A method for removing alkali metals from electrolytic aluminum liquid

By using silicon tetrachloride gas to decompose and generate silicon dioxide particles and chlorine gas under high temperature and micro-oxygen conditions, the carbon pollution and chlorine volume instability problems in the removal of alkali metals and alkaline earth metals in the prior art are solved, and the purification of aluminum liquid with high efficiency and environmental protection is achieved.

CN121496499BActive Publication Date: 2026-11-17ZHEJIANG QIAOLAOYE ALUMINIUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511853850.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-10
Publication Date
2026-11-17
Estimated Expiration
2045-12-10

AI Technical Summary

Technical Problem

Existing technologies for removing alkali and alkaline earth metals from molten aluminum suffer from carbon pollution and environmental pollution and equipment corrosion caused by unstable chlorine gas volume.

Method used

Silicon tetrachloride gas is decomposed under high temperature and low oxygen conditions to produce silicon dioxide particles and chlorine gas. Taking advantage of the fact that the density of silicon dioxide particles is less than that of molten aluminum, they float to the surface to form a slag layer. Chlorine gas reacts with alkali metals to generate chlorides that are enriched in the slag layer, thus avoiding the introduction of carbon and hydrogen.

Benefits of technology

It effectively removes alkali and alkaline earth metals from molten aluminum, avoiding the degradation of aluminum product performance caused by carbon and hydrogen, and reducing environmental pollution and equipment corrosion risks.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This disclosure relates to the field of impurity removal technology for electrolytic aluminum, specifically a method for removing alkali metals from molten aluminum. The method includes the following: in a closed reaction apparatus containing molten aluminum, silicon tetrachloride gas is injected into the molten aluminum through a gas inlet located at the bottom of the closed reaction apparatus. This disclosure innovatively utilizes silicon tetrachloride gas obtained after preheating the silicon tetrachloride liquid to remove alkali metals and alkaline earth metals from the molten aluminum; the silicon tetrachloride gas decomposes under high temperature and low oxygen conditions to produce silica particles and chlorine gas; this disclosure utilizes the characteristic that the density of silica particles is less than that of aluminum, causing the silica particles to float to the surface of the molten aluminum and form slag; furthermore, silicon tetrachloride itself does not contain C and H, thus avoiding the introduction of C and H that would degrade the performance of the aluminum product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of impurity removal technology in electrolytic aluminum, specifically a method for removing alkali metals from electrolytic aluminum liquid. Background Technology

[0002] The alkali and alkaline earth metals in molten aluminum mainly originate from the alkali and alkaline earth metal elements produced during aluminum electrolysis, such as Na, Li, and Ca. They also come from fluxes used in aluminum alloys. These fluxes are generally composed of chlorides and fluorides of alkali and alkaline earth metals, with key components including KCl, NaCl, NaF, CaF, Na3AlF6, and Na2SiF6. After using flux, these alkali and alkaline earth metals remain in the melt. Taking sodium as an example, sodium is almost insoluble in aluminum, with a maximum solid solubility of less than 0.0025%. In Al-Mg alloys, when the magnesium content exceeds 2%, magnesium abstracts silicon, precipitating free sodium. During solidification, sodium exists at grain boundaries. During plastic deformation, due to its low melting point, it reverts to a free state, thus forming crack initiation points. As the deformation increases, these cracks converge and form open fractures, a phenomenon known as sodium embrittlement. Calcium in aluminum alloys forms new phases, CaAl4 and CaAl2, with aluminum. The formation of these new phases reduces the amount of strengthening phases in the aluminum alloy. These new phases are insoluble in the aluminum matrix and cannot undergo precipitation strengthening. Therefore, calcium in aluminum alloys reduces the as-cast hardness, and as the calcium content increases, the hardness of the aluminum alloy after heat treatment also decreases. Furthermore, Ca reduces the fluidity of the molten aluminum alloy, making it more prone to gas absorption and the formation of microscopic pinholes or porosity. In severe cases, it can produce segregated hard and brittle compounds, significantly increasing the scrap rate of castings and reducing the heat treatment strengthening effect of the aluminum alloy.

[0003] In the existing technology, the method to remove alkali metals from aluminum melt is to use chlorine gas, chlorine-containing refining agents (such as hexachloroethane, carbon tetrachloride, etc.) or fluoride-containing refining agents in a holding furnace to refine the melt. Common chlorine-containing refining agents inevitably have the following disadvantages: (1) Organic substances such as hexachloroethane and carbon tetrachloride inevitably produce carbon pollution and form a new Al4Cl3 phase; (2) As a liquid, carbon tetrachloride releases chlorine gas in a volume much larger than its own volume, which will cause explosive release. A large amount of chlorine gas cannot react completely and leaves the aluminum melt, which not only leads to waste and environmental pollution, but also causes corrosion of the reaction device and affects its service life. Summary of the Invention

[0004] This disclosure provides a method for removing alkali metals from electrolytic aluminum liquid to address the shortcomings of related technologies.

[0005] According to a first aspect of the present disclosure, a method for removing alkali metals from electrolytic aluminum liquid is provided, the method comprising the following: In a closed reaction apparatus containing molten aluminum, silicon tetrachloride gas is injected into the molten aluminum through a gas inlet located at the bottom of the closed reaction apparatus.

[0006] In one aspect of this disclosure, the atmosphere within the sealed reaction apparatus may be a mixture of argon and oxygen; the partial pressure of the oxygen is 10. -8 Up to 10 -6 atm; the volume fraction of oxygen is 0.001-0.015% of the integral of argon gas.

[0007] In one aspect of the embodiments of this disclosure, the atmosphere in the closed reaction device may be a mixture of carbon dioxide and carbon monoxide; the volume ratio of carbon monoxide to carbon dioxide is selected from (75-85):(15-25).

[0008] In one aspect of this disclosure, the atmosphere within the sealed reaction apparatus may be pure argon.

[0009] In one aspect of this disclosure, the silicon tetrachloride gas is pre-dried and heated, and the purity of the silicon tetrachloride gas is ≥99.9%, and it does not contain organic solvents or water.

[0010] In one aspect of this disclosure, the silicon tetrachloride gas decomposes in a high-temperature, low-oxygen environment to produce silicon dioxide particles and chlorine gas; the density of the silicon dioxide particles is less than that of the molten aluminum, forming a slag layer on the surface of the molten aluminum. Chlorine reacts with floating alkali and alkaline earth metals to form chlorides, the density of which is less than that of molten aluminum, and the chlorides are enriched in the slag layer.

[0011] In one aspect of the embodiments of this disclosure, the sealed reaction device is a sealed heat-insulating bag; the top of the sealed heat-insulating bag is provided with a gas outlet and a slag outlet; the bottom of the sealed heat-insulating bag is provided with a gas inlet and a liquid outlet.

[0012] In one aspect of this disclosure, the silicon tetrachloride gas is preheated to 100°C-150°C to prevent localized overcooling of the electrolytic aluminum liquid.

[0013] In one aspect of this disclosure, the processing temperature of the electrolytic aluminum liquid is selected from 730℃-750℃; the processing time is selected from 5-10 min.

[0014] In one aspect of this disclosure, the mixed gas discharged from the gas outlet is condensed to recover silicon tetrachloride.

[0015] Compared with the prior art, the beneficial effects of this disclosure are: This disclosure creatively utilizes silicon tetrachloride gas obtained by preheating silicon tetrachloride liquid to remove alkali metals and alkaline earth metals from electrolytic aluminum liquid; the silicon tetrachloride gas decomposes under high temperature and micro-oxygen conditions to produce silicon dioxide particles and chlorine gas; this disclosure utilizes the characteristic that the density of silicon dioxide particles is less than that of aluminum, causing the silicon dioxide particles to float to the surface of the aluminum liquid and form slag; furthermore, silicon tetrachloride itself does not contain C and H; it avoids the introduction of C and H causing a decrease in the performance of aluminum products. Detailed Implementation

[0016] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. The embodiments described herein are illustrative in nature and are used to provide a basic understanding of this application. The embodiments of this application should not be construed as limiting this application.

[0017] For the sake of brevity, this article only discloses a few specific numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0018] In this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0019] In this disclosure, under high-temperature, oxygen-free conditions, SiCl4 is difficult to decompose into Si and Cl2, and it remains essentially stable in molten aluminum; however, under high-temperature, low-oxygen conditions (oxygen partial pressure approximately 10), SiCl4 is difficult to decompose into Si and Cl2, and it remains relatively stable in molten aluminum. -6 Under the conditions of atm), the main reaction is: SiCl4 + 2O2 → SiO2(s) + 2Cl2(g), ΔG = -450 kJ / mol; while the side reaction is: SiCl4 → Si(s) + 2Cl2(g), ΔG = +85 kJ / mol (suppressed); since silicon dioxide and aluminum do not react, the method used in this disclosure introduces almost no silicon impurities.

[0020] In this disclosure, the partial pressure of oxygen is 10. -8 Up to 10 -6 atm; specifically, it can be 1×10 -6 atm, 5×10 -7 atm, 8×10 -7 atm, 2.5×10 -7 atm, 10 -7 atm, etc.

[0021] In this disclosure, the volume fraction of oxygen is 0.001-0.015% of the volume fraction of argon gas; specifically, it can be 0.001%, 0.005%, 0.010%, or 0.015%.

[0022] In this disclosure, the rate of silicon tetrachloride gas introduced after drying and heating can be 5-20 L / min; however, this disclosure is not limited to this; it can be specifically set according to the size of the reaction apparatus and the amount of molten aluminum.

[0023] In this disclosure, silicon tetrachloride gas is preheated to 100°C-150°C to prevent localized overcooling of the electrolytic aluminum liquid; specifically, it can be preheated to 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, or 150°C; this disclosure is not limited thereto.

[0024] In this disclosure, the density of the generated silica particles is 2.2 g / cm³. 3 The chlorine gas automatically floats to the surface of the molten aluminum to form a slag layer; the chlorine gas reacts with the floating sodium, potassium and calcium metals to generate chlorides, which are enriched in the slag layer; the tail gas after the reaction is condensed and recovered, and the increase in silicon in the molten aluminum is controlled within 10 ppm, and the sodium, potassium and calcium contents are all ≤5 ppm.

[0025] In this disclosure, the slag layer is removed by skimming.

[0026] In this disclosure, the treatment temperature of the electrolytic aluminum liquid is selected from 730℃-750℃, specifically 730℃, 735℃, 740℃, 745℃, or 750℃. The treatment time of the electrolytic aluminum liquid is selected from 5-10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes; more specifically, the treatment temperature of the electrolytic aluminum liquid is 740℃, and the treatment time is 10 minutes.

[0027] In this disclosure, the oxygen flow rate within the reaction apparatus is precisely regulated by a mass flow controller.

[0028] In this disclosure, the mixed gas discharged from the top of the reaction device is condensed to recover silicon tetrachloride, and the uncondensed gas is absorbed by alkaline solution to remove chlorine. The argon gas is then returned to the reactor for reuse via a circulating pump.

[0029] The present disclosure will be further described below by way of specific embodiments.

[0030] Example 1 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet, slag outlet and oxygen sensor interface at the top, and a gas inlet and liquid outlet at the bottom.

[0031] Argon: Purity ≥ 99.999%, dried by molecular sieve before use; Oxygen: Purity ≥ 99.9%, precisely regulated by mass flow controller (MFC); Oxygen volume fraction: 0.0010% (oxygen partial pressure pO2 = 8 × 10⁻⁶). -7 SiCl4 is stored in a liquid storage tank made of 316L stainless steel, with a built-in molecular sieve desiccant. The SiCl4 is preheated to 125±5℃ using a vaporizer to obtain SiCl4 gas, and the SiCl4 gas flow rate is controlled at approximately 20L / min using a gas flow valve.

[0032] 300 kg of molten aluminum was poured into the insulation bag, sealed, and then evacuated to 10 Pa. An argon-oxygen mixture was then introduced. Heating was started, and the temperature of the molten aluminum was stabilized at 740 ± 2 °C. The bottom gas inlet was opened, and SiCl4 gas was injected through the gas flow valve. After 5 minutes of injection, the injection was stopped, and the mixture was allowed to stand for 5 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0033] The composition of the molten aluminum was determined using ICP-OES: Na was 2.8 ppm, Ca was 1.5 ppm, and Si increased by 3.2 ppm. The slag layer was analyzed using a LECO analyzer, revealing a NaCl + CaCl2 content of approximately 12 wt% and a SiO2 content of approximately 82%.

[0034] Example 2 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet and slag outlet at the top, and a gas inlet and liquid outlet at the bottom.

[0035] Argon: purity ≥99.999%, used after being dried by molecular sieve; SiCl4 is stored in a liquid storage tank made of 316L stainless steel with built-in molecular sieve desiccant; SiCl4 is preheated to 125±5℃ using a vaporizer to obtain SiCl4 gas, and the SiCl4 gas flow rate is controlled to be about 20L / min using a gas flow valve.

[0036] 300 kg of molten aluminum was poured into the insulation bag, sealed, and then evacuated to 10 Pa before being filled with argon gas. Heating was started to stabilize the temperature of the molten aluminum at 740 ± 2 °C. The gas inlet at the bottom was opened, and SiCl4 gas was injected through the gas flow valve. After 5 minutes of injection, the injection was stopped, and the mixture was allowed to stand for 5 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0037] The composition of the molten aluminum was determined by ICP-OES: Na was 66.7 ppm, Ca was 23.5 ppm, and Si increased by 14.2 ppm.

[0038] Example 3 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet, slag outlet and oxygen sensor interface at the top, and a gas inlet and liquid outlet at the bottom.

[0039] Argon: Purity ≥ 99.999%, dried by molecular sieve before use; Oxygen: Purity ≥ 99.9%, precisely regulated by mass flow controller (MFC); Oxygen volume fraction: 0.0010% (oxygen partial pressure pO2 = 8 × 10⁻⁶). -7 SiCl4 is stored in a liquid storage tank made of 316L stainless steel, with a built-in molecular sieve desiccant. The SiCl4 is preheated to 125±5℃ using a vaporizer to obtain SiCl4 gas, and the SiCl4 gas flow rate is controlled at approximately 20L / min using a gas flow valve.

[0040] 300 kg of molten aluminum was poured into the insulation bag, sealed, and then evacuated to 10 Pa. An argon-oxygen mixture was then introduced. Heating was started, and the temperature of the molten aluminum was stabilized at 770 ± 2 °C. The bottom gas inlet was opened, and SiCl4 gas was injected through the gas flow valve. After 5 minutes of injection, the injection was stopped, and the mixture was allowed to stand for 5 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0041] The composition of the molten aluminum was determined using ICP-OES: Na was 4.2 ppm, Ca was 1.9 ppm, and Si increased by 4.0 ppm. The slag layer was analyzed using a LECO analyzer, revealing a NaCl + CaCl2 content of approximately 11 wt% and a SiO2 content of approximately 83%.

[0042] Example 4 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet, slag outlet and oxygen sensor interface at the top, and a gas inlet and liquid outlet at the bottom.

[0043] Argon: Purity ≥ 99.999%, dried by molecular sieve before use; Oxygen: Purity ≥ 99.9%, precisely regulated by mass flow controller (MFC); Oxygen volume fraction: 0.0010% (oxygen partial pressure pO2 = 8 × 10⁻⁶). -7SiCl4 is stored in a liquid storage tank made of 316L stainless steel, with a built-in molecular sieve desiccant. The SiCl4 is preheated to 125±5℃ using a vaporizer to obtain SiCl4 gas, and the SiCl4 gas flow rate is controlled at approximately 20L / min using a gas flow valve.

[0044] 300 kg of molten aluminum was poured into the insulation bag, sealed, and then evacuated to 10 Pa. An argon-oxygen mixture was then introduced. Heating was started, and the temperature of the molten aluminum was stabilized at 710 ± 2 °C. The bottom gas inlet was opened, and SiCl4 gas was injected through the gas flow valve. After 5 minutes of injection, the injection was stopped, and the mixture was allowed to stand for 5 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0045] The composition of the molten aluminum was determined using ICP-OES: Na was 5.4 ppm, Ca was 2.7 ppm, and Si increased by 3.6 ppm. The slag layer was analyzed using a LECO analyzer, revealing a NaCl + CaCl2 content of approximately 11 wt% and a SiO2 content of approximately 83%.

[0046] Comparative Example 1 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet, slag outlet and graphite tube at the top, and a liquid discharge port at the bottom.

[0047] Argon: purity ≥99.999%, dried with molecular sieve before use; carbon tetrachloride is injected into the molten aluminum via a graphite tube using a dripping method. A pumping system is used to maintain a constant flow rate; the dripping volume is controlled at 450g, and the dripping time is controlled at 12 minutes (to prevent burst release). A graphite tube with an inner diameter of 8mm is used, inserted to a depth of 125mm from the bottom of the ladle.

[0048] 300 kg of molten aluminum was injected into the insulation bag, sealed, and evacuated to 10 Pa before being filled with argon gas. Heating was started to stabilize the temperature of the molten aluminum at 740 ± 2 °C. The pumping system was turned on to maintain a constant flow rate. The dripping volume was controlled at 450 g, and the dripping time was controlled at 12 minutes. Carbon tetrachloride was injected through a graphite tube. After 12 minutes, the injection was stopped, and the mixture was allowed to stand for 8 minutes. The slag layer on the surface was then removed by opening the slag port.

[0049] The composition of the molten aluminum was determined by ICP-OES: Na was 12.0 ppm, Ca was 9.5 ppm, and the increase in C was 20.6 ppm.

[0050] Comparative Example 2 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet and slag outlet at the top, and a gas inlet and liquid outlet at the bottom.

[0051] Argon: purity ≥99.999%, used after being dried by molecular sieve; carbon tetrachloride is stored in a liquid storage tank made of 316L stainless steel with built-in molecular sieve desiccant; carbon tetrachloride is preheated to 105±5℃ using a vaporizer to obtain carbon tetrachloride gas, and the flow rate of carbon tetrachloride gas is controlled at about 20L / min using a gas flow valve.

[0052] 300 kg of molten aluminum was poured into the insulation bag, sealed, and then evacuated to 10 Pa before being filled with argon gas. Heating was started to stabilize the temperature of the molten aluminum at 740 ± 2 °C. The gas inlet at the bottom was opened, and carbon tetrachloride gas was injected through the gas flow valve. After 5 minutes of injection, the injection was stopped, and the mixture was allowed to stand for 5 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0053] The composition of the molten aluminum was determined by ICP-OES: Na was 15.4 ppm, Ca was 11.7 ppm, and the increase in C was 14.6 ppm.

[0054] Comparative Example 3 It adopts a 500L sealed insulation bag, lined with silicon nitride refractory material, with a gas outlet and slag outlet at the top, a liquid discharge outlet at the bottom, and a closed screw feeder in the middle.

[0055] Argon: purity ≥99.999%, dried by molecular sieve before use; hexachloroethane is added to the molten aluminum via a closed screw feeder. A pumping system is used to maintain a constant feed rate; the total mass of the material is controlled at 400g, and the feeding time is controlled at 8 minutes (to prevent burst release).

[0056] 300 kg of molten aluminum was injected into the insulation bag, sealed, and then evacuated to 10 Pa before being filled with argon gas. Heating was started to stabilize the temperature of the molten aluminum at 740 ± 2 °C. The pumping system was turned on to maintain a constant feeding rate. The total mass of the material was controlled at 400 g, and the feeding time was controlled at 8 minutes. Hexachloroethane was added to the molten aluminum through a closed screw feeder. After 8 minutes, the injection was stopped, and the mixture was allowed to stand for 6 minutes. The slag layer on the surface was then removed by opening the slag outlet.

[0057] The composition of the molten aluminum was determined by ICP-OES: Na was 9.5 ppm, Ca was 7.3 ppm, and the increase in C was 14.4 ppm.

[0058] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This disclosure is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein.

Claims

1. A method for removing alkali metals from electrolytic aluminum liquid, characterized in that, The method includes the following: In a closed reaction apparatus containing molten aluminum, silicon tetrachloride gas is injected into the molten aluminum through a gas inlet located at the bottom of the closed reaction apparatus. The atmosphere inside the sealed reaction device is a slightly oxygenated atmosphere formed by argon and oxygen; the partial pressure of the oxygen is 10. -8 Up to 10 -6 atm; the volume fraction of oxygen is 0.001-0.015% of the integral of argon gas; The silicon tetrachloride gas is pre-dried and heated, and the purity of the silicon tetrachloride gas is ≥99.9%, and it does not contain organic solvents or water; The sealed reaction device is a sealed insulated bag; the top of the sealed insulated bag is provided with a gas outlet and a slag outlet; the bottom of the sealed insulated bag is provided with a gas inlet and a liquid outlet. The silicon tetrachloride gas is preheated to 100℃-150℃ to prevent localized overcooling of the electrolytic aluminum liquid.

2. The method for removing alkali metals from electrolytic aluminum liquid according to claim 1, characterized in that, The treatment temperature of the electrolytic aluminum liquid is selected from 730℃-750℃; the treatment time is selected from 5-10min.

3. The method for removing alkali metals from electrolytic aluminum liquid according to claim 1, characterized in that, The mixed gas discharged from the gas outlet is condensed to recover silicon tetrachloride.