A method for preparing a drive wheel for an ultrathin powder metallurgy card component
By employing gradient pressing, segmented sintering, and surface strengthening processes, the challenges of densification and precision control in ultra-thin drive wheels were solved, enabling the fabrication of high-performance ultra-thin drive wheels and improving the wear resistance and strength of the parts.
Patent Information
- Application Number
- CN202511910693.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-12-17
AI Technical Summary
Traditional powder metallurgy processes are difficult to fabricate ultra-thin drive wheels, and there are problems such as uneven compact density, easy cracking, delamination, warping deformation, difficulty in controlling dimensional accuracy, and insufficient strength and toughness.
The process involves gradient pressing, segmented sintering, precision shaping, and surface strengthening. This includes mixing metal-based powder with alloy additives, gradient pressure forming, segmented sintering, cold finishing, and low-temperature nitriding to ensure the densification and high precision of ultra-thin parts.
This technology enables high-density, defect-free blanking of ultra-thin drive wheels, ensuring dimensional stability and high precision, improving the wear resistance and fatigue strength of parts, and meeting the requirements for high-load service.
Smart Images

Figure CN121669937B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of powder metallurgy card manufacturing technology, and in particular to a method for manufacturing a drive wheel for an ultrathin powder metallurgy card. Background Technology
[0002] Powder metallurgy technology is widely used in the manufacture of precision mechanical parts such as gears and drive wheels due to its advantages such as near-net-shape forming, high material utilization, and the ability to produce complex-shaped parts. However, as part structures tend to become ultra-thin, traditional powder metallurgy processes face severe challenges. In the pressing stage, it is difficult to achieve uniform filling and densification of powder in thin-walled cavities, which can easily lead to uneven compact density, cracks, or delamination. In the sintering stage, ultra-thin parts are more sensitive to thermal stress due to their large specific surface area and low structural stiffness, making them prone to warping and deformation, and difficult to control dimensional accuracy.
[0003] In addition, thin-walled parts prepared by conventional processes often lack strength and toughness and have poor surface wear resistance, making it difficult to meet the service requirements of drive wheels under high load and cyclic stress.
[0004] Therefore, developing a dedicated powder metallurgy process that can balance high-precision forming, low-deformation sintering, and high-performance strengthening has become a technical bottleneck in the preparation of high-performance ultra-thin drive wheels. Summary of the Invention
[0005] The purpose of this invention is to solve the above-mentioned problems and to propose a method for preparing an ultrathin structure powder metallurgy driving wheel.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: a method for preparing an ultrathin structure powder metallurgy driving wheel, comprising the following steps:
[0007] S1. Raw material preparation: Mix metal-based powder, alloy additives and lubricants in a certain proportion to obtain mixed powder;
[0008] S2. Gradient pressing: The mixed powder is filled into a customized mold cavity, and a drive wheel blank is prepared by gradient pressure pressing process. The minimum thickness of the drive wheel blank is 0.5 mm.
[0009] S3. Segmented sintering: The drive wheel blank is placed in the sintering furnace and subjected to low-temperature pre-firing and high-temperature main firing in sequence to obtain the sintered blank.
[0010] S4. Precision shaping: The dimensions of the sintered billet are corrected by a cold finishing process to obtain the initial-formed drive wheel;
[0011] S5. Surface strengthening: The initial-formed drive wheel is subjected to surface strengthening treatment to finally obtain an ultra-thin structure powder metallurgy card drive wheel. The finished drive wheel has a density ≥7.2g / cm³ and a flatness ≤0.05mm.
[0012] Preferably, in step S1:
[0013] The metal-based powder is atomized pure iron powder with a particle size of 50-150μm and a loose packing density of 2.8-3.2g / cm³.
[0014] The alloy additive comprises copper powder, nickel powder, and molybdenum powder, with the three components accounting for 2%–4%, 1%–3%, and 0.5%–1.5% of the mass of the metal-based powder, respectively.
[0015] The lubricant is zinc stearate, and its mass percentage is 0.8%–1.2% of the total mass of the mixed powder.
[0016] Preferably, the mixing process in step S1 is performed using a high-speed mixer:
[0017] The mixer speed is set to 8-12 r / min, and the mixing time is 20-30 min.
[0018] During the mixing process, the material temperature is controlled to be ≤40℃ by jacket water cooling. After the mixing is completed, the mixed powder is sieved through a 100-mesh sieve.
[0019] Preferably, the gradient pressing process parameters in step S2 include:
[0020] The pressing equipment is a servo CNC press, and the mold preheating temperature is 40-60℃;
[0021] The gradient pressure is divided into two stages: the first stage pressure is 450-550MPa, and the holding time is 5-8s; the second stage pressure is 650-700MPa, and the holding time is 10-15s.
[0022] The density of the pressed drive wheel blank is 7.15-7.25 g / cm³, and the dimensional tolerance is controlled within ±0.1 mm.
[0023] Preferably, the segmented sintering process parameters in step S3 include:
[0024] Low-temperature pre-firing stage: heating rate is 5-8℃ / min, heating to 700-750℃, holding time is 30-45min, atmosphere is air;
[0025] High-temperature main combustion stage: After pre-firing, the temperature is increased to 1100-1150℃ at a rate of 10-12℃ / min, and held for 30-60min. The atmosphere is an ammonia decomposition atmosphere with a hydrogen gas integral of ≥99.9%.
[0026] During the sintering process, the shrinkage rate of the drive wheel blank is controlled at 1.8%–2.2%, and a horizontally placed tray is used.
[0027] Preferably, the precision shaping process in step S4 uses a custom-made precision shaping mold:
[0028] The shaping equipment is a four-column hydraulic press with a shaping pressure of 700-750MPa and a holding time of 8-12s.
[0029] The surface roughness Ra of the forming mold cavity is ≤0.1μm;
[0030] After shaping, the inner diameter tolerance of the drive wheel is grade H7, the outer diameter tolerance is grade h7, and the flatness is ≤0.05mm.
[0031] Preferably, the surface strengthening treatment in step S5 is a low-temperature nitriding process:
[0032] The nitriding equipment is a vacuum nitriding furnace, with a nitriding temperature of 500-550℃ and a holding time of 120-180 minutes;
[0033] The nitriding atmosphere is a mixture of nitrogen and hydrogen gas with a volume ratio of 1:3, and the pressure inside the furnace is maintained at 0.15-0.2 MPa.
[0034] The thickness of the nitrided layer on the surface of the reinforced drive wheel is 15-25μm, the surface Vickers hardness is ≥550HV0.2, and the core Vickers hardness is ≥280HV0.2.
[0035] Preferably, a metal-based powder pretreatment step S0 is included before step S1:
[0036] The atomized pure iron powder was placed in a vacuum drying oven and dried for 2-3 hours at 80-100℃ and a vacuum degree ≤-0.09MPa.
[0037] After drying, the iron powder was classified using an air classifier, and powder with a particle size of 50-150μm was selected as metal-based powder.
[0038] Preferably, step S5 is followed by a finished product inspection step S6:
[0039] Density testing: The density of the drive wheel was measured using the water displacement method. Five samples were randomly selected from each batch, and the arithmetic mean was taken.
[0040] Hardness testing: The surface and core hardness were tested using a Vickers hardness tester. Three evenly distributed points were selected for surface testing, and the core was tested by wire cutting.
[0041] Dimensional inspection: The inner diameter, outer diameter, and flatness are inspected using a coordinate measuring machine.
[0042] Preferably, in step S2, the cavity structure of the customized mold is adapted to the drive wheel structure:
[0043] The mold cavity includes a hub hole forming section, a tooth forming section, and a rim forming section;
[0044] The tooth profile of the gear forming section adopts an involute tooth profile with a module of 1.5mm and 6 teeth. The mold material is high-speed steel, and the cavity surface is nitrided with a surface hardness of ≥60HRC and a service life of ≥300,000 pressing cycles.
[0045] Compared with the prior art, the advantages and positive effects of the present invention are as follows:
[0046] It promotes the uniform flow and densification of powder in the ultra-thin cavity, resulting in a high-density, defect-free compact, which lays a good geometric and physical foundation for subsequent processes. The innovative segmented sintering system removes lubricant and initially forms particle bonds through low-temperature pre-firing, and then transfers to high-temperature main firing to complete alloying and densification. This process significantly alleviates the deformation caused by thermal stress concentration and ensures the dimensional stability of the ultra-thin compact.
[0047] Cold straightening was performed to correct the unavoidable minor deformations after sintering, ultimately ensuring that the critical dimensional accuracy of the parts reached H7 / h7 level, and the flatness was strictly controlled within 0.05mm, meeting the requirements for high-precision assembly.
[0048] Finally, through surface strengthening treatment, a high-hardness nitrided layer is formed on the surface of the part, which greatly improves the wear resistance and fatigue strength of the drive wheel tooth surface, while the core still maintains good toughness. The whole method works synergistically. Attached Figure Description
[0049] Figure 1 This is a flowchart of the method of the present invention. Detailed Implementation
[0050] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0051] according to Figure 1 The present invention proposes a method for preparing an ultrathin powder metallurgy drive wheel, comprising the following steps:
[0052] S1. Raw material preparation: Metal-based powder, alloy additives, lubricants, and composite plasticizers are mixed in proportion to obtain a mixed powder;
[0053] S2. Gradient pressing: The mixed powder is filled into a customized mold cavity, and a drive wheel blank is prepared by gradient pressure pressing process. The minimum thickness of the drive wheel blank is 0.5 mm.
[0054] S3. Segmented sintering: The drive wheel blank is placed in the sintering furnace and subjected to low-temperature pre-firing and high-temperature main firing in sequence to obtain the sintered blank.
[0055] S4. Precision shaping: The dimensions of the sintered billet are corrected by a cold finishing process to obtain the initial-formed drive wheel;
[0056] S5. Surface strengthening: The initial-formed drive wheel is subjected to surface strengthening treatment to finally obtain an ultra-thin structure powder metallurgy card drive wheel. The finished drive wheel has a density ≥7.2g / cm³ and a flatness ≤0.05mm.
[0057] As an optional embodiment, in step S1:
[0058] The metal-based powder is atomized pure iron powder with a particle size of 50-150μm and a loose packing density of 2.8-3.2g / cm³.
[0059] The alloy additive comprises copper powder, nickel powder, and molybdenum powder, with the three components accounting for 2%–4%, 1%–3%, and 0.5%–1.5% of the mass of the metal-based powder, respectively.
[0060] The lubricant is zinc stearate, and its mass percentage is 0.8%–1.2% of the total mass of the mixed powder.
[0061] As an optional embodiment, the mixing process in step S1 is performed using a high-speed mixer:
[0062] The mixer speed is set to 8-12 r / min, and the mixing time is 20-30 min.
[0063] During the mixing process, the material temperature is controlled to be ≤40℃ by jacket water cooling. After the mixing is completed, the mixed powder is sieved through a 100-mesh sieve.
[0064] As an optional embodiment, the gradient pressing process parameters in step S2 include:
[0065] The pressing equipment is a servo CNC press, and the mold preheating temperature is 40-60℃;
[0066] The gradient pressure is divided into two stages: the first stage pressure is 450-550MPa, and the holding time is 5-8s; the second stage pressure is 650-700MPa, and the holding time is 10-15s.
[0067] The density of the pressed drive wheel blank is 7.15-7.25 g / cm³, and the dimensional tolerance is controlled within ±0.1 mm.
[0068] As an optional embodiment, the segmented sintering process parameters in step S3 include:
[0069] Low-temperature preheating stage: heating rate is 5-8℃ / min, heating to 400-500℃, holding time is 30-45min, atmosphere is air;
[0070] High-temperature main combustion stage: After pre-firing, the temperature is increased to 1100-1150℃ at a rate of 10-12℃ / min, and held for 30-60min. The atmosphere is an ammonia decomposition atmosphere with a hydrogen gas integral of ≥99.9%.
[0071] During the sintering process, the shrinkage rate of the drive wheel blank is controlled at 1.8%–2.2%, and a horizontally placed tray is used.
[0072] As an optional embodiment, the precision shaping process in step S4 employs a custom-made precision shaping mold:
[0073] The shaping equipment is a four-column hydraulic press with a shaping pressure of 700-750MPa and a holding time of 8-12s.
[0074] The surface roughness Ra of the forming mold cavity is ≤0.02μm;
[0075] After shaping, the inner diameter tolerance of the drive wheel is grade H7, the outer diameter tolerance is grade h7, and the flatness is ≤0.05mm.
[0076] As an optional embodiment, the surface strengthening treatment in step S5 is a low-temperature nitriding process:
[0077] The nitriding equipment is a vacuum nitriding furnace, with a nitriding temperature of 500-550℃ and a holding time of 120-180 minutes;
[0078] The nitriding atmosphere is a mixture of nitrogen and hydrogen gas with a volume ratio of 1:3, and the pressure inside the furnace is maintained at 0.15-0.2 MPa.
[0079] The thickness of the nitrided layer on the surface of the reinforced drive wheel is 15-25μm, the surface Vickers hardness is ≥550HV0.2, and the core Vickers hardness is ≥280HV0.2.
[0080] As an optional embodiment, a metal-based powder pretreatment step S0 is included before step S1:
[0081] The atomized pure iron powder was placed in a vacuum drying oven and dried for 2-3 hours at 80-100℃ and a vacuum degree ≤-0.09MPa.
[0082] After drying, the iron powder was classified using an air classifier, and powder with a particle size of 50-150μm was selected as metal-based powder.
[0083] As an optional embodiment, step S5 is followed by a finished product inspection step S6:
[0084] Density testing: The density of the drive wheel was measured using the water displacement method. Five samples were randomly selected from each batch, and the arithmetic mean was taken.
[0085] Hardness testing: The surface and core hardness were tested using a Vickers hardness tester. Three evenly distributed points were selected for surface testing, and the core was tested by wire cutting.
[0086] Dimensional inspection: The inner diameter, outer diameter, and flatness are inspected using a coordinate measuring machine.
[0087] As an optional embodiment, in step S2, the cavity structure of the customized mold is adapted to the drive wheel structure:
[0088] The mold cavity includes a hub hole forming section, a tooth forming section, and a rim forming section;
[0089] The tooth profile of the gear forming section adopts an involute tooth profile with a module of 1.5mm and 6 teeth. The mold material is high-speed steel, and the cavity surface is nitrided with a surface hardness of ≥60HRC and a service life of ≥300,000 pressing cycles.
[0090] Example 1:
[0091] Fabrication of drive wheels for ultrathin powder metallurgy card components;
[0092] 1. Experimental materials and equipment;
[0093] 1.1 Experimental materials;
[0094] Metal-based powder: atomized pure iron powder (commercially available product), particle size 80μm (detected by laser particle size analyzer), loose packing density 3.0g / cm³ (compliant with GB / T1479.1-2019 standard);
[0095] Alloy additives: electrolytic copper powder (particle size 45μm, purity ≥99.9%), carbonyl nickel powder (particle size 3μm, purity ≥99.8%), and molybdenum powder (particle size 10μm, purity ≥99.5%), all of which are commercially available products;
[0096] Lubricant: Zinc stearate (analytical grade, particle size 5μm), commercially available product;
[0097] 1.2 Experimental equipment;
[0098] Mixer: GHJ-5 type, with jacketed water cooling system, speed range 0-30r / min;
[0099] Servo CNC press: YQ32-100 model, maximum pressure 1000kN, pressure control accuracy ±1MPa;
[0100] Sintering furnace: RX-1200 type, with ammonia decomposition atmosphere generator, temperature control accuracy ±5℃;
[0101] Four-column hydraulic press: Y32-200 model, maximum pressure 2000kN, adjustable pressure holding time;
[0102] Vacuum nitriding furnace: LD-Z-60 type, vacuum degree ≤-0.098MPa, temperature control accuracy ±3℃;
[0103] Customized pressing mold: made of high-speed steel, with gear tooth forming section (involute tooth shape, module 1.5mm, number of teeth 6), and the cavity surface is nitrided (surface hardness 62HRC).
[0104] Testing equipment: Laser particle size analyzer (model Mastersizer3000), water displacement density analyzer (model MDJ-300), Vickers hardness tester (model HV-1000), coordinate measuring machine (model GlobalAdvantage), metallographic microscope (model AxioObserver7).
[0105] 2. Specific preparation steps;
[0106] Step S0: Pretreatment of metal-based powder;
[0107] Place the atomized pure iron powder into a ceramic tray, spread it evenly with a thickness of ≤10mm, and put it into a vacuum drying oven.
[0108] Set the drying oven temperature to 90℃ and the vacuum degree to -0.095MPa, and dry for 2.5 hours;
[0109] After drying, the iron powder is poured into an air classifier (model QLM-100), the classifying air velocity is set to 8m / s, and iron powder with a particle size of 50-150μm is screened out for later use.
[0110] Step S1: Raw material preparation (mixed powder preparation);
[0111] Weigh the raw materials according to the following mass ratio: 1000g of pretreated pure iron powder, 30g of copper powder (accounting for 3% of the mass of pure iron powder), 20g of nickel powder (accounting for 2% of the mass of pure iron powder), 10g of molybdenum powder (accounting for 1% of the mass of pure iron powder), and 12g of zinc stearate (accounting for 1.1% of the total mass of the mixed powder).
[0112] Add the above ingredients to the mixing tank of the mixer in sequence, and then tighten the lid.
[0113] Set the mixer speed to 10 r / min, turn on the jacket water cooling (circulate 25℃ water), and start mixing; record the material temperature every 5 minutes during the mixing process to ensure that the temperature is ≤40℃.
[0114] After mixing for 25 minutes, stop the machine and pour the mixed powder into a 100-mesh standard sieve (0.154 mm aperture). Manually sieve to remove a small amount of agglomerated particles, collect the sieved mixed powder, and set it aside for later use.
[0115] Step S2: Gradient pressing (preparation of driving wheel blank);
[0116] Turn on the servo CNC press, install the customized pressing mold on the press worktable, set the mold preheating temperature to 50℃, and preheat for 30 minutes;
[0117] Start the suppression program and execute gradient pressure:
[0118] First stage: Pressure rises to 500MPa, held for 6 seconds;
[0119] Second stage: Pressure rises to 680MPa, held for 12 seconds;
[0120] After pressing is completed, the mold opens automatically, and the blank is removed by the drive wheel with a soft brush;
[0121] Step S3: Segmented sintering (preparation of sintered green body);
[0122] Start the sintering furnace and ammonia decomposition atmosphere generator in advance, and preheat the furnace body to 300°C.
[0123] The drive wheel blanks are laid flat on the tray (10 blanks per tray, with a spacing of ≥5mm), and the trays are sent into the sintering furnace chamber.
[0124] Setting the segmented sintering program:
[0125] Low-temperature preheating: Heat to 450℃ at a rate of 6℃ / min, hold for 40min, and use air as the atmosphere;
[0126] High-temperature main combustion: After the pre-combustion is completed, switch the atmosphere to ammonia decomposition atmosphere, and raise the temperature to 1120℃ at a rate of 11℃ / min, and hold for 75min;
[0127] After sintering, turn off the heating and maintain the ammonia decomposition atmosphere until the furnace temperature drops below 200°C. Open the furnace door and allow it to cool naturally to room temperature before removing the sintered billet.
[0128] Step S4: Precision shaping (preliminary preparation of the drive wheel);
[0129] The sintered green body and the customized finishing mold (cavity surface roughness Ra=0.015μm) are installed on the worktable of a four-column hydraulic press, and the mold is fixed after positioning;
[0130] Set the shaping pressure to 700MPa, hold the pressure for 10 seconds, and start the shaping program;
[0131] After shaping, remove the partially formed drive wheel;
[0132] Step S5: Surface strengthening (finished product preparation);
[0133] The initial forming drive wheel is installed into the tooling frame of the vacuum nitriding furnace. The tooling frame is made of stainless steel and the drive wheel spacing is ≥3mm.
[0134] Close the furnace door, evacuate to -0.095 MPa, and introduce a mixture of nitrogen and hydrogen (volume ratio 1:3) to raise the pressure inside the furnace to 0.18 MPa.
[0135] Set the nitriding program: heat to 520℃ at a rate of 8℃ / min, and hold for 150min;
[0136] After nitriding is completed, the heating is turned off, and the mixed gas is continued to be introduced until the furnace temperature drops below 150°C. After depressurization, the furnace door is opened, and the drive wheel of the ultra-thin structure powder metallurgy card is removed.
[0137] Step S6: Finished product inspection;
[0138] Density test: Using the water displacement method, five finished product samples were taken and their densities were measured to be 7.32 g / cm³, 7.38 g / cm³, 7.35 g / cm³, 7.36 g / cm³, and 7.34 g / cm³, respectively. The arithmetic mean of 7.35 g / cm³ was ≥ 7.2 g / cm³.
[0139] Hardness testing: Vickers hardness tester (load 500g, holding pressure 10s) was used to test the hardness of three points on the surface, which were 575HV, 585HV and 580HV respectively, with an average value of 580HV ≥ 550HV; wire cutting was used to cut the core sample, and the hardness was tested at 290HV, 300HV and 295HV, with an average value of 295HV ≥ 280HV;
[0140] Dimensional inspection: The inner diameter tolerance is H7 grade and the outer diameter tolerance is h7 grade. The flatness is 0.03mm≤0.05mm. The thickness of the nitrided layer is inspected with a metallographic microscope. The thickness of the nitrided layer in the cross section is 20μm, which meets the requirements.
[0141] Comparison with Example 2, which did not employ segmented sintering:
[0142] Using the same raw materials, equipment, and process as in Example 1, only the segmented sintering in step S3 is replaced with direct high-temperature sintering (1120℃, holding for 115 min, ammonia decomposition atmosphere), while the other steps remain unchanged:
[0143] Oxidation spots appeared on the surface of the green body after sintering (due to the failure to pre-fire to remove lubricant / plasticizer residues).
[0144] The finished product has a density of 7.05 g / cm³ (lower than 7.35 g / cm³ in Example 1) and a surface hardness of 520 HV (lower than 580 HV in Example 1), which does not meet the usage requirements.
[0145] Conclusion of the Example;
[0146] This embodiment successfully fabricated an ultra-thin powder metallurgy driving wheel with a minimum thickness of 0.5 mm through a continuous process of powder pretreatment, gradient pressing, segmented sintering, precision shaping, and low-temperature nitriding. The finished product's density, hardness, and dimensional accuracy all meet the requirements. Comparative examples show that gradient pressing can avoid cracking of ultra-thin compacts and ensure uniform density, while segmented sintering can control shrinkage and avoid oxidation. The overall process solves the technical problems of easy cracking, uneven shrinkage, and difficulty in controlling precision when preparing ultra-thin parts using traditional powder metallurgy, and has significant process advantages.
[0147] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments that can be applied to other fields. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A method for preparing a drive wheel for an ultrathin powder metallurgy card component, characterized in that, Includes the following steps: S1. Raw material preparation: Mix metal-based powder, alloy additives and lubricants in a certain proportion to obtain mixed powder; S2. Gradient pressing: The mixed powder is filled into a customized mold cavity, and a drive wheel blank is prepared by gradient pressure pressing process. The minimum thickness of the drive wheel blank is 0.5 mm. S3. Segmented sintering: The drive wheel blank is placed in the sintering furnace and subjected to low-temperature pre-firing and high-temperature main firing in sequence to obtain the sintered blank. S4. Precision shaping: The dimensions of the sintered billet are corrected by a cold finishing process to obtain the initial-formed drive wheel; S5. Surface Strengthening: The initially formed drive wheel undergoes surface strengthening treatment to finally obtain an ultra-thin structure powder metallurgy drive wheel. The density of the finished drive wheel is ≥7.2 g / cm³. 3 Flatness ≤ 0.05mm; In step S1: The metal-based powder is atomized pure iron powder with a particle size of 50-150 μm and a loose packing density of 2.8-3.2 g / cm³. The alloy additive comprises copper powder, nickel powder, and molybdenum powder, with the three components accounting for 2%–4%, 1%–3%, and 0.5%–1.5% of the mass of the metal-based powder, respectively. The lubricant is zinc stearate, and its mass percentage is 0.8%–1.2% of the total mass of the mixed powder. The gradient pressing process parameters in step S2 include: The pressing equipment is a servo CNC press, and the mold preheating temperature is 40-60℃; The gradient pressure is divided into two stages: the first stage pressure is 450-550MPa, and the holding time is 5-8s; the second stage pressure is 650-700MPa, and the holding time is 10-15s. The density of the pressed drive wheel blank is 7.15-7.25 g / cm³, and the dimensional tolerance is controlled within ±0.1 mm; the segmented sintering process parameters in step S3 include: Low-temperature pre-firing stage: heating rate is 5-8℃ / min, heating to 700-750℃, holding time is 30-45min, atmosphere is air; High-temperature main combustion stage: After pre-combustion, the temperature is increased to 1100-1150℃ at a rate of 10-12℃ / min, and the holding time is 30-60min. The atmosphere is an ammonia decomposition atmosphere. During the sintering process, the shrinkage rate of the drive wheel compact is controlled at 1.8%–2.2%, and a horizontally placed tray is used; The precision shaping process in step S4 uses a custom-made precision mold: The shaping equipment is a four-column hydraulic press with a shaping pressure of 700-750MPa and a holding time of 8-12s. The surface roughness Ra of the forming mold cavity is ≤0.02μm; After shaping, the inner diameter tolerance of the drive wheel is H7 grade, the outer diameter tolerance is h7 grade, and the flatness is ≤0.05mm; the surface strengthening treatment in step S5 is a low-temperature nitriding process. The nitriding equipment is a vacuum nitriding furnace, with a nitriding temperature of 500-550℃ and a holding time of 120-180 minutes; The nitriding atmosphere is a mixture of nitrogen and hydrogen gas with a volume ratio of 1:3, and the pressure inside the furnace is maintained at 0.15-0.2 MPa.
2. The method for preparing an ultrathin powder metallurgy driving wheel according to claim 1, characterized in that, The mixing process in step S1 is performed using a high-speed mixer: The mixer speed is set to 8-12 r / min, and the mixing time is 20-30 min. During the mixing process, the material temperature is controlled to be ≤40℃ by jacket water cooling. After the mixing is completed, the mixed powder is sieved through a 100-mesh sieve.
3. The method for preparing an ultrathin powder metallurgy driving wheel according to claim 1, characterized in that, Step S1 is preceded by a metal-based powder pretreatment step S0: The atomized pure iron powder was placed in a vacuum drying oven and dried for 2-3 hours at 80-100℃ and a vacuum degree ≤-0.09MPa. After drying, the iron powder was classified using an air classifier, and powder with a particle size of 50-150μm was selected as metal-based powder.
4. The method for preparing an ultrathin powder metallurgy driving wheel according to claim 1, characterized in that, Step S5 is followed by a finished product inspection step S6: Density testing: The density of the drive wheel was measured using the water displacement method. Five samples were randomly selected from each batch, and the arithmetic mean was taken. Hardness testing: The surface and core hardness were tested using a Vickers hardness tester. Three evenly distributed points were selected for surface testing, and the core was tested by wire cutting. Dimensional inspection: The inner diameter, outer diameter, and flatness are inspected using a coordinate measuring machine.
5. The method for preparing an ultrathin structure powder metallurgy driving wheel according to claim 1, characterized in that, In step S2, the cavity structure of the customized mold is adapted to the drive wheel structure: The mold cavity includes a hub hole forming section, a tooth forming section, and a rim forming section; The tooth profile of the gear forming section adopts an involute tooth profile with a module of 1.5mm and 6 teeth.
Citation Information
Patent Citations
Method for producing a swashplate
CN108150379A