A heavy-duty bearing with a silver-copper bimetallic composite structure and its preparation method
By using green and blue light composite laser welding technology, the problem of difficult bonding at the silver-copper interface has been solved, achieving rapid heat dissipation and high-strength bonding in silver-copper bimetallic bearings, thereby improving the bearing's service life and wear resistance.
Patent Information
- Application Number
- CN202610063097.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-16
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-01-16
AI Technical Summary
In existing technologies, it is difficult to achieve atomic-level metallurgical bonding at the interface between silver and copper, resulting in poor heat dissipation performance of copper-silver bearings, which cannot meet the high-temperature requirements of heavy-duty bearings. Furthermore, traditional welding methods pose a risk of equipment damage.
The technology employs a composite laser welding technique using green and blue light. It utilizes green light with wavelengths of 500nm~560nm and blue light with wavelengths of 400nm~500nm as a composite light source to reduce the metal reflectivity, increase the absorption rate, achieve localized rapid heating and melting, and perform atomic-level metallurgical bonding. The blue laser power is then gradually reduced to assist in cooling.
This technology enables rapid heat dissipation and cooling of silver-copper bimetallic bearings, improves bonding strength, reduces equipment wear, and enhances bearing life and wear resistance.
Smart Images

Figure CN121649571B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bearing processing technology, and more specifically, to a heavy-duty bearing with a silver-copper bimetallic composite structure and its preparation method. Background Technology
[0002] In large, heavy-duty machinery, heavy-duty bearings often use high-strength steel or copper as the backing material for support, while softer materials like Babbitt metal and aluminum serve as bearing bushes to reduce friction and increase wear. During operation, the bearing temperature rises significantly, leading to substantial heat accumulation. Among commonly used metal bearings, copper, aluminum, iron, and tin have thermal conductivity values of 397 W / (m·K), 237 W / (m·K), 50 W / (m·K), and 60 W / (m·K), respectively. This shows that the thermal conductivity of different metals varies considerably or is generally low. This difference in thermal conductivity can easily lead to poor heat dissipation in bearings, causing heat accumulation. Furthermore, the viscosity of the lubricating oil inside the bearing decreases at high temperatures, posing a risk of failure. Therefore, in specialized fields such as national defense and military industries, bearing components with high thermal conductivity and good heat dissipation performance are crucial limiting factors.
[0003] The base and bearing shell of sliding bearings are primarily bimetallic composite structures. Currently, commonly used composite structures mainly use steel, copper, Babbitt metal, and aluminum. When two metals are combined, the difference in thermal conductivity leads to poor heat dissipation, posing a risk of failure at high temperatures. However, silver and copper composite bearings have similar thermal conductivity, both around 400 W / (m·K), with silver's thermal conductivity at 429 W / (m·K), not significantly different from copper. Both are high thermal conductivity materials, resulting in excellent heat dissipation. The combination of copper and silver, as materials for heavy-duty bearings, provides excellent heat dissipation and significantly extends service life. Therefore, this type of bimetallic composite bearing with excellent heat dissipation has unique advantages in specialized fields such as national defense.
[0004] However, this leads to the problem of bonding the copper-silver interface. Using traditional arc additive manufacturing methods, when depositing silver onto a copper substrate, the weld seam turns black and becomes unformed, making it impossible to weld. Brazing, a common method for joining dissimilar metals, is suitable for small parts. In the context of large-area composite silver-copper bearings, the capillary action of the brazing filler metal alone cannot meet the workpiece's bonding requirements. Furthermore, brazing is a difficult process and not suitable for this application. When using laser additive manufacturing, the high reflectivity of silver and copper at this wavelength, limited by the wavelength of ordinary lasers, makes it difficult to melt the interface and form an effective metallurgical bond. The high reflectivity can also damage equipment, such as causing severe lens burn-out. Ultimately, copper and silver cannot achieve atomic-level metallurgical bonding, failing to meet workpiece strength requirements and providing adequate heat dissipation, wear reduction, and durability.
[0005] Therefore, this invention is proposed to address the manufacturing challenges of copper-silver bearings and to solve the problem of difficult interface formation. Summary of the Invention
[0006] The purpose of this invention is to address the shortcomings of existing technologies by providing a heavy-duty bearing with a silver-copper bimetallic composite structure and its preparation method. Utilizing the high thermal conductivity of copper and silver, it achieves rapid heat dissipation and cooling, reduces thermal wear, and extends the service life of the workpiece. Composite laser welding is employed for additive manufacturing, significantly reducing the reflectivity of the two metals to the laser and increasing their absorption rate. Localized rapid heating and melting achieve the welding purpose, realizing atomic-level metallurgical bonding, improving the bimetallic bonding strength, and simultaneously reducing equipment wear.
[0007] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: A heavy-duty bearing with a silver-copper bimetallic composite structure, wherein the backing material of the bearing is copper and the bearing bush material is silver, is manufactured by additive manufacturing using green and blue light composite laser welding.
[0008] Furthermore, the backing material of the bearing is at least one of copper, brass, or bronze; the bearing bush material is high-silver material.
[0009] The preparation method of the above-mentioned heavy-duty bearing with silver-copper bimetallic composite structure includes the following steps: Step S1: Copper part machining and copper part surface treatment; Step S2: Fix the copper part on the welding platform, combine green laser and blue laser, use silver-based welding material, and perform composite laser welding additive manufacturing to obtain a silver-copper bimetallic composite structure. Step S3: The silver-copper bimetallic composite structure is finely processed to obtain the silver bearing layer.
[0010] Furthermore, in step S2, the composite laser consists of green light with a wavelength of 500nm~560nm and blue light with a wavelength of 400nm~500nm; the silver-based welding material is selected from silver-based welding wire, silver-based welding sheet, silver-based welding strip or silver-based welding powder.
[0011] Furthermore, in step S2, the silver-based welding material is pure Ag welding wire with a wire diameter of 1.0~2.4mm.
[0012] Furthermore, in step S2, the welding process adopts a coaxial wire feeding method, and the angle between the welding wire and the base material is between 35 and 60 degrees.
[0013] Furthermore, in step S2, the composite laser welding process is carried out in the form of reciprocating motion, and the overlap rate of adjacent welds is 10%~50%.
[0014] Furthermore, in step S2, the centers of the combined green and blue laser beams coincide, and the beam size and power of each laser beam can be adjusted independently.
[0015] Furthermore, the composite laser welding additive manufacturing in step S2 includes the following steps: Step S2.1, using composite laser welding to form the bottom layer; Step S2.2, continuing to use composite laser welding for overlay welding.
[0016] Further, in step S2.1, during the composite laser welding for the root layer, the green laser power is 500~1500W, the blue laser power is 800~1400W, the spot diameter is 1~4mm, the welding rate is 2~6mm / s, the wire feed speed is 5~15mm / s, the defocusing amount is -3mm~-0.5mm, and the layer height is 1~3mm; in step S2.2, during the composite laser surfacing process, the green laser power is 300~1000W, the blue laser power is 1000~1400W, the spot diameter is 2~5mm, the welding rate is 5~15mm / s, the wire feed speed is 10~20mm / s, the defocusing amount is 0.5~3mm, and the layer height is 2~4mm; the number of surfacing layers using the reciprocating motion of the composite laser is 3~10 layers.
[0017] Furthermore, in step S2.1, during the composite laser welding for the root pass, the shielding gas flow rate is 5-15 L / min; the shielding gas is one or a combination of argon, helium, and nitrogen; in step S2.2, during the composite laser welding process, the shielding gas flow rate is 10-20 L / min; the shielding gas is one or a combination of argon, nitrogen, and helium.
[0018] Furthermore, in step S2, the composite laser welding additive manufacturing also includes using a blue laser with a power gradient reduction to decrease the cooling rate during the cooling process. The specific process of laser-assisted slow cooling is as follows: Step S2.3: After the welding is completed, only the green laser is turned off, and the blue laser power is adjusted to 100~800w, the spot diameter is 5~10mm, and no wire is fed. The reciprocating motion continues according to the welding process at a speed of 10~30mm / s for 5~10 minutes; Step S2.4: The blue laser power is gradually reduced, and the reciprocating motion continues at a speed of 10~30mm / s for 5~10 minutes; Step S2.5: Step S2.4 is repeated until the workpiece is cooled to below 300℃.
[0019] Furthermore, in step S3, the silver-copper bimetallic composite structure is further refined to obtain a silver bearing layer with a thickness of 3~17mm.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The present invention relates to a heavy-duty bearing with a silver-copper bimetallic composite structure, which uses copper as the backing material of the bearing and high-silver material as the bearing bush material. During the operation of the bearing, the high thermal conductivity of copper and silver is utilized to achieve rapid heat dissipation and cooling, reduce thermal wear, and improve the service life of the workpiece.
[0021] 2. The method for preparing the heavy-duty bearing with silver-copper bimetallic composite structure of the present invention uses green light with a wavelength of 500nm~560nm and blue light with a wavelength of 400nm~500nm as a composite light source, which greatly reduces the reflectivity of the two metals to the laser, increases the absorption rate, and achieves local rapid heating and melting to achieve the purpose of welding, realizes metallurgical bonding at the atomic level, improves the bimetallic bonding strength, and reduces equipment wear.
[0022] 3. The method for preparing the heavy-duty bearing with silver-copper bimetallic composite structure of the present invention involves using a gradient reduction of blue laser power for auxiliary cooling during the cooling process after composite laser welding. By utilizing the inverse relationship between laser spot size and power density, the spot size is increased while the blue laser power is gradually reduced, so that the workpiece still has a certain amount of heat input during the cooling process, thereby achieving the purpose of slow cooling and preventing excessive cooling rate, which would cause excessive internal stress in the workpiece and have an adverse effect on subsequent processing and application.
[0023] 4. The heavy-duty bearing with silver-copper bimetallic composite structure of the present invention is easy to repair locally. Silver and copper bimetals are used as the backing material and bearing bush material of the bearing, respectively. The composite laser welding is used for additive manufacturing. Taking advantage of its high speed, large depth and small deformation, local rapid repair can be achieved. Strong metallurgical bonding is achieved in the depth direction, reducing the maintenance cost of the workpiece in the later stage. Attached Figure Description
[0024] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0025] Figure 1 This is a high-magnification image of the metallographic interface of the silver-copper bimetallic composite structure in the heavy-duty bearing prepared in Example 1 of the present invention. Figure 2 This describes the surface morphology of the pure Ag welding wire laser additive manufacturing process in Embodiment 1 of the present invention. Figure 3 Photograph of a traditional CMT weld seam. Detailed Implementation
[0026] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0027] In existing technologies, when silver is used as the bearing material, the traditional arc additive manufacturing method results in blackened welds that cannot be properly formed when silver is deposited on a copper substrate. Figure 3 As shown, traditional CMT welding results in poor weld formation and blackening. When brazing is used, due to the large-area composite structure of the bearing bush and the substrate, the capillary action of the brazing filler metal alone cannot meet the connection requirements, and brazing is also difficult. When using laser cladding for additive manufacturing, the wavelength factor and the high reflectivity of copper and silver to ordinary lasers, as well as their own high thermal conductivity, result in insufficient interface temperature, preventing the formation of a metallurgical bond.
[0028] This invention provides a heavy-duty bearing with a silver-copper bimetallic composite structure. The bearing backing material is copper, and the bearing bush material is silver. It is manufactured by additive manufacturing using green and blue light composite laser welding.
[0029] Preferably, the backing material of the bearing is at least one of copper, brass, or bronze; Preferably, the bearing material is high-silver material.
[0030] Silver-copper bimetallic bearings use copper as the backing material and high-silver material as the bearing bush material. During the bearing's operation, the high thermal conductivity of copper and silver (copper has a thermal conductivity of 397 W / (m·K), and silver has a thermal conductivity of 429 W / (m·K)) is utilized to achieve rapid heat dissipation and cooling, reduce thermal wear, and improve the service life of the workpiece.
[0031] This invention also provides a method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure, comprising the following steps: Step S1: Copper part machining and copper part surface treatment; Step S2: Fix the copper part on the welding platform, combine green laser and blue laser, use silver-based welding material, and perform composite laser welding additive manufacturing to obtain a silver-copper bimetallic composite structure. Step S3: The silver-copper bimetallic composite structure is finely processed to obtain the silver bearing layer.
[0032] Preferably, the surface treatment of the copper part in step S1 includes cleaning the surface of the workpiece and removing the oxide layer.
[0033] Preferably, in step S2, the composite laser consists of green light with a wavelength of 500nm to 560nm and blue light with a wavelength of 400nm to 500nm; the wavelength of the green light includes, but is not limited to, values of 500nm, 510nm, 520nm, 530nm, 540nm, 550nm, and 560nm or a range between two values; the wavelength of the blue light includes, but is not limited to, values of 400nm, 410nm, 420nm, 430nm, 440nm, 450nm, 460nm, 470nm, 480nm, 490nm, and 500nm or a range between two values.
[0034] Conventional laser welding machines use a laser wavelength of 1064nm. Copper and silver have high reflectivity to this wavelength, and their excellent thermal conductivity prevents them from rapidly heating up and melting. Therefore, this invention uses green light with wavelengths between 500nm and 560nm and blue light between 400nm and 500nm as a composite light source. This significantly reduces the reflectivity of the two metals to the laser, increases the absorption rate, and enables localized rapid heating and melting, achieving the welding purpose. This results in atomic-level metallurgical bonding, improves the bimetallic bond strength, and reduces equipment wear.
[0035] Preferably, in step S2, the silver-based solder is selected from welding wire, welding sheet, welding strip, welding powder, or other forms of silver-based solder that can be used in additive manufacturing.
[0036] Preferably, in step S2, the silver-based welding material is pure Ag welding wire with a wire diameter of 1.0~2.4mm, including but not limited to 1.0mm, 1.2mm, 1.4mm, 1.6mm, 1.8mm, 2.0mm, 2.2mm, and 2.4mm.
[0037] Preferably, in step S2, the welding process adopts a coaxial wire feeding method, and the angle between the welding wire and the base material is between 35 and 60 degrees, including but not limited to 35 degrees, 40 degrees, 45 degrees, 50 degrees, 55 degrees, and 60 degrees.
[0038] Preferably, the welding process of composite laser welding in step S2 is carried out in the form of reciprocating motion, and the overlap rate of two adjacent welds is 10% to 50%, including but not limited to point values of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, and 50% or the range between two point values.
[0039] Preferably, in step S2, the centers of the combined green and blue laser beams coincide, and the beam size and power of each laser beam can be adjusted independently.
[0040] Preferably, step S2, composite laser welding additive manufacturing, includes the following steps: Step S2.1: Apply composite laser welding to create the base layer; Step S2.2: Continue to use composite laser for surfacing.
[0041] Preferably, in step S2.1, during the composite laser welding for the root pass, the green laser power is 500~1500W (including but not limited to 500W, 600W, 800W, 1000W, 1200W, 1400W, 1500W), the blue laser power is 800~1400W (including but not limited to 800W, 1000W, 1200W, 1400W), the spot diameter is 1~4mm (including but not limited to 1mm, 2mm, 3mm, 4mm), the welding speed is 2~6mm / s (including but not limited to 2mm / s, 3mm / s, 4mm / s, 5mm / s, 6mm / s), the wire feed speed is 5~15mm / s (including but not limited to 5mm / s, 10mm / s, 15mm / s), and the defocusing amount is -3mm~. -0.5mm (including but not limited to -3mm, -2.5mm, -2.0mm, -1.5mm, -1.0mm, -0.5mm), and the floor height is 1~3mm (including but not limited to 1mm, 1.5mm, 2mm, 2.5mm, 3mm).
[0042] Preferably, in step S2.1, during the composite laser welding root pass, the shielding gas flow rate is 5~15L / min, including but not limited to 5L / min, 7L / min, 10L / min, 12L / min, and 15L / min; the shielding gas is one or a combination of inert gases such as argon, helium, and nitrogen.
[0043] Preferably, in step S2.2, during the composite laser welding process, the green laser power is 300~1000w (including but not limited to 300w, 500w, 600w, 800w, 1000w), the blue laser power is 1000~1400w (including but not limited to 1000w, 1100w, 1200w, 1400w), the spot diameter is 2~5mm (including but not limited to 2mm, 3mm, 4mm, 5mm), and the welding speed is 5~15mm / s (including but not limited to 5mm / s). The wire feeding speed is 10-20 mm / s (including but not limited to 10 mm / s, 12 mm / s, 14 mm / s, 16 mm / s, 18 mm / s, 20 mm / s), the defocusing amount is 0.5-3 mm (including but not limited to 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm), and the layer height is 2-4 mm (including but not limited to 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm).
[0044] Preferably, in step S2.2, during the composite laser welding process, the shielding gas flow rate is 10-20 L / min, including but not limited to 10 L / min, 12 L / min, 14 L / min, 16 L / min, 18 L / min, and 20 L / min; the shielding gas is one or a combination of inert gases such as argon, nitrogen, and helium.
[0045] Preferably, in step S2.2, the number of layers welded by the reciprocating motion of the composite laser is 3 to 10 (including but not limited to 3, 5, 7, and 10 layers), and the final weld height is 6 to 40 mm (including but not limited to 6 mm, 10 mm, 14 mm, 18 mm, 20 mm, 22 mm, 26 mm, 30 mm, 34 mm, 38 mm, and 40 mm), preferably 6 to 20 mm.
[0046] Preferably, in step S2, the composite laser welding additive manufacturing further includes using a blue laser with a reduced power gradient to decrease the cooling rate during the cooling process.
[0047] Preferably, the specific process of laser-assisted slow cooling in step S2 is as follows: Step S2.3: After the welding is completed, turn off only the green laser and adjust the blue laser power to 100~800w, with a spot diameter of 5~10mm (including but not limited to 5mm, 6mm, 7mm, 8mm, 9mm, 10mm). Do not feed wire and continue to reciprocate according to the welding process at a speed of 10~30mm / s (including but not limited to 10mm / s, 15mm / s, 20mm / s, 25mm / s, 30mm / s) for 5~10 minutes (including but not limited to 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes). Step S2.4: Gradually reduce the blue laser power and continue reciprocating motion at a speed of 10~30mm / s (including but not limited to 10mm / s, 15mm / s, 20mm / s, 25mm / s, 30mm / s), for 5~10 minutes (including but not limited to 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes). Step S2.5, repeat step S2.4, until the workpiece temperature drops below 300℃.
[0048] In the cooling process of this invention, the blue laser power is gradually reduced to assist in cooling. Taking advantage of the inverse relationship between laser spot size and power density, the spot size is increased while the blue laser power is gradually reduced, so that the workpiece still has a certain amount of heat input during the cooling process, thereby achieving the purpose of slow cooling. This prevents the cooling rate from being too fast, which would cause excessive internal stress in the workpiece and have an adverse effect on subsequent processing and application.
[0049] Preferably, in step S3, the silver-copper bimetallic composite structure is finely processed to obtain a silver bearing layer with a thickness of 3~17mm (including but not limited to 3mm, 6mm, 9mm, 10mm, 12mm, 15mm, 17mm).
[0050] This invention uses silver-copper bimetal as the backing material and bearing bush material of the bearing, and performs additive manufacturing by laser welding. Taking advantage of its high speed, large depth and small deformation, it can realize rapid local repair, achieve strong metallurgical bonding in the depth direction, reduce the maintenance cost of the workpiece in the later stage, and facilitate local repair.
[0051] Example 1 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and combine a 532nm green laser and a 450nm blue laser. After the two lasers are combined, the centers of the laser spots coincide. Step 3: Use pure Ag welding wire with a diameter of 1.2mm and feed the wire using a wire feeding mechanism; Step 4: When performing composite laser welding for the root layer, the green laser power is 1200w, the blue laser power is 1000w, the spot diameter is 2mm, the welding rate is 3mm / s, the wire feed speed is 7mm / s, the defocusing amount is -0.7mm, and the shielding gas used during the welding process is argon gas with a flow rate of 12 L / min and a layer height of 1mm. Step 5: After welding the root layer, continue to use composite laser for overlay welding. At this time, the green light power is 800w, the blue light power is 1400w, the spot diameter is 2.5mm, the welding speed is 6mm / s, the wire feed speed is 15mm / s, the defocusing amount is 1mm, the shielding gas flow rate is 15L / min, and the layer height is 2mm. Step 6: The welding process uses a reciprocating motion, with an overlap rate of 15% between adjacent weld seams; Step 7: Using the reciprocating motion of the composite laser, four layers are deposited, resulting in a final deposit height of 8mm, and a total height of 9mm for the root pass and the deposit. Step 8: After the welding is completed, turn off only the green laser and adjust the blue laser power to 800w with a spot diameter of 6mm. Do not feed wire and continue the reciprocating motion according to the welding process at a speed of 20mm / s. After 10 minutes of cycling, reduce the blue laser power to 600w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 18mm / s. After 10 minutes of cycling, reduce the blue laser power to 400w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. After 8 minutes of cycling, reduce the blue laser power to 200w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. Repeat this cycle until the workpiece temperature drops below 300℃. Step 9: The composite metal structure prepared in Step 8 is then precision-machined to obtain a silver bearing layer with a thickness of 7 mm. Example 2 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and combine a 532nm green laser and a 450nm blue laser. After the two lasers are combined, the centers of the laser spots coincide. Step 3: Use pure Ag welding wire with a diameter of 1.6mm and feed the wire using a wire feeding mechanism; Step 4: When performing composite laser welding for the root layer, the green laser power is 1400w, the blue laser power is 1200w, the spot diameter is 2.5mm, the welding speed is 4mm / s, the wire feed speed is 15mm / s, the defocusing amount is -1mm, the shielding gas used in the welding process is argon gas with a flow rate of 13 L / min, and the layer height is 1.8mm. Step 5: After welding the root layer, continue to use composite laser for overlay welding. At this time, the green light power is 900w, the blue light power is 1400w, the spot diameter is 3mm, the welding speed is 6mm / s, the wire feed speed is 18mm / s, the defocusing amount is 1.2mm, the shielding gas flow rate is 17L / min, and the layer height is 2.5mm. Step 6: The welding process adopts a reciprocating motion, and the overlap rate between adjacent welds is 17%. Step 7: Using the reciprocating motion of the composite laser, 5 layers are deposited, resulting in a final deposit height of 12.5mm, and a total height of 14.3mm for the root pass and the deposit. Step 8: After the welding is completed, turn off only the green laser and adjust the blue laser power to 800w with a spot diameter of 7mm. Do not feed wire and continue the reciprocating motion according to the welding process at a speed of 18mm / s. After 6 minutes of cycling, reduce the blue laser power to 600w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 16mm / s. After 6 minutes of cycling, reduce the blue laser power to 400w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 14mm / s. After 8 minutes of cycling, reduce the blue laser power to 200w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. Repeat this cycle until the workpiece temperature drops below 300℃. Step 9: The composite metal structure prepared in Step 8 is finely processed to obtain a silver bearing layer with a thickness of 12 mm.
[0052] Example 3 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and combine a 532nm green laser and a 450nm blue laser. After the two lasers are combined, the centers of the laser spots coincide. Step 3: Use pure Ag welding wire with a diameter of 1.6mm and feed the wire using a wire feeding mechanism; Step 4: When performing composite laser welding for the root layer, the green laser power is 1350w, the blue laser power is 1250w, the spot diameter is 2.5mm, the welding speed is 4mm / s, the wire feed speed is 15mm / s, the defocusing amount is -0.8mm, the shielding gas used in the welding process is argon gas with a flow rate of 14 L / min, and the layer height is 1.8mm. Step 5: After welding the root layer, continue to use composite laser for overlay welding. At this time, the green light power is 950w, the blue light power is 1400w, the spot diameter is 3mm, the welding speed is 6mm / s, the wire feed speed is 18mm / s, the defocusing amount is 1.3mm, the shielding gas flow rate is 16L / min, and the layer height is 2.5mm. Step 6: The welding process adopts a reciprocating motion, and the overlap rate between adjacent welds is 17%. Step 7: Using the reciprocating motion of the composite laser, 5 layers are deposited, resulting in a final deposit height of 12.5mm, and a total height of 14.3mm for the root pass and the deposit. Step 8: The composite metal structure prepared in Step 7 is finely processed to obtain a silver bearing layer with a thickness of 11 mm.
[0053] Comparative Example 1 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and use a blue laser with a wavelength of 450nm; Step 3: Use pure Ag welding wire with a diameter of 1.2mm and feed the wire using a wire feeding mechanism; Step 4: When applying the base layer, the blue laser power is 2600w, the spot diameter is 2.5mm, the welding rate is 3mm / s, the wire feed speed is 8mm / s, the defocusing amount is -0.5mm, the shielding gas used in the welding process is argon gas with a flow rate of 12 L / min, and the layer height is 1mm. Step 5: After welding the root layer, continue to use blue laser for overlay welding. At this time, the power is 2300w, the spot diameter is 2.6mm, the welding speed is 8mm / s, the wire feed speed is 19 mm / s, the defocusing amount is 0.8mm, the shielding gas flow rate is 15L / min, and the layer height is 2mm. Step 6: The welding process uses a reciprocating motion, with an overlap rate of 15% between adjacent weld seams; Step 7: Using the reciprocating motion of the laser, four layers are deposited, resulting in a final deposit height of 8mm, and a total height of 9mm for the root pass and the deposit. Step 8: After the welding is completed, adjust the blue laser power to 800w, the spot diameter to 7mm, do not feed wire, and continue the reciprocating motion according to the welding process at a speed of 20mm / s. After 10 minutes of cycling, reduce the blue laser power to 600w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 19mm / s. After 10 minutes of cycling, reduce the blue laser power to 400w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. After 8 minutes of cycling, reduce the blue laser power to 200w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. Repeat this cycle until the workpiece temperature drops below 300℃. Step 9: The composite metal structure prepared in Step 8 is finely processed to obtain a silver bearing layer with a thickness of 7 mm.
[0054] Comparative Example 2 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and use a 532nm green laser for welding; Step 3: Use pure Ag welding wire with a diameter of 1.6mm and feed the wire using a wire feeding mechanism; Step 4: When welding the root layer, the green laser power is 2500w, the spot diameter is 2.8mm, the welding speed is 5mm / s, the wire feed speed is 15mm / s, the defocusing amount is -0.7mm, the shielding gas used in the welding process is argon gas with a flow rate of 13 L / min and a layer height of 1.8mm. Step 5: After welding the root layer, continue to use green laser for overlay welding. At this time, the green laser power is 2200w, the spot diameter is 2.8mm, the welding speed is 7mm / s, the wire feed speed is 20mm / s, the defocusing amount is 0.9mm, the shielding gas flow rate is 17L / min, and the layer height is 2.5mm. Step 6: The welding process adopts a reciprocating motion, and the overlap rate between adjacent welds is 17%. Step 7: Using the reciprocating motion of the laser, 5 layers are deposited, resulting in a final deposit height of 12.5mm, and a total height of 14.3mm for the root pass and the deposit. Step 8: After the welding is completed, adjust the green laser power to 800w, the spot diameter to 8mm, do not feed wire, and continue the reciprocating motion according to the welding process at a speed of 20mm / s. After 8 minutes of cycling, reduce the green laser power to 600w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 18mm / s. After 6 minutes of cycling, reduce the green laser power to 400w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 16mm / s. After 8 minutes of cycling, reduce the green laser power to 200w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. Repeat this cycle until the workpiece temperature drops below 300℃. Step 9: The composite metal structure prepared in Step 8 is finely processed to obtain a silver bearing layer with a thickness of 11 mm.
[0055] Comparative Example 3 A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure includes the following steps (some of which are parameter limitations of other steps and do not represent the order of steps): Step 1: Process the copper into the required size and shape, and perform surface treatment to remove stains and oxide layers from the workpiece surface; Step 2: Use tools to fix the processed copper parts on the welding platform, and combine a 532nm green laser and a 450nm blue laser. After the two lasers are combined, the centers of the laser spots coincide. Step 3: Use pure Ag welding wire with a diameter of 1.2mm and feed the wire using a wire feeding mechanism; Step 4: When performing composite laser welding for the root layer, the green laser power is 600w, the blue laser power is 1600w, the spot diameter is 1.6mm, the welding rate is 2.5mm / s, the wire feed speed is 8 mm / s, the defocusing amount is -0.4mm, the shielding gas used during the welding process is argon gas with a flow rate of 15 L / min and a layer height of 1mm. Step 5: After welding the root layer, continue to use composite laser for overlay welding. At this time, the green laser power is 400w, the blue laser power is 1800w, the spot diameter is 1.8mm, the welding speed is 4mm / s, the wire feed speed is 15mm / s, the defocusing amount is 0.3mm, the shielding gas flow rate is 15L / min, and the layer height is 2mm. Step 6: The welding process uses a reciprocating motion, with an overlap rate of 15% between adjacent weld seams; Step 7: Use the reciprocating motion of the composite laser to deposit 4 layers, ultimately forming a deposit height of 8mm, and the total height of the root pass and the deposit is 9mm; Step 8: After the welding is completed, turn off only the green light, adjust the blue laser power to 800w, the spot diameter to 7mm, do not feed wire, and continue the reciprocating motion according to the welding process at a speed of 20mm / s. After 10 minutes of cycling, reduce the blue laser power to 600w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 18mm / s. After 10 minutes of cycling, reduce the blue laser power to 400w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. After 8 minutes of cycling, reduce the blue laser power to 200w, keep the spot diameter unchanged, and continue the reciprocating motion at a speed of 15mm / s. Repeat this cycle until the workpiece temperature drops below 300℃. Step 9: The composite metal structure prepared in Step 8 is finely processed to obtain a silver bearing layer with a thickness of 7 mm.
[0056] Test case I. The metallurgical bonding of the workpiece is shown through the interfacial metallographic structure; like Figure 1 The high-magnification image of the metallographic interface of the silver-copper bimetallic composite structure in the heavy-duty bearing prepared in Example 1 is shown. The dark area on the left is the brass matrix, the white area on the right is the pure silver solder, and the middle area is the interface between the two. As can be seen from the figure, the two materials form a solid solution or intermetallic compound at the interface, with silver as the matrix. The solid solution or compound is mainly granular, with some appearing as needles.
[0057] II. Example 1: Surface morphology of pure Ag welding wire laser additive manufacturing (see attached). Figure 2 See traditional CMT welding weld photos. Figure 3 .
[0058] like Figure 2As shown, silver is deposited on the substrate using pure Ag welding wire laser additive manufacturing. Unlike the melting method of CMT, the laser mainly uses a high-density energy beam to concentrate on a single point, causing the base material and welding wire to melt. The substrate then cools down and the surface dissipates heat to achieve a cooling and solidification effect, resulting in good weld formation and relatively controllable heat input.
[0059] like Figure 3 As shown, when using the traditional arc additive manufacturing method to deposit silver on a copper substrate, the weld seam turns black and cannot be formed. Traditional CMT welding results in poor weld seam formation and blackening.
[0060] 3. The strength of the workpiece shall be tested in accordance with the standard GB / T 12948 "Sliding bearings - Bimetallic bond strength destructive test method"; During the heat dissipation performance test, the entire workpiece was heated to 200℃, kept at that temperature for 1 hour, and then taken out for natural cooling. The surface temperature of the silver bearing was measured at regular intervals, and the time required for the silver surface to cool down to 80℃ was calculated. The heat dissipation performance was judged based on the duration. The wear reduction and wear resistance of silver bearing bushes are mainly determined by friction and wear tests. The HT-1000 high-temperature friction and wear testing machine is used to conduct friction and wear tests on copper-based silver bearing bushes under a certain load.
[0061] The main test results are shown in Table 1: Table 1. Performance test results of heavy-duty bearings with silver-copper bimetallic composite structures prepared in Examples 1-3 and Comparative Examples 1-3.
[0062] Table 1 shows that different processing parameters have different effects on the performance of the specimens. Green light mainly focuses on the weld penetration, while blue light is beneficial to the weld density. Therefore, compared with a single light source, the composite light source in the examples significantly improves the weld strength. In Example 3, gradient-assisted cooling with blue light was not performed. Without this auxiliary cooling, the residual stress inside the workpiece increases, leading to a decrease in workpiece strength, which can severely affect the finishing of the workpiece. Gradient-assisted cooling with blue light is used to reduce the cooling rate of the workpiece, prevent stress problems caused by rapid cooling that could lead to dimensional fluctuations, alleviate internal stress, reduce defects, and minimize machining errors caused by stress, thus providing conditions for subsequent precision assembly.
[0063] Regarding the heat dissipation performance of the workpiece, under the condition that the material is the same, it is only related to the size of the workpiece. In Example 1, Comparative Example 1 and Comparative Example 3, the final workpiece size is 7mm, so the heat dissipation time of the three is not much different. However, in Example 2, the workpiece size is the largest, so the heat dissipation time is the longest. The coefficient of friction is a key performance of the bearing material, and its value is only related to the material's own properties, so the coefficient of friction is basically the same.
Claims
1. A method for preparing a heavy-duty bearing with a silver-copper bimetallic composite structure, characterized in that, Includes the following steps: Step S1: Copper part machining and copper part surface treatment; Step S2: Fix the copper part on the welding platform, combine green laser and blue laser, use silver-based welding material, and perform composite laser welding additive manufacturing to obtain a silver-copper bimetallic composite structure. Step S3: The silver-copper bimetallic composite structure is precision machined to obtain the silver bearing layer; The bearing's backing material is copper, and the bearing bush material is silver. It is manufactured using additive manufacturing with green and blue light composite laser welding. The silver-based welding material mentioned in step S2 is selected from silver-based welding wire, silver-based welding sheet or silver-based welding strip; In step S2, the centers of the combined green and blue laser beams coincide. Step S2, composite laser welding additive manufacturing, includes the following steps: Step S2.1: Apply composite laser welding to create the base layer; Step S2.2: Continue to use composite laser for welding; In step S2.1, during the composite laser welding process for the root layer, the green laser power is 500~1500w, the blue laser power is 800~1400w, the spot diameter is 1~4mm, the welding rate is 2~6mm / s, the wire feed speed is 5~15mm / s, the defocusing amount is -3mm~-0.5mm, and the layer height is 1~3mm. In step S2.2, during the composite laser welding process, the green laser power is 300~1000w, the blue laser power is 1000~1400w, the spot diameter is 2~5mm, the welding rate is 5~15mm / s, the wire feed speed is 10~20mm / s, the defocusing amount is 0.5~3mm, and the layer height is 2~4mm.
2. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 1, characterized in that, The backing material of the bearing is at least one of copper, brass, or bronze; the bearing bush material is high-silver material.
3. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 1, characterized in that, In step S2, the composite laser consists of green light with a wavelength of 500nm~560nm and blue light with a wavelength of 400nm~500nm.
4. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 3, characterized in that, It should include at least one of the following technical features: (1) In step S2, the silver-based welding material is pure Ag welding wire with a wire diameter of 1.0~2.4mm; (2) In step S2, the welding process adopts a coaxial wire feeding method, and the angle between the welding wire and the base material is between 35 and 60 degrees; (3) In step S2, the composite laser welding process is carried out in the form of reciprocating motion, and the overlap rate of adjacent welds is 10%~50%; (4) In step S2, the spot size and power of the green laser and the blue laser can be adjusted independently.
5. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 4, characterized in that, In step S2.2, the number of layers welded using the reciprocating motion of the composite laser is 3 to 10.
6. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 1, characterized in that, In step S2.1, during the composite laser welding process for the root pass, the shielding gas flow rate is 5~15L / min; the shielding gas is one or a combination of inert gases. In step S2.2, during the composite laser welding process, the shielding gas flow rate is 10-20 L / min; the shielding gas is one or a combination of inert gases.
7. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 5 or 6, characterized in that, Step S2 in the composite laser welding additive manufacturing process also includes using a blue laser with a reduced power gradient to decrease the cooling rate during the cooling process. The specific process of laser-assisted slow cooling is as follows: Step S2.3: After the welding is completed, turn off only the green laser, adjust the blue laser power to 100~800w, the spot diameter to 5~10mm, do not feed wire, and continue to reciprocate according to the welding process at a speed of 10~30mm / s for 5~10 minutes. Step S2.4: Gradually reduce the blue laser power and continue reciprocating motion at a speed of 10~30mm / s for 5~10 minutes. Step S2.5, repeat step S2.4, until the workpiece temperature drops below 300℃.
8. The method for preparing the heavy-duty bearing with a silver-copper bimetallic composite structure according to claim 5 or 6, characterized in that, In step S3, the silver-copper bimetallic composite structure is finely processed to obtain a silver bearing layer with a thickness of 3~17mm.
Citation Information
Patent Citations
Method for manufacturing functionally graded material through copper-silver dissimilar metal blue laser additive