A low-temperature resistant carbon fiber reinforced polyamide material for drones in cold regions and its preparation method
By combining PEBAX polyether amide elastomer modified with nano-modified toughening agents and amino-modified carbon nanotubes with silane-modified carbon fibers, the problem of brittle fracture of traditional materials in low-temperature environments was solved, achieving high modulus and toughening effect of UAV materials in cold regions, and improving the low-temperature performance of UAVs.
Patent Information
- Application Number
- CN202511973239.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-12-25
AI Technical Summary
Traditional polyamide materials are prone to brittle fracture at low temperatures, and carbon fiber reinforcement reduces toughness. Existing toughening systems are not effective in ultra-low temperature environments, making drones more susceptible to crashes when used in cold regions.
By using nano-modified toughening agents and aminated carbon nanotubes to modify PEBAX polyether amide elastomers and silane-modified carbon fibers, microphase separation is generated at the microscale and interfacial compatibility is improved. Combined with long-chain carbon nylon substrates, low-temperature resistant carbon fiber reinforced polyamide materials are prepared.
While maintaining high modulus, it significantly improves the low-temperature toughness and interlaminar strength of the material, enhances the material's performance in cold regions, and prevents brittle fracture of UAV structural components.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-performance nylon composite materials, specifically relating to a low-temperature resistant carbon fiber reinforced polyamide (PA) material suitable for drones in cold regions, its preparation method, and its application. Background Technology
[0002] Polyamide (PA) has become the preferred thermoplastic material for UAV shells, arms, propellers, and other structural components due to its lightweight, high strength, oil resistance, and ease of processing. However, when the service environment temperature is below -40°C, the traditional PA6 / PA66 matrix will experience brittle fracture under instantaneous impact (landing, gusts, catapult takeoff), leading to crashes. Existing toughening systems generally use maleic anhydride-grafted POE (POE-g-MAH), but its glass transition temperature is still insufficient for the harsh environment of ultra-low temperatures, and the retention rate of low-temperature notched impact strength needs to be improved.
[0003] While carbon fiber (CF) can significantly improve the rigidity of polycarbonate (PA), it further reduces toughness and exacerbates low-temperature brittleness. Simultaneously, the high surface inertness of CF results in low interfacial shear strength with PA, making interlaminar delamination a new potential risk for fatigue failure in UAVs. Therefore, achieving both high modulus and ultra-low temperature toughening has become a bottleneck in the field of materials for cold-weather UAVs.
[0004] PEBAX (polyether-polyamide block copolymer) has an extremely low glass transition temperature (Tg) in its polyether segments, resulting in good compatibility with PA materials due to its structural characteristics. The polyether segments of PEBAX can maintain chain segment movement at low temperatures, making it an ideal low-temperature toughening agent. However, PEBAX has a low melt viscosity, and the heat resistance of the polyether segments poses a risk of thermal degradation. Directly extruding and blending PEBAX with PA materials carries the risk of degradation and chain breakage, leading to lower-than-expected toughening efficiency. Furthermore, commercially available carbon fibers (CFs) are mostly epoxy or PU coated, exhibiting poor compatibility with the PA matrix and low interfacial shear strength, making it difficult to fully realize the reinforcing potential of carbon fibers. Summary of the Invention
[0005] To address the shortcomings and deficiencies of existing technologies, the primary objective of this invention is to provide a low-temperature resistant carbon fiber reinforced polyamide (PA) material suitable for drones operating in cold regions. This material, while maintaining the high modulus and durability of carbon fiber reinforced polyamide (PA), effectively improves the low-temperature performance of drones, meeting the complex operational needs of drones in special environments such as high-latitude regions.
[0006] The second objective of this invention is to provide a method for preparing the aforementioned low-temperature resistant carbon fiber reinforced polyamide (PA) material suitable for drones in cold regions.
[0007] A third objective of this invention is to provide an application of a low-temperature resistant carbon fiber reinforced polyamide (PA) material suitable for drones in cold regions.
[0008] The primary objective of this invention is achieved through the following technical solution: A low-temperature resistant carbon fiber reinforced polyamide (PA) material for drones used in high-altitude and cold-weather regions is composed of the following components by weight percentage: Nylon resin 65.0%–85.0% Silane-modified carbon fiber 10.0–30.0% Nano-modified toughening agent 1.0–6.0% Processing aids 0.1–1.0% Antioxidant 0.1–1.0% The sum of the mass percentages of the above components is 100%; The preparation method of the silane-modified carbon fiber is as follows: after degumming the carbon fiber, it is impregnated with a modifier of 0.3%-0.5% by mass, and then air-dried or oven-dried to obtain silane-modified carbon fiber; the carbon fiber is at least one of chopped strands with a tensile strength grade of T-700 or T-800; the modifier is KH-550 aminosilane coupling agent; the mass ratio of the carbon fiber to the modifier is 1:9~3:7. The preparation method of the nano-modified toughening agent is as follows: PEBAX polyether amide elastomer is mixed with aminated carbon nanotubes (CNT-NH2) and then cut into small particles, which are the nano-modified toughening agent; the mass fraction of aminated carbon nanotubes (CNT-NH2) in the nano-modified toughening agent is 0.5~1.5%; the mixing temperature is 150-180℃ and the mixing time is 3~5 min.
[0009] Preferably, the nylon resin is at least one of nylon 610, nylon 612, nylon 1010, nylon 1012, nylon 1212, nylon 11, and nylon 12 long carbon chain nylon resin.
[0010] Preferably, the processing aid is at least one of the following: silicone-based lubricants, fatty acid amides, metal stearates, waxes, ester lubricants, and polytetrafluoroethylene (PTFE) micropowders.
[0011] Preferably, the antioxidant is at least one of hindered phenolic antioxidants, thioester antioxidants, phosphite antioxidants, and ester antioxidants.
[0012] The second objective of this invention is achieved through the following technical solution: A method for preparing low-temperature resistant carbon fiber reinforced polyamide (PA) material for unmanned aerial vehicles (UAVs) in cold regions includes the following steps: (1) Nylon resin, compatibilizer, processing aid, nano-modified toughening agent and antioxidant are mixed at high speed to obtain premix I; (2) Add premix I from the main feed port of the twin-screw extruder, melt extrude and granulate. Set the temperature of each section of the twin-screw extruder to 180℃, 240℃, 245℃, 250℃, 260℃, 230℃, 230℃, 220℃, 220℃, and the die head temperature to 240℃. The screw speed is 300-600 rpm. (3) The silane-modified carbon fiber is added from the side feed port of the twin-screw extruder, which is located in the sixth section of the extruder barrel; (4) After melting and extruding all the raw materials, cooling, air drying, pelletizing, vibrating and sieving, and homogenizing, low-temperature resistant carbon fiber reinforced polyamide (PA) material for UAVs in cold regions can be prepared.
[0013] Preferably, the high-speed mixing speed in step (1) is 800-1500 rpm, and the high-speed mixing time is 1-2 minutes.
[0014] The third objective of this invention is achieved through the following technical solution: Application of a low-temperature resistant carbon fiber reinforced polyamide (PA) material suitable for drones in cold regions in drone equipment.
[0015] Specifically, the UAV structural components include the UAV frame, arms, propellers, propeller guards, and mid-frame.
[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The preparation method of the present invention uses a nano-modified toughening agent. Based on the traditional low-temperature toughened carbon fiber reinforced PA material with maleic anhydride grafted POE, the PEBAX polyether amide elastomer with better low-temperature resistance is used. Its unique polyether and amide soft and hard segment structure can produce micro-phase separation at the micro scale, which effectively improves the toughness of the toughening agent. Furthermore, because of its intrinsic compatibility with PA material, the nano-modified toughening agent has better bonding properties than traditional general polyolefin toughening agents. (2) In this invention, conventional PEBAX polyether amide elastomer is modified by nano-hybridization. Aminated carbon nanotubes are mixed with PEBAX polyether amide elastomer at 150-180°C. Under these conditions, PEBAX will not easily degrade during the mixing process because the soft segment has a relatively low melting point. Moreover, carbon nanotubes can be distributed more in the soft segment rubber phase of PEBAX, resulting in better microphase toughening effect.
[0017] (3) The present invention adds carbon nanotubes to conventional PEBAX to effectively improve the toughening effect. Firstly, PEBAX provides toughness mainly by the plastic deformation of the soft segment. When subjected to impact, carbon nanotubes are distributed in the soft segment to "hold" the soft segment, and at the same time generate a large number of nanoscale cavities, which can effectively improve the energy absorption capacity of PEBAX.
[0018] (4) This invention selects special aminated carbon nanotubes and simultaneously modifies the carbon fibers with aminosilane coupling. The combined effect of these two points is as follows: during the processing and molding process, the carbon nanotubes present in the PEBAX toughening agent combine with the aminosilane groups on the surface of the carbon fiber, allowing a thin layer of toughening agent to adhere to the surface of the carbon fiber, effectively improving the interlayer strength and preventing a significant decrease in strength due to the addition of the toughening agent. Furthermore, the aminated carbon nanotubes also have good compatibility with the nylon substrate itself, improving the overall integrity of the material.
[0019] (5) Based on the traditional PA6 and PA66, the present invention uses long carbon chain nylon as the base material. The long carbon chain in its structure has good compatibility with the polyester soft segment of PEBAX and the processing temperature is lower, which further prevents the degradation of PEBAX elastomer. Detailed Implementation
[0020] The present invention will be further described in detail below with reference to embodiments, but the embodiments of the present invention are not limited thereto. All raw materials involved in the present invention can be purchased directly from the market. For process parameters not specifically specified, conventional techniques can be referred to.
[0021] The raw materials used in the embodiments and comparative examples of this invention are as follows: Polyhexamethylene sebacate (Nylon 610 resin): PA610, Shandong Xianglong New Materials Co., Ltd.; Chopped strand carbon fiber (T-700): CFUW-MC C-6, Toray Industries, Japan; Polyetheramide elastomer (PEBAX): PEBAX 2533, ARKEMA, France. Maleic anhydride grafted POE: N493, Dow Chemical, USA; Aminated carbon nanotubes: Beijing Deco Island Gold Technology Co., Ltd.; Silane coupling agent: KH550, Hangzhou Jessica Chemical Co., Ltd.; Antioxidant: 1098 (N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexamethylenediamine), Ciba, Switzerland; TFB 117, Clariant, Switzerland; Processing aids: SG-100A; silicone powder Examples 1 to 7 Those skilled in the art, combining conventional knowledge and referring to the preparation steps in Table 1, can make adaptive modifications to Examples 1 to 7 of the present invention.
[0022] Weigh the raw materials according to the formulas described in Table 1, and then prepare the materials. The materials described in Examples 1 to 7 of this invention are prepared according to the following steps: (1) Slowly and thoroughly mix polyether amide elastomer (PEBAX) with 1% by mass of aminated carbon nanotubes (CNT-NH2), then put it into an internal mixer and mix at 150-180℃ for 3-5 minutes to obtain nano-modified toughening agent material blocks; (2) Cut the nano-modified toughening agent block into rice-grain-sized particles to obtain the nano-modified toughening agent; (3) The carbon fiber is first placed in a low temperature muffle furnace at 450℃ for surface degumming treatment, and then the treated carbon fiber is impregnated with a KH-550 water-alcohol solution with a mass fraction of 0.3%-0.5% (between 1 / 9 and 3 / 7), and then air-dried or oven-dried to obtain silane modified carbon fiber. (4) Nylon resin, compatibilizer, processing aid, nano-modified toughening agent and antioxidant are mixed at high speed to obtain premix I; the high speed mixing speed is 800-1500 rpm and the high speed mixing time is 1-2 minutes; (5) Add premix I from the main feed port of the twin-screw extruder, melt extrude and granulate. Set the temperature of each section of the twin-screw extruder to 180℃, 240℃, 245℃, 250℃, 260℃, 230℃, 230℃, 220℃, 220℃, the die head temperature to 240℃, and the screw speed to 300-600 rpm. (6) Add silane-modified carbon fiber from the side feed port of the twin-screw extruder. The side feed port is located in the sixth section of the extruder barrel and is fed according to the proportion. (7) The raw materials of the formulation system are melted, extruded, cooled, air-dried, granulated, vibrated and sieved, and homogenized to prepare the product.
[0023] Table 1
[0024] Note: Density was tested according to ISO 1183-1 standard; tensile strength was tested according to ISO 527-2 standard; flexural strength and flexural modulus were tested according to ISO 178 standard; cantilever beam notched impact and low-temperature cantilever beam notched impact strength were tested according to ISO 180 standard, with the low-temperature impact specimens frozen for 24 hours.
[0025] As shown in Table 1 above, comparing Examples 1 to 3, adding maleic anhydride-grafted POE and PEBAX elastomer to the carbon fiber reinforced long-chain nylon system can both have a significant toughening effect. At room temperature, the toughening efficiency of the two is not significantly different, with PEBAX showing a slightly better toughening effect than maleic anhydride-grafted POE. However, the strength and modulus of the carbon fiber reinforced PA material toughened by PEBAX are actually higher, indicating that PEBAX can play a compatibilizing role between carbon fiber and long-chain nylon. Moreover, under extreme low-temperature conditions, the toughening effect of PEBAX elastomer is more obvious due to its lower glass transition temperature (-65℃). Comparing Examples 3 and 4, it can be seen that increasing the amount of PEBAX from 3 parts to 6 parts significantly improves the impact strength, but excessive addition leads to a significant decrease in tensile strength and modulus of the product, thus affecting the carbon fiber... The performance advantages of reinforced nylon materials are negated, and the amount of PEBAX toughening agent added should be controlled in actual use. Comparing Examples 3 and 5, it can be seen that the addition of carbon nanotubes improves the toughening efficiency of the PEBAX toughening agent. This is due to the reinforcing effect of carbon nanotubes at the microscale; their special structure can hold the toughening agent in place when the material is impacted, effectively dissipating the energy from the impact. Comparing Examples 6 and 7, it can be seen that in actual use, adding aminated carbon nanotubes alone has no significant difference in effect, and the toughening efficiency remains basically unchanged. However, when the nano-modified toughening agent (aminated carbon nanotube-modified PEBAX elastomer) and aminosilane-modified carbon fiber are used simultaneously, their synergistic effect is more obvious. The combination of the two can achieve a better toughening effect, and the modulus decrease caused by the addition of the toughening agent is significantly reduced. After the nano-modified toughening agent (aminated carbon nanotube-modified PEBAX elastomer) and aminosilane-modified carbon fiber are combined, the interlaminar strength between the carbon fiber and the substrate is improved, strengthening the overall performance of the material.
[0026] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A low-temperature resistant carbon fiber reinforced polyamide material for unmanned aerial vehicles (UAVs) in cold regions, characterized in that, It consists of the following components by mass percentage: Nylon resin 65.0%–85.0% Silane-modified carbon fiber 10.0–30.0% Nano-modified toughening agent 1.0–6.0% Processing aids 0.1–1.0% Antioxidant 0.1–1.0% The sum of the mass percentages of the above components is 100%; The preparation method of the silane-modified carbon fiber is as follows: after degumming the carbon fiber, it is impregnated with a modifier of 0.3%-0.5% by mass, and then air-dried or oven-dried to obtain silane-modified carbon fiber; the carbon fiber is at least one of chopped strands with a tensile strength grade of T-700 or T-800; the modifier is KH-550 aminosilane coupling agent; the mass ratio of the carbon fiber to the modifier is 1:9~3:
7. The preparation method of the nano-modified toughening agent is as follows: PEBAX polyether amide elastomer is mixed with aminated carbon nanotubes and then cut into small particles, which are the nano-modified toughening agent; the mass fraction of aminated carbon nanotubes in the nano-modified toughening agent is 0.5~1.5%; the mixing temperature is 150-180℃ and the mixing time is 3~5min.
2. The low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions according to claim 1, characterized in that, The nylon resin is at least one of nylon 610, nylon 612, nylon 1010, nylon 1012, nylon 1212, nylon 11, and nylon 12 long carbon chain nylon resin.
3. The low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions according to claim 1, characterized in that, The processing aid is at least one of the following: silicone-based lubricants, fatty acid amides, metal stearates, waxes, ester lubricants, and polytetrafluoroethylene micropowders.
4. The low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions according to claim 1, characterized in that, The antioxidant is at least one of hindered phenolic antioxidants, thioester antioxidants, phosphite antioxidants, and ester antioxidants.
5. A method for preparing a low-temperature resistant carbon fiber reinforced polyamide material for unmanned aerial vehicles (UAVs) in cold regions according to any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Nylon resin, compatibilizer, processing aid, nano-modified toughening agent and antioxidant are mixed at high speed to obtain premix I; (2) Add premix I from the main feed port of the twin-screw extruder, melt extrude and granulate. Set the temperature of each section of the twin-screw extruder to 180℃, 240℃, 245℃, 250℃, 260℃, 230℃, 230℃, 220℃, 220℃, and the die head temperature to 240℃. The screw speed is 300-600 rpm. (3) The silane-modified carbon fiber is added from the side feed port of the twin-screw extruder, which is located in the sixth section of the extruder barrel; (4) After melting, extruding, cooling, air drying, pelletizing, vibrating and sieving, and homogenizing all the raw materials, low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions can be prepared.
6. The method for preparing low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions according to claim 5, characterized in that, The high-speed mixing speed in step (1) is 800-1500 rpm, and the high-speed mixing time is 1-2 minutes.
7. The application of a low-temperature resistant carbon fiber reinforced polyamide material for unmanned aerial vehicles (UAVs) in cold regions according to any one of claims 1 to 4 in UAV equipment.
8. The application of the low-temperature resistant carbon fiber reinforced polyamide material for UAVs in cold regions according to claim 7 in UAV structural components, characterized in that, The structural components of the UAV include the UAV frame, arms, propellers, propeller guards, and mid-frame.
Citation Information
Patent Citations
Carbon fiber reinforced polyamide composite material and preparation method thereof
CN102229747A
Carbon fiber reinforced polyamide composite material product and preparation method thereof
CN110423462A