A process for refining molten aluminum

By using a refining agent with a specific composition and adjusting the gas pressure in the aluminum refining process, the problems of hydrogen and inclusions in aluminum alloys were solved, achieving hydrogen removal, impurity removal, and grain refinement, thereby improving the material's performance.

CN121674730BActive Publication Date: 2026-11-17ZHEJIANG QIAOLAOYE ALUMINIUM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202511955236.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-23
Publication Date
2026-11-17
Estimated Expiration
2045-12-23

AI Technical Summary

Technical Problem

Existing aluminum and aluminum alloy melts contain hydrogen, alkali metals, and non-metallic inclusions, which leads to a decline in material properties, especially in high-end applications where it is difficult to meet the stringent requirements for hydrogen content and inclusion size.

Method used

An aluminum refining process is adopted, which uses a refining agent containing NaCl, KCl, Na2SiF6, Na3AlF6, Na2SO4, CaF2, NaNO3 and CeO2 nanoparticles. The refining agent is inserted into the aluminum liquid through a refining tube and the gas pressure is adjusted. Combined with slag removal and settling steps, hydrogen removal, impurity removal and grain refinement are achieved.

Benefits of technology

It effectively reduces the hydrogen content and inclusion size in molten aluminum, improves the mechanical and formability properties of the material, and meets the requirements of high-end applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This disclosure relates to the field of aluminum alloy smelting and refining, specifically an aluminum molten metal refining process. This process includes the following steps: aluminum alloy is added to a smelting furnace and heated to 660℃-710℃; after the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 730℃-750℃; then a refining agent is added to the refining tank; the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted; a refining tube is inserted into the molten aluminum and moved back and forth until refining is complete; after refining, the product is obtained by skimming off slag and allowing the mixture to settle. This disclosure provides an aluminum molten metal refining process that can simultaneously complete hydrogen removal, impurity removal, and grain refinement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of aluminum alloy smelting and refining, specifically an aluminum molten refining process. Background Technology

[0002] Currently, aluminum and aluminum alloy melts inevitably contain hydrogen, alkali metals (Na, K, Li), and non-metallic inclusions (Al2O3, SiO2, MgO, etc.). These impurities significantly reduce the mechanical properties, corrosion resistance, and formability of the material. Especially in high-end applications such as 3C exterior parts, automotive sheet metal, and aerospace forgings, the hydrogen content requirement is below 0.10 mL / 100gAl, and the inclusion size needs to be controlled below 10 μm. Therefore, melt refining is an indispensable and crucial step in the aluminum processing flow.

[0003] Therefore, there is an urgent need for an aluminum refining process that can simultaneously remove hydrogen, impurities, and refine grain size. Summary of the Invention

[0004] This disclosure provides an aluminum refining process to address the shortcomings of related technologies.

[0005] According to a first aspect of the present disclosure, an aluminum refining process is provided, the aluminum refining process comprising the following steps: Step 1: Add aluminum alloy into the melting furnace and heat it to 660℃-710℃; Step 2: After the aluminum alloy has completely melted, raise the temperature of the molten aluminum to 730℃-750℃; add the refining agent to the refining tank; then open the powder outlet valve of the refining machine and adjust the refining degassing pressure; Step 3: Insert the refining tube into the molten aluminum and move it back and forth until refining is complete; Step 4: After refining, the product is obtained by removing the residue and letting it stand.

[0006] In one aspect of the embodiments of this disclosure, the aluminum alloy used in step 1 is selected from any of the following: 1060 type aluminum alloy, 1100 type aluminum alloy, 3003 type aluminum alloy, 3004 type aluminum alloy, 3104 type aluminum alloy, 5005 type aluminum alloy, 5050 type aluminum alloy, 6060 type aluminum alloy, 6063 type aluminum alloy, 6061 type aluminum alloy, A356 type aluminum alloy, ZL101 type aluminum alloy, ADC10 type aluminum alloy, or ADC12 type aluminum alloy.

[0007] In one aspect of the embodiments of this disclosure, specifically, the aluminum alloy used in step 1 is selected from 1060 type aluminum alloy, 1100 type aluminum alloy, 6060 type aluminum alloy, ZL101 type aluminum alloy, ADC10 type aluminum alloy or ADC12 type aluminum alloy.

[0008] In one aspect of this disclosure, the refining agent comprises the following compounds in weight percentages: 20wt%-30wt% NaCl, 15wt%-25wt% KCl, 10wt%-15wt% Na2SiF6, 5wt%-10wt% Na3AlF6, 3wt%-8wt% Na2SO4, 2wt%-7wt% CaF2, 1wt%-6wt% NaNO3, and 15wt%-25wt% CeO2 nanoparticles.

[0009] In one aspect of this disclosure, preferably, the refining agent comprises the following compounds in weight percentages: 25wt%-30wt% NaCl, 18wt%-22wt% KCl, 10wt%-15wt% Na2SiF6, 5wt%-10wt% Na3AlF6, 5wt%-7wt% Na2SO4, 3wt%-6wt% CaF2, 3wt%-6wt% NaNO3, and 18wt%-22wt% CeO2 nanoparticles.

[0010] In one aspect of this disclosure, specifically, the refining agent comprises the following compounds in weight percentages: 25wt% NaCl, 20wt% KCl, 12wt% Na2SiF6, 8wt% Na3AlF6, 6wt% Na2SO4, 5wt% CaF2, 4wt% NaNO3 and 20wt% CeO2 nanoparticles.

[0011] In one aspect of this disclosure, the CeO2 nanoparticles are prepared by the following steps: Step 1-a: Dissolve Ce(NO3)3·6H2O and PVP in ethylene glycol, then add HCl dropwise; after stirring and mixing, transfer to a reaction vessel; Step 2-a: React at 150℃-170℃ for 2-5 hours; after the reaction is complete, cool to room temperature, wash and dry to obtain the intermediate product; Step 3-a: The intermediate product obtained in step 2-a is calcined to obtain the CeO2 nanoparticles.

[0012] In one aspect of this disclosure, the CeO2 nanoparticles are prepared by the following steps: Step 1-a: Dissolve 5g of Ce(NO3)3·6H2O and 2g of PVP in 45-60mL of ethylene glycol, then add 10mL of 1mol / L HCl dropwise; after stirring and mixing, transfer to a reaction vessel; Step 2-a: React at 160℃ for 3 hours in an electrically heated drying oven; after the reaction is completed, cool to room temperature, and obtain the intermediate product after washing and drying. Step 3-a: The intermediate product obtained in step 2-a is placed in a muffle furnace and heated from room temperature to 500°C at a rate of 1°C / mL for 4 hours; then cooled to room temperature to obtain the CeO2 nanoparticles.

[0013] In one aspect of this disclosure, the amount of the refining agent is 0.35%-0.7% of the mass of the molten aluminum.

[0014] In one aspect of the embodiments of this disclosure, the degassing pressure is selected from 0.1-0.4 MPa.

[0015] In one aspect of this disclosure, the aluminum refining process includes the following steps: Step 1: Add aluminum alloy into the melting furnace and heat it to 700℃; Step 2: After the aluminum alloy has completely melted, adjust the composition of the molten aluminum. Step 3: Raise the temperature of the aluminum liquid obtained in Step 2 to 740℃; add the refining agent to the refining tank, the amount of the refining agent being 0.35%-0.7% of the mass of the aluminum liquid; then open the powder outlet valve of the refining machine and adjust the refining degassing pressure to 0.1-0.4MPa; Step 4: Insert the refining tube into the molten aluminum obtained in Step 2 and move it back and forth until the refining is complete; Step 5: After refining, the product is obtained by removing the residue and letting it stand.

[0016] Compared with the prior art, the beneficial effects of this disclosure are: this disclosure provides an aluminum refining process that can simultaneously complete hydrogen removal, impurity removal and grain refinement. Detailed Implementation

[0017] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present application will now be described in detail with reference to the embodiments.

[0018] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this disclosure. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this disclosure as detailed in the appended claims.

[0019] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. The embodiments described herein are illustrative in nature and are used to provide a basic understanding of this application. The embodiments of this application should not be construed as limiting this application.

[0020] For the sake of brevity, this article only discloses a few specific numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0021] In this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0022] In this description, unless otherwise stated, "above" and "below" include the stated number.

[0023] Unless otherwise stated, the terms used in this disclosure have their common meanings as commonly understood by those skilled in the art. Unless otherwise stated, the values ​​of the parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this disclosure).

[0024] The term "about" is used to describe and indicate small variations. When used in conjunction with an event or situation, the term may refer to examples in which the event or situation occurred precisely or in examples in which the event or situation occurred very approximately. For example, when used in conjunction with numerical values, the term may refer to a range of variation less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. Additionally, quantities, ratios, and other numerical values ​​are sometimes presented in range format herein. It should be understood that such range format is for convenience and brevity and should be interpreted flexibly to include not only numerical values ​​explicitly specified as range limits but also all individual numerical values ​​or subranges covered within the range, as if each numerical value and subrange were explicitly specified.

[0025] The list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another instance, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.

[0026] In this disclosure, the composition adjustment of molten aluminum refers to the adaptive addition of elements not present in the refining agent; for example, when using ADC12 aluminum alloy as raw material, the composition of the molten aluminum is adjusted to Fe of 0.9wt%-1.0% and Cu of 1.65wt%-3.5wt%. This disclosure does not limit the specific content of the composition adjustment, which can be adaptively selected according to different raw materials.

[0027] In this disclosure, the role of NaCl and KCl in the refining agent is to form a low-melting eutectic, reduce the overall melting point and viscosity, and cover the liquid surface to isolate it from air.

[0028] In this disclosure, the role of Na2SiF6 in the refining agent is to carry hydrogen and inclusions to the surface after decomposition.

[0029] In this disclosure, the role of Na3AlF6 in the refining agent is to dissolve the oxide film, causing it to change from a solid-solid interface to a solid-liquid slag phase, which facilitates its aggregation and removal.

[0030] In this disclosure, the role of Na2SO4 in the refining agent is to oxidize impurities such as Fe and Cr, helping them to float to the surface.

[0031] In this disclosure, the role of CaF2 in the refining agent is to increase the interfacial tension between the refining agent and the molten aluminum, which facilitates the removal of slag phase aggregates.

[0032] In this disclosure, the role of NaNO3 in the refining agent is to enhance the oxidizing atmosphere and assist in the removal of hydrogen and slag.

[0033] In this disclosure, in the refining agent, the role of CeO2 nanoparticles is to provide oxygen-rich vacancies on the surface (CeO2 nanoparticles). 4+ / Ce 3+ (Circulation) The reaction of Al2O3 film causes lattice distortion and fragmentation of inclusions; at the same time, it serves as a heterogeneous nucleation substrate to refine α-Al and eutectic silicon.

[0034] The present disclosure will be further described below by way of specific embodiments. Unless otherwise specified, all chemical reagents used in the embodiments of this disclosure are obtained through conventional commercial means. Unless otherwise specified, all contents mentioned below are mass contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.

[0035] Examples and Comparative Examples Example 1 Example 1 includes the following steps: 1. Preparation of CeO2 nanoparticles: 5g of Ce(NO3)3·6H2O and 2g of PVP were dissolved in 48mL of ethylene glycol, and then 10mL of 1mol / L HCl was added dropwise. After stirring and mixing, the mixture was transferred to a reaction vessel and reacted at 160℃ for 3h in an electric heating drying oven. After the reaction was completed, the mixture was cooled to room temperature, washed, and dried to obtain an intermediate product. The intermediate product was placed in a muffle furnace and calcined at 500℃ for 4h by increasing the temperature from room temperature to 1℃ / mL. Then it was cooled to room temperature to obtain CeO2 nanoparticles.

[0036] The above steps can be repeated multiple times to prepare enough CeO2 nanoparticles for the following reaction.

[0037] 2. Preparation of refining agent: 25 parts by weight of NaCl, 20 parts by weight of KCl, 12 parts by weight of Na2SiF6, 8 parts by weight of Na3AlF6, 6 parts by weight of Na2SO4, 5 parts by weight of CaF2, 4 parts by weight of NaNO3 and 20 parts by weight of the aforementioned prepared CeO2 nanoparticles were added to a V-type mixer and mixed at 50 rpm for 5 min to obtain a refining agent.

[0038] 3. Aluminum refining: 6060 aluminum alloy is added to a smelting furnace and heated to 700°C. After the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 740°C. A refining agent is added to the refining tank at a rate of 0.5% of the mass of the molten aluminum. Then, the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted to 0.25 MPa. The refining tube is inserted into the molten aluminum and moved back and forth until the refining is completed. After slag removal and settling, the product is obtained.

[0039] Example 2 Example 2 includes the following steps: 1. Preparation of CeO2 nanoparticles: 5g of Ce(NO3)3·6H2O and 2g of PVP were dissolved in 48mL of ethylene glycol and then transferred to a reaction vessel. The mixture was reacted at 160℃ for 3h in an electrically heated drying oven. After the reaction was completed, the mixture was cooled to room temperature, washed, and dried to obtain an intermediate product. The intermediate product was placed in a muffle furnace and calcined at 500℃ for 4h by increasing the temperature from room temperature to 1℃ / mL. The mixture was then cooled to room temperature to obtain CeO2 nanoparticles.

[0040] The above steps can be repeated multiple times to prepare enough CeO2 nanoparticles for the following reaction.

[0041] 2. Preparation of refining agent: 25 parts by weight of NaCl, 20 parts by weight of KCl, 12 parts by weight of Na2SiF6, 8 parts by weight of Na3AlF6, 6 parts by weight of Na2SO4, 5 parts by weight of CaF2, 4 parts by weight of NaNO3 and 20 parts by weight of the aforementioned prepared CeO2 nanoparticles were added to a V-type mixer and mixed at 50 rpm for 5 min to obtain a refining agent.

[0042] 3. Aluminum refining: 6060 aluminum alloy is added to a smelting furnace and heated to 700°C. After the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 740°C. A refining agent is added to the refining tank at a rate of 0.5% of the mass of the molten aluminum. Then, the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted to 0.25 MPa. The refining tube is inserted into the molten aluminum and moved back and forth until the refining is completed. After slag removal and settling, the product is obtained.

[0043] Example 3 Example 3 includes the following steps: 1. Preparation of CeO2 nanoparticles: 5 mmol of Ce(NO3)3·6H2O was dissolved in 70 mL of water, then 9 mmol of urea was added and mixed with stirring. Then 10 mL of H2O2 was added. The mixture was then reacted at 230 °C for 10 h. After the reaction was completed, the mixture was cooled to room temperature, washed, and dried to obtain an intermediate product. The intermediate product was placed in a muffle furnace and heated from room temperature to 500 °C at a rate of 1 °C / mL for 4 h. The mixture was then cooled to room temperature to obtain CeO2 nanoparticles.

[0044] The above steps can be repeated multiple times to prepare enough CeO2 nanoparticles for the following reaction.

[0045] 2. Preparation of refining agent: 25 parts by weight of NaCl, 20 parts by weight of KCl, 12 parts by weight of Na2SiF6, 8 parts by weight of Na3AlF6, 6 parts by weight of Na2SO4, 5 parts by weight of CaF2, 4 parts by weight of NaNO3 and 20 parts by weight of the aforementioned prepared CeO2 nanoparticles were added to a V-type mixer and mixed at 50 rpm for 5 min to obtain a refining agent.

[0046] 3. Aluminum refining: 6060 aluminum alloy is added to a smelting furnace and heated to 700°C. After the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 740°C. A refining agent is added to the refining tank at a rate of 0.5% of the mass of the molten aluminum. Then, the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted to 0.25 MPa. The refining tube is inserted into the molten aluminum and moved back and forth until the refining is completed. After slag removal and settling, the product is obtained.

[0047] Example 4 Example 4 includes the following steps: 1. Preparation of CeO2 nanoparticles: 8g of glucose was dissolved in 40mL of water and then transferred to a reaction vessel. The mixture was reacted at 150℃ for 4h to obtain carbon spheres as templates. 30mL of 0.012mol / L Ce(NO3)3 aqueous solution was prepared, and 0.2g of the carbon spheres as templates were added. Then, 0.58g of HMT (hexamethylenetetramine) was added, and the mixture was refluxed in an oil bath at 75℃ for 2h. After the reaction was completed, the mixture was cooled to room temperature, washed, and dried to obtain an intermediate product. The intermediate product was placed in a muffle furnace and calcined at 600℃ for 5h by increasing the temperature from room temperature to 1℃ / mL. The mixture was then cooled to room temperature to obtain CeO2 nanoparticles.

[0048] The above steps can be repeated multiple times to prepare enough CeO2 nanoparticles for the following reaction.

[0049] 2. Preparation of refining agent: 25 parts by weight of NaCl, 20 parts by weight of KCl, 12 parts by weight of Na2SiF6, 8 parts by weight of Na3AlF6, 6 parts by weight of Na2SO4, 5 parts by weight of CaF2, 4 parts by weight of NaNO3 and 20 parts by weight of the aforementioned prepared CeO2 nanoparticles were added to a V-type mixer and mixed at 50 rpm for 5 min to obtain a refining agent.

[0050] 3. Aluminum refining: 6060 aluminum alloy is added to a smelting furnace and heated to 700°C. After the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 740°C. A refining agent is added to the refining tank at a rate of 0.5% of the mass of the molten aluminum. Then, the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted to 0.25 MPa. The refining tube is inserted into the molten aluminum and moved back and forth until the refining is completed. After slag removal and settling, the product is obtained.

[0051] Comparative Example 1 Comparative Example 1 includes the following steps: 1. Preparation of refining agent: 25 parts by weight of NaCl, 20 parts by weight of KCl, 12 parts by weight of Na2SiF6, 8 parts by weight of Na3AlF6, 6 parts by weight of Na2SO4, 5 parts by weight of CaF2 and 4 parts by weight of NaNO3 were added to a V-type mixer and mixed at 50 rpm for 5 min to obtain the refining agent.

[0052] 2. Aluminum refining: 6060 aluminum alloy is added to a smelting furnace and heated to 700°C. After the aluminum alloy is completely melted, the temperature of the molten aluminum is raised to 740°C. A refining agent is added to the refining tank at a rate of 0.5% of the mass of the molten aluminum. Then, the powder outlet valve of the refining machine is opened, and the refining degassing pressure is adjusted to 0.25 MPa. The refining tube is inserted into the molten aluminum and moved back and forth until the refining is completed. After slag removal and settling, the product is obtained.

[0053] The specific surface area and pore volume data of the CeO2 nanoparticles prepared in Examples 1 to 4 were obtained by N2 physisorption analysis. The testing instrument was an Autosorb-iQ-AG-MP fully automated specific surface area and pore volume analyzer. Before analysis, the prepared CeO2 nanoparticles were degassed at 300℃ for 3 h for pretreatment. The specific surface area and pore volume data were calculated using the Brunauer-Emmett-Teller (BET) method and the Barrett-Joyner-Halenda (BJH) method, respectively. The results are shown in the table below.

[0054] <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> Example 1 109.2 0.352 Example 2 47.1 0.073 Example 3 84.5 0.159 Example 4 142.9 0.136 The hydrogen and slag contents of the products obtained in the examples and comparative examples were detected using a hydrogen analyzer and a slag analyzer, and the results are shown in the table below. The products obtained in the examples and comparative examples were cast into aluminum alloy ingots, and then samples were taken to test the tensile strength, and the results are shown in the table below.

[0055] Hydrogen content (mL / 100gAl) <![CDATA[Slag content (mm 2 / kgAl)]]> Tensile strength (MPa) Example 1 0.118 0.075 224 Example 2 0.198 0.136 187 Example 3 0.167 0.122 195 Example 4 0.150 0.118 209 Comparative Example 1 0.227 0.204 180 As can be seen, the performance of the product in Example 1 is significantly better than that of the other examples and comparative examples. This is because CeO2 in Example 1 has both a high specific surface area and a high pore volume. The higher specific surface area can provide more exposed crystal faces; it can cause the Al2O3 film to undergo a regenerative reaction, resulting in lattice distortion and breakage of inclusions; at the same time, it can serve as a heterogeneous nucleation substrate, refining α-Al and eutectic silicon; while the high pore volume can store the products of the decomposition of other compounds in the refining agent, such as the SiF4 microbubble portion decomposed by Na3AlF6, in the pores and then slowly release them into the aluminum melt, prolonging the bubble-inclusion collision time and improving the slag and hydrogen removal capabilities.

[0056] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This disclosure is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein.

Claims

1. An aluminum refining process, characterized in that, The aluminum refining process includes the following steps: Step 1: Add aluminum alloy into the melting furnace and heat it to 660℃-710℃; Step 2: After the aluminum alloy has completely melted, raise the temperature of the molten aluminum to 730℃-750℃; add the refining agent to the refining tank; then open the powder outlet valve of the refining machine and adjust the refining degassing pressure; Step 3: Insert the refining tube into the molten aluminum and move it back and forth until refining is complete; Step 4: After refining, the product is obtained by removing the residue and letting it stand. The refining agent contains the following compounds in weight percentage: 20wt%-30wt% NaCl, 15wt%-25wt% KCl, 10wt%-15wt% Na2SiF6, 5wt%-10wt% Na3AlF6, 3wt%-8wt% Na2SO4, 2wt%-7wt% CaF2, 1wt%-6wt% NaNO3, and 15wt%-25wt% CeO2 nanoparticles; The CeO2 nanoparticles were prepared by the following steps: Step 1-a: Dissolve 5g of Ce(NO3)3·6H2O and 2g of PVP in 45-60mL of ethylene glycol, then add 10mL of 1mol / L HCl dropwise; after stirring and mixing, transfer to a reaction vessel; Step 2-a: React at 160℃ for 3 hours in an electrically heated drying oven; after the reaction is completed, cool to room temperature, and obtain the intermediate product after washing and drying. Step 3-a: The intermediate product obtained in step 2-a is placed in a muffle furnace and heated from room temperature to 500°C at a rate of 1°C / min, and calcined for 4 hours; then cooled to room temperature to obtain the CeO2 nanoparticles.

2. The aluminum refining process according to claim 1, characterized in that, The aluminum alloy used in step 1 is selected from any of the following: 1060 type aluminum alloy, 1100 type aluminum alloy, 3003 type aluminum alloy, 3004 type aluminum alloy, 3104 type aluminum alloy, 5005 type aluminum alloy, 5050 type aluminum alloy, 6060 type aluminum alloy, 6063 type aluminum alloy, 6061 type aluminum alloy, A356 type aluminum alloy, ZL101 type aluminum alloy, ADC10 type aluminum alloy, or ADC12 type aluminum alloy.

3. The aluminum refining process according to claim 1, characterized in that, The refining agent contains the following compounds in weight percentage: 25wt% NaCl, 20wt% KCl, 12wt% Na2SiF6, 8wt% Na3AlF6, 6wt% Na2SO4, 5wt% CaF2, 4wt% NaNO3 and 20wt% CeO2 nanoparticles.

4. The aluminum refining process according to claim 1, characterized in that, The amount of the refining agent used is 0.35%-0.7% of the mass of the molten aluminum.

5. The aluminum refining process according to claim 1, characterized in that, The degassing pressure is selected from 0.1-0.4 MPa.

6. The aluminum refining process according to claim 1, characterized in that, The aluminum refining process includes the following steps: Step 1: Add aluminum alloy into the melting furnace and heat it to 700℃; Step 2: After the aluminum alloy has completely melted, adjust the composition of the molten aluminum. Step 3: Raise the temperature of the aluminum liquid obtained in Step 2 to 740℃; add the refining agent to the refining tank, the amount of the refining agent being 0.35%-0.7% of the mass of the aluminum liquid; then open the powder outlet valve of the refining machine and adjust the refining degassing pressure to 0.1-0.4MPa; Step 4: Insert the refining tube into the molten aluminum obtained in Step 2 and move it back and forth until the refining is complete; Step 5: After refining, the product is obtained by removing the residue and letting it stand.

Citation Information

Patent Citations

  • Environment-friendly secondary aluminum refining agent and using method thereof

    CN108359810A

  • Hollow-structure CeO2@C core-shell nano composite material as well as preparation method and application thereof

    CN108807943A

  • Refining method for reducing impurity content of molten aluminum

    CN115109957A