Preparation method of polyetherimide
By employing a solvent-free synthesis technique in a high-pressure reactor, the problems of solvent residue and wide molecular weight distribution in the synthesis of polyetherimide have been solved, achieving efficient and low-cost preparation of polyetherimide. The product exhibits good thermal stability and a light color.
Patent Information
- Application Number
- CN202511988277.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-26
- Publication Date
- 2026-02-06
AI Technical Summary
Existing polyetherimide synthesis processes suffer from problems such as solvent residue, low reaction efficiency, wide molecular weight distribution, high end-group residue, and easy coloring of products due to high-temperature oxidation.
Solvent-free synthesis was carried out using a high-pressure reactor. An oxygen-free environment was ensured by replacing air with nitrogen. The material ratio and temperature were controlled to achieve melt extrusion granulation and prepare polyetherimide.
This method enables the preparation of polyetherimides with narrow molecular weight distribution, low end-group residue, good high thermal oxidation stability, and light color, thereby improving production efficiency and reducing solvent costs and processing steps.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of high polymer materials, and particularly relates to a preparation method of polyetherimide. BACKGROUND
[0002] Polyetherimide (PEI) is widely used in aerospace, electronic devices and other fields due to its excellent heat resistance, mechanical strength and transparency. The traditional synthesis process is mainly divided into two categories: Chinese patent application CN105121511A discloses a method for preparing a polyetherimide resin, comprising charging a reactor with a liquid reaction solvent, bisphenol A dianhydride, m-phenylenediamine and a chain terminator selected from the group consisting of phthalic anhydride and aniline, introducing a stream of dry inert gas below the surface of the liquid reactor contents, and selectively removing water from the reactor by dispersing the inert gas in the liquid reactor contents and venting the inert gas and water from the headspace of the reactor, thereby preparing the polyetherimide resin. This method needs to introduce o-dichlorobenzene solvent for reaction in the process.
[0003] The solvent method uses dichloromethane, o-dichlorobenzene solvent, NMP, etc. as the solvent, and is prepared by two steps of low-temperature solution polycondensation and high-temperature imidization. This method has problems such as yellowing of the product caused by solvent residue, high cost of subsequent solvent recovery, environmental pollution, and low reaction efficiency.
[0004] Chinese patent application CN111133031A discloses a method for preparing polyetherimide by melt polymerization under vacuum conditions. In the process, dichloromethane and other solvents are first introduced for preliminary reaction, and then the solvents are evaporated for reaction.
[0005] Some melt polycondensation methods also introduce solvents to cause the occurrence of solvent residue phenomenon, and the atmospheric pressure reaction needs a long time of high temperature dehydration, which leads to wide molecular weight distribution, high end group residue content, and easy coloring of the product caused by high temperature oxidation. In the reaction process, the reaction steps are more and the reaction treatment time is longer, and the production efficiency is low.
[0006] Therefore, it is urgent to provide a polyetherimide preparation method without solvent in the reaction process, with narrow molecular weight distribution of the product, low end group residue content, and good high-temperature oxidation stability. SUMMARY
[0007] The first object of the present application is to solve the above technical problems, and to provide a polyetherimide preparation method without solvent, with narrow molecular weight distribution of the product, low end group residue content, good high-temperature oxidation stability, and light color.
[0008] The second object of the present application is to provide a polyetherimide.
[0009] The third object of the present application is to provide a polyetherimide part.
[0010] The present application is realized by the following technical solutions: A polyetherimide preparation method comprises the following steps: (a) adding a first monomer into a high-pressure reaction kettle equipped with a mechanical stirring device; replacing air with nitrogen in the reaction kettle, increasing pressure, and increasing temperature to melt the material; (b) adding a second monomer preheated to a molten state into the reaction kettle through a feeding pump in multiple times; during the addition of the second monomer, increasing the temperature by 10-30 DEG C for every 8-12% of the molar amount of the second monomer, and finally increasing the temperature to 350-500 DEG C, and the feeding process lasts for 30-60 minutes; (c) keeping the temperature for 10-20 minutes after the feeding is completed; (d) discharging water vapor through an exhaust port to reduce the pressure to 0.1-0.2 MPa, and stopping the exhaust; (e) recharging nitrogen to increase the pressure to 0.4-0.6 MPa; (f) extruding the molten material from the reaction kettle, and granulating after cooling; The first monomer and the second monomer are one of aromatic bisether anhydride and the other is diamine; and the PDI value of the polyetherimide is 2.0-2.2.
[0011] In the present application, the PDI value means the molecular weight distribution index, PDI = Mw / Mn. Wherein, Mw is the weight average molecular weight, and Mn is the number average molecular weight.
[0012] In the present application, the PDI value can be: 2.00, 2.01, 2.02, 2.03, 2.04, 2.05, 2.06, 2.07, 2.08, 2.09, 2.10, 2.11, 2.12, 2.13, 2.14, 2.15, 2.16, 2.17, 2.18, 2.19, 2.20, or a range interval formed by any two of the above values.
[0013] Preferably, the PDI value is 2.0-2.15.
[0014] The polyetherimide preparation method provided by the present application effectively avoids oxidation of the amine end, accurately controls the material ratio, so that the amine end is basically completely reacted without adding a capping agent, and at the same time, the high pressure makes the reaction more easily carried out, and the molecular weight of the molecular weight with a smaller chain length is further increased, thereby narrowing the molecular weight distribution.
[0015] Preferably, in step (a), the air is replaced with nitrogen at least three times.
[0016] In the present application, the at least three times of replacing air with nitrogen in step (a) is achieved by the following process: nitrogen is introduced into the closed high-pressure reactor, the pressure in the reactor is increased to 0.6-0.8 MPa, then the exhaust port is opened to discharge the gas (mainly a mixture of nitrogen and air) in the reactor, and the pressure is reduced to normal pressure. This "pressurization-exhaustion" process is referred to as one complete replacement. This process is repeated at least three times to ensure that the oxygen concentration in the reaction system is reduced to a very low level. After the replacement is completed, nitrogen is finally charged into the reactor and maintained at a certain pressure (such as 0.3-0.5 MPa), and after 30 minutes, if the pressure does not decrease, the subsequent operation is carried out.
[0017] It should be noted that the above-mentioned "pressurization-exhaustion" nitrogen replacement air method is only one preferred and efficient implementation scheme for achieving an oxygen-free environment in the reaction system. Under the concept of the present application, any technical means that can effectively reduce the oxygen concentration in the reactor to achieve the same technical effect as the "nitrogen replacement air" described in the present application falls within the scope of the present application. This includes but is not limited to: using a "vacuum-pumping nitrogen" cycle replacement method; using a dynamic replacement method with continuous nitrogen blowing at the inlet and outlet of the reactor; any existing or future gas replacement technology that can achieve the same oxygen-free environment effect.
[0018] Therefore, simple replacement or equivalent changes to the replacement method should be considered within the scope of the present application if they do not deviate from the core inventive idea of creating an oxygen-free environment.
[0019] Preferably, in step (a), the pressure is increased to 0.3-0.5 MPa.
[0020] In the present application, the pressure (unit: MPa) maintained during the reaction in step (a) can be: 0.3, 0.32, 0.35, 0.38, 0.4, 0.43, 0.45, 0.47, 0.50, or a range interval formed by any two of the above values.
[0021] Preferably, in step (a), the temperature is increased to 70-300°C.
[0022] In the present application, in step (a), the temperature (unit: °C) can be increased to: 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, or a range interval formed by any two of the above values.
[0023] Preferably, in step (a), the temperature is raised to 150-300°C.
[0024] In the present application, the single addition mole mass (unit: %) of the second monomer in step (b) can be 8, 9, 10, 11, 12, or a range interval formed by any two of the above values.
[0025] In some specific embodiments, the single addition mole mass of the second monomer is 10%.
[0026] Preferably, when the second monomer in step (b) is selected from diamines, the preheating temperature is 80-150°C; when the second monomer in step (b) is selected from aromatic bisether anhydrides, the preheating temperature is 140-200°C.
[0027] In the present application, when the second monomer in step (b) is selected from diamines, the preheating temperature can be 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, or a range interval formed by any two of the above values.
[0028] In the present application, when the second monomer in step (b) is selected from aromatic bisether anhydrides, the preheating temperature can be 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188, 189, 190, 191, 192, 193, 194, 195, 196, 197, 198, 199, 200, or a range interval formed by any two of the above values.
[0029] In some specific embodiments, before adding the second monomer to the high-pressure reactor, the temperature inside the reactor is 200°C. For every 10% molar amount of the second monomer added, the temperature is increased by 20°C. That is, the second monomer is divided into 10 equal parts, with 10% molar amount added each time. The temperature is increased by 20°C each time the second monomer is added. After the first addition, the temperature rises to 220°C, after the second to 240°C, and so on, until the tenth addition is completed, at which point the reaction temperature reaches 400°C.
[0030] Preferably, in step (c), the pressure is maintained at 0.3-0.5 MPa during the reaction.
[0031] In this invention, in step (c), the pressure (unit: MPa) maintained during the reaction process can be: 0.3, 0.32, 0.35, 0.38, 0.4, 0.43, 0.45, 0.47, 0.50, or any range formed by any two of the above values.
[0032] Preferably, in step (c), the pressure is maintained at 0.35-0.45 MPa during the reaction.
[0033] Preferably, in step (d), the exhaust is performed at 330-380°C.
[0034] In this invention, in step (d), the exhaust temperature can be 330, 335, 340, 345, 350, 355, 360, 365, 370, 375, 380, or any range formed by any two of the above values.
[0035] Preferably, in step (d), the exhaust is performed at 350-370°C.
[0036] Preferably, the pressure after re-inflation in step (e) is 0.45-0.55 MPa.
[0037] In this invention, in step (e), the pressure after re-inflating can be 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, or a range formed by any two of the above values.
[0038] Preferably, the aromatic diether anhydride is selected from bisphenol A type dianhydride, diphenyl ether type dianhydride, diphenyl sulfide type dianhydride, benzophenone type dianhydride, diphenyl sulfone type dianhydride, or other dianhydrides with different structures.
[0039] More preferably, the aromatic diether anhydride is selected from bisphenol A dianhydrides.
[0040] In the present application, the aromatic bis-ether anhydride can be selected from at least one of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 3,3-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl ether dianhydride, 4,4-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4-bis(3,4-dicarboxyphenoxy)benzophenone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl ether dianhydride, 4,4-bis(2,3-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4-bis(2,3-dicarboxyphenoxy)benzophenone dianhydride, 4,4-bis(2,3-dicarboxyphenoxy)diphenyl sulfone dianhydride, 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl-2,2-propane dianhydride, 4-(2,3-dicarboxyphenoxy)-4-(3,4-dicarboxyphenoxy)diphenyl ether dianhydride, 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)phenyl sulfide dianhydride, 4-(2,3-dicarboxyphenoxy)-4-(3,4-dicarboxyphenoxy)benzophenone dianhydride, 4,4-(hexafluoroisopropylidene)diphthalic anhydride, 4-(2,3-dicarboxyphenoxy)-4-(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride, 3,3,4,4-triphenyl ether tetraacid dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, p-phenylene-bisbenzotrifurandianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride.
[0041] Preferably, the aromatic bis-ether anhydride is selected from any one of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 3,3-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 4,4-bis(3,4-dicarboxyphenoxy)benzophenone dianhydride, 3,3,4,4-triphenyl ether tetraacid dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, p-phenylene-bisbenzotrifurandianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride. The aromatic bis-ether anhydride monomer of the present application should be able to transform into a molten state suitable for performing polycondensation reaction under the heating conditions of the present application. Generally, it is a solid crystal with a melting point of 50-400℃, and the detection standard is GB / T 28724-2012, and the detection method is differential scanning calorimetry.
[0042] Preferably, the melting point of the aromatic bis-ether anhydride monomer is 80-350℃.
[0043] Preferably, the diamine is selected from at least one of aliphatic diamine, alicyclic diamine, aromatic diamine.
[0044] In the present application, the diamine can be selected from at least one of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, 1,18-octadecanediamine, 3-methylheptamethylenediamine, 4,4-dimethylheptamethylenediamine, 4-methylnonamethylenediamine, 5-methylnonamethylenediamine, 2,5-dimethylhexamethylenediamine, 2,5-dimethylheptamethylenediamine, 2,2-dimethylpropylenediamine, N-methyl-bis-(3-aminopropyl)amine, 3-methoxyhexamethylenediamine, 1,2-bis(3-aminopropoxy)ethane, bis(3-aminopropyl) sulfide, 1,4-cyclohexanediamine, bis-(4-aminocyclohexyl)methane, m-phenylenediamine, p-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene, m-xylylenediamine, p-phenylenediamine, 2-methyl-4,6-diethyl-l,3-phenylenediamine, 5-methyl-4,6-diethyl-l,3-phenylenediamine, diphenylamine, 3,3'-dimethylphenylamine, 3,3'-dimethoxyphenylamine, 1,5-diaminonaphthalene, bis-(4-aminophenyl)methane, bis-(2-chloro-4-amino-3,5-diethylphenyl)methane, bis-(4-aminophenyl)sulfide, bis-(4-aminophenyl)sulfone and bis-(4-aminophenyl)ether, 3,5-diaminobenzoic acid, 3,4'-diaminodiphenylmethane, diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diamino-2,2'-bistrifluoromethylbiphenyl.
[0045] Preferably, the diamine is selected from at least one of m-phenylenediamine, p-phenylenediamine.
[0046] Further preferably, the diamine is selected from m-phenylenediamine.
[0047] The diamine can also be selected from at least one of isomers of any region of the above-mentioned compounds.
[0048] The diamine monomer in the present application should be able to transform into a molten flow state suitable for carrying out polycondensation reaction under the heating conditions described in the present application, and maintain chemical stability in this state. Generally, the diamine monomer in the present application is solid at room temperature, and the melting point is 70-350℃, detected according to GB / T 19466.3-2022 by differential scanning calorimetry.
[0049] Preferably, the melting point of the diamine monomer is 80-300℃.
[0050] For diamine monomers that are liquid at room temperature (such as some aliphatic diamines), the boiling point should be higher than the temperature of the polymerization reaction of the present application to ensure that the monomer ratio and the reaction progress are not affected by volatilization during the reaction. Those skilled in the art can adjust the preheating temperature to achieve the appropriate fluidity according to the physical properties of the selected diamine.
[0051] The melting point and other physical parameters of the monomer compounds described in the present application may vary reasonably due to differences in measuring instruments, measuring methods, purity, and crystalline form. The key to the use of the monomers as polymer monomers lies in their chemical reaction characteristics determined by their molecular structure, rather than their specific physical parameters. Those skilled in the art can understand that as long as the monomer has the core molecular structure claimed in the present application, the specific value of the melting point does not substantially affect the technical effects of the present application.
[0052] The preparation method of polyetherimide provided by the present application can be used to prepare polyetherimides of different structural types, mainly including: (1) polyetherimide obtained by polymerization of a single-structure diamine and a single-structure aromatic diether anhydride; (2) polyetherimide obtained by polymerization of mixed diamines and / or mixed aromatic diether anhydrides.
[0053] Among them, mixed diamines refer to combinations of two or more diamines of different structures; mixed aromatic diether anhydrides refer to combinations of two or more aromatic diether anhydrides of different structures.
[0054] In the process of preparing polyetherimide obtained by polymerization of a single-structure diamine and a single-structure aromatic diether anhydride through the preparation method of polyetherimide provided by the present application, the diamine is selected from any one of 3,5-diaminobenzoic acid, m-phenylenediamine, 3,4'-diaminodiphenylmethane, p-phenylenediamine, diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, and 4,4'-diamino-2,2'-bistrifluoromethylbiphenyl; The aromatic diether anhydride is selected from any one of bisphenol A type diether dianhydride, 3,3,4,4-biphenyl ether tetraacid dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, p-phenylene-bisphenyltricarboxylate dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride.
[0055] In the process of preparing the polyetherimide by the preparation method of the polyetherimide provided in the application, the diamine is selected from any one or more than two kinds of mixture of 3,5-diaminobenzoic acid, m-phenylenediamine, 3,4'-diaminodiphenyl methane, p-phenylenediamine, diaminodiphenyl ether, 4,4'-diaminodiphenyl methane, 4,4'-diamino-2,2'-bistrifluoromethyl biphenyl; the aromatic bis-ether anhydride is selected from a bis-ether dianhydride of one structure or a mixture composed of a bis-ether dianhydride and another aromatic dianhydride of non-ether bond structure. In the mixture, the mole percentage of the bis-ether dianhydride accounts for 90% to 100% of the total dianhydride monomers, and the mole percentage of the other aromatic dianhydride accounts for 0% to 10%. The aromatic bis-ether dianhydride includes a mixture of one or more of bisphenol A type bis-ether dianhydride and 3,3',4,4'-triphenyl ether tetraacid dianhydride; the other aromatic dianhydride includes a mixture of one or more of biphenyl tetraacid dianhydride, pyromellitic dianhydride, benzophenone tetraacid dianhydride, diphenyl ether tetraacid dianhydride and hexafluoro dianhydride.
[0056] In the application, the polyetherimide obtained by polymerization of a single-structure diamine and a single-structure dianhydride refers to that all the diamine chain segments in the polymer chain are of the same structure, and all the dianhydride chain segments are of the same structure.
[0057] In the application, the polyetherimide obtained by polymerization of a mixed diamine and / or a mixed aromatic bis-ether anhydride refers to that the polymer chain contains at least two different structures of diamine chain segments, or at least two different structures of dianhydride chain segments, or both.
[0058] The application provides a polyetherimide prepared by the above preparation method.
[0059] Preferably, the polyetherimide is a thermoplastic polyetherimide.
[0060] The application also provides a polyetherimide article, wherein the polyetherimide is prepared by the above preparation method.
[0061] Preferably, the article can be an aerospace article, an automobile article, a mechanical industry article, an electronic and electrical article, a precision machinery article.
[0062] More preferably, the article can be an electronic and electrical article.
[0063] Specifically, the electronic and electrical article can be a wafer carrier, an insulating film, a connector, a socket and the like.
[0064] Compared with the prior art, the application has the following beneficial effects: The present application effectively shortens the reaction time of the material by introducing a high-pressure reaction kettle. After the reaction is completed, the step of melting, discharging, extruding and granulating can be directly carried out, which can effectively save the material processing step and improve the production efficiency. And effectively solve the problem of color change of the material caused by the invasion of oxidizing gas such as air into the system.
[0065] The present application uses a solvent-free reaction, which can effectively reduce the cost of solvent, reduce the subsequent process of treating the solvent, and does not need to recover the solvent, and the material produced does not have the problem of solvent residue.
[0066] The present application provides a new melt polymerization system capable of synthesizing polyetherimide. The polyetherimide prepared by the method of the present application has narrow molecular weight distribution, low end group residue, good thermal oxidative stability and light color. DETAILED DESCRIPTION
[0067] The present application will be described in detail below in conjunction with specific examples. The following examples will help those skilled in the art to further understand the present application, but do not limit the present application in any form. It should be pointed out that for those skilled in the art, without departing from the concept of the present application, a number of modifications and improvements can be made. These all belong to the protection scope of the present application.
[0068] The raw materials used in the present application are derived from commercial sources.
[0069] Test methods: Molecular weight: GBT 36214.1-5-2018 Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography (using polystyrene standard sample as standard curve) Mobile phase and sample configuration: DMF containing 0.1% mass fraction of LiBr is used as the mobile phase, and the mobile phase is configured to contain 0.5% mass fraction of sample liquid.
[0070] Test equipment: Agilent 1260 Infinity II GPC / SEC system, PolarGel chromatographic column.
[0071] Test conditions: column temperature: 35℃, flow rate: 1mL / min, sample size: 20uL.
[0072] End group content: GB-T 9725-2007 Chemical reagents General method for potentiometric titration Sample configuration: 1g of material is placed in a 25mL volumetric flask, N,N-dimethylformamide (DMF) is used as the solvent, and the solution is dissolved into a light yellow solution under ultrasonic oscillation in a water bath at 40℃, and the same method is used to configure a blank sample.
[0073] The potentiometric titration is performed by using a Mettler automatic potentiometric titrator, the electrode is DG i113-SC, the reference electrolyte is 1 mol / L LiCl ethanol solution, and the standard solution is 0.01 mol / L HCl standard solution.
[0074] Firstly, the N, N-dimethylformamide (DMF) blank sample is titrated for correction, and no obvious potential change peak appears in three repetitions, which proves that the sample solution has no influence.
[0075] After blank correction, the titration of the sample is performed, and the average result is obtained by repeating three experiments.
[0076] Thermal stability: GB / T 27761-2011 test method for weight loss and residual amount of thermogravimetric analyzer A certain mass of sample is accurately weighed and placed into a WRRS thermogravimetric analyzer, and the thermal weight loss is observed at a temperature increasing speed of 20 ℃ / min to 800 ℃.
[0077] If the thermal weight loss at 530 ℃ is less than 5%, it proves that the sample stability is excellent, and the average value is obtained by repeating three experiments.
[0078] Color: visually, the sample prepared in the experiment is injection molded into a color plate, and then compared with the standard sample, the color is better or consistent with the standard sample.
[0079] The embodiments of the application are prepared by the following methods: (a) a first monomer is added to a high-pressure reaction kettle provided with a mechanical metal stirring paddle, and the high-pressure kettle is closed. Nitrogen is used to replace the gas in the high-pressure kettle, the stirring is started at 20 rpm / min, the temperature is increased to the melting point of the first monomer, nitrogen is filled to increase the pressure in the kettle for the first time; (b) the molten second monomer is pumped into the reaction kettle by using a feeding pump; (c) every time 10% of the molar amount of the second monomer is added, the temperature is increased in steps, and the stirring speed is gradually increased to 100 rpm / min, and the temperature is increased to the final temperature; (d) the final temperature is maintained for reaction; (e) the water vapor in the reaction kettle is discharged by opening the gas discharge valve, and the pressure gradually decreases during the discharging process, and the discharging is stopped; (f) nitrogen is filled to increase the gas pressure in the pressure kettle again; (g) then the reaction material is discharged from the bottom of the high-pressure kettle to a cooling water tank to form a strip-shaped polyetherimide, and the strip-shaped polyetherimide is placed into a granulator to be granulated to obtain the finished polyetherimide.
[0080] Table 1 preparation method and test results of each embodiment of examples 1-4
[0081] Table 2. Preparation method and test results for each of Examples 5-10
[0082] Comparative Example 1 In a glass reactor equipped with a mechanical stirrer, the monomers BPADA, m- phenylenediamine and chain terminator PA were dissolved in dichloromethane, stirred in an ultrasonic bath for 2 hours, the solvent was removed in a rotary evaporator at 50°C and 75,000 Pa and dried in a vacuum oven at 30°C and 10,000 Pa overnight. BPADA contained more than or equal to 95 mol% of 3,4 isomer.
[0083] The temperature of the reactor was increased to melt the dry mixture of monomers at 225°C for 10 minutes. Stirring was started at the beginning of the melting phase at 225°C and increased to 20 rpm. Then, the temperature was increased to the reaction set point of 350°C. Stirring was increased sequentially during the reaction to reach a maximum of 80 rpm. At 80 rpm, the pressure was decreased from atmospheric pressure to 1,000 Pa, keeping the vacuum constant until the end of the reaction.
[0084] The polyetherimide prepared in Comparative Example 1 had a molecular weight of Mn 13,000, Mw 43,000, PDI 3.3, an end group content of 50 mol / t, a thermal stability of 5% thermogravimetric temperature of 505°C, and a color of yellow.
[0085] Comparative Example 2 In a 1 L three-necked flask equipped with a mechanical stirrer, a thermometer, 0.1 mol of BPADA was added, 1 mol of molecular sieve treated N-methylpyrrolidone (NMP) was poured in, the system temperature was controlled below 5°C with an ice bath, and nitrogen protection. After the BPADA was completely dissolved, 10.8 g (0.1 mol) of m-phenylenediamine was added in three batches, stirring was continued, the ice bath was maintained, and the reaction was carried out for 8 h. At this time, yellow viscous polyetherimide acid was obtained, and the nitrogen and ice bath were removed. Acetic anhydride / pyridine (0.15 mol / 0.125 mol) was added to the flask, heated to 160°C, and reacted for 3 h. After the reaction was completed, the liquid in the flask was poured into a large amount of anhydrous ethanol to obtain PEI solid. The solid was collected, washed repeatedly with distilled water and anhydrous ethanol, and vacuum dried.
[0086] The polyetherimide prepared in Comparative Example 2 had a molecular weight of Mn 12,800, Mw 40,000, PDI 3.1, an end group content of 62 mol / t, a thermal stability of 5% thermogravimetric temperature of 510°C, and a color of yellow.
[0087] Comparative Example 3 The m-phenylenediamine preheated to a molten state was added into the high-pressure reaction kettle at one time, and the temperature was raised to the final temperature, and the others were the same as in Example 1. The polyetherimide prepared in Comparative Example 3 had a molecular weight of Mn 14000, Mw 44000, PD 3.1, an end group content of 65 mol / t, a thermal stability of 5% thermal weight loss temperature 514℃, and a color of yellow.
[0088] Comparative Example 4 The m-phenylenediamine preheated to a molten state was divided into 10 portions and added into the high-pressure reaction kettle in 10 times, and the temperature was directly raised to the final temperature after the last portion was added, and the others were the same as in Example 1. The polyetherimide prepared in Comparative Example 4 had a molecular weight of Mn 12000, Mw 35000, PD 2.9, an end group content of 60 mol / t, a thermal stability of 5% thermal weight loss temperature 520℃, and a color of yellow.
[0089] As can be seen from the examples, the polyetherimide provided in the examples has a PDI of 2.00-2.20, an end group content of ≤40 mol / t, a 5% thermal weight loss temperature of ≤520℃, and a color mainly of light yellow.
[0090] As can be seen from the comparative examples, the polyetherimide provided in the comparative examples has a PDI of 2.9-3.3, an end group content of ≥50 mol / t, a 5% thermal weight loss temperature of ≥530℃, and a color of yellow.
[0091] Finally, it should be noted that the above examples are only used to illustrate the technical solutions of the present application and not to limit the protection scope of the present application. Although the present application has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present application.
Claims
1. A method for preparing polyetherimide, characterized in that, Includes the following steps: (a) Add the first monomer to a high-pressure reactor equipped with a mechanical stirrer; purge the reactor with nitrogen to replace the air, increase the pressure and temperature to melt the material; (b) The second monomer, preheated to a molten state, is added to the reactor in multiple batches via a feed pump. During the addition of the second monomer, the temperature is raised by 10-30°C for every 8-12% molar amount of the second monomer added, until the final temperature reaches 350-500°C. The feeding process lasts for 30-60 minutes. (c) After the material is added, maintain the temperature and react for 10-20 minutes; (d) Open the exhaust port to release water vapor, reduce the pressure to 0.1-0.2 MPa, and then stop venting; (e) Refill with nitrogen to raise the pressure to 0.4-0.6 MPa; (f) The molten material is extruded from the reactor, cooled, and then granulated; Wherein, one of the first monomer and the second monomer is an aromatic diether anhydride and the other is a diamine; the PDI value of the polyetherimide is 2.0-2.
2.
2. The method for preparing polyetherimide according to claim 1, characterized in that, In step (a), the air is replaced with nitrogen at least three times; the pressure is increased to 0.3-0.5 MPa; and the temperature is increased to 70-300°C, preferably to 150-300°C.
3. The method for preparing polyetherimide according to claim 1, characterized in that, When the second monomer in step (b) is selected from diamine, the preheating temperature is 80-150℃; when the second monomer in step (b) is selected from aromatic diether anhydride, the preheating temperature is 140-200℃.
4. The method for preparing polyetherimide according to claim 1, characterized in that, In step (c), the pressure is maintained at 0.3-0.5 MPa, preferably 0.35-0.45 MPa, during the reaction.
5. The method for preparing polyetherimide according to claim 1, characterized in that, In step (d), exhaust is performed at 330-380°C, preferably 350-370°C.
6. The method for preparing polyetherimide according to claim 1, characterized in that, After refilling in step (e), the pressure is 0.45-0.55 MPa.
7. The method for preparing polyetherimide according to claim 1, characterized in that, The aromatic diether anhydride is selected from bisphenol A type dianhydride, diphenyl ether type dianhydride, diphenyl sulfide type dianhydride, benzophenone type dianhydride, diphenyl sulfone type dianhydride or other dianhydrides, preferably bisphenol A type dianhydride.
8. The method for preparing polyetherimide according to claim 1, characterized in that, The diamine is selected from at least one of aliphatic diamines, alicyclic diamines, and aromatic diamines.
9. A polyetherimide, characterized in that, It is prepared by any one of the preparation methods of claims 1-8.
10. A polyetherimide component, characterized in that, The polyetherimide therein is prepared by any one of the preparation methods of claims 1-8.
Citation Information
Patent Citations
Process for the production of polyetherimides
CN105121511A
Melt polymerization method for polyetherimides
CN111133031A