A self-circulating deodorization treatment process for hydrogen-containing organic waste gas
The self-circulating deodorization process using gradient-doped activated carbon and composite catalysts overcomes the limitations of traditional methods, achieving efficient, energy-saving, and environmentally friendly treatment of hydrogen-containing organic waste gas and ensuring stable treatment of waste gas during the production of 2-thiophene ethanol.
Patent Information
- Application Number
- CN202511680926.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-11-17
AI Technical Summary
Traditional methods for treating hydrogen-containing organic waste gas have limitations. For example, adsorption methods require frequent replacement of adsorbents, and combustion methods consume a lot of energy and may produce secondary pollutants. They cannot treat hydrogen-containing organic waste gas efficiently, energy-savingly, or in an environmentally friendly manner.
A composite catalyst is used for self-circulating deodorization treatment, including gradient-doped activated carbon, a Pt-Pd alloy nanoparticle layer and a La2O3-Al2O3 composite oxide shell. Volatile organic compounds are decomposed and transformed through catalytic self-circulating reaction, combined with pretreatment by a plate absorption tower and ultraviolet photodegradation.
It achieves efficient removal of VOCs and odor substances from exhaust gas, reduces operating costs, improves treatment efficiency, and maintains stable performance under fluctuating humidity and sulfur content.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of waste gas treatment technology, specifically to a self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Background Technology
[0002] 2-Thiophene ethanol is a traditional Chinese medicine organic intermediate used in the synthesis of platelet aggregation inhibitors and thiophenepicillin-type drugs for antithrombosis. As a fine chemical product with important applications, 2-thiophene ethanol has promising prospects. The main synthesis processes can be summarized as follows: ① Butyllithium process: Thiophene reacts with butyllithium to achieve metal substitution, then reacts with ethylene oxide, and finally hydrolyzes to obtain the target product; however, the reaction conditions are harsh, and the yield is only 79%; ② Grignard reagent process: Thiophene is used as a raw material, undergoing bromination and Grignard reaction to obtain a Grignard reagent, which then reacts with ethylene oxide and undergoes hydrolysis to obtain the target product, achieving a yield of 80%; however, the reaction conditions are harsh and unsuitable for large-scale industrial application; ③ Ester reduction process: 2-Thiophene acetate is used as a raw material, sodium borohydride is used as a reducing agent, and a quaternary ammonium salt is used as a phase transfer catalyst for reduction. The yield is low, and the reducing agent sodium borohydride is expensive, resulting in high costs.
[0003] Currently, to address the problems of stringent experimental conditions and expensive raw materials in the synthesis of 2-thiophene ethanol, which make it unsuitable for industrial production, traditional production processes have been improved and optimized. The process involves: preparing a mixed system containing sodium sand using sodium blocks as raw material; adding thiophene, isoprene, etc., to the sodium sand-containing mixed system for a metallization reaction; then adding ethylene oxide for epoxidation, hydrolysis, acid washing, water washing, atmospheric distillation, vacuum distillation, and high-vacuum distillation to obtain 2-thiophene ethanol. The waste gas generated during the process mainly comes from synthesis, distillation, and extraction / stratification. Based on the waste gas concentration and whether it contains hydrogen, it is classified into three categories: hydrogen-containing waste gas, low-concentration waste gas, and high-concentration process waste gas. Given the hazardous nature of hydrogen-containing waste gas, it is not included in the main waste gas pipeline and is not treated by RTO incineration; instead, the hydrogen-producing process waste gas needs to be collected, treated, and discharged separately. This hydrogen-containing waste gas contains hydrogen as well as volatile organic compounds such as toluene, tetrahydrofuran, isoprene, thiophene, 2-methyl-1-butene, 1,2-dimethylcyclopropane, ethylene oxide, and 2-thiophene ethanol. Effective control measures are needed to improve the plant environment. Currently, traditional methods for treating hydrogen-containing organic waste gas have many limitations. For example, while adsorption can effectively remove organic pollutants from waste gas, the adsorbent is easily saturated and requires frequent replacement, resulting in high operating costs. Combustion, while converting organic pollutants into carbon dioxide and water, consumes a large amount of energy and may produce secondary pollutants such as nitrogen oxides. Therefore, developing a highly efficient, energy-saving, and environmentally friendly process for treating hydrogen-containing organic waste gas is urgently needed. Summary of the Invention
[0004] The purpose of this invention is to provide a self-circulating deodorization treatment process for hydrogen-containing organic waste gas, solving the following technical problems:
[0005] Traditional methods for treating hydrogen-containing organic waste gas have many limitations.
[0006] The objective of this invention can be achieved through the following technical solutions:
[0007] A self-circulating deodorization treatment process for hydrogen-containing organic waste gas includes the following steps:
[0008] S1: Hydrogen-containing organic waste gas is pretreated by a plate absorption tower to obtain pretreated waste gas;
[0009] S2: The pretreated waste gas is subjected to a catalytic self-circulation reaction to obtain pre-purified waste gas;
[0010] S3: The pre-purified waste gas undergoes further treatment to complete the self-circulating deodorization process;
[0011] The catalytic self-circulating reaction involves the recycling of pretreated waste gas using a composite catalyst.
[0012] The preparation method of the composite catalyst includes the following steps:
[0013] S1: Place the activated carbon in Ce 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 2-4 hours, then dry; then place in Ce 4+ / Zr 4+ The activated carbon was impregnated in a low-concentration impregnation solution at room temperature for 4-8 hours, dried, and calcined under a nitrogen atmosphere to obtain gradient-doped activated carbon.
[0014] S2: Gradient-doped activated carbon is immersed in an active solution containing Pt(NO3)2, Pd(NO3)2, La(NO3)3·6H2O, and Al(NO3)3·9H2O, and then dried; it is then placed in a microwave plasma reaction chamber for reduction treatment to obtain the core-shell material.
[0015] S3: Methyltriethoxysilane and anhydrous ethanol are mixed and sprayed onto the surface of the core-shell material, cured under a nitrogen atmosphere, crushed and sieved to obtain a composite catalyst.
[0016] As a further aspect of the present invention, the specific steps of the curing treatment under a nitrogen atmosphere are as follows: treatment at 100-120°C for 2-4 hours under a nitrogen atmosphere.
[0017] As a further aspect of the present invention: Ce 4+ / Zr 4+The preparation method of high-concentration impregnation solution includes the following steps: Ce(NO3)4·6H2O, Zr(NO3)4·5H2O, and deionized water are mixed, and 5wt% nitric acid solution is added to adjust the pH to 2-3 to obtain Ce. 4+ / Zr 4+ High-concentration impregnation solution; Ce 4+ / Zr 4+ The mass ratio of Ce(NO3)4·6H2O to Zr(NO3)4·5H2O in the high-concentration impregnation solution is 1:1; per milliliter of Ce 4+ / Zr 4+ The high-concentration impregnation solution contained 15 mg of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O; activated carbon and Ce 4+ / Zr 4+ The solid-liquid ratio of the high-concentration impregnation solution is 1g:8-10mL;
[0018] Ce 4+ / Zr 4+ The preparation method of low-concentration impregnation solution includes the following steps: Ce(NO3)4·6H2O, Zr(NO3)4·5H2O, and deionized water are mixed, and 5wt% nitric acid solution is added to adjust the pH to 2-3 to obtain Ce. 4+ / Zr 4+ Low concentration impregnation solution; Ce 4+ / Zr 4 + The mass ratio of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in the low-concentration impregnation solution is 1:1; per milliliter of Ce 4+ / Zr 4+ The low-concentration impregnation solution contained 5 mg of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O; activated carbon and Ce 4+ / Zr 4+ The solid-liquid ratio of the low-concentration impregnation solution is 1g:8-10mL.
[0019] As a further aspect of the present invention: the active solution comprises the following raw materials by weight percentage: 0.81%-1.35% Pt(NO3)2, 0.92%-1.54% Pd(NO3)2, 3.05%-4.58% La(NO3)3·6H2O, 2.37%-3.56% Al(NO3)3·9H2O, with the balance being deionized water, and the sum of the weight percentages of the raw materials is 100%; the solid-liquid ratio of the gradient-doped activated carbon to the active solution is 1g:6-8mL.
[0020] As a further aspect of the present invention: the impregnation treatment in S2 is specifically: ultrasonic-assisted co-impregnation for 1-2 hours; the reduction treatment in S2 is specifically: reduction in an argon atmosphere at a pressure of 0.04-0.06 MPa and a power of 300-500 W for 10-30 minutes.
[0021] As a further embodiment of the present invention: the addition ratio of methyltriethoxysilane, anhydrous ethanol, and core-shell material in S3 is 0.4-0.8g: 10-20mL: 100g.
[0022] As a further aspect of the present invention, the method for preparing activated carbon includes the following steps: ultrasonically soaking activated carbon in nitric acid solution, washing with water, and drying to obtain activated carbon.
[0023] As a further aspect of the present invention: the temperature of the self-circulating reaction is 220-300℃ and the pressure is 0.1-0.3MPa; the pretreated waste gas circulates and stays in the reaction device storing the composite catalyst for 30-40 minutes.
[0024] As a further embodiment of the present invention: the plate absorption tower is a 6-8 layer sieve plate tower; the specific steps of the pretreatment are: spraying the pretreatment liquid from the distributor at the top of the tower absorption tower, and making it cross-flow contact with the hydrogen-containing organic waste gas entering from the bottom of the tower.
[0025] As a further aspect of the present invention: the liquid-to-gas ratio of the pretreatment liquid to the hydrogen-containing organic waste gas is controlled at 3-5 L / m³. 3 The pretreatment solution comprises the following raw materials by weight percentage: 10%-15% weak alkaline component, 0.5-1% rhamnolipid, 0.1%-0.3% disodium ethylenediaminetetraacetate, 0.01-0.03% polydimethylsiloxane defoamer, and the balance being deionized water; the sum of the raw material percentages is 100%.
[0026] The weak alkaline component is either sodium hydroxide or sodium carbonate; the defoamer is a polydimethylsiloxane defoamer.
[0027] As a further aspect of the present invention, the preparation method of the pretreatment solution includes the following steps: adding deionized water and a weak alkali to a stirred tank and stirring to dissolve; adding rhamnolipid and stirring to disperse; adding disodium ethylenediaminetetraacetate and an antifoaming agent and stirring to disperse; filtering to obtain the pretreatment solution. The pretreatment solution specifically absorbs ethylene oxide, rhamnolipid enhances the solubility of thiophene, and disodium ethylenediaminetetraacetate prevents component stratification and failure.
[0028] The specific steps for stirring and dissolving are as follows: heat to 50-60℃, stir at 200-300r / min for 30-40 minutes.
[0029] The specific stirring and dispersion process is as follows: at room temperature, stir at a speed of 200-300 r / min for 15-20 min.
[0030] As a further aspect of the present invention, the deep treatment includes ultraviolet photodegradation.
[0031] As a further aspect of the present invention: the wavelength of ultraviolet photolysis is 185nm-254nm, and the irradiation time is 5-10min.
[0032] The beneficial effects of this invention are:
[0033] (1) Plate absorption tower for pretreatment of hydrogen-containing waste gas
[0034] This application first passes hydrogen-containing waste gas through a plate absorption tower, employing a cross-flow contact method. The pretreatment liquid is evenly sprayed from a distributor at the top of the tower onto each layer of sieve plates. The hydrogen-containing waste gas enters from the bottom of the tower and rises layer by layer, forming sufficient gas-liquid contact with the pretreatment liquid on the sieve plates. The pretreatment liquid contains various active ingredients that can chemically react with some water-soluble pollutants in the waste gas (especially ethylene oxide), dissolving and removing them. Simultaneously, gas-liquid heat exchange achieves cooling and humidification of the waste gas, creating suitable conditions for subsequent self-circulation reactions.
[0035] (2) Gradient doping of Ce on the surface of activated carbon after activation 4+ -Zr 4+
[0036] This application utilizes nitric acid to activate activated carbon, generating a large number of oxygen-containing functional groups (such as hydroxyl and carboxyl groups) on the surface, providing anchor sites for subsequent adsorption and coordination of metal ions. This application also utilizes Ce... 4+ -Zr 4+ High concentration impregnation solution, Ce 4+ -Zr 4+ Low-concentration impregnation solution is used to dope activated carbon to obtain gradient-doped activated carbon; the oxygen storage / release capacity of Ce-Zr solid solution is used to enhance the oxidative degradation of cyclic ether components; and gradient doping not only ensures the density of active sites on the surface, but also improves the interfacial bonding force between activated carbon and the Pt-Pd alloy nanoparticle layer / La2O3-Al2O3 composite oxide shell.
[0037] (3) A Pt-Pd alloy nanoparticle layer and a La2O3-Al2O3 composite oxide shell layer are sequentially deposited on the surface of gradient doped activated carbon.
[0038] This application involves impregnating graded-doped activated carbon with a Pt-containing... 2+ / Pd 2+ / La 3+ / Al 3+In the mixed solution of precursors, the surface of the gradient-doped activated carbon support is rich in oxygen-containing functional groups, and the Ce-Zr doping sites have strong electron attraction, which can preferentially capture Pt through electrostatic adsorption and coordination. 2+ / Pd 2+ This allows Pt to rapidly accumulate on the surface and shallow pores of the carrier, forming an active center enrichment region, and encapsulating Pt on the surface of the gradient-doped activated carbon. 2+ / Pd 2+ Core precursor; subsequently, La 3+ / Al 3+ Pt already adsorbed 2+ / Pd 2+ A loose precursor coating layer is formed on the outer side of the core region; and a continuous core-shell structure is formed under ultrasonic-assisted co-impregnation treatment; then microwave plasma reduction treatment is performed to first form a Pt-Pd alloy nanoparticle layer on the surface of gradient doped activated carbon, and then wrap it with a La2O3-Al2O3 composite oxide shell layer to obtain a core-shell material.
[0039] Pt-Pd alloy nanoparticle layers efficiently catalyze the reaction of toluene, isoprene, thiophene, etc.; La2O3-Al2O3 composite oxide shells contain La 3+ It preferentially combines with sulfur species to form stable La2S3, avoiding the combination of sulfur species with the active centers of Pt-Pd alloy nanoparticles; Al2O3 enhances the shell dispersion and structural stability, preventing shell agglomeration and blockage of active sites.
[0040] Methyltriethoxysilane is also used for hydrophobic treatment. This hydrophobic treatment is suitable for the humidity environment of hydrogen-containing waste gas after pretreatment, avoiding the decrease in activity caused by moisture adsorption and ensuring stable performance under fluctuating conditions of 2-thiophene ethanol production waste gas.
[0041] This application addresses the problems of catalyst poisoning caused by sulfur-containing components such as thiophene in 2-thiophene ethanol production waste gas, and the reluctance to degrade cyclic ethers such as tetrahydrofuran. It proposes a composite catalyst with a core-shell structure exhibiting sulfur resistance and gradient doping. The pretreated waste gas enters a self-circulating reaction device, where it comes into full contact with the composite catalyst. Under specific temperature and pressure conditions, a chemical reaction is initiated, decomposing and transforming volatile organic compounds (VOCs). Through multiple cycles of the reaction, the treatment efficiency of the waste gas is continuously improved, ensuring that VOCs and odorous substances are fully removed. Detailed Implementation
[0042] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0043] Example 1: The preparation method of the composite catalyst includes the following steps:
[0044] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0045] Ce(NO3)4·6H2O and Zr(NO3)4·5H2O were mixed with deionized water in a mass ratio of 1:1, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to prepare Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ Low concentration impregnation solution;
[0046] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0047] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:8mL. 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 2 hours, then dry at 100℃ for 2 hours; according to a solid-liquid ratio of 1g:6mL, then place in Ce... 4+ / Zr 4+ Gradient-doped activated carbon was obtained by impregnating in a low-concentration impregnation solution at room temperature for 4 hours, drying at 110℃ for 6 hours, and calcining at 350℃ under nitrogen atmosphere for 3 hours.
[0048] S2: Prepare an active solution according to the following raw material weight percentage ratio: 0.81% Pt(NO3)2, 1.54% Pd(NO3)2, 3.05% La(NO3)3·6H2O, 2.37% Al(NO3)3·9H2O, and 92.23% deionized water;
[0049] According to the solid-liquid ratio of gradient-doped activated carbon to activated solution of 1g:6mL, the gradient-doped activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h; then it was placed in a microwave plasma reaction chamber under argon flow rate of 50mL / min, pressure of 0.05MPa, and power of 500W for 15min to obtain the core-shell material.
[0050] S3: 0.4g of methyltriethoxysilane and 10mL of anhydrous ethanol were mixed and sprayed onto the surface of 100g of core-shell material. The mixture was cured at 100℃ for 2h under a nitrogen atmosphere, pulverized, and passed through a 40-mesh sieve to obtain the composite catalyst.
[0051] Example 2: The preparation method of the composite catalyst includes the following steps:
[0052] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0053] Ce(NO3)4·6H2O and Zr(NO3)4·5H2O were mixed with deionized water in a mass ratio of 1:1, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to prepare Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ Low concentration impregnation solution;
[0054] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0055] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:9mL. 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 3 hours, then dry at 100℃ for 2 hours; according to a solid-liquid ratio of 1g:7mL, then place in Ce... 4+ / Zr 4+ Gradient-doped activated carbon was obtained by impregnating in a low-concentration impregnation solution at room temperature for 6 hours, drying at 110℃ for 6 hours, and calcining at 350℃ under nitrogen atmosphere for 3 hours.
[0056] S2: Prepare an active solution according to the following raw material weight percentage ratio: 1.14% Pt(NO3)2, 1.23% Pd(NO3)2, 3.67% La(NO3)3·6H2O, 2.96% Al(NO3)3·9H2O, and 91% deionized water;
[0057] According to the solid-liquid ratio of gradient-doped activated carbon to activated solution of 1g:7mL, the gradient-doped activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h. Then it was placed in a microwave plasma reaction chamber under argon flow rate of 50mL / min, pressure of 0.05MPa, and power of 500W for 15min to obtain the core-shell material.
[0058] S3: 0.6g of methyltriethoxysilane and 10mL of anhydrous ethanol were mixed and sprayed onto the surface of 100g of core-shell material. The mixture was cured at 110℃ for 3h under a nitrogen atmosphere, pulverized, and passed through a 40-mesh sieve to obtain the composite catalyst.
[0059] Example 3: The preparation method of the composite catalyst includes the following steps:
[0060] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0061] Ce(NO3)4·6H2O and Zr(NO3)4·5H2O were mixed with deionized water in a mass ratio of 1:1, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to prepare Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ Low concentration impregnation solution;
[0062] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0063] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:10mL. 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 4 hours, then dry at 100℃ for 2 hours; according to a solid-liquid ratio of 1g:8mL, then place in Ce... 4+ / Zr 4+ Gradient-doped activated carbon was obtained by impregnating in a low-concentration impregnation solution at room temperature for 8 hours, drying at 110℃ for 6 hours, and calcining at 350℃ under nitrogen atmosphere for 3 hours.
[0064] S2: Prepare the active solution according to the following raw material weight percentage ratio: 1.35% Pt(NO3)2, 1.54% Pd(NO3)2, 4.58% La(NO3)3·6H2O, 3.56% Al(NO3)3·9H2O, 88.97% deionized water;
[0065] According to the solid-liquid ratio of gradient-doped activated carbon to activated solution of 1g:8mL, the gradient-doped activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h; then it was placed in a microwave plasma reaction chamber under argon flow rate of 50mL / min, pressure of 0.05MPa, and power of 500W for 15min to obtain the core-shell material.
[0066] S3: 0.8g of methyltriethoxysilane and 10mL of anhydrous ethanol were mixed and sprayed onto the surface of 100g of core-shell material. The mixture was cured at 120℃ for 4h under a nitrogen atmosphere, pulverized, and passed through a 40-mesh sieve to obtain the composite catalyst.
[0067] Example 4: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas, comprising the following steps:
[0068] S1: Add 8572g of deionized water and 1500g of sodium carbonate to a stirred tank, control the temperature at 30℃, and stir at 200r / min until dissolved. Add 50g of rhamnolipid, raise the temperature to 50-60℃, and stir at 200r / min for 30min. Add 20g of disodium EDTA and 2g of defoamer, and stir at 200r / min for 20min at room temperature. Filter to obtain the pretreated solution.
[0069] The pretreatment liquid is sprayed from the top distributor of the 8-layer sieve plate tower, and comes into cross-flow contact with the hydrogen-containing organic waste gas entering from the bottom of the tower. The liquid-to-gas ratio of the pretreatment liquid to the hydrogen-containing organic waste gas is controlled at 4 L / m³. 3 The pretreated waste gas is obtained;
[0070] S2: The pretreated waste gas is passed into a self-circulating device equipped with the composite catalyst prepared in Example 1 for catalytic self-circulation reaction. The temperature of the self-circulation reaction is 270°C and the pressure is 0.2 MPa. The pretreated waste gas circulates and stays in the reaction device storing the composite catalyst for 40 minutes to obtain the initially purified waste gas.
[0071] S3: The pre-purified exhaust gas is irradiated with ultraviolet light with a wavelength of 185nm-254nm for 5 minutes to complete the self-circulating deodorization process.
[0072] Example 5: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, the only difference is that the composite catalyst prepared in Example 1 used in Example 4 is replaced with an equal amount of the composite catalyst prepared in Example 2. The remaining components and processes are completely consistent with Example 4.
[0073] Example 6: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, the only difference is that the composite catalyst prepared in Example 1 used in Example 4 is replaced in equal amounts with the composite catalyst prepared in Example 3. The remaining components and processes are completely consistent with Example 4.
[0074] Comparative Example 1: The preparation method of the composite catalyst includes the following steps:
[0075] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0076] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0077] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:9mL. 4+ / Zr 4+ The activated carbon was impregnated in a high-concentration impregnation solution at room temperature for 3 hours, dried at 100°C for 2 hours, and then calcined at 350°C in a nitrogen atmosphere for 3 hours to obtain doped activated carbon.
[0078] S2: Prepare an active solution according to the following raw material weight percentage ratio: 1.14% Pt(NO3)2, 1.23% Pd(NO3)2, 3.67% La(NO3)3·6H2O, 2.96% Al(NO3)3·9H2O, and 91% deionized water;
[0079] According to the solid-liquid ratio of doped activated carbon to activated solution of 1g:7mL, the doped activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h; then it was placed in a microwave plasma reaction chamber under argon flow rate of 50mL / min, pressure of 0.05MPa, and power of 500W for 15min to obtain the core-shell material.
[0080] S3: 0.6g of methyltriethoxysilane and 10mL of anhydrous ethanol were mixed and sprayed onto the surface of 100g of core-shell material. The mixture was cured at 110℃ for 3h under a nitrogen atmosphere, pulverized, and passed through a 40-mesh sieve to obtain the composite catalyst.
[0081] Comparative Example 2: The preparation method of the composite catalyst includes the following steps:
[0082] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0083] Ce(NO3)4·6H2O and Zr(NO3)4·5H2O were mixed with deionized water in a mass ratio of 1:1, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to prepare Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ Low concentration impregnation solution;
[0084] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0085] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:9mL. 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 3 hours, then dry at 100℃ for 2 hours; according to a solid-liquid ratio of 1g:7mL, then place in Ce... 4+ / Zr 4+ Gradient-doped activated carbon was obtained by impregnating in a low-concentration impregnation solution at room temperature for 6 hours, drying at 110℃ for 6 hours, and calcining at 350℃ under nitrogen atmosphere for 3 hours.
[0086] S2: Prepare an active solution according to the following raw material weight percentage ratio: 1.14% Pt(NO3)2, 1.23% Pd(NO3)2, and 97.63% deionized water;
[0087] According to the solid-liquid ratio of gradient-doped activated carbon to activated solution of 1g:7mL, the gradient-doped activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h. Then, it was placed in a microwave plasma reaction chamber under argon flow rate of 50mL / min, pressure of 0.05MPa, and power of 500W for 15min to obtain the composite material.
[0088] S3: 0.6g of methyltriethoxysilane and 10mL of anhydrous ethanol were mixed and sprayed onto the surface of 100g of composite material. The mixture was cured at 110℃ for 3h under a nitrogen atmosphere, pulverized, and passed through a 40-mesh sieve to obtain the composite catalyst.
[0089] The preparation method of the composite catalyst in Comparative Example 3 includes the following steps:
[0090] S1: Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in a mass ratio of 1:1 were mixed with deionized water, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to obtain Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ High-concentration impregnation solution;
[0091] Ce(NO3)4·6H2O and Zr(NO3)4·5H2O were mixed with deionized water in a mass ratio of 1:1, and the pH was adjusted to 2 by adding 5wt% nitric acid solution to prepare Ce(NO3)4·6H2O and Zr(NO3)4·5H2O per liter. 4+ / Zr 4+ Low concentration impregnation solution;
[0092] Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0093] Activated carbon was placed in Ce at a solid-liquid ratio of 1g:9mL. 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 3 hours, then dry at 100℃ for 2 hours; according to a solid-liquid ratio of 1g:7mL, then place in Ce... 4+ / Zr 4+ Gradient-doped activated carbon was obtained by impregnating in a low-concentration impregnation solution at room temperature for 6 hours, drying at 110℃ for 6 hours, and calcining at 350℃ under nitrogen atmosphere for 3 hours.
[0094] S2: Prepare an active solution according to the following raw material weight percentage ratio: 1.14% Pt(NO3)2, 1.23% Pd(NO3)2, 3.67% La(NO3)3·6H2O, 2.96% Al(NO3)3·9H2O, and 91% deionized water;
[0095] According to the solid-liquid ratio of gradient-doped activated carbon to active solution of 1g:7mL, the gradient-doped activated carbon was placed in the active solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h. Then, it was placed in a microwave plasma reaction chamber for reduction treatment at an argon flow rate of 50mL / min, a pressure of 0.05MPa, and a power of 500W for 15min. After pulverization and passing through a 40-mesh sieve, the composite catalyst was obtained.
[0096] The preparation method of the composite catalyst in Comparative Example 4 includes the following steps:
[0097] S1: Activated carbon (particle size 2mm, specific surface area 1000m²) 2 / g) was placed in a 5% nitric acid solution, ultrasonically soaked at 40kHz and 300W for 2h, washed with water until neutral, and dried at 110℃ for 4h to obtain activated carbon;
[0098] S2: Prepare an active solution according to the following raw material weight percentage ratio: 1.14% Pt(NO3)2, 1.23% Pd(NO3)2, and 97.63% deionized water;
[0099] According to the solid-liquid ratio of activated carbon to activated solution of 1g:7mL, the activated carbon was placed in the activated solution and ultrasonically impregnated at 40kHz and 300W for 60min, and then vacuum dried at 80℃ for 4h. Then, it was placed in a microwave plasma reaction chamber and reduced for 15min under an argon flow rate of 50mL / min, a pressure of 0.05MPa, and a power of 500W to obtain the composite catalyst.
[0100] Comparative Example 5: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, only the composite catalyst prepared in Example 1 used in Example 4 is replaced with an equal amount of the composite catalyst prepared in Comparative Example 1. The remaining components and processes are completely consistent with Example 4.
[0101] Comparative Example 6: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, only the composite catalyst prepared in Example 1 used in Example 4 is replaced in equal amounts with the composite catalyst prepared in Comparative Example 2. The remaining components and processes are completely consistent with Example 4.
[0102] Comparative Example 7: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, only the composite catalyst prepared in Example 1 used in Example 4 was replaced in equal amounts with the composite catalyst prepared in Comparative Example 3. The remaining components and processes were completely consistent with Example 4.
[0103] Comparative Example 8: A self-circulating deodorization treatment process for hydrogen-containing organic waste gas. Compared with Example 4, only the composite catalyst prepared in Example 1 used in Example 4 is replaced with an equal amount of the composite catalyst prepared in Comparative Example 4. The remaining components and processes are completely consistent with Example 4.
[0104] Performance testing
[0105] Simulated exhaust gas composition: H2 5%-10%, toluene 5%, tetrahydrofuran 8%, thiophene 3%, isoprene 4%, balance inert gas; the following indicators were tested:
[0106] (1) VOCs degradation efficiency: The concentrations of toluene, tetrahydrofuran, thiophene, and isoprene in the waste gas before and after treatment were determined by gas chromatography, and the degradation rate was calculated.
[0107] Degradation rate = (Initial concentration - Residual concentration) / Initial concentration × 100%
[0108] (2) Resistance to sulfur poisoning: After 100 hours of continuous operation, the retention value of the degradation rate of thiophene by the composite catalyst was measured:
[0109] Retention value = (Degradation rate after 100 hours / Initial degradation rate) × 100%
[0110] (3) Humidity adaptability: Under fluctuating operating conditions where the exhaust gas humidity (relative humidity) increases from 30% to 80%, the change range of tetrahydrofuran degradation rate was measured:
[0111] Variation range = [(Highest degradation rate - Lowest degradation rate) / Initial degradation rate] × 100%
[0112] (4) Specificity of cyclic ether degradation: Degradation rate of tetrahydrofuran was determined separately;
[0113] Table 1: Performance Test Data Statistics of Examples 4-6 and Comparative Examples 5-8
[0114]
[0115] As shown in Table 1, compared with Comparative Example 1, Examples 4-6 show that Comparative Example 1, due to the lack of gradient doping, has a lower degradation rate of cyclic ethers and a lower degradation rate of total VOCs. Furthermore, insufficient interfacial bonding leads to the shedding of the active layer, which indirectly reduces stability.
[0116] Compared to Comparative Example 2, Examples 4-6 show a decrease in the thiophene degradation rate retention value due to the absence of La2O3-Al2O3 in Comparative Example 2. The La2O3-Al2O3 composite oxide shell is the key to the long-term stable operation of the catalyst.
[0117] Compared to Comparative Example 3, Examples 4-6 show that Comparative Example 3, lacking hydrophobic treatment, exhibits a greater variation in tetrahydrofuran degradation rate under humidity fluctuations.
[0118] Compared to Comparative Example 4, Examples 4-6 lacked gradient doping, hydrophobic treatment, and the La2O3-Al2O3 composite oxide shell, resulting in a significant decrease in total VOCs degradation rate and extremely poor sulfur resistance and humidity adaptability.
[0119] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.
Claims
1. A self-circulating deodorization treatment process for hydrogen-containing organic waste gas, characterized in that, The process includes the following steps: A1: Hydrogen-containing organic waste gas is pretreated by a plate absorption tower to obtain pretreated waste gas; A2: The pretreated waste gas is subjected to a catalytic self-circulation reaction to obtain initially purified waste gas; A3: The pre-purified waste gas undergoes further treatment to complete the self-circulating deodorization process; The catalytic self-circulation reaction is a process in which the pretreated waste gas is recycled using a composite catalyst. The preparation method of the composite catalyst includes the following steps: S1: Place the activated carbon in Ce 4+ / Zr 4+ Immerse in a high-concentration impregnation solution at room temperature for 2-4 hours, then dry; then place in Ce 4+ / Zr 4+ The activated carbon was impregnated in a low-concentration impregnation solution at room temperature for 4-8 hours, dried, and calcined under a nitrogen atmosphere to obtain gradient-doped activated carbon. S2: Gradient-doped activated carbon is immersed in an active solution containing Pt(NO3)2, Pd(NO3)2, La(NO3)3·6H2O, and Al(NO3)3·9H2O, and then dried; it is then placed in a microwave plasma reaction chamber for reduction treatment to obtain the core-shell material. S3: Methyltriethoxysilane and anhydrous ethanol were mixed and sprayed onto the surface of the core-shell material, cured under a nitrogen atmosphere, crushed and sieved to obtain a composite catalyst. Ce 4+ / Zr 4+ The mass ratio of Ce(NO3)4·6H2O to Zr(NO3)4·5H2O in the high-concentration impregnation solution is 1:1; per milliliter of Ce 4+ / Zr 4+ The high-concentration impregnation solution contained 15 mg of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O; activated carbon and Ce 4+ / Zr 4+ The solid-liquid ratio of the high-concentration impregnation solution is 1g:8-10mL; Ce 4+ / Zr 4+ The mass ratio of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O in the low-concentration impregnation solution is 1:1; per milliliter of Ce 4+ / Zr 4 + The low-concentration impregnation solution contained 5 mg of Ce(NO3)4·6H2O and Zr(NO3)4·5H2O; activated carbon and Ce 4+ / Zr 4+ The solid-liquid ratio of the low-concentration impregnation solution is 1g:8-10mL; The method for preparing activated carbon includes the following steps: ultrasonically soaking activated carbon in nitric acid solution, washing with water, and drying to obtain activated carbon.
2. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The Ce 4 + / Zr 4+ The preparation method of high-concentration impregnation solution includes the following steps: Ce(NO3)4·6H2O, Zr(NO3)4·5H2O, and deionized water are mixed, and 5wt% nitric acid solution is added to adjust the pH to 2-3 to obtain Ce. 4+ / Zr 4+ High-concentration impregnation solution; The Ce 4+ / Zr 4+ The preparation method of low-concentration impregnation solution includes the following steps: Ce(NO3)4·6H2O, Zr(NO3)4·5H2O, and deionized water are mixed, and 5wt% nitric acid solution is added to adjust the pH to 2-3 to obtain Ce. 4+ / Zr 4+ Low-concentration impregnation solution.
3. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The active solution contains the following raw materials by weight percentage: 0.81%-1.35% Pt(NO3)2, 0.92%-1.54% Pd(NO3)2, 3.05%-4.58% La(NO3)3·6H2O, 2.37%-3.56% Al(NO3)3·9H2O, with the balance being deionized water. The sum of the raw material weight percentages is 100%. The solid-liquid ratio of the gradient-doped activated carbon to the active solution is 1g:6-8mL.
4. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The impregnation treatment in S2 is as follows: ultrasonic-assisted co-impregnation for 1-2 hours; the reduction treatment in S2 is as follows: reduction in an argon atmosphere at a pressure of 0.04-0.06 MPa and a power of 300-500 W for 10-30 minutes.
5. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The addition ratio of methyltriethoxysilane, anhydrous ethanol, and core-shell material in S3 is 0.4-0.8g: 10-20mL: 100g.
6. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The temperature of the self-circulating reaction is 220-300℃ and the pressure is 0.1-0.3MPa; the pretreated waste gas circulates and stays in the reaction device storing the composite catalyst for 30-40 minutes.
7. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The plate absorption tower is a 6-8 layer sieve plate tower; the specific steps of the pretreatment are: spraying the pretreatment liquid from the distributor at the top of the tower absorption tower, and making it cross-flow contact with the hydrogen-containing organic waste gas entering from the bottom of the tower.
8. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 7, characterized in that, The liquid-to-gas ratio of the pretreated liquid to the hydrogen-containing organic waste gas is controlled at 3-5 L / m³. 3 The pretreatment solution comprises the following raw materials by weight percentage: 10%-15% weak alkaline component, 0.5-1% rhamnolipid, 0.1%-0.3% disodium EDTA, 0.01-0.03% defoamer, and the balance being deionized water; the sum of the raw material percentages is 100%. The weak base component is either sodium hydroxide or sodium carbonate.
9. The self-circulating deodorization treatment process for hydrogen-containing organic waste gas according to claim 1, characterized in that, The deep processing includes ultraviolet photodegradation.
Citation Information
Patent Citations
Catalysts comprising substantially pure alpha-alumina carrier for treating exhaust gases
US5856263A
Catalyst composition
US5981427A