High-strength collision-resistant cable and preparation method thereof

Through multi-layer structural design and synergistic effects of components, the problem of improving the performance of existing cables under complex working conditions has been solved, achieving comprehensive performance improvement in high strength, impact resistance, insulation and flame retardancy, thereby enhancing the structural stability and service life of the cable.

CN121439336APending Publication Date: 2026-01-30浙江华普电缆有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511801839.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-02
Publication Date
2026-01-30

AI Technical Summary

Technical Problem

Existing cables struggle to achieve a synergistic improvement in high strength, impact resistance, insulation, and flame retardancy under complex operating conditions. Furthermore, the poor compatibility between the buffer structure and the reinforcement structure makes the cables prone to cracking, interlayer peeling, and insulation breakdown.

Method used

It adopts a multi-layer structure design consisting of oxygen-free copper conductor, modified insulation layer, multi-functional buffer layer, high-strength armor layer and wear-resistant outer sheath. It utilizes components such as modified cross-linked polyethylene, polyisobutylene grafted maleic anhydride-nano boron nitride composite, and modified high-performance polypropylene-graphene quantum dot composite to form a complementary system of flexible buffer and rigid support through modification treatment and extrusion coating process. Combined with the flame retardant and reinforcing effect of melamine cyanurate, the processing fluidity of calcium stearate and the aging delay effect of antioxidant, the overall performance is improved.

Benefits of technology

This achieves a synergistic improvement in the cable's high strength, impact resistance, insulation, and flame retardancy, enhancing its structural stability and weather resistance, and extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121439336A_ABST
    Figure CN121439336A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength collision-resistant cable and a preparation method thereof. The high-strength collision-resistant cable comprises an oxygen-free copper conductor, a modified insulating layer, a multifunctional buffer layer, a high-strength armor layer and a wear-resistant outer sheath which are sequentially arranged from inside to outside, the invention relates to a preparation method of an anti-aging agent. The high-strength collision-resistant cable is prepared from the following raw materials: 35 to 45 parts of modified crosslinked polyethylene, 12 to 18 parts of polyisobutene grafted maleic anhydride-nano boron nitride compound, 8 to 15 parts of modified high-performance polypropylene-graphene quantum dot compound, 3 to 6 parts of nano titanium dioxide, 7 to 12 parts of aramid staple fiber, 5 to 10 parts of melamine cyanurate and 0.8 to 1.5 parts of calcium stearate. 0.5 to 1.0 part of a silane coupling agent, 6 to 10 parts of polycaprolactone and 0.3 to 0.8 part of an antioxidant. The obtained cable has excellent comprehensive performance of high strength, impact resistance, insulation, flame retardance and weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cable technology, specifically to a high-strength, impact-resistant cable and its preparation method. Background Technology

[0002] As the core carrier of power transmission and signal conduction, cables are widely used in various fields such as industrial production, construction engineering, and transportation. Their operating environments often involve complex conditions such as mechanical collisions, temperature fluctuations, and external extrusion, thus placing stringent requirements on the mechanical strength, impact resistance, insulation stability, and overall service capability of cables. Existing cables typically employ a multi-layered composite structure of "conductor, insulation layer, and sheath," optimizing individual properties by selecting different base materials and adding conventional fillers to meet basic usage requirements.

[0003] Existing cables often have limitations in performance design, making it difficult to achieve a synergistic improvement in key properties such as high strength, impact resistance, insulation, and flame retardancy. Although some cables have improved mechanical strength by increasing sheath thickness or using conventional reinforcing fillers, their insulation performance is easily affected. Furthermore, when subjected to external impact, the poor coordination between the buffer structure and the reinforcement structure results in the inability to effectively disperse impact energy, leading to problems such as cracks, interlayer peeling, and even insulation breakdown. This makes them unsuitable for complex and harsh operating environments and limits their application in scenarios with high reliability requirements. Summary of the Invention

[0004] To address the problems existing in the prior art, the present invention provides a high-strength impact-resistant cable and its preparation method, which enables the cable to possess excellent comprehensive properties of high strength, impact resistance, insulation, flame retardancy and weather resistance.

[0005] To achieve the above objectives, the present invention provides the following technical solution: This application discloses a high-strength impact-resistant cable, which includes, from the inside out, an oxygen-free copper conductor, a modified insulation layer, a multifunctional buffer layer, a high-strength armor layer, and a wear-resistant outer sheath. By weight, the raw materials comprising the high-strength impact-resistant cable include: 35-45 parts of modified cross-linked polyethylene, 12-18 parts of polyisobutylene-grafted maleic anhydride-nano boron nitride composite, 8-15 parts of modified high-performance polypropylene-graphene quantum dot composite, 3-6 parts of nano titanium dioxide, 7-12 parts of aramid staple fiber, 5-10 parts of melamine cyanurate, 0.8-1.5 parts of calcium stearate, 0.5-1.0 parts of silane coupling agent, 6-10 parts of polycaprolactone, and 0.3-0.8 parts of antioxidant.

[0006] By setting the above technical scheme, the modified cross-linked polyethylene as the core base material of the modified insulation layer, cooperates with the nano titanium dioxide and the silane coupling agent to optimize the insulation performance and structural stability; the polyisobutylene grafted maleic anhydride-nano boron nitride compound and the modified high-performance polypropylene-graphene quantum dot compound form a complementary system of flexible buffer and rigid support, and are matched with polycaprolactone to improve flexibility, aramid short fibers to inhibit crack propagation, effectively strengthen the crashworthiness and mechanical strength; melamine cyanurate has the functions of flame retardation and reinforcement, calcium stearate ensures the processing fluidity, antioxidants delay material aging, and the mechanical enhancement of the high-strength armored layer and the protection effect of the wear-resistant outer protective sleeve, the synergistic effect of each component and the multilayer structure from the inside to the outside makes the cable have excellent high strength, impact resistance, insulation, flame retardation and weather resistance comprehensive performance.

[0007] Preferably, the weight average molecular weight of the modified cross-linked polyethylene is 50000-80000 Da, the particle size of the nano titanium dioxide is 20-50 nm, the length of the aramid short fiber is 100-200 μm, and the weight average molecular weight of the polycaprolactone is 10000-20000 Da.

[0008] By setting the above technical scheme, the modified cross-linked polyethylene with a weight average molecular weight of 50000-80000 Da can have excellent insulation performance and mechanical strength, the nano titanium dioxide with a particle size of 20-50 nm has good dispersibility and enhancement characteristics, can improve the wear resistance and anti-aging ability of the material, the aramid short fiber with a length of 100-200 μm can fully play the crack bridging effect to inhibit crack propagation, and the polycaprolactone with a weight average molecular weight of 10000-20000 Da can optimize the flexibility and low-temperature adaptability of the material, and the synergistic effect of each component effectively improves the comprehensive mechanical strength, impact resistance, anti-aging ability and wide-temperature-range stable service effect of the cable.

[0009] Preferably, the silane coupling agent is one of KH-550, KH-560 or KH-570, and the antioxidant is one of antioxidant 1010, antioxidant 168 or antioxidant 1076.

[0010] By setting the above technical scheme, the silane coupling agent KH-550, KH-560 or KH-570 can bridge the organic components and inorganic components through chemical bonding, reduce interface defects, improve the compatibility and bonding force between components, and avoid material aggregation; the antioxidant 1010, antioxidant 168 or antioxidant 1076 can effectively capture free radicals generated during material processing and use, inhibit thermal oxidative aging, and delay performance degradation, and the synergistic effect of the two makes the cable have stable mechanical properties, structural integrity and long-term service ability.

[0011] Preferably, the raw materials of the polyisobutylene grafted maleic anhydride-nano boron nitride composite include, in parts by weight, polyisobutylene 90-100, maleic anhydride 8-12, benzoyl peroxide 1.2-1.8, nano boron nitride 8-12, anhydrous toluene 140-180, silane coupling agent KH-570 2-4.

[0012] By setting the above technical solution, polyisobutylene provides excellent elastic foundation for the composite, maleic anhydride as a grafting monomer can introduce reactive groups, benzoyl peroxide initiates grafting reaction to realize chemical bonding of polyisobutylene and maleic anhydride, nano boron nitride gives the material thermal conductivity and mechanical enhancement effect, anhydrous toluene ensures uniform dispersion and smooth reaction of each raw material, silane coupling agent KH-570 optimizes the compatibility of nano boron nitride and organic matrix, and the synergistic effect of each component makes the prepared composite have the comprehensive performance of elastic buffer, interface compatibility, efficient thermal conductivity and mechanical enhancement, which can effectively improve the impact energy absorption capacity and structural stability of the material.

[0013] Preferably, the preparation method of the polyisobutylene grafted maleic anhydride-nano boron nitride composite includes the following steps: 1) Add nano boron nitride to 3 / 7 of the total amount of anhydrous toluene, disperse under the condition of ultrasonic frequency 20-30 kHz and ultrasonic power 250-300 W for 30-40 min, add silane coupling agent KH-570 dropwise, stir at a speed of 250-350 r / min at 70-80°C for 2-3 h, filter, and dry at 88-90°C under vacuum condition of -0.09 MPa to -0.08 MPa for 6-8 h to obtain modified nano boron nitride; 2) Add polyisobutylene to the remaining anhydrous toluene, heat to 85-95°C and stir to dissolve, add maleic anhydride and benzoyl peroxide, stir at a speed of 300-400 r / min under nitrogen atmosphere for 5-7 h, and then remove 80-90% of the anhydrous toluene by reduced pressure distillation to obtain a polyisobutylene grafted maleic anhydride concentrate; 3) Add the modified nano boron nitride to the polyisobutylene grafted maleic anhydride concentrate, high-speed stir at a speed of 350-450 r / min at 100-110°C for 3-4 h, then pour into 150-200 parts of petroleum ether to precipitate, filter, dry at 78-82°C under vacuum condition of -0.10 MPa to -0.09 MPa for 10-12 h, and crush through a 200-300 mesh sieve to obtain a polyisobutylene grafted maleic anhydride-nano boron nitride composite.

[0014] By setting the above technical scheme, the preparation method improves the dispersibility of the nano boron nitride and the compatibility with the organic phase through modification and ultrasonic dispersion treatment of silane coupling agent KH-570, realizes the stable combination of the active groups introduced through the grafting reaction of polyisobutylene and maleic anhydride and the modified nano boron nitride, removes impurities and unreacted monomers through vacuum distillation concentration, petroleum ether precipitation purification, vacuum drying to ensure the purity of the product, and crushing and sieving to optimize the uniformity of the particle size, and finally obtains a polyisobutylene grafted maleic anhydride-nano boron nitride compound which is uniformly dispersed, has a tight interface, high purity and regular particle size. The elasticity of polyisobutylene, the reactivity of maleic anhydride and the thermal conductivity of nano boron nitride form a synergistic effect to ensure the stability of the comprehensive performance of the compound.

[0015] Preferably, the weight average molecular weight of the polyisobutylene is 8000-12000 Da, and the particle size of the nano boron nitride is 50-100 nm.

[0016] By setting the above technical scheme, the weight average molecular weight of the polyisobutylene is 8000-12000 Da, which can ensure that it has appropriate chain segment flexibility and processing fluidity, can fully play the role of elastic buffer, and can be highly compatible with other components; the particle size of the nano boron nitride is 50-100 nm, which can avoid particle agglomeration, ensure uniform dispersion in the polyisobutylene grafted maleic anhydride matrix, and fully play the high-efficiency thermal conductivity performance, and the synergistic effect of the two makes the compound have good elastic buffer capacity, high-efficiency thermal conductivity and excellent dispersion compatibility, laying a foundation for subsequent performance synergy.

[0017] Preferably, the composition of the modified high-performance polypropylene-graphene quantum dot compound includes, in terms of weight parts: high-performance polypropylene 90-100 parts, graphene quantum dots 3-5 parts, glycidyl methacrylate 6-10 parts, di-tert-butyl peroxide 0.8-1.2 parts, anhydrous ethanol 50-70 parts, and antioxidant 168 0.4-0.6 parts; the high-performance polypropylene is impact copolymerized polypropylene or homopolymerized polypropylene, and the weight average molecular weight is 40000-60000 Da; the particle size of the graphene quantum dots is 3-5 nm.

[0018] By setting the above technical scheme, the impact copolymerized polypropylene or homopolymerized polypropylene (weight average molecular weight 40000-60000 Da) provides basic rigid support for the compound, the 3-5 nm particle size graphene quantum dots strengthen the mechanical properties by virtue of high specific surface area, the glycidyl methacrylate can improve the bonding force between components, the di-tert-butyl peroxide can initiate grafting reaction to promote component compatibility, the anhydrous ethanol helps the uniform dispersion of graphene quantum dots, and the antioxidant 168 inhibits thermal oxidation during the processing process. The synergistic effect of each component makes the compound have excellent rigidity, mechanical enhancement effect and structural stability, while ensuring the performance consistency during the processing process.

[0019] Preferably, the preparation method of the modified high-performance polypropylene-graphene quantum dot composite comprises the following steps: a. dispersing graphene quantum dots in anhydrous ethanol, and dispersing for 25-35 min under the conditions of an ultrasonic frequency of 20-30 kHz and an ultrasonic power of 250-300 W to obtain a graphene quantum dot dispersion; b. adding high-performance polypropylene, glycidyl methacrylate, di-t-butyl peroxide and antioxidant 168 into a high-speed mixer, mixing at a speed of 800-1000 r / min at 110-120℃ for 15-20 min to obtain a premix; c. feeding the premix into a double-screw extruder, and setting the extrusion temperature as follows: zone 1, 150-160℃; zone 2, 165-175℃; zone 3, 175-185℃; zone 4, 180-190℃, and setting the screw rotation speed as 300-400 r / min; after extrusion, water cooling and granulation are performed to obtain a polypropylene-glycidyl methacrylate graft; d. mixing the polypropylene-glycidyl methacrylate graft with the graphene quantum dot dispersion, stirring at a speed of 200-300 r / min at 70-80℃, evaporating anhydrous ethanol until no free liquid is visible in the system, and then drying at 118-122℃ under a vacuum condition of -0.09 MPa to -0.08 MPa for 8-10 h to obtain a modified high-performance polypropylene-graphene quantum dot composite.

[0020] By setting the above technical solution, ultrasonic dispersion can ensure that graphene quantum dots are uniformly dispersed in anhydrous ethanol, and agglomeration is avoided to fully exert the high specific surface area reinforcing effect; high-performance polypropylene and glycidyl methacrylate are subjected to efficient grafting reaction through high-speed mixing and double-screw extrusion process, a polypropylene-glycidyl methacrylate graft containing active groups is generated, and the bonding force with graphene quantum dots is improved; then, impurities are removed through stirring evaporation and vacuum drying to ensure the cleanliness of the system, and finally, a modified high-performance polypropylene-graphene quantum dot composite which is uniformly dispersed, firmly bonded at the interface, high in purity, and has rigidity support and excellent mechanical properties is obtained.

[0021] The application also discloses a preparation method of the high-strength impact-resistant cable. S1, pretreatment of an oxygen-free copper conductor: A plurality of fine copper wires (with a diameter of 0.1-0.2 mm) are twisted into an oxygen-free copper conductor according to a pitch ratio of 8:1-10:1, and then dried at 120-140℃ for 2-3 h; subsequently, the oxygen-free copper conductor is activated by using a plasma treatment machine at a power of 350-450 W for 4-6 min. S2, modification of an insulating layer: Modified cross-linked polyethylene, nano-titanium dioxide, silane coupling agent were added into a high-speed mixer and mixed at 105-115℃ and 750-950r / min for 12-16min to obtain the insulation layer mixture; The mixture was coated on the pretreated copper conductor by a single screw extruder, the extrusion temperature was 145-155℃ for feeding section, 165-175℃ for compression section and 175-185℃ for homogenization section, the screw rotation speed was 280-380r / min, the coating thickness was 1.8-2.5mm, and the cooling and shaping were performed in 20-25℃ cooling water for 5-8min to obtain the insulated core wire; S3, multifunctional buffer layer preparation: Polyisobutylene grafted maleic anhydride-nano boron nitride compound, modified high-performance polypropylene-graphene quantum dot compound, polycaprolactone, calcium stearate were added into an internal mixer and mixed at 95-105℃ and 650-850r / min for 15-20min; Aramid short fibers and melamine cyanurate were added and mixed at 110-120℃ and 300-400r / min for 20-25min to obtain the buffer layer mixture; The buffer layer mixture was coated on the insulated core wire by extrusion coating process, the extrusion temperature was 135-145℃, the screw rotation speed was 220-320r / min, the coating thickness was 1.5-2.0mm, and the cooling and shaping were performed in 20-25℃ cooling water for 6-10min; S4, high-strength armored layer composite: Double-stranded galvanized steel wire (diameter 0.3-0.5mm) was cross-woven, the weaving density was ≥95%, the weaving tension was 6-9N, and the weaving pitch was 6-8 times the diameter of the cable to form a high-strength armored layer; S5, wear-resistant outer sheath extrusion molding: Polyether TPU material was selected and antioxidant was added, and the armored layer was coated by a double-screw extruder, the extrusion temperature was 165-175℃ for feeding section, 185-195℃ for compression section and 195-205℃ for homogenization section, the screw rotation speed was 280-380r / min, the coating thickness was 1.8-2.2mm, the cooling and shaping were performed in 20-25℃ cooling water for 8-12min, and the cooling vacuum degree was -0.35MPa to -0.25MPa to obtain the high-strength impact-resistant cable.

[0022] Through the above technical scheme, the plasma activation treatment can improve the surface activity of the oxygen-free copper conductor, and enhance the interfacial bonding force with the modified insulation layer; the components are uniformly dispersed through the full mixing and dense mixing process, the extrusion coating and cooling and shaping ensure that the layers are dense and tightly combined, the high weaving density and specific tension of the high-strength armored layer strengthen the mechanical support of the high-strength armored layer, and the extrusion process of the wear-resistant outer sheath makes the cable have good protection performance; the whole preparation process cooperates to ensure that the performance of the modified crosslinked polyethylene, polyisobutylene grafted maleic anhydride-nano boron nitride compound, and modified high-performance polypropylene-graphene quantum dot compound components can be fully utilized, so that the cable has excellent high-strength, impact-resistant, weather-resistant and structural stability performance.

[0023] Preferably, in step S5, the Shore hardness of the polyether TPU material is 75-85D.

[0024] Through the above technical scheme, the cable outer sheath is provided with a suitable balance of rigidity and flexibility, which not only ensures excellent wear resistance and scratch resistance of the outer sheath, and can resist external mechanical friction and slight impact, but also avoids brittle fracture caused by excessive hardness, and at the same time can closely fit the high-strength armored layer to form a synergistic protection, thereby improving the overall structural stability of the cable and prolonging the service life of the cable.

[0025] The beneficial effects of the present application are: The modified crosslinked polyethylene as the core base material of the modified insulation layer cooperates with the nano titanium dioxide and silane coupling agent to optimize the insulation performance and structural stability; the polyisobutylene grafted maleic anhydride-nano boron nitride compound and the modified high-performance polypropylene-graphene quantum dot compound form a complementary system of flexible cushioning and rigid support, and are matched with polycaprolactone to improve flexibility, aramid short fibers to inhibit crack propagation, effectively enhancing the impact resistance and mechanical strength; melamine cyanurate has the functions of flame retardation and reinforcement, calcium stearate ensures processing fluidity, and antioxidants delay material aging, in combination with the mechanical reinforcement of the high-strength armored layer and the protection effect of the wear-resistant outer sheath, the synergistic effect of the various components and the multilayer structure from the inside to the outside makes the cable have excellent high-strength, impact-resistant, insulating, flame-retardant and weather-resistant comprehensive performance.

[0026] The polyisobutylene provides excellent elastic basis for the compound, the maleic anhydride as the grafting monomer can introduce reactive groups, the benzoyl peroxide initiates the grafting reaction to realize the chemical bonding of polyisobutylene and maleic anhydride, the nano boron nitride gives the material thermal conductivity and mechanical reinforcement effect, the anhydrous toluene ensures uniform dispersion and smooth reaction of the raw materials, and the silane coupling agent KH-570 optimizes the compatibility of the nano boron nitride and the organic matrix, so that the prepared compound has the comprehensive performance of elastic cushioning, interface compatibility, thermal conductivity and mechanical reinforcement, which can effectively improve the impact energy absorption capacity and structural stability of the material. BRIEF DESCRIPTION OF DRAWINGS

[0027] Figure 1 Structure diagram of high-strength impact-resistant cable in the present application; In the figure, 1, oxygen-free copper conductor; 2, modified insulation layer; 3, multifunctional buffer layer; 4, high-strength armored layer; 5, wear-resistant outer sheath. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of protection of the present application.

[0029] Embodiment 1 The present embodiment discloses a high-strength impact-resistant cable, which comprises, from inside to outside, an oxygen-free copper conductor 1, a modified insulation layer 2, a multifunctional buffer layer 3, a high-strength armored layer 4, and a wear-resistant outer sheath 5. The composition of the high-strength impact-resistant cable includes, in parts by weight, modified cross-linked polyethylene with a weight average molecular weight of 50,000 Da 35 parts, polyisobutylene grafted maleic anhydride-nano boron nitride composite 12 parts, modified high-performance polypropylene-graphene quantum dot composite 8 parts, nano titanium dioxide with a particle size of 20 nm 3 parts, aramid short fiber with a length of 100 μm 7 parts, melamine cyanurate 5 parts, calcium stearate 0.8 parts, silane coupling agent KH-550 0.5 parts, polycaprolactone with a weight average molecular weight of 10,000 Da 6 parts, and antioxidant 168 0.3 parts.

[0030] The composition of the polyisobutylene grafted maleic anhydride-nano boron nitride composite includes, in parts by weight, polyisobutylene with a weight average molecular weight of 8,000 Da 90 parts, maleic anhydride 8 parts, benzoyl peroxide 1.2 parts, nano boron nitride with a particle size of 50 nm 8 parts, anhydrous toluene 140 parts, and silane coupling agent KH-570 2 parts.

[0031] The preparation method of the polyisobutylene grafted maleic anhydride-nano boron nitride composite includes the following steps: 1) The nano boron nitride is added to 3 / 7 of the total amount of anhydrous toluene, dispersed for 30 min under the condition of ultrasonic frequency 20 kHz and ultrasonic power 250 W, and then the silane coupling agent KH-570 is added dropwise, stirred at a speed of 250 r / min at 70°C for 2 h, filtered, and dried at 88°C under the condition of vacuum of -0.09 MPa for 6 h to obtain modified nano boron nitride. 2) polyisobutylene is added into the remaining anhydrous toluene, heated to 85℃ and stirred to dissolve, maleic anhydride and benzoyl peroxide are added, stirred at 300r / min for 5h under nitrogen atmosphere, after the reaction is completed, 80% of the anhydrous toluene is removed by reduced pressure distillation, and a polyisobutylene grafted maleic anhydride concentrate is obtained; 3) modified nano boron nitride is added into the polyisobutylene grafted maleic anhydride concentrate, stirred at 350r / min for 3h at 100℃, then poured into 150 parts of petroleum ether to precipitate, filtered and dried at 78℃ under vacuum condition of -0.10MPa for 10h, crushed through a 200 mesh sieve, and a polyisobutylene grafted maleic anhydride-nano boron nitride composite is obtained.

[0032] The modified high-performance polypropylene-graphene quantum dot composite includes, in terms of weight parts, high-performance polypropylene 90 parts, graphene quantum dots 3 parts, glycidyl methacrylate 6 parts, di-tert-butyl peroxide 0.8 parts, anhydrous ethanol 50 parts, and antioxidant 168 0.4 parts. The high-performance polypropylene is an impact copolymerized polypropylene with a weight average molecular weight of 40,000 Da. The particle size of the graphene quantum dots is 3 nm.

[0033] The preparation method of the modified high-performance polypropylene-graphene quantum dot composite includes the following steps: a. The graphene quantum dots are dispersed in anhydrous ethanol under the condition of an ultrasonic frequency of 20 kHz and an ultrasonic power of 250 W for 25 min to obtain a graphene quantum dot dispersion liquid; b. The high-performance polypropylene, glycidyl methacrylate, di-tert-butyl peroxide, and antioxidant 168 are added into a high-speed mixer and mixed at 800r / min for 15 min at 110℃ to obtain a premix; c. The premix is fed into a twin-screw extruder, and the extrusion temperature is 150℃ for the first zone, 165℃ for the second zone, 175℃ for the third zone, and 180℃ for the fourth zone. The screw rotation speed is 300r / min. After extrusion, the product is water-cooled and pelletized to obtain a polypropylene-glycidyl methacrylate grafting product; d. The polypropylene-glycidyl methacrylate grafting product is mixed with the graphene quantum dot dispersion liquid, stirred at 200r / min at 70℃, and the anhydrous ethanol is evaporated until no free liquid is visible in the system. Then, the product is dried under vacuum condition of 118℃ and -0.09MPa for 8h to obtain a modified high-performance polypropylene-graphene quantum dot composite.

[0034] The embodiment also discloses a preparation method of the high-strength impact-resistant cable, which includes the following steps: S1, oxygen-free copper conductor pretreatment: A plurality of thin copper wires (diameter 0.1 mm) were twisted into an oxygen-free copper conductor at a pitch ratio of 8:1, dried at 120°C for 2 h, and then activated by a plasma treatment machine at a power of 350 W for 4 min; S2, modification of the insulating layer: The modified cross-linked polyethylene, nano-titanium dioxide, and silane coupling agent KH-550 were added to a high-speed mixer, mixed at 105°C at a speed of 750 r / min for 12 min, and an insulating layer mixture was obtained. The mixture was coated on the pretreated copper conductor by a single-screw extruder, the extrusion temperature was 145°C for the feeding section, 165°C for the compression section, and 175°C for the homogenization section, the screw speed was 280 r / min, the coating thickness was 1.8 mm, and the cooling and shaping were performed in 20°C cooling water for 5 min, and an insulating core wire was obtained. S3, preparation of a multifunctional buffer layer: The polyisobutylene grafted maleic anhydride-nano-boron nitride composite, modified high-performance polypropylene-graphene quantum dot composite, polycaprolactone, and calcium stearate were added to an internal mixer, and mixed at 95°C at a speed of 650 r / min for 15 min. The aramid short fibers and melamine cyanurate were added, and mixed at 110°C at a speed of 300 r / min for 20 min, and a buffer layer mixture was obtained. The buffer layer mixture was coated on the insulating core wire by an extrusion coating process, the extrusion temperature was 135°C, the screw speed was 220 r / min, the coating thickness was 1.5 mm, and the cooling and shaping were performed in 20°C cooling water for 6 min. S4, high-strength armored layer composite: Double-strand galvanized steel wires (diameter 0.3 mm) were cross-woven, the weaving density was ≥95%, the weaving tension was 6 N, and the weaving pitch was 6 times the diameter of the cable, and a high-strength armored layer was formed. S5, extrusion molding of wear-resistant outer sheath: A polyether TPU material with a Shore hardness of 75D was selected, antioxidant 168 was added, and the armored layer was coated by a double-screw extruder, the extrusion temperature was 165°C for the feeding section, 185°C for the compression section, and 195°C for the homogenization section, the screw speed was 280 r / min, the coating thickness was 1.8 mm, the cooling and shaping were performed in 20°C cooling water for 8 min, and the cooling vacuum degree was -0.35 MPa, and a high-strength impact-resistant cable was obtained.

[0035] Example 2: The embodiment discloses a high-strength anti-collision cable, which comprises, from inside to outside, an oxygen-free copper conductor 1, a modified insulation layer 2, a multifunctional buffer layer 3, a high-strength armored layer 4 and a wear-resistant outer sheath 5. The high-strength anti-collision cable comprises, in terms of weight parts, the following components: modified cross-linked polyethylene with a weight average molecular weight of 80000 Da 45 parts, polyisobutylene grafted maleic anhydride-nano boron nitride compound 18 parts, modified high-performance polypropylene-graphene quantum dot compound 15 parts, nano titanium dioxide with a particle size of 50 nm 6 parts, aramid short fiber with a length of 200 microns 12 parts, melamine cyanurate 10 parts, calcium stearate 1.5 parts, silane coupling agent KH-570 1.0 part, polycaprolactone with a weight average molecular weight of 20000 Da 10 parts and antioxidant 1010 0.8 part.

[0036] The polyisobutylene grafted maleic anhydride-nano boron nitride compound comprises, in terms of weight parts, the following components: polyisobutylene with a weight average molecular weight of 12000 Da 100 parts, maleic anhydride 12 parts, benzoyl peroxide 1.8 parts, nano boron nitride with a particle size of 100 nm 12 parts, anhydrous toluene 180 parts and silane coupling agent KH-570 4 parts.

[0037] The polyisobutylene grafted maleic anhydride-nano boron nitride compound is prepared by the following steps. 1) The nano boron nitride is added to 3 / 7 of the total amount of anhydrous toluene, dispersed for 40 min under the condition of an ultrasonic frequency of 30 kHz and an ultrasonic power of 300 W, and then the silane coupling agent KH-570 is added dropwise, and the reaction is carried out at 80 DEG C under the condition of stirring at a rotating speed of 350 r / min for 3 h, and then the modified nano boron nitride is obtained by filtering and drying at 90 DEG C under the condition of a vacuum of -0.08 MPa for 8 h. 2) The polyisobutylene is added to the remaining anhydrous toluene, and then the temperature is raised to 95 DEG C for stirring and dissolving, and then the maleic anhydride and the benzoyl peroxide are added, and the reaction is carried out under the condition of stirring at a rotating speed of 400 r / min for 7 h in a nitrogen atmosphere, and then 90% of the anhydrous toluene is removed by reduced pressure distillation to obtain a polyisobutylene grafted maleic anhydride concentrate. 3) The modified nano boron nitride is added to the polyisobutylene grafted maleic anhydride concentrate, and then the high-speed stirring is carried out at 110 DEG C under the condition of a rotating speed of 450 r / min for 4 h, and then the polyisobutylene grafted maleic anhydride-nano boron nitride compound is obtained by precipitating in 200 parts of petroleum ether, filtering, drying at 82 DEG C under the condition of a vacuum of -0.09 MPa for 12 h and crushing through a 300-mesh sieve.

[0038] The composition of the modified high-performance polypropylene-graphene quantum dot composite includes, in parts by weight, 100 parts of high-performance polypropylene, 5 parts of graphene quantum dots, 10 parts of glycidyl methacrylate, 1.2 parts of di-tert-butyl peroxide, 70 parts of anhydrous ethanol, and 0.6 parts of antioxidant 168; the high-performance polypropylene is homopolymer polypropylene with a weight average molecular weight of 60,000 Da; and the graphene quantum dots have a particle size of 5 nm.

[0039] The preparation method of the modified high-performance polypropylene-graphene quantum dot composite includes the following steps: a. dispersing the graphene quantum dots in anhydrous ethanol, and dispersing for 35 min under the conditions of an ultrasonic frequency of 30 kHz and an ultrasonic power of 300 W to obtain a graphene quantum dot dispersion liquid; b. adding the high-performance polypropylene, glycidyl methacrylate, di-tert-butyl peroxide, and antioxidant 168 into a high-speed mixer, and mixing at 120°C and a rotating speed of 1,000 r / min for 20 min to obtain a premix; c. feeding the premix into a double-screw extruder, and setting the extrusion temperature as 160°C for the first zone, 175°C for the second zone, 185°C for the third zone, and 190°C for the fourth zone, and setting the screw rotating speed as 400 r / min; after extrusion, water cooling and pelletizing are performed to obtain a polypropylene-glycidyl methacrylate grafting product; d. mixing the polypropylene-glycidyl methacrylate grafting product with the graphene quantum dot dispersion liquid, stirring at 80°C and a rotating speed of 300 r / min, evaporating the anhydrous ethanol until no free liquid is visible in the system, and then drying under the conditions of 122°C and a vacuum of -0.08 MPa for 10 h to obtain the modified high-performance polypropylene-graphene quantum dot composite.

[0040] The embodiment also discloses a preparation method of the high-strength and collision-resistant cable, which includes the following steps: S1, pretreatment of the oxygen-free copper conductor: a plurality of fine copper wires (with a diameter of 0.2 mm) are stranded into an oxygen-free copper conductor according to a pitch ratio of 10:1, and then dried at 140°C for 3 h; subsequently, a plasma treatment machine is used to activate and treat the oxygen-free copper conductor at a power of 450 W for 6 min; S2, coating of the modified insulating layer: modified crosslinked polyethylene, nano-titanium dioxide, and silane coupling agent KH-570 are added into a high-speed mixer, and mixed at 115°C and a rotating speed of 950 r / min for 16 min to obtain an insulating layer mixture; the mixture is coated on the pretreated copper conductor through a single-screw extruder, and the extrusion temperature is set as 155°C for a feeding section, 175°C for a compression section, and 185°C for a homogenization section, and the screw rotating speed is set as 380 r / min; the coating thickness is 2.5 mm, and the insulating core wire is cooled and shaped in 25°C cooling water for 8 min; S3, multifunctional buffer layer preparation: The polyisobutylene grafted maleic anhydride-nano boron nitride compound, modified high-performance polypropylene-graphene quantum dot compound, polycaprolactone, calcium stearate are added to the internal mixer, and the internal mixing is carried out at 105℃ and a rotating speed of 850r / min for 20min; The aramid short fiber and melamine cyanurate are added, and the internal mixing is carried out at 120℃ and a rotating speed of 400r / min for 25min to obtain the buffer layer mixture; The buffer layer mixture is coated on the insulating core wire by using the extrusion coating process, the extrusion temperature is 145℃, the screw rotating speed is 320r / min, the coating thickness is 2.0mm, and the cooling and shaping are carried out in 25℃ cooling water for 10min; S4, high-strength armored layer composite: The double-strand galvanized steel wire (diameter 0.5mm) is cross-woven, the weaving density is greater than or equal to 95%, the weaving tension is 9N, and the weaving pitch is 8 times of the diameter of the cable, so as to form the high-strength armored layer; S5, wear-resistant outer sheath extrusion molding: The polyether TPU material with a Shore hardness of 85D is selected, the antioxidant 1010 is added, and the armored layer is coated by using the double-screw extruder, the extrusion temperature is: the feeding section is 175℃, the compression section is 195℃, the homogenization section is 205℃, the screw rotating speed is 380r / min, the coating thickness is 2.2mm, the cooling and shaping are carried out in 25℃ cooling water for 12min, the cooling vacuum degree is-0.25MPa, and the high-strength impact-resistant cable is obtained.

[0041] Embodiment 3: The embodiment discloses a high-strength impact-resistant cable, which comprises an oxygen-free copper conductor 1, a modified insulating layer 2, a multifunctional buffer layer 3, a high-strength armored layer 4 and a wear-resistant outer sheath 5 arranged in sequence from inside to outside; the high-strength impact-resistant cable comprises the following components in parts by weight: modified cross-linked polyethylene with a weight average molecular weight of 65,000 Da 40 parts, polyisobutylene grafted maleic anhydride-nano boron nitride compound 15 parts, modified high-performance polypropylene-graphene quantum dot compound 11 parts, nano titanium dioxide with a particle size of 35 nm 5 parts, aramid short fiber with a length of 150 microns 10 parts, melamine cyanurate 7 parts, calcium stearate 1.1 parts, silane coupling agent KH-560 0.7 parts, polycaprolactone with a weight average molecular weight of 15,000 Da 8 parts and antioxidant 1076 0.5 parts.

[0042] The polyisobutylene grafted maleic anhydride-nano boron nitride compound comprises the following components in parts by weight: polyisobutylene with a weight average molecular weight of 10,000 Da 95 parts, maleic anhydride 10 parts, benzoyl peroxide 1.5 parts, nano boron nitride with a particle size of 75 nm 10 parts, anhydrous toluene 160 parts and silane coupling agent KH-570 3 parts.

[0043] The preparation method of the polyisobutylene grafted maleic anhydride-nano boron nitride composite comprises the following steps: 1) The nano boron nitride is added into 3 / 7 of the total amount of anhydrous toluene, dispersed for 35 min under the condition of ultrasonic frequency 25 kHz and ultrasonic power 275 W, and then the silane coupling agent KH-570 is added dropwise, and the reaction is carried out at 75℃ under the condition of stirring at a speed of 300 r / min for 2.5 h, and then the modified nano boron nitride is obtained by filtering and drying at 89℃ under the condition of vacuum of -0.085 MPa for 7 h; 2) The polyisobutylene is added into the remaining anhydrous toluene, and then the temperature is increased to 90℃ for stirring and dissolving, and then the maleic anhydride and the benzoyl peroxide are added, and the reaction is carried out under the condition of stirring at a speed of 350 r / min for 6 h in a nitrogen atmosphere, and then 85% of the anhydrous toluene is removed by reduced pressure distillation to obtain a polyisobutylene grafted maleic anhydride concentrate; 3) The modified nano boron nitride is added into the polyisobutylene grafted maleic anhydride concentrate, and then the high-speed stirring is carried out at 105℃ under the condition of a speed of 400 r / min for 3.5 h, and then the polyisobutylene grafted maleic anhydride-nano boron nitride composite is obtained by precipitating into 175 parts of petroleum ether, filtering, drying at 80℃ under the condition of vacuum of -0.095 MPa for 11 h, and crushing through a 250 mesh sieve.

[0044] The composition of the modified high-performance polypropylene-graphene quantum dot composite includes, in terms of weight parts, high-performance polypropylene 95 parts, graphene quantum dots 4 parts, glycidyl methacrylate 8 parts, di-tert-butyl peroxide 1 part, anhydrous ethanol 60 parts, and antioxidant 168 0.5 parts. The high-performance polypropylene is homopolymer polypropylene with a weight average molecular weight of 50000 Da. The particle size of the graphene quantum dots is 4 nm.

[0045] The preparation method of the modified high-performance polypropylene-graphene quantum dot composite comprises the following steps: a. The graphene quantum dots are dispersed in anhydrous ethanol under the condition of ultrasonic frequency 25 kHz and ultrasonic power 275 W for 30 min to obtain a graphene quantum dot dispersion; b. The high-performance polypropylene, glycidyl methacrylate, di-tert-butyl peroxide, and antioxidant 168 are added into a high-speed mixer, and then mixed at a speed of 900 r / min at 115℃ for 17 min to obtain a premix; c. The premix is fed into a twin-screw extruder, and the extrusion temperature is: zone 1 155℃, zone 2 170℃, zone 3 180℃, and zone 4 185℃, and the screw rotation speed is 350 r / min. After extrusion, the polypropylene-glycidyl methacrylate graft is obtained by water cooling and pelletizing; d.The polypropylene-glycidyl methacrylate graft was mixed with the graphene quantum dot dispersion liquid, stirred at 75℃ and 250r / min, and the anhydrous ethanol was removed by evaporation until no free liquid was visible in the system, then dried at 120℃ under vacuum condition of-0.085MPa for 9h to obtain the modified high-performance polypropylene-graphene quantum dot composite.

[0046] The embodiment also discloses a preparation method of the high-strength impact-resistant cable. S1, pretreatment of oxygen-free copper conductor: A plurality of fine copper wires (diameter 0.15mm) were stranded into an oxygen-free copper conductor according to a pitch ratio of 9:1, dried at 130℃ for 2.5h, and then activated by a plasma treatment machine at a power of 400W for 5min; S2, modification of insulating layer: Modified cross-linked polyethylene, nano-titanium dioxide and silane coupling agent KH-560 were added into a high-speed mixer, mixed at 110℃ and 850r / min for 14min to obtain an insulating layer mixture; The mixture was coated on the pretreated copper conductor by a single-screw extruder, the extrusion temperature was 150℃ for the feeding section, 170℃ for the compression section and 180℃ for the homogenization section, the screw rotation speed was 330r / min, the coating thickness was 2.1mm, and the insulating core wire was obtained by cooling and shaping in 22℃ cooling water for 7min; S3, preparation of multifunctional buffer layer: Polyisobutylene grafted maleic anhydride-nano-boron nitride composite, modified high-performance polypropylene-graphene quantum dot composite, polycaprolactone and calcium stearate were added into an internal mixer, and mixed at 100℃ and 750r / min for 17min; Aramid short fibers and melamine cyanurate were added, and mixed at 115℃ and 350r / min for 22min to obtain a buffer layer mixture; The buffer layer mixture was coated on the insulating core wire by an extrusion coating process, the extrusion temperature was 140℃, the screw rotation speed was 270r / min, the coating thickness was 1.7mm, and the buffer layer was cooled and shaped in 22℃ cooling water for 8min; S4, high-strength armored layer compounding: Double-strand galvanized steel wires (diameter 0.4mm) were cross-woven, the weaving density was greater than or equal to 95%, the weaving tension was 8N, and the weaving pitch was 7 times the diameter of the cable to form a high-strength armored layer. S5, extrusion molding of wear-resistant outer sheath: A polyether TPU material with a Shore hardness of 80D is selected, antioxidant 1076 is added, and a sheath layer is coated outside the armored layer through a double-screw extruder, the extrusion temperature is 170℃ for the feeding section, 190℃ for the compression section, and 200℃ for the homogenization section, the screw speed is 330r / min, the coating thickness is 2mm, and the cooling is performed in 22℃ cooling water for 10min, the cooling vacuum degree is-0.3MPa, and a high-strength impact-resistant cable is obtained.

[0047] Comparative Example 1: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that the polyisobutylene grafted maleic anhydride-nano boron nitride composite is not added, and is replaced by an equal amount of pure polyisobutylene.

[0048] Comparative Example 2: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that the modified high-performance polypropylene-graphene quantum dot composite is not added, and is replaced by an equal amount of homopolymer polypropylene.

[0049] Comparative Example 3: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that the polyisobutylene grafted maleic anhydride-nano boron nitride composite is not modified with nano boron nitride (only polyisobutylene grafted maleic anhydride).

[0050] Comparative Example 4: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that the modified high-performance polypropylene-graphene quantum dot composite is not modified with graphene quantum dots (only polypropylene-glycidyl methacrylate grafting).

[0051] Comparative Example 5: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that aramid short fibers are not added.

[0052] Comparative Example 6: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that melamine cyanurate is not added.

[0053] Comparative Example 7: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that silane coupling agent KH-560 is not added.

[0054] Comparative Example 8: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is only that polycaprolactone is not added.

[0055] Comparative Example 9: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is that no antioxidant 1076 is added.

[0056] Comparative Example 10: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is that the conductor plasma pretreatment step is omitted.

[0057] Comparative Example 11: A high-strength impact-resistant cable and a preparation method thereof, the difference between which and Example 3 is that nano-titanium dioxide is replaced with an equal amount of nano-calcium carbonate.

[0058] The cables obtained in Examples 1-3 and Comparative Examples 1-11 were subjected to performance testing of tensile strength, notched impact strength, impact damage resistance, breakdown voltage, elongation at break, low-temperature toughness, high-temperature stability, and flame-retardant grade, and the performance testing methods and standards are as follows: 1. Tensile strength: according to “Determination of tensile properties of plastics - Part 2: test conditions for moulded and extruded plastics” (GB / T 1040.2-2006), dumbbell type I samples were used, the tensile speed was 50 mm / min, 5 samples were tested for each group, and the average value was taken; 2. Notched impact strength: according to “Determination of Izod impact strength of plastics” (GB / T 1843-2008), A-type notched samples were used, the impact energy was 5 J, the environmental temperature was (23±2) °C, 6 samples were tested for each group, and the average value was taken; 3. Impact damage resistance: according to “General test methods for cables and optical cables - Insulation and sheath materials” (GB / T 2951.51-2017), a falling weight impact tester was used for testing, the impact mass was 2.5 kg, the impact height was 1.2 m, each sample was impacted 10 times, and the damage rate = (the number of damaged impacts / the total number of impacts) x 100%; 4. Breakdown voltage: according to “Insulating materials - Determination of electrical strength - Part 1: test at power frequency” (GB / T 1408.1-2016), flat electrodes were used, the voltage was raised at a speed of 2.5 kV / s, the environmental temperature was (23±2) °C, the relative humidity was (50±5)%, 4 samples were tested for each group, and the average value was taken; 5. Elongation at break: according to “Determination of tensile properties of plastics - Part 2: test conditions for moulded and extruded plastics” (GB / T 1040.2-2006), it was tested synchronously with the tensile strength, 5 samples were tested for each group, and the average value was taken; 6. Low-temperature toughness: according to “Determination of low-temperature brittleness of plastics - Part 1: impact method” (GB / T 1842-2008), the cable sample was frozen at -45 °C for 2 h, then subjected to 180° bending for 10 times, and whether cracks were generated was observed; 7. High temperature stability: according to the "Plastics Thermal Aging Test Method" (GB / T 7141-2008), the cable buffer / sheath material sample is aged at 90°C for 168h, the tensile strength after aging is tested, and the tensile strength retention rate = (tensile strength after aging / tensile strength before aging) x 100%; 8. Flame retardant grade: according to "Determination of the Burning Behavior of Plastics - Part 2: Horizontal and Vertical Methods" (GB / T 2408-2008), vertical burning test is carried out to evaluate the flame retardant grade.

[0059] The results are shown in Table 1.

[0060] Table 1 Performance parameters of cables obtained in Examples 1-3 and Comparative Examples 1-11

[0061] The performance differences and reason analysis of Comparative Examples 1-11 are as follows, taking Example 3 as the control group: Comparative Example 1: The tensile strength decreased from 51.3 MPa to 34.7 MPa, with a decrease of 32.4%; the notched impact strength decreased from 65.7 kJ / m 2 to 42.3 kJ / m 2 , with a decrease of 35.6%; the impact damage resistance rate increased from 0% to 45%. The reason is that the polyisobutylene grafted maleic anhydride-nano boron nitride composite is not added, and is replaced by an equal amount of pure polyisobutylene, which loses the elastic buffer and high efficient heat conduction function of the composite, and the impact energy cannot be effectively dispersed. At the same time, the lack of maleic anhydride grafting groups in polyisobutylene leads to a decrease in interfacial compatibility, which further weakens the mechanical properties and impact resistance of the cable.

[0062] Comparative Example 2: The tensile strength decreased from 51.3 MPa to 33.5 MPa, with a decrease of 34.7%; the notched impact strength decreased from 65.7 kJ / m 2 to 40.8 kJ / m 2 , with a decrease of 37.9%; the impact damage resistance rate increased from 0% to 50%. Since the modified high-performance polypropylene-graphene quantum dot composite is not added, and is replaced by an equal amount of homopolymer polypropylene (high-performance polypropylene), the rigid support of high-performance polypropylene and the synergistic reinforcing effect of graphene quantum dots are lacking, and a "soft-rigid-heat conducting" synergistic system cannot be formed, and the overall mechanical support capacity of the protective layer is greatly reduced.

[0063] Comparative Example 3: The tensile strength decreased from 51.3 MPa to 38.2 MPa, with a decrease of 25.5%; the notched impact strength decreased from 65.7 kJ / m 2 to 47.5 kJ / m 2, the drop of 27.7%; the impact damage resistance rate increased from 0% to 35%; the low-temperature toughness changed from no crack to slight crack. The polyisobutylene grafted maleic anhydride-nano boron nitride composite was not modified by nano boron nitride, but only polyisobutylene grafted maleic anhydride, which led to the decrease of thermal conductivity and dispersibility of the material, the weakening of the interfacial bonding force between components, and the significant reduction of synergistic enhancement effect.

[0064] Comparative Example 4: the tensile strength decreased from 51.3 MPa to 37.6 MPa, a drop of 26.7%; the notched impact strength decreased from 65.7 kJ / m 2 to 46.2 kJ / m 2 , a drop of 29.7%; the impact damage resistance rate increased from 0% to 38%; the low-temperature toughness changed from no crack to slight crack. The modified high-performance polypropylene-graphene quantum dot composite was not modified by graphene quantum dots, but only polypropylene-glycidyl methacrylate graft, which lacked the high specific surface area enhancement effect of graphene quantum dots, and the mechanical properties and impact resistance of the material decreased significantly.

[0065] Comparative Example 5: the tensile strength decreased from 51.3 MPa to 41.5 MPa, a drop of 19.1%; the notched impact strength decreased from 65.7 kJ / m 2 to 52.1 kJ / m 2 , a drop of 20.7%; the impact damage resistance rate increased from 0% to 25%. After the aramid short fibers were not added, the "crack bridging" effect was lost, and the crack was easy to expand under impact load, resulting in the weakening of the mechanical properties and impact resistance of the cable.

[0066] Comparative Example 6: the impact damage resistance rate increased from 0% to 20%; the flame retardant grade decreased from UL94 V-0 to V-2. After the melamine cyanurate was not added, the flame-retardant carbon layer and inert gas buffer effect generated by its decomposition were lacking, the material structure was easy to be damaged during combustion, the flame retardant performance decreased significantly, and the reinforcing effect brought by the particle filling was also lost, and the auxiliary gain of impact resistance disappeared.

[0067] Comparative Example 7: the tensile strength decreased from 51.3 MPa to 36.9 MPa, a drop of 28.1%; the notched impact strength decreased from 65.7 kJ / m 2 to 45.7 kJ / m 2 , a drop of 30.4%; the impact damage resistance rate increased from 0% to 40%; the breakdown voltage decreased from 35.2 kV to 25.3 kV, a drop of 28.1%; the low-temperature toughness changed from no crack to crack. After the silane coupling agent KH-560 was not added, the organic matrix and inorganic fillers could not form effective chemical bonding, the interfacial compatibility was poor, the inorganic fillers were easy to agglomerate, the interfacial defects increased, and the mechanical properties, insulation properties and environmental resistance of the cable decreased simultaneously.

[0068] Comparative Example 8: The tensile strength decreased from 51.3 MPa to 39.4 MPa, a decrease of 23.2%; the notched impact strength decreased from 65.7 kJ / m 2 to 49.3 kJ / m 2 , a decrease of 25.0%; the impact damage resistance increased from 0% to 32%; and the low-temperature toughness changed from no cracks to slight cracks. After not adding polycaprolactone (PCL), the buffer layer lost the low-temperature elasticity adjustment effect of the flexible polymer, and the material was insufficiently flexible in a low-temperature environment, and the impact energy absorption efficiency decreased.

[0069] Comparative Example 9: The high-temperature tensile strength retention rate decreased from 98% to 75%, a decrease of 23.5%. After not adding antioxidant 1076, the free radicals generated during the processing and use of the material cannot be effectively captured, thermal oxidation is aggravated, and the performance in a long-term high-temperature environment is significantly attenuated.

[0070] Comparative Example 10: The tensile strength decreased from 51.3 MPa to 35.8 MPa, a decrease of 29.9%; the notched impact strength decreased from 65.7 kJ / m 2 to 43.5 kJ / m 2 , a decrease of 33.8%; the impact damage resistance increased from 0% to 42%; the breakdown voltage decreased from 35.2 kV to 25.1 kV, a decrease of 28.7%; and the low-temperature toughness changed from no cracks to cracks. After omitting the conductor plasma pretreatment step, the surface activity of the conductor is insufficient, the interfacial adhesion between the conductor and the insulating layer is poor, interlayer peeling occurs under impact load, the overall structural stability decreases, and the comprehensive performance weakens.

[0071] Comparative Example 11: The tensile strength decreased from 51.3 MPa to 40.1 MPa, a decrease of 21.8%; the notched impact strength decreased from 65.7 kJ / m 2 to 50.2 kJ / m 2 , a decrease of 23.6%; the impact damage resistance increased from 0% to 30%; and the breakdown voltage decreased from 35.2 kV to 28.9 kV, a decrease of 17.9%. After replacing nano-titanium dioxide with an equal amount of nano-calcium carbonate, the hardness and dispersibility of nano-calcium carbonate are both inferior to those of nano-titanium dioxide, the filling and reinforcing effect is weaker than that of nano-titanium dioxide, the structural density of the insulating layer decreases, the strengthening effect of the insulating layer weakens, and the mechanical and insulating properties of the cable decrease.

[0072] In summary, the polyisobutylene grafted maleic anhydride-nano boron nitride composite provides elastic buffering and efficient heat conduction, the modified high-performance polypropylene-graphene quantum dot composite strengthens rigid support and mechanical enhancement, and the two synergistically build a "soft-rigid-heat-conductive" system, which greatly improves the impact resistance and wide-temperature-range stability. The modified cross-linked polyethylene is combined with nano-titanium dioxide and silane coupling agent KH-560 to improve the synergistic adaptability of the insulating and impact resistance.

[0073] The above examples are only used to illustrate the technical solutions of the present application, but not to limit the present application; although the present application has been described in detail with reference to the foregoing examples, those ordinarily skilled in the art should understand: the technical solutions recorded in the foregoing examples can be modified, or some technical features can be replaced equivalently; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A high strength impact resistant cable, characterized by, The high-strength anti-collision cable comprises, from inside to outside, an oxygen-free copper conductor, a modified insulation layer, a multi-functional buffer layer, a high-strength armored layer and a wear-resistant outer sheath. The high-strength anti-collision cable comprises, by weight, 35-45 parts of modified cross-linked polyethylene, 12-18 parts of polyisobutylene grafted maleic anhydride-nano boron nitride compound, 8-15 parts of modified high-performance polypropylene-graphene quantum dot compound, 3-6 parts of nano titanium dioxide, 7-12 parts of aramid short fiber, 5-10 parts of melamine cyanurate, 0.8-1.5 parts of calcium stearate, 0.5-1.0 parts of silane coupling agent, 6-10 parts of polycaprolactone and 0.3-0.8 parts of antioxidant.

2. The high strength crush resistant cable of claim 1, wherein, The weight average molecular weight of the modified cross-linked polyethylene is 50,000-80,000 Da, the particle size of the nano titanium dioxide is 20-50 nm, the length of the aramid short fiber is 100-200 μm and the weight average molecular weight of the polycaprolactone is 10,000-20,000 Da.

3. The high strength crush resistant cable of claim 1, wherein, The silane coupling agent is one of KH-550, KH-560 and KH-570, and the antioxidant is one of antioxidant 1010, antioxidant 168 and antioxidant 1076.

4. The high strength crush resistant cable of claim 1, wherein, The polyisobutylene grafted maleic anhydride-nano boron nitride compound comprises, by weight, 90-100 parts of polyisobutylene, 8-12 parts of maleic anhydride, 1.2-1.8 parts of benzoyl peroxide, 8-12 parts of nano boron nitride, 140-180 parts of anhydrous toluene and 2-4 parts of silane coupling agent KH-570.

5. The high strength crush resistant cable of claim 4, wherein, The preparation method of the polyisobutylene grafted maleic anhydride-nano boron nitride compound comprises the following steps: 1) the nano boron nitride is added into 3 / 7 of the total amount of anhydrous toluene, dispersed for 30-40 min under the conditions of ultrasonic frequency of 20-30 kHz and ultrasonic power of 250-300 W, and then the silane coupling agent KH-570 is added dropwise, stirred and reacted at 70-80 ℃ and a rotating speed of 250-350 r / min for 2-3 h, filtered, and dried at 88-90 ℃ under the vacuum condition of-0.09 MPa to-0.08 MPa for 6-8 h to obtain modified nano boron nitride; 2) the polyisobutylene is added into the remaining anhydrous toluene, heated to 85-95 ℃ and stirred and dissolved, and then the maleic anhydride and the benzoyl peroxide are added, stirred and reacted under the nitrogen atmosphere at a rotating speed of 300-400 r / min for 5-7 h, and then 80-90% of the anhydrous toluene is removed by reduced pressure distillation to obtain a polyisobutylene grafted maleic anhydride concentrated solution; 3) the modified nano boron nitride is added into the polyisobutylene grafted maleic anhydride concentrated solution, high-speed stirred at 100-110 ℃ and a rotating speed of 350-450 r / min for 3-4 h, and then poured into 150-200 parts of petroleum ether for precipitation, filtered, and dried at 78-82 ℃ under the vacuum condition of-0.10 MPa to-0.09 MPa for 10-12 h, and then crushed through a 200-300 mesh sieve to obtain the polyisobutylene grafted maleic anhydride-nano boron nitride compound.

6. The high strength crush resistant cable of claim 4, wherein, The weight average molecular weight of the polyisobutylene is 8,000-12,000 Da, and the particle size of the nano boron nitride is 50-100 nm.

7. The high strength crush resistant cable of claim 1, wherein, The modified high-performance polypropylene-graphene quantum dot composite comprises, in parts by weight, 90-100 parts of high-performance polypropylene, 3-5 parts of graphene quantum dots, 6-10 parts of glycidyl methacrylate, 0.8-1.2 parts of di-tert-butyl peroxide, 50-70 parts of anhydrous ethanol, and 0.4-0.6 parts of antioxidant 168, wherein the high-performance polypropylene is impact copolymerized polypropylene or homopolymerized polypropylene, and has a weight average molecular weight of 40,000-60,000 Da; and the graphene quantum dots have a particle size of 3-5 nm.

8. The high strength crush resistant cable of claim 7, wherein, The preparation method of the modified high-performance polypropylene-graphene quantum dot composite comprises the following steps: a. dispersing the graphene quantum dots in anhydrous ethanol, and dispersing for 25-35 min under the conditions of an ultrasonic frequency of 20-30 kHz and an ultrasonic power of 250-300 W to obtain a graphene quantum dot dispersion liquid; b. adding the high-performance polypropylene, glycidyl methacrylate, di-tert-butyl peroxide, and antioxidant 168 into a high-speed mixer, and mixing at a speed of 800-1,000 r / min at 110-120 ℃ for 15-20 min to obtain a premix; c. feeding the premix into a double-screw extruder, and setting the extrusion temperature as follows: 150-160 ℃ for the first zone, 165-175 ℃ for the second zone, 175-185 ℃ for the third zone, and 180-190 ℃ for the fourth zone, and setting the screw rotation speed as 300-400 r / min, and then performing water cooling and pelletizing after extrusion to obtain a polypropylene-glycidyl methacrylate grafting product; d. mixing the polypropylene-glycidyl methacrylate grafting product with the graphene quantum dot dispersion liquid, stirring at a speed of 200-300 r / min at 70-80 ℃, evaporating the anhydrous ethanol until no free liquid is visible in the system, and then drying at 118-122 ℃ under a vacuum condition of -0.09 MPa to -0.08 MPa for 8-10 h to obtain the modified high-performance polypropylene-graphene quantum dot composite.

9. A method of manufacturing a high strength crash resistant cable according to any one of claims 1-8, characterized in that, The method comprises the following steps: S1, oxygen-free copper conductor pretreatment: a plurality of fine copper wires are twisted into an oxygen-free copper conductor according to a pitch ratio of 8:1-10:1, and then dried at 120-140 ℃ for 2-3 h, and then activated and treated by using a plasma treatment machine at a power of 350-450 W for 4-6 min; S2, modified insulation layer coating: a modified crosslinked polyethylene, nano-titanium dioxide, and a silane coupling agent are added into a high-speed mixer, and mixed at a speed of 750-950 r / min at 105-115 ℃ for 12-16 min to obtain an insulation layer mixture; the mixture is coated on the pretreated copper conductor by using a single-screw extruder, and the extrusion temperature is set as follows: 145-155 ℃ for a feeding section, 165-175 ℃ for a compression section, and 175-185 ℃ for a homogenization section, the screw rotation speed is set as 280-380 r / min, the coating thickness is set as 1.8-2.5 mm, and the insulation core wire is obtained by cooling and shaping in 20-25 ℃ cooling water for 5-8 min; S3, multifunctional buffer layer preparation: Polyisobutylene grafted maleic anhydride-nano boron nitride compound, modified high-performance polypropylene-graphene quantum dot compound, polycaprolactone, calcium stearate are added into the internal mixer, and are mixed at 95-105 DEG C for 15-20 min at a rotating speed of 650-850 r / min; Aramid short fiber and melamine cyanurate are added, and are mixed at 110-120 DEG C for 20-25 min at a rotating speed of 300-400 r / min to obtain a buffer layer mixture; The buffer layer mixture is coated on the insulating core wire by using an extrusion coating process, the extrusion temperature is 135-145 DEG C, the screw rotating speed is 220-320 r / min, the coating thickness is 1.5-2.0 mm, and the coating is cooled and shaped in 20-25 DEG C cooling water for 6-10 min; S4, high-strength armored layer composite: Double galvanized steel wires are cross-woven to form a high-strength armored layer, the weaving density is greater than or equal to 95%, the weaving tension is 6-9 N, and the weaving pitch is 6-8 times the diameter of the cable; S5, wear-resistant outer sheath extrusion molding: Polyether TPU material is selected, an antioxidant is added, and the armored layer is coated outside by using a double-screw extruder, the extrusion temperature is: the feeding section is 165-175 DEG C, the compression section is 185-195 DEG C, the homogenization section is 195-205 DEG C, the screw rotating speed is 280-380 r / min, the coating thickness is 1.8-2.2 mm, the coating is cooled and shaped in 20-25 DEG C cooling water for 8-12 min, the cooling vacuum degree is-0.35 MPa to-0.25 MPa, and a high-strength impact-resistant cable is obtained.

10. The method of making a high strength crush resistant cable of claim 9, wherein, In step S5, the Shore hardness of the polyether TPU material is 75-85D.