Few-layer Ti3C2 heterostructure constructed by bifunctional molecular bridge as well as preparation method and application of few-layer Ti3C2 heterostructure

By using 11-aminoundecanoic acid as a bifunctional molecular bridge, the interlayer spacing of MoS2 is expanded and stable bonds are formed with the surface of few-layer MXene, which solves the problems of narrow interlayer spacing of MoS2 and aggregation of traditional intercalating agents, and realizes the stable construction and performance improvement of heterostructures.

CN122035865APending Publication Date: 2026-05-15HUAIBEI NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610176338.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-06
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

In the prior art, the narrow interlayer spacing of MoS2 leads to low conductivity, which limits its electrochemical performance. Furthermore, traditional organic cationic intercalating agents are prone to aggregation and competitive adsorption during the construction of heterostructures, hindering the uniform construction of heterostructures.

Method used

Using 11-aminoundecanoic acid as a bifunctional molecular bridge, the interlayer spacing is extended by coordination between -NH3+ at one end and the MoS2 precursor [Mo7O24]6-, and a stable bond is formed between -COOH at the other end and -OH on the surface of few-layer MXene. This enables the in-situ growth of intercalated MoS2 on the FLM surface, thus constructing a continuous and stable FLM/AUAm/MoS2 heterostructure.

Benefits of technology

It improves the utilization efficiency of active sites, achieves uniform construction of heterostructures and enhances electrochemical performance, exhibiting excellent cycling stability and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122035865A_ABST
    Figure CN122035865A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrochemical energy storage materials, in particular to a few-layer Ti3C2 heterostructure constructed by a bifunctional molecular bridge technology as well as a preparation method and application thereof, and the preparation method comprises the following steps: uniformly mixing 11-aminoundecanoic acid (AUAm), (NH4) 6Mo7O24. 4H2O, a few-layer transition metal carbide solution (FLM) and CH4N2S with water, and carrying out hydrothermal reaction to obtain a few-layer Ti3C2 heterostructure material. The molecular bridge designed by the invention has a bifunctional characteristic, the-NH2 group of the molecular bridge can be inserted between MoS2 layers to expand the interlayer spacing, the-COOH group of the molecular bridge and-OH on the surface of FLM form a covalent bond, the in-situ growth of intercalated MoS2 on few-layer metal carbide is realized, the construction of an FLM / AUAm / MoS2 heterostructure is promoted, and the material designed by the technology can be used as a supercapacitor electrode material and has a wide application prospect. The excellent electrochemical performance is shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochemical energy storage materials technology, specifically to a few-layer Ti3C2 heterostructure constructed with bifunctional molecular bridges, its preparation method, and its applications. Background Technology

[0002] Constructing heterostructures is an important strategy for effectively improving the electrochemical performance of materials. By organically combining different components, not only can the inherent advantages of each component be integrated, but synergistic effects can also be induced at the interface scale, thereby overcoming the inherent limitations of single-component materials in terms of structure and performance. Heterostructure engineering, by regulating interfacial interactions, helps to optimize electron and ion transport behavior, thereby developing functional materials with excellent electrochemical performance.

[0003] Transition metal carbides (MXenes) are considered ideal conductive substrates for constructing heterostructures due to their excellent intrinsic electrical conductivity and tunable surface chemistry. Molybdenum disulfide (MoS2), with its unique layered structure and rich physicochemical properties, has been widely used as a functional component and has been combined with MXenes to construct various high-performance heterostructure systems, such as CF / MoS2 / Ti3C2Tx, Ti3C2Tx / B-MoS2, MnPMo8V6 / MXene / MoS2, MoS2 / Mo2CTx, Ti3C2Tx-MWCNT / MoS2, 2D / 2D MXene / MoS2, and MoS2 / Mo 1.33 In existing heterostructure construction processes, Ti3C2MXene often exists as an incompletely exfoliated multilayer bulk, causing MoS2 to primarily grow on the outer surface of Ti3C2MXene. This makes it difficult to fully utilize the numerous potential active sites contained within the interlayer of Ti3C2MXene, thus limiting the potential for performance improvement in heterostructures. Therefore, to expose more active sites for heterostructure growth, few-layer Ti3C2MXene (FLM) should be prepared to construct a heterostructure between few-layer MXene and MoS2.

[0004] However, while traditional MoS2 possesses good chemical stability and is easy to prepare on a large scale, its intrinsic semiconductor properties result in low conductivity. Furthermore, its relatively narrow interlayer spacing hinders the insertion and extraction of electrolyte ions. These factors collectively limit the electrochemical performance of MoS2, thus restricting its application in high-performance electrochemical devices. To address these issues, an organic cation intercalator (STA) is introduced. + CTA + TEA + TBA + TMA +This process can expand the interlayer spacing of 2H-MoS2 and regulate its microstructure and surface chemical properties, thereby promoting ion transport and storage and improving its electrochemical performance. However, during isomer growth, free organic cations in the precursor solution easily disrupt the charge distribution on the FLM surface, causing its Zeta potential to drop below the colloidal stability threshold, thus inducing irreversible aggregation and sedimentation. Simultaneously, free organic cations can also adsorb various negatively charged substances, inducing competitive adsorption, such as the -OH and -O functional groups and molybdate anions [Mo7O] on the FLM surface. 24 ] 6- The competitive adsorption between molecules leads to localized enrichment of components and phase separation, which is detrimental to the uniform construction of heterostructures. Limited by these factors, existing organic molecules containing only a single functional group cannot simultaneously achieve effective control over the MoS2 intercalation process and stable anchoring interactions with the FLM surface, thus hindering the construction of heterostructures. Summary of the Invention

[0005] To address the aforementioned problems, this invention proposes a technique for constructing FLM heterostructures based on bifunctional molecular bridges, along with its preparation method and applications. Organic cationic intercalating agents with single functional groups not only cause the aggregation of FLM dispersions but also induce the formation of functional groups such as -OH and [Mo7O] on the FLM surface. 24 ] 6- Competitive adsorption between molecules hinders the construction of heterostructures. This invention selects 11-aminoundecanoic acid as the molecular bridging unit, with one end having a -NH3 group. + The interlayer structure of MoS2 is expanded to form intercalated MoS2, while the -COOH group at the other end forms a covalent bond with few-layer MXene, enabling in-situ growth of intercalated MoS2 on the FLM surface. This successfully constructs a heterostructure between intercalated MoS2 and few-layer MXene. It possesses both amino and carboxyl functional groups, allowing for effective synergistic regulation of the heterostructure construction process.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] The first aspect of this invention provides a few-layer Ti3C2 heterostructure constructed with a bifunctional molecular bridge. In a hydrothermal reaction, a few-layer transition metal carbide solution, a MoS2 precursor solution, and 11-aminoundecanoic acid are reacted, and the -NH3 group at one end of the 11-aminoundecanoic acid... + [Mo7O] in MoS2 precursor solution 24 ] 6-Coordination is performed to expand the interlayer spacing of MoS2, resulting in intercalated MoS2. The -COOH group at the other end forms Ti-OC with the -OH group on the surface of the few-layer transition metal carbide, anchoring the intercalated MoS2 on the transition metal carbide surface, thus obtaining the FLM / AUAm / MoS2 heterostructure, i.e., the few-layer Ti3C2 heterostructure. Specifically, the amino group -NH2 can be protonated to -NH3 in the reaction system. + It can react with the MoS2 precursor molybdate anion [Mo7O] 24 ] 6- Coordination occurs, inducing and promoting the formation of intercalated MoS2, thereby effectively expanding the interlayer spacing of MoS2. Simultaneously, the carboxyl group (-COOH) at the other end of the molecule reacts chemically with the -OH group on the FLM surface, forming a stable Ti-OC bond, achieving stable fixation of intercalated MoS2 on the FLM surface. Through the synergistic effect of the above-mentioned bifunctional molecular bridges, this invention constructs a continuous and stable heterostructure interface structure between FLM and intercalated MoS2, not only avoiding the limitations of monofunctional molecules in interface regulation but also significantly improving the utilization efficiency of active sites. The resulting FLM heterostructure composite material exhibits higher electrochemical performance, fully demonstrating the effectiveness and superiority of this molecular bridge strategy in interface engineering regulation and electrochemical performance enhancement. The molecular bridge strategy designed in this invention not only effectively regulates the MoS2 interlayer spacing and alleviates the competitive adsorption effect but also achieves the anchoring of intercalated MoS2 on the FLM surface, thereby promoting the construction of heterostructures. The few-layer Ti3C2 heterostructure consists of MoS2 nanoflower structures uniformly distributed on few-layer transition metal carbide nanosheets.

[0008] In another preferred embodiment, the MoS2 precursor is (NH4)6Mo7O 24 ·4H2O and CH4N2S; 11-Aminoundecanoic acid, (NH4)6Mo7O 24 The mass ratio of 4H2O to CH4N2S is 0.1~0.2:1.4484:2.8418.

[0009] In another preferred embodiment, the mass ratio of 11-aminoundecanoic acid to transition metal carbide is 3~4:0.6~0.8.

[0010] The second aspect of this invention provides a method for preparing the few-layer Ti3C2 heterostructure constructed from the aforementioned bifunctional molecular bridge, comprising the following steps: An aqueous solution of 11-aminoundecanoic acid was reacted with (NH4)6Mo7O 24 • Mix the aqueous solution of 4H2O with stirring, add a solution of a few layers of transition metal carbides and continue stirring, then mix with CH4N2S to obtain a mixed solution; After reacting the mixture solution at 200℃~220℃ for 16h~20h, the precipitate was collected by centrifugation, washed, and dried to obtain the few-layer Ti3C2 heterostructure. During the hydrothermal reaction: the amounts of 11-aminoundecanoic acid and (NH4)6Mo7O were controlled. 24 The order in which 4H2O and the few-layer transition metal carbide solution are added ensures stable dispersion of the solution because the electrostatic repulsion between free functional groups prevents significant aggregation of the few-layer transition metal carbide.

[0011] 11-Aminoundecanoic acid, (NH4)6Mo7O 24 The order of addition of 4H2O and the few-layer transition metal carbide solution is: 11-aminoundecanoic acid and (NH4)6Mo7O. 24 • Mix with 4H2O first, then add a few-layer transition metal carbide solution to the mixed solution; or mix a few-layer transition metal carbide solution and 11-aminoundecanoic acid first, then add (NH4)6Mo7O 24 • Add 4H2O to the mixed solution; or a few-layer transition metal carbide solution and (NH4)6Mo7O 24 Mix the ingredients first with 4H2O, then add 11-aminoundecanoic acid to the mixed solution.

[0012] In another preferred embodiment, the specific process for obtaining the few-layer transition metal carbide solution is as follows: Etching of the Ti3AlC2MAX phase with LiF-HCl solution yielded a few-layer transition metal carbide solution; the relative molecular mass ratio of LiF to Ti3AlC2MAX phase was 6.2:0.5. The LiF-HCl solution is obtained by dissolving LiF in HCl, wherein the mass-to-volume ratio of LiF to HCl is 1.4g~1.8g:25mL~35mL; and the concentration of HCl is 6M~9M.

[0013] A third aspect of the present invention provides a working electrode, which is prepared by the following method: A binder, conductive agent, and active material are dispersed in an organic solvent at a mass ratio of 0.005~0.0055:0.005~0.0055:0.04~0.044 to obtain a slurry; the active material is the aforementioned few-layer Ti3C2 heterostructure material. The slurry is coated onto the current collector and dried to obtain the working electrode.

[0014] In another preferred embodiment, the adhesive is PVDF; the conductive agent is acetylene black; the organic solvent is NMP; and the current collector is nickel foam.

[0015] A fourth aspect of the present invention provides a supercapacitor including the aforementioned working electrode.

[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention aims to address the interaction between the -NH2 group at one end of the 11-aminoundecanoic acid molecule and the MoS2 precursor [Mo7O] during the construction of heterostructures. 24 ]6 - Coordination promotes the formation of intercalated MoS2 and effectively expands the interlayer spacing of MoS2, resulting in intercalated MoS2. The -CCOH at the other end forms stable chemical bonds with the -OH on the surface of the few-layer transition metal carbide, enabling the intercalated MoS2 to grow in situ on the FLM surface, promoting the construction of the FLM / AUAm / MoS2 heterostructure and achieving stable interfacial connectivity. Compared to existing single-group intercalating agents that can only expand the interlayer spacing of MoS2 but cannot achieve uniform construction of heterostructures, the construction method in this invention not only effectively controls the MoS2 intercalation process but also stabilizes and anchors the few-layer Ti3C2, thereby promoting the construction of heterostructures and successfully obtaining structurally stable few-layer Ti3C2 heterostructure materials.

[0017] This invention utilizes a hydrothermal method to prepare few-layer Ti3C2 heterostructure materials, which exhibit excellent cycle stability under long-term charge-discharge cycles. The method employed in this invention is highly innovative, the fabrication process is simple, environmentally friendly, and safe, the experimental temperature is low, and the product has good morphology and high purity, making it suitable for industrial-scale application. Attached Figure Description

[0018] Figure 1 This is a comparison diagram of the preparation process of few-layer Ti3C2 heterostructure materials according to the present invention and the preparation process using a traditional single intercalating agent.

[0019] Figure 2 These are the XRD data of the few-layer Ti3C2 heterostructure material prepared in Example 1.

[0020] Figure 3 These are SEM images of few-layer Ti3C2 heterostructure materials obtained by different preparation methods. a is an SEM image of FLM / MoS2-DATB prepared using the traditional monofunctional intercalating agent decaalkyltrimethylammonium bromide, and b is an SEM image of FLM / AUAm / MoS2 prepared using Example 1 of this invention.

[0021] Figure 4 The diagram shows the structural analysis of the few-layer Ti3C2 heterostructure material prepared in Example 1; a is the Fourier transform infrared spectrum, b is the high-resolution C 1s XPS spectrum, and c is the high-resolution O 1s XPS spectrum.

[0022] Figure 5 These are XPS spectra of the few-layer Ti3C2 heterostructure material prepared in Example 1. a is the high-resolution N 1s XPS spectrum, b is the Mo 3d XPS spectrum, and c is the S 2p XPS spectrum.

[0023] Figure 6 These are the cyclic voltammetry and constant current charge-discharge curves of the working electrode prepared in Example 4; a is the cyclic voltammetry curve of the working electrode in Example 4, and b is the constant current charge-discharge curve of the working electrode in Example 4.

[0024] Figure 7 These are the cyclic voltammetry and constant current charge-discharge curves of the working electrode prepared in Example 1; a is the cyclic voltammetry curve of the working electrode in Example 1, and b is the constant current charge-discharge curve of the working electrode in Example 1.

[0025] Figure 8 The graphs show a performance comparison of the working electrodes prepared in Application Example 1 and Application Example 4; a is the cyclic voltammetry curve of the working electrodes in Application Example 1 and Application Example 4, and b is the constant current charge-discharge curve of the working electrodes in Application Example 1 and Application Example 4.

[0026] Figure 9 The specific capacitance values ​​of the working electrodes in Application Example 1 and Application Example 4 at different current densities.

[0027] Figure 10 The working electrode prepared in Example 1 is used at 15A g. -1 Stability data after 10,000 cycles of continuous charge and discharge at current density. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0029] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] Few-layer MXene (FLM) is considered an ideal substrate material due to its large specific surface area and abundant surface functional groups. In practical applications, while 2H-phase MoS2 exhibits good chemical stability and is easy to prepare on a large scale, its intrinsic semiconductor properties result in low conductivity. Furthermore, its relatively narrow interlayer spacing hinders the insertion and extraction of electrolyte ions. These factors collectively limit the electrochemical performance of 2H-MoS2, thus restricting its application in high-performance electrochemical devices. Based on the above, organic ion intercalation (such as STA...) is... + CTA + TEA + TBA + TMA + Intercalation has become an effective strategy for expanding the 2H-MoS2 spacing and optimizing the microstructure / surface chemistry, thereby promoting ion transport / storage and achieving high intercalation pseudocapacitance. This has prompted the exploration of constructing heterostructures between intercalated MoS2 and FLM. However, during heterogeneous growth, free organic cations in the precursor solution disrupt the surface charge distribution of FLM, causing its Zeta potential to drop below the critical stability threshold and inducing irreversible aggregation and sedimentation. In addition, free organic cations compete for adsorption with various negatively charged substances, such as FLM surface functional groups (-OH, -O) and molybdate anions ([Mo7O3]2). 24 ] 6- Therefore, organic molecules with monofunctional groups cannot simultaneously promote the intercalation of MoS2 and effectively interact with the FLM surface. This not only leads to localized and non-uniform intercalation but also hinders the construction of heterostructures.

[0031] Therefore, to solve the above problems and achieve in-situ growth of intercalated MoS2 on the FLM surface, the present invention aims to provide a method for constructing FLM / AUAm / MoS2 heterostructure materials through bifunctional molecular bridges, as well as its preparation and applications.

[0032] The following section details the preparation method and applications of a bifunctional molecular bridging technique for constructing few-layer Ti3C2 heterostructures.

[0033] In the following examples, FLM is few-layer Ti3C2; AUMan is 11-aminoundecanoic acid; DTAB is decaalkyltrimethylammonium bromide; (NH4)6Mo7O 24 ·4H2O is ammonium molybdate; CH4N2S is thiourea.

[0034] Ti3AlC2MAX phase powder was purchased from Foshan Xinxi Technology Co., Ltd. in Guangdong Province; 11-aminomonoalkyl acid was purchased from Wokai; and decaalkyltrimethylammonium bromide was purchased from Wokai.

[0035] Example 1 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in 30mL of PTFE reactor containing 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension at 120W for 20min to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0036] S2. Weigh 0.15g of AUAm and dissolve it in 30mL of deionized water. Stir with a magnetic stirrer for 30min to form a homogeneous solution, obtaining the AUAm solution. Then, add 1.4484g of (NH4)6Mo7O 24 • 4H₂O was dissolved in 15 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH₄)₆Mo₇O. 24 ·4H2O solution; (NH4)6Mo7O 24 • Add 4H2O solution dropwise to AUAm solution with continuous magnetic stirring for a total of 30 min to obtain a mixed solution; add 1 mL of 10 mg / mL FLM solution to the mixed solution and stir for 30 min. Then transfer the mixture to a beaker containing 2.8418 g CH4N2S and stir for another 30 min to obtain the reaction solution.

[0037] S3. The reaction solution in the beaker is transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor is dried at 210°C for 18 hours in a constant temperature forced air drying oven and then removed. The precipitate is collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate is collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder sample, which is a few-layer Ti3C2 heterostructure.

[0038] Example 2 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0039] S2, Weigh 1.4484g of (NH4)6Mo7O 24 • Dissolve 4H2O in 15mL of deionized water and stir with a magnetic stirrer for 10min to form a homogeneous (NH4)6Mo7O 24 • 4H₂O solution; then add 1 mL of 10 mg / mL FLM solution dropwise to (NH₄)₆Mo₇O 24 In a 4H₂O solution, maintain magnetic stirring for 30 minutes throughout the process. Dissolve 0.15 g of AUAm in a beaker containing 30 mL of deionized water and stir with a magnetic stirrer for 30 minutes to form a homogeneous solution. Finally, transfer the solution containing the complex to a beaker containing 2.8418 CH₄N₂S and stir with a magnetic stirrer for 30 minutes to ensure complete dissolution, obtaining the reaction solution.

[0040] S3. The reaction solution is transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell for reaction. The hydrothermal reactor is dried in a constant temperature forced air drying oven at 210°C for 18 hours and then removed. The precipitate is collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate is collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder sample, which is a few-layer Ti3C2 heterostructure.

[0041] Example 3 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature of 25℃, which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches about 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power 120W) to further promote the diffusion of Ti3C2 sheets. After sonication, centrifuge the colloidal suspension at 3500 rpm for 10min to separate the black supernatant, and finally obtain a 10mg / mL FLM solution.

[0042] S2. Weigh 0.15g of AUAm and dissolve it in a beaker containing 30mL of deionized water. Stir with a magnetic stirrer for 30min to form a homogeneous solution, obtaining the AUAm solution. Then, add 1mL of 10mg / mL FLM solution dropwise to the AUAm solution, maintaining magnetic stirring throughout the process. After stirring for 30min, add 1.4484g of (NH4)6Mo7O 24 ·4H2O was dissolved in a beaker containing 15 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH4)6Mo7O. 24 ·4H2O solution; (NH4)6Mo7O 24 • 4H2O solution was added dropwise to AUAm solution, and magnetic stirring was maintained throughout the process. After stirring for 30 minutes, the solution containing the complex was transferred to a beaker containing 2.8418 g of CH4N2S, and stirred for another 30 minutes to obtain the solution to be reacted.

[0043] S3. The reaction solution was transferred to a polytetrafluoroethylene-lined reactor housed in a stainless steel reactor shell. The hydrothermal reactor was dried in a constant-temperature forced-air drying oven at 210°C for 18 hours before being removed. The precipitate was collected by centrifugation and washed repeatedly with deionized water and anhydrous ethanol. The final washed precipitate was collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder samples.

[0044] To further illustrate the effect of using AUAm in this invention, DTAB is used to replace AUAm, and its preparation process is compared to that of... Figure 1 As shown, the specific experimental design is as follows.

[0045] Comparative Example 1 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0046] S2. Weigh 0.15g of DTAB and dissolve it in 30mL of deionized water. Stir with a magnetic stirrer for 30min to form a homogeneous solution, thus obtaining the DTAB solution. Then, add 1.4484g of (NH4)6Mo7O 24 • 4H₂O was dissolved in 15 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH₄)₆Mo₇O. 24 ·4H₂O solution. Subsequently, (NH₄)₆Mo₇O 24 • The 4H2O solution was added dropwise to the DTAB solution, and the entire process was continuously magnetically stirred for 30 min. Subsequently, 1 mL of 10 mg / mL FLM solution was added to the mixed solution, and after stirring for 30 min, it was transferred to a beaker containing 2.8418 g of CH4N2S, and stirred for another 30 min to obtain the reaction solution.

[0047] S3. The solution to be reacted in the beaker was transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor was dried in a constant-temperature forced air drying oven at 210°C for 18 hours and then removed. The precipitate was collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate was collected and dried in a constant-temperature drying oven for 24 hours to obtain FLM / MoS2-DTAB powder samples.

[0048] Comparative Example 2 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0049] S2, Weigh 1.4484g of (NH4)6Mo7O 24 • Dissolve 4H2O in 15mL of deionized water and stir with a magnetic stirrer for 10min to form a homogeneous (NH4)6Mo7O 24 • 4H₂O solution; then add 1 mL of 10 mg / mL FLM solution dropwise to (NH₄)₆Mo₇O 24 In a 4H₂O solution, maintain magnetic stirring for 30 minutes throughout the process. Dissolve 0.15 g of AUAm in a beaker containing 30 mL of deionized water and stir with a magnetic stirrer for 30 minutes to form a homogeneous solution. Finally, transfer the solution containing the complex to a beaker containing 2.8418 CH₄N₂S and stir with a magnetic stirrer for 30 minutes to ensure complete dissolution, obtaining the reaction solution.

[0050] S3. The reaction solution in the beaker was transferred to a polytetrafluoroethylene-lined reactor housed in a stainless steel reactor shell. The hydrothermal reactor was dried in a constant-temperature forced-air drying oven at 210°C for 18 hours before being removed. The precipitate was collected by centrifugation and washed repeatedly with deionized water and anhydrous ethanol. The final washed precipitate was collected and dried in a vacuum drying oven for 24 hours to obtain FLM / MoS2-DTAB powder samples.

[0051] Comparative Example 3 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0052] S2. Weigh 0.15g of DTAB and dissolve it in 30mL of deionized water. Stir with a magnetic stirrer for 30 minutes to form a homogeneous solution, obtaining the DTAB solution. Then, add 1mL of 10mg / mL FLM solution dropwise to the DTAB solution, maintaining magnetic stirring throughout the process. After stirring for 30 minutes, add 1.4484g of (NH4)6Mo7O 24 • Dissolve 4H₂O in a beaker containing 15 mL of deionized water and stir with a magnetic stirrer for 10 min to form a homogeneous solution. Then add (NH₄)₆Mo₇O₇. 24 • 4H2O solution was added dropwise to DTAB solution, and magnetic stirring was maintained throughout the process. After stirring for 30 minutes, the solution containing the complex was transferred to a beaker containing 2.8418g CH4N2S, and stirred for another 30 minutes to obtain the reaction solution.

[0053] S3. The solution to be reacted in the beaker was transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor was dried at 210°C for 18 hours in a constant temperature forced air drying oven and then removed. The precipitate was collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate was collected and dried in a vacuum drying oven for 24 hours to obtain FLM / MoS2-DTAB powder samples.

[0054] To illustrate the role of AUAm, experiments were conducted below with no AUAm added and with different amounts of AUAm added.

[0055] Comparative Example 4 A method for preparing FLM / MoS2 composite material, which differs from Example 1 in that AUAm material is not added, and the specific method includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0056] S2, Weigh 1.4484g of (NH4)6Mo7O 24 • 4H₂O was dissolved in 45 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH₄)₆Mo₇O. 24 • 4H2O solution; Add 1 mL of 10 mg / mL FLM solution to the mixed solution, stir for 30 min, then transfer to a beaker containing 2.8418 g CH4N2S, stir for another 30 min to obtain the reaction solution.

[0057] The reaction solution in the beaker was transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor was dried at 210°C for 18 hours in a constant-temperature forced air drying oven before being removed. The precipitate was collected by centrifugation and washed repeatedly with deionized water and anhydrous ethanol. Finally, the washed precipitate was collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder samples, which are few-layer Ti3C2 heterostructures.

[0058] Comparative Example 5 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0059] S2. Weigh 0.1g of AUAm and dissolve it in 30mL of deionized water. Stir with a magnetic stirrer for 30min to form a homogeneous solution, obtaining the AUAm solution. Then, add 1.4484g of (NH4)6Mo7O 24 • 4H₂O was dissolved in 15 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH₄)₆Mo₇O. 24 ·4H2O solution; (NH4)6Mo7O 24 • Add 4H2O solution dropwise to AUAm solution with continuous magnetic stirring for a total of 30 min to obtain a mixed solution; add 1 mL of 10 mg / mL FLM solution to the mixed solution and stir for 30 min. Then transfer the mixture to a beaker containing 2.8418 g CH4N2S and stir for another 30 min to obtain the reaction solution.

[0060] S3. The reaction solution in the beaker is transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor is dried at 210°C for 18 hours in a constant temperature forced air drying oven and then removed. The precipitate is collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate is collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder sample, which is a few-layer Ti3C2 heterostructure.

[0061] Comparative Example 6 A method for preparing a few-layer Ti3C2 heterostructure material includes the following steps: S1. Weigh 1.6g of LiF and dissolve it in a PTFE reactor containing 30mL of 9M HCl. Stir with a magnetic stirrer for 5min to form a homogeneous solution at room temperature (25°C), which is the LiF / HCl solution. Then, add 1g of Ti3AlC2MAX phase powder to the LiF / HCl solution and etch at 40°C for 24h. After etching, wash the mixture three times with 3M HCl, and then centrifuge thoroughly with deionized water until the pH of the supernatant reaches approximately 6. During each centrifugation step, discard the supernatant and manually shake to redisperse the precipitate in deionized water to obtain a colloidal suspension. Sonicate the colloidal suspension for 20min (power: 120W) to further promote the Ti3C2T x The diffusion of the film; after ultrasonic treatment, the colloidal suspension was centrifuged at 3500 rpm for 10 min to separate the black supernatant, and finally a 10 mg / mL FLM solution was obtained.

[0062] S2. Weigh 0.2g of AUAm and dissolve it in 30mL of deionized water. Stir with a magnetic stirrer for 30min to form a homogeneous solution, obtaining the AUAm solution. Then, add 1.4484g of (NH4)6Mo7O 24 • 4H₂O was dissolved in 15 mL of deionized water and stirred with a magnetic stirrer for 10 min to form a homogeneous solution, yielding (NH₄)₆Mo₇O. 24 ·4H2O solution; (NH4)6Mo7O 24 • Add 4H2O solution dropwise to AUAm solution with continuous magnetic stirring for a total of 30 min to obtain a mixed solution; add 1 mL of 10 mg / mL FLM solution to the mixed solution and stir for 30 min. Then transfer the mixture to a beaker containing 2.8418 g CH4N2S and stir for another 30 min to obtain the reaction solution.

[0063] S3. The reaction solution in the beaker is transferred to a polytetrafluoroethylene-lined reactor installed in a stainless steel reactor shell. The hydrothermal reactor is dried at 210°C for 18 hours in a constant temperature forced air drying oven and then removed. The precipitate is collected by centrifugation and washed multiple times with deionized water and anhydrous ethanol. Finally, the washed precipitate is collected and dried in a vacuum drying oven for 24 hours to obtain FLM / AUAm / MoS2 powder sample, which is a few-layer Ti3C2 heterostructure.

[0064] Application Example 1 A method for preparing a working electrode includes the following steps: Weigh out 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, which is the FLM / AUAm / MoS2 heterostructure material of Example 1.

[0065] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The carbon sheet coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0066] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 1; the electrolyte is a 1M sodium sulfate solution.

[0067] Application Example 2 A method for preparing a working electrode includes the following steps: Weigh out 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, which is the few-layer Ti3C2 heterostructure material of Example 2.

[0068] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0069] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 2; the electrolyte is a 1M sodium sulfate solution.

[0070] Application Example 3 A method for preparing a working electrode includes the following steps: Weigh out 0.005g of PVDF, 0.005g of acetylene black and 0.04g of active material, the active material being the few-layer Ti3C2 heterostructure material of Example 3.

[0071] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0072] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 3; the electrolyte is a 1M sodium sulfate solution.

[0073] Application Example 4 A method for preparing a working electrode includes the following steps: Weigh out 0.005g PVDF, 0.005g acetylene black and 0.04g active material. The active material is the few-layer Ti3C2 heterostructure material of Comparative Example 1.

[0074] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0075] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 4; the electrolyte is a 1M sodium sulfate solution.

[0076] Application Example 5 A method for preparing a working electrode includes the following steps: Weigh out 0.005g PVDF, 0.005g acetylene black and 0.04g active material. The active material is the few-layer Ti3C2 heterostructure material of Comparative Example 2.

[0077] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0078] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 5; the electrolyte is a 1M sodium sulfate solution.

[0079] Application Example 6 A method for preparing a working electrode includes the following steps: Weigh out 0.005g PVDF, 0.005g acetylene black and 0.04g active material, which is the few-layer Ti3C2 heterostructure material of Comparative Example 3.

[0080] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0081] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 6; the electrolyte is a 1M sodium sulfate solution.

[0082] Application Example 7 A method for preparing a working electrode includes the following steps: Weigh out 0.005 g PVDF, 0.005 g acetylene black and 0.04 g active material, which is the FLM / MoS2 composite material of Comparative Example 4.

[0083] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0084] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 7; the electrolyte is a 1M sodium sulfate solution.

[0085] Application Example 8 A method for preparing a working electrode includes the following steps: Weigh out 0.005 g PVDF, 0.005 g acetylene black and 0.04 g active material, which is the few-layer Ti3C2 heterostructure composite material of Comparative Example 5.

[0086] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The nickel foam coated with the slurry was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0087] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 8; the electrolyte is a 1M sodium sulfate solution.

[0088] Application Example 9 A method for preparing a working electrode includes the following steps: Weigh out 0.005g of PVDF, 0.005g of acetylene black and 0.04g of active material. The active material is the few-layer Ti3C2 heterostructure composite material of Comparative Example 6.

[0089] The weighed PVDF, acetylene black and active material were placed into an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 minutes to obtain a slurry. The slurry was evenly coated onto the nickel foam, with a coating area of ​​1cm × 1cm. The carbon sheet coated with nickel foam was then placed in a vacuum drying oven and dried at 60°C to obtain the working electrode.

[0090] A supercapacitor includes a reference electrode, a counter electrode, a working electrode, and an electrolyte to form a three-electrode testing system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, and the working electrode is the working electrode prepared using Application Example 9; the electrolyte is a 1M sodium sulfate solution.

[0091] The products prepared in the above embodiments were subjected to performance analysis.

[0092] Test 1: X-ray diffraction analysis X-ray diffraction (XRD) analysis was performed on the FLM / AUAm / MoS2 heterostructure material prepared in Example 1. The results are shown in the figure. Figure 2 . Figure 2 This is the X-ray diffraction pattern of the few-layer Ti3C2 heterostructure material prepared in Example 1. Figure 2The XRD pattern shows that the prepared few-layer Ti3C2 heterostructure not only has the (002) characteristic peak of few-layer Ti3C2, but also has the (002) characteristic peak representing the expansion of the interlayer spacing of MoS2 after the addition of AUAm, which confirms that the material is a composite of FLM, AUAm and MoS2, and that the addition of AUAm successfully expanded the interlayer spacing of MoS2.

[0093] Test 2: Scanning Electron Microscopy Analysis The few-layer Ti3C2 heterostructure material prepared in Example 1 was analyzed by scanning electron microscopy (SEM), and the results are shown in the figure. Figure 3 . Figure 3 The images shown are scanning electron microscope (SEM) images of the few-layer Ti3C2 heterostructures prepared in Example 1 and Comparative Example 1, respectively, at the same magnification. Figure 3 SEM images show that FLM nanosheets grow uniformly on MoS2 nanoflowers. This is because the bifunctional properties of AUAm effectively alleviate competitive adsorption in the few-layer Ti3C2 heterostructure, promoting robust integration of the interface.

[0094] Test 3: Fourier transform infrared spectrum and high-resolution XPS spectra of C 1s, O 1s, N 1s, Mo 3d and S 2p of the few-layer Ti3C2 heterostructure material prepared in Example 1.

[0095] Fourier transform infrared spectroscopy and high-resolution C 1s and O 1s XPS spectroscopy were performed on the few-layer Ti3C2 heterostructure material prepared in Example 1. The results are shown in the figure. Figure 4 It can be observed from the Fourier transform infrared spectrum that, compared with FLM, at ~3400 cm⁻¹ -1 The weakening of the -OH stretching band at the α-OH position in FLM / AUAm / MoS2 indicates an esterification reaction between the -COOH groups of AUMan and the -OH groups on the FLM surface, suggesting interfacial coupling between AUMan and FLM. High-resolution C 1s XPS spectra reveal a new peak at 288.7 eV corresponding to C=O in the prepared few-layer Ti3C2 heterostructure compared to FLM, confirming the interaction between the AUMan and FLM surfaces. Similarly, high-resolution O 1s XPS spectra show a new peak at 533.0 eV corresponding to the Ti-OC bond in the prepared few-layer Ti3C2 heterostructure compared to FLM, further confirming the interaction between AUMan and the upper surface of FLM.

[0096] High-resolution XPS spectroscopic analysis of N 1s, Mo 3d, and S 2p was performed on the few-layer Ti3C2 heterostructure material prepared in Example 1. The results are shown in [Figure 1]. Figure 5The N 1s peak can be attributed to the pyridine nitrogen (-C=NC-) in the thiourea derivative, from (NH4)6Mo7O 24 The undissolved pyrrole nitrogen (CN, -NH-) in the CH4N2S residue is noteworthy. New N2 was also observed in FLM / AUAm / MoS2. + The (ammonium center) peak, originating from -NH2 in AUAm, elucidates the interaction between -NH2 and MoS2. Simultaneously, significant changes in the S 2p and Mo 3d spectra, including Mo... 5+ and Mo 6+ The coexistence of species further reflects changes in the local chemical environment associated with intercalation-induced structural evolution.

[0097] Test 4: Cyclic voltammetry and constant current charge-discharge curves of the working electrodes prepared in Application Examples 1 and 4 pass Figure 6 and Figure 7 The results of the cyclic voltammetry curves and constant current charge-discharge curves of the working electrodes prepared in Application Example 1 and Application Example 4, respectively, show that the working electrodes of Application Example 1 and Application Example 4 exhibit an approximately rectangular characteristic in the cyclic voltammetry test curve and a linear characteristic in the constant current charge-discharge curve, demonstrating the ideal behavior of supercapacitor electrode materials.

[0098] Figure 8 The results of the cyclic voltammetry and galvanostatic charge-discharge curves show that, compared with Application Example 4, the working electrode prepared in Application Example 1 has a larger area of ​​cyclic voltammetry and a longer duration of galvanostatic charge-discharge, confirming the electrochemical improvement brought about by the successful construction of the heterostructure. Meanwhile... Figure 9 The study demonstrates that the specific capacitance of the working electrode prepared in Example 1 is higher than that of the working electrode prepared in Example 4 at different current densities, further illustrating the advantages of successfully constructing a heterostructure. Furthermore... Figure 9 The exhibition also showcases working electrodes prepared in Application Examples 1 and 4 at 1 A g. -1 At current density, the specific capacitance values ​​are 205 F g. -1 and 120 F g -1 .

[0099] Test 5: The working electrode prepared in Example 1 was tested at 15 A g. -1 Cyclic stability test after 10,000 cycles of continuous charge and discharge at current density.

[0100] The working electrode prepared in Application Example 1 was subjected to a cycle test of up to 10,000 times. The results are shown in [Figure 1]. Figure 10Cyclic test results show that even after the working electrode of Example 1 has undergone 10,000 charge-discharge tests, its specific capacitance value can still maintain 92% of the initial capacitance value, demonstrating excellent cyclic stability.

[0101] A bifunctional molecular bridge based on AUAm was proposed and verified, enabling the in-situ growth of MoS2 with increased interlayer spacing on the surface of FLM, thus successfully constructing a stable FLM / AUAm / MoS2 heterostructure. A comparison was made with decaalkyltrimethylammonium bromide (DTAB), which has the same alkyl chain length but only a single functional group, to highlight the unique role of AUAm. Figure 1 As shown.

[0102] Test 6: The few-layer Ti3C2 heterostructure materials prepared in Example 1 and Comparative Examples 4 to 6 were respectively subjected to a test at 1 A·g -1 The specific capacitance was tested under the specified conditions, and it was found that the FLM / MoS2 prepared without the addition of AUAm, i.e., the product prepared in Comparative Example 4, had a specific capacitance of 1 A·g. -1 The specific capacitance at that time was 58 F·g -1 The FLM / AUAm / MoS2 prepared by adding 0.1 g of AUAm, which is the product prepared in Comparative Example 5, has a concentration of 1 A·g. -1 The specific capacitance at that time was 116 F·g -1 FLM / AUAm / MoS2 prepared by adding 0.2g of AUAm at 1A·g -1 The specific capacitance at that time was 167 F·g -1 The results above show that the specific capacitance increases with the increase of AUAm content, indicating that adding AUAm can give the few-layer Ti3C2 heterostructure material excellent charge storage capacity.

[0103] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A few-layer Ti3C2 heterostructure constructed from bifunctional molecular bridges, characterized in that, In a hydrothermal reaction, a few-layer transition metal carbide solution, a MoS2 precursor solution, and 11-aminoundecanoic acid react to form the -NH3 group at the 11-aminoundecanoic acid end. + [Mo7O] in MoS2 precursor solution 24 ]6 - Coordination is performed to expand the interlayer spacing of MoS2, resulting in intercalated MoS2. The -COOH at the other end forms Ti-OC with the -OH group on the surface of the transition metal carbide, thereby anchoring the intercalated MoS2 on the surface of the transition metal carbide, resulting in the FLM / AUAm / MoS2 heterostructure, i.e., the few-layer Ti3C2 heterostructure.

2. The few-layer Ti3C2 heterostructure constructed by the bifunctional molecular bridge according to claim 1, characterized in that, The MoS2 precursor is (NH4)6Mo7O 24 ·4H2O and CH4N2S; 11-Aminoundecanoic acid, (NH4)6Mo7O 24 The mass ratio of 4H2O to CH4N2S is 0.1~0.2:1.4484:2.8418.

3. The few-layer Ti3C2 heterostructure constructed by the bifunctional molecular bridge according to claim 2, characterized in that, The mass ratio of 11-aminoundecanoic acid to transition metal carbides is 3~4:0.6~0.

8.

4. A method for preparing a few-layer Ti3C2 heterostructure constructed from bifunctional molecular bridges as described in claim 3, characterized in that, Includes the following steps: An aqueous solution of 11-aminoundecanoic acid was reacted with (NH4)6Mo7O 24 • Mix 4H2O aqueous solution with stirring, add transition metal carbide solution and continue stirring, then mix with CH4N2S to obtain a mixed solution; After reacting the mixture solution at 200℃~220℃ for 16h~20h, centrifuge to collect the precipitate, wash and dry it to obtain the few-layer Ti3C2 heterostructure.

5. The method for preparing the few-layer Ti3C2 heterostructure constructed by bifunctional molecular bridges according to claim 4, characterized in that, The specific process for obtaining the few-layer transition metal carbide solution is as follows: Etching of the Ti3AlC2 MAX phase with LiF-HCl solution yielded a few-layer transition metal carbide solution; the mass ratio of LiF to Ti3AlC2 MAX phase was 6.0~6.5:0.50~0.

60. The LiF-HCl solution is obtained by dissolving LiF in HCl, wherein the mass-to-volume ratio of LiF to HCl is 1.4g~1.8g:25mL~35mL; and the concentration of HCl is 6M~9M.

6. A working electrode, characterized in that, It was prepared using the following method: A binder, a conductive agent, and an active material are dispersed in an organic solvent at a mass ratio of 0.005~0.0055:0.005~0.0055:0.04~0.044 to obtain a slurry; the active material is the few-layer Ti3C2 heterostructure material as described in claim 3. The slurry is coated onto the current collector and dried to obtain the working electrode.

7. The working electrode according to claim 6, characterized in that, The adhesive is polyvinylidene fluoride; the conductive agent is acetylene black; the organic solvent is N-methylpyrrolidone (NMP); and the current collector is nickel foam.

8. A supercapacitor, characterized in that, Includes the working electrode as described in claim 6.