A high-rate silicon-based solid-state anode battery and its fabrication method

By using lithium polyacrylate@nano-silicon/N-doped porous carbon as the negative electrode active material in solid-state batteries, the structural pulverization problem caused by the volume expansion of silicon negative electrodes was solved, and silicon-based negative electrode solid-state batteries with high rate and excellent cycle performance were realized.

CN122118102BActive Publication Date: 2026-11-10YANCHENG INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610255707.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-03-04
Publication Date
2026-11-10
Estimated Expiration
2046-03-04

AI Technical Summary

Technical Problem

The dramatic volume expansion of silicon anodes during charging and discharging leads to mechanical pulverization of the electrode structure and deterioration of interface dynamics, which seriously affects the high-rate charge-discharge performance and cycle life of solid-state batteries.

Method used

Lithium polyacrylate@nano-silicon/N-doped porous carbon is used as the negative electrode active material. Through the core-shell structure design, the nano-silicon particles are uniformly dispersed in the porous carbon. The carbon wall provides buffer space and mechanical support, while the lithium polyacrylate provides lithium source and adhesion force, forming an elastic shell to prevent silicon particles from falling off.

Benefits of technology

It significantly improves the rate performance and cycle stability of solid-state batteries, suppresses the pulverization of electrode materials, and improves the initial coulombic efficiency and the integrity of the electrode structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of solid-state battery technology, specifically to a high-rate silicon-based anode solid-state battery and its preparation method. The silicon-based anode solid-state battery prepared by this invention comprises a silicon-based anode, a sulfide solid electrolyte, and a cathode; wherein the silicon-based anode is formed by pressing a silicon-based anode material, which is a mixture of lithium polyacrylate@nano-silicon / N-doped porous carbon, a sulfide solid electrolyte, and a conductive agent; the lithium polyacrylate@nano-silicon / N-doped porous carbon in this invention, as the anode active material, differs from traditional nano-silicon and can significantly improve the rate performance and cycle stability of the solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid-state battery technology, specifically to a high-rate silicon-based anode solid-state battery and its preparation method. Background Technology

[0002] With the rapid popularization of electric vehicles and the increasingly urgent need for large-scale energy storage in smart grids, all-solid-state batteries, due to their use of non-flammable solid electrolytes, theoretically can break through the energy density limit of traditional lithium-ion batteries and fundamentally solve safety issues, and are considered one of the most promising technological routes. However, their commercialization process is still constrained by the performance bottleneck of key electrode materials, especially on the negative electrode side.

[0003] Silicon, with its theoretical specific capacity of up to 3579 mAh / g (approximately ten times that of graphite) and suitable delithiation potential, has become the inevitable choice for achieving a leap in energy density in solid-state batteries. However, the dramatic volume expansion (>300%) of silicon anodes during charge and discharge not only leads to mechanical pulverization of the electrode structure and failure of solid-state electrolyte contacts, but also severely deteriorates its interfacial kinetics and cycle life under high-rate charge and discharge conditions. Therefore, developing silicon-based composite anodes capable of operating at high rates, and using them as a basis for producing high-rate, high-cycle-performance solid-state batteries, is currently a cutting-edge research hotspot in the field of electrochemical energy storage. Summary of the Invention

[0004] The purpose of this invention is to provide a high-rate silicon-based anode solid-state battery and its preparation method, so as to solve the problems mentioned in the background art.

[0005] To address the aforementioned technical problems, this invention provides the following technical solution: a high-rate silicon-based anode solid-state battery and its preparation method, comprising the following steps:

[0006] Step S1: Using a homogenizer, lithium polyacrylate@nano silicon / N-doped porous carbon, sulfide solid electrolyte and conductive agent are thoroughly mixed in a mass ratio of 60:35:5 to obtain silicon-based anode material;

[0007] Step S2: Press the sulfide solid electrolyte to form a solid electrolyte layer, then press a silicon-based anode material on one side of the solid electrolyte layer to form a silicon-based anode, and press a cathode material on the other side to form a cathode. Then perform electrochemical performance testing to obtain a high-rate silicon-based anode solid battery.

[0008] Furthermore, the lithium polyacrylate@nano-silicon / N-doped porous carbon is prepared by KH570-modified grafting of nano-silicon / N-doped porous carbon, followed by polymerization and coating with acrylic acid as monomer, and finally by modification with lithium hydroxide.

[0009] Furthermore, the nano-silicon / N-doped porous carbon is prepared by ball milling nano-silicon and then loading it onto N-doped porous carbon; the N-doped porous carbon is prepared by mixing and grinding carbon precursor, urea and potassium oxalate, and then calcining at high temperature, while the carbon precursor is prepared by reacting citric acid monohydrate and magnesium nitrate hexahydrate.

[0010] Furthermore, the preparation method of the lithium polyacrylate@nano-silicon / N-doped porous carbon includes the following steps:

[0011] Step A1: Disperse nano-silicon / N-doped porous carbon in an ethanol-water solution (ethanol to water volume ratio of 9:1) for 1 hour, adjust the pH to 4.2, add KH570, then heat to 60℃ and stir for 5 hours. Wash with ethanol and deionized water three times alternately, and dry under vacuum to obtain grafted modified nano-silicon / N-doped porous carbon.

[0012] Step A2: Disperse the grafted modified nano-silicon / N-doped porous carbon evenly in deionized water, add isobutanol, adjust the pH to 9.5, sonicate for 1 h, then add emulsifier OP-10 and stir for 12 h, purge with nitrogen, add sodium bicarbonate and potassium persulfate and stir evenly, then slowly add acrylic acid dropwise and heat to 75℃ for polymerization reaction for 5.5-6.5 h, wash with water until neutral, adjust the pH to 6-7, then add 0.8-1.2 mol / L lithium hydroxide aqueous solution and stir for 5-8 h, wash with ethanol until neutral, and dry to obtain lithium polyacrylate@nano-silicon / N-doped porous carbon.

[0013] Further, in step A1, the ratio of the amount of nano-silicon / N-doped porous carbon, ethanol aqueous solution and KH570 is 1g:100mL:0.05-0.15g;

[0014] Further, in step A1, the nano-silicon / N-doped porous carbon is prepared by the following steps:

[0015] N-doped porous carbon and nano-silicon powder were uniformly mixed, anhydrous ethanol was added and mixed thoroughly, then transferred to a ball mill jar filled with argon gas, stainless steel grinding balls were added, and then the ball mill jar was placed in a planetary ball mill for ball milling and vacuum drying to obtain nano-silicon / N-doped porous carbon.

[0016] Furthermore, the mass ratio of the N-doped porous carbon, nano-silicon powder, and anhydrous ethanol is 7-9:1-3:1-3;

[0017] Furthermore, the ball-to-material ratio in the ball milling process is 1-2:1, the ball milling time is 30-36 hours, and the rotation speed is 1000-1200 r / min.

[0018] Furthermore, the N-doped porous carbon is prepared by the following steps:

[0019] Step B1: Add citric acid monohydrate and magnesium nitrate hexahydrate to deionized water, then transfer to a 90°C water bath and stir until the solvent evaporates. Then place at 180°C for 2 hours to foam and obtain carbon precursor.

[0020] Step B2: Mix carbon precursor, urea and potassium oxalate and grind them. Then transfer them to a tube furnace, heat them to a specific temperature under a nitrogen atmosphere and hold for 2 hours. Then acid wash them until neutral and dry them to obtain N-doped porous carbon.

[0021] Furthermore, in step B1, the ratio of citric acid monohydrate, magnesium nitrate hexahydrate, and deionized water is 0.8-1.2g:2-2.5g:20mL;

[0022] Furthermore, in step B2, the mass ratio of carbon precursor, urea, and potassium oxalate is 1:2:2;

[0023] Furthermore, the heat preservation temperature in step B2 is 750-850℃, and the heating rate is 3℃ / min;

[0024] Further, the pickling in step B2 involves pickling with 3 mol / L hydrochloric acid for 8-10 hours.

[0025] Further, in step A2, the ratio of the amount of grafted modified nano-silicon / N-doped porous carbon, deionized water, isobutanol, emulsifier OP-10, sodium bicarbonate, potassium persulfate, acrylic acid, and lithium hydroxide aqueous solution is 0.5-1.5g:100mL:0.4-1mL:0.2-0.6g:0.3-0.9g:0.04-0.12g:2-6g:50mL.

[0026] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: The present invention provides a method for preparing a high-rate silicon-based anode solid-state battery, wherein the silicon-based anode solid-state battery includes a silicon-based anode, a sulfide solid electrolyte, and a cathode; the silicon-based anode is formed by pressing a silicon-based anode material, wherein the silicon-based anode material is a mixture of lithium polyacrylate@nano-silicon / N-doped porous carbon, sulfide solid electrolyte, and conductive agent; the lithium polyacrylate@nano-silicon / N-doped porous carbon in the present invention, as an anode active material, differs from traditional nano-silicon and can significantly improve the rate performance and cycle stability of the solid-state battery.

[0027] The lithium polyacrylate@nano-silicon / N-doped porous carbon prepared in this invention has a core-shell-like structure. The pores (especially micropores and mesopores) in the N-doped porous carbon provide a uniformly dispersed and fixed "room" for the nano-silicon particles. This not only prevents silicon particles from failing due to agglomeration during cycling, but more importantly, the carbon walls surrounding the pores provide a buffer space for the huge volume expansion of silicon during charging and discharging, effectively suppressing the overall pulverization of the electrode material. Furthermore, the good mechanical strength of the carbon material forms a continuous conductive and mechanical support network, maintaining the integrity of the electrode structure. In addition, as an excellent electronic conductor, the N-doped porous carbon provides a rapid electron transport pathway for the non-conductive silicon, significantly improving the rate performance of the battery. The nano-silicon in the carbon material reduces bulk silicon to the nanoscale, greatly shortening the solid-phase diffusion distance of lithium ions within the silicon particles. Compared to small volume changes, nanoparticles are more able to withstand the internal stress caused by volume expansion and are less prone to breakage. The outermost layer of lithium polyacrylate provides a lithium source, allowing lithium ions in the lithium polyacrylate to preferentially participate in the formation of the solid electrolyte interphase (SEI) film during the first cycle. This effectively compensates for the active lithium consumed in the formation of the SEI and improves the first coulombic efficiency. The carboxylic acid lithium groups of the lithium polyacrylate can form strong hydrogen bonds with the natural oxide layer on the silicon surface and the oxygen-containing groups on the carbon material surface, providing adhesion far exceeding that of traditional PVDF adhesives. As an elastic polymer shell, it acts like a "cling film" to wrap and bind the nano-silicon / N-doped porous carbon together. When the internal silicon volume expands, this elastic shell can stretch and apply a retraction force, tightly "holding" the expanded silicon particles to prevent them from falling off and also preventing the fresh silicon surface from being exposed due to particle expansion. Detailed Implementation

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] Materials and sources used in this invention: Nano-silicon was synthesized by gas phase laser method and came from Alfa Esa (China) Chemical Reagent Co., Ltd.; The sulfide electrolyte was Li6PS5Cl, which came from Guangdong Qianjin Chemical Reagent Co., Ltd., and was of analytical grade AR.

[0030] In the following embodiments, the positive electrode material was prepared by the following steps: the active material NCM111, the sulfide electrolyte Li6PS5Cl and the conductive agent were thoroughly mixed using a homogenizer at a mass ratio of 70:25:5 to obtain the positive electrode material; the conductive agent was conductive carbon VGCF, which was obtained from Zhejiang Yamei Nanotechnology Co., Ltd., and the model number was C-F0050.

[0031] Example 1: This example provides a lithium polyacrylate@nano-silicon / N-doped porous carbon method, which includes the following steps:

[0032] Step A1: Disperse 1g of nano-silicon / N-doped porous carbon in 100mL of ethanol-water solution (ethanol to water volume ratio of 9:1) for 1h by ultrasonication, adjust the pH to 4.2, add 0.05g of KH570, then heat to 60℃ and stir for 5h. Wash with ethanol and deionized water three times alternately, and vacuum dry to obtain grafted modified nano-silicon / N-doped porous carbon.

[0033] Step A2: Disperse 0.5g of grafted modified nano-silicon / N-doped porous carbon evenly in 100mL of deionized water, add 0.4mL of isobutanol, adjust the pH to 9.5, sonicate for 1h, then add 0.2g of emulsifier OP-10 and stir for 12h, purge with nitrogen, add 0.3g of sodium bicarbonate and 0.04g of potassium persulfate and stir evenly, then slowly add 2g of acrylic acid and heat to 75℃ for polymerization reaction for 5.5h, wash with water until neutral, adjust the pH to 6, then add 50mL of 0.8mol / L lithium hydroxide aqueous solution and stir for 5h, wash with ethanol until neutral, and dry to obtain lithium polyacrylate@nano-silicon / N-doped porous carbon;

[0034] In step A1, the nano-silicon / N-doped porous carbon is prepared by the following steps:

[0035] 7g of N-doped porous carbon and 1g of nano-silicon powder were uniformly mixed, and 1g of anhydrous ethanol was added and mixed thoroughly. Then, the mixture was transferred to a ball milling jar filled with argon gas and stainless steel grinding balls were added. The ball milling jar was then placed in a planetary ball mill for ball milling and vacuum drying to obtain nano-silicon / N-doped porous carbon. The ball-to-material ratio for ball milling was 1:1, the ball milling time was 30h, and the rotation speed was 1000r / min.

[0036] The method for preparing the N-doped porous carbon includes the following steps:

[0037] Step B1: Add 0.8g of citric acid monohydrate and 2g of magnesium nitrate hexahydrate to 20mL of deionized water, then transfer to a 90℃ water bath and stir until the solvent evaporates. Then place it at 180℃ for 2h to foam and obtain the carbon precursor.

[0038] Step B2: Mix 1g of carbon precursor, 2g of urea and 2g of potassium oxalate and grind them. Then transfer the mixture to a tube furnace, heat it to a specific temperature under a nitrogen atmosphere and hold it there. Then acid wash it until it is neutral and dry it to obtain N-doped porous carbon. The holding temperature is 750℃, the heating rate is 3℃ / min, and the holding time is 2h. Acid washing: use 3mol / L hydrochloric acid to acid wash for 8h.

[0039] Example 2: This example provides a lithium polyacrylate@nano-silicon / N-doped porous carbon preparation method including the following steps:

[0040] Step A1: Disperse 1g of nano-silicon / N-doped porous carbon in 100mL of ethanol-water solution (ethanol to water volume ratio of 9:1) for 1h by ultrasonication, adjust the pH to 4.2, add 0.1g of KH570, then heat to 60℃ and stir for 5h. Wash with ethanol and deionized water three times alternately, and dry under vacuum to obtain grafted modified nano-silicon / N-doped porous carbon.

[0041] Step A2: Disperse 1g of grafted modified nano-silicon / N-doped porous carbon evenly in 100mL of deionized water, add 0.7mL of isobutanol, adjust the pH to 9.5, sonicate for 1h, then add 0.4g of emulsifier OP-10 and stir for 12h, purge with nitrogen, add 0.6g of sodium bicarbonate and 0.08g of potassium persulfate and stir evenly, then slowly add 4g of acrylic acid and heat to 75℃ for polymerization reaction for 6h, wash with water until neutral, adjust the pH to 6.5, then add 50mL of 1mol / L lithium hydroxide aqueous solution and stir for 6.5h, wash with ethanol until neutral, and dry to obtain lithium polyacrylate@nano-silicon / N-doped porous carbon;

[0042] In step A1, nano-silicon / N-doped porous carbon is prepared by the following steps:

[0043] 8g of N-doped porous carbon and 2g of nano-silicon powder were uniformly mixed, and 2g of anhydrous ethanol was added and mixed thoroughly. Then, the mixture was transferred to a ball mill jar filled with argon gas and stainless steel grinding balls were added. The ball mill jar was then placed in a planetary ball mill for ball milling and vacuum drying to obtain nano-silicon / N-doped porous carbon. The ball-to-material ratio for ball milling was 1.5:1, the ball milling time was 33h, and the rotation speed was 1100r / min.

[0044] The method for preparing N-doped porous carbon includes the following steps:

[0045] Step B1: Add 1g of citric acid monohydrate and 2.3g of magnesium nitrate hexahydrate to 20mL of deionized water, then transfer to a 90℃ water bath and stir until the solvent evaporates. Then place it at 180℃ for 2h to foam and obtain the carbon precursor.

[0046] Step B2: Mix 1g of carbon precursor, 2g of urea and 2g of potassium oxalate and grind them. Then transfer the mixture to a tube furnace, heat it to a specific temperature under a nitrogen atmosphere and hold it there. Then perform acid washing, wash until neutral, and dry to obtain N-doped porous carbon. The holding temperature is 800℃, the heating rate is 3℃ / min, and the holding time is 2h. Acid washing: use 3mol / L hydrochloric acid for 9h.

[0047] Example 3: This example provides a lithium polyacrylate@nano-silicon / N-doped porous carbon method, which includes the following steps:

[0048] Step A1: Disperse 1g of nano-silicon / N-doped porous carbon in 100mL of ethanol-water solution (ethanol to water volume ratio of 9:1) for 1h by ultrasonication, adjust the pH to 4.2, add 0.15g of KH570, then heat to 60℃ and stir for 5h. Wash with ethanol and deionized water three times alternately, and vacuum dry to obtain grafted modified nano-silicon / N-doped porous carbon.

[0049] Step A2: Disperse 1.5g of grafted modified nano-silicon / N-doped porous carbon evenly in 100mL of deionized water, add 1mL of isobutanol, adjust the pH to 9.5, sonicate for 1h, then add 0.6g of emulsifier OP-10 and stir for 12h. Purge with nitrogen, add 0.9g of sodium bicarbonate and 0.12g of potassium persulfate and stir evenly. Then slowly add 6g of acrylic acid and heat to 75℃ for polymerization reaction for 6.5h. Wash with water until neutral, then adjust the pH to 7. Then add 50mL of 1.2mol / L lithium hydroxide aqueous solution and stir for 8h. Wash with ethanol until neutral and dry to obtain lithium polyacrylate@nano-silicon / N-doped porous carbon.

[0050] In step A1, nano-silicon / N-doped porous carbon is prepared by the following steps:

[0051] 9g of N-doped porous carbon and 3g of nano-silicon powder were uniformly mixed, and 3g of anhydrous ethanol was added and mixed thoroughly. Then, the mixture was transferred to a ball milling jar filled with argon gas and stainless steel grinding balls were added. The ball milling jar was then placed in a planetary ball mill for ball milling and vacuum drying to obtain nano-silicon / N-doped porous carbon. The ball-to-material ratio for ball milling was 2:1, the ball milling time was 36h, and the rotation speed was 1200r / min.

[0052] The N-doped porous carbon is prepared by the following steps:

[0053] Step B1: Add 1.2g of citric acid monohydrate and 2.5g of magnesium nitrate hexahydrate to 20mL of deionized water, then transfer to a 90℃ water bath and stir until the solvent evaporates. Then place at 180℃ for 2h to foam and obtain carbon precursor.

[0054] Step B2: Mix 1g of carbon precursor, 2g of urea and 2g of potassium oxalate and grind them. Then transfer the mixture to a tube furnace, heat it to a specific temperature under a nitrogen atmosphere and hold it there. Then perform acid washing, wash until neutral, and dry to obtain N-doped porous carbon. The holding temperature is 850℃, the heating rate is 3℃ / min, and the holding time is 2h. Acid washing: use 3mol / L hydrochloric acid to wash for 10h.

[0055] Example 4: This example provides a high-rate silicon-based solid-state anode battery, the preparation method of which includes the following steps:

[0056] Step S1: Using a homogenizer, the lithium polyacrylate@nano-silicon / N-doped porous carbon, sulfide solid electrolyte Li6PS5Cl, and conductive agent carbon black prepared in Example 1 are thoroughly mixed in a mass ratio of 60:35:5 to obtain the silicon-based anode material.

[0057] Step S2: Using a 10mm diameter mold, 100mg of sulfide solid electrolyte Li6PS5Cl is pressed at 300MPa for 2 minutes to form a solid electrolyte layer. 38mg of positive electrode material is evenly spread on one side of the solid electrolyte layer and pressed at 300MPa for 2 minutes to form the positive electrode. Then, 2.3mg of silicon-based negative electrode material is evenly spread on the other side of the solid electrolyte layer and pressed at 900MPa for 2 minutes to form the silicon-based negative electrode. Finally, a first pressure of 100MPa is applied to the mold battery using a stainless steel clamp to assemble the prefabricated solid battery for further electrochemical testing, thus obtaining a high-rate silicon-based negative electrode solid battery. The entire assembly process is carried out in an argon-filled glove box, with an environmental requirement of water content <0.01ppm and oxygen content <0.01ppm.

[0058] Example 5: This example provides a high-rate silicon-based anode solid-state battery. The difference from Example 4 is that lithium polyacrylate@nano-silicon / N-doped porous carbon prepared in Example 2 is used instead of lithium polyacrylate@nano-silicon / N-doped porous carbon prepared in Example 1; all other aspects are the same.

[0059] Example 6: This example provides a high-rate silicon-based anode solid-state battery. The difference from Example 4 is that lithium polyacrylate@nano silicon / N-doped porous carbon prepared in Example 3 is used instead of lithium polyacrylate@nano silicon / N-doped porous carbon prepared in Example 1; all other aspects are the same.

[0060] Comparative Example 1: This comparative example is a silicon-based anode solid-state battery. The difference from Example 6 is that nano-silicon is used instead of lithium polyacrylate@nano-silicon / N-doped porous carbon prepared in Example 3. All other aspects are the same.

[0061] Comparative Example 2: This comparative example is a silicon-based anode solid-state battery. The difference from Example 6 is that the nano-silicon / N-doped porous carbon prepared in Example 3 is used instead of the lithium polyacrylate@nano-silicon / N-doped porous carbon prepared in Example 3. All other aspects are the same.

[0062] The silicon-based anode solid-state batteries prepared in Examples 4-6 and Comparative Examples 1-2 were first pretreated and then subjected to electrochemical performance testing. The specific steps are as follows:

[0063] Pretreatment method: The assembled pre-formed solid-state batteries were transferred to a constant temperature chamber at an ambient temperature of 45°C and left to stand for 12 hours. Then, the pre-formed solid-state batteries were subjected to rate charge-discharge tests using the Neware battery testing system. The first three cycles were charged and discharged at 0.1C. After the first charge to 4.2V (i.e., 100% state of charge) at 0.1C, the pre-formed solid-state batteries were removed from the stainless steel fixture and pressed again under a second pressure of 900MPa for 2 minutes. Then, the first pressure of 100MPa was applied to the mold battery again using the stainless steel fixture. The battery was then placed back in the constant temperature chamber and left to stand for 30 minutes before being discharged to 2.4V at 0.1C. The battery was then cycled for 2 more cycles at 0.1C to complete the formation process. Subsequently, the batteries were cycled for 3 more cycles at 0.2C, 0.5C, 1C, and 2C respectively.

[0064] Electrochemical performance testing method: Cyclic voltammetry tests were performed on the battery using an Autolab PGSTAT302N electrochemical workstation. The test range was 0-3V, and the scan rate was 0.1mV / s. The initial coulombic efficiency and capacity retention after 500 cycles were measured during charge-discharge cycles at 0.1C, 0.2C, 0.5C, 1C, 2C, and 5C.

[0065] The electrochemical performance test results are shown in Table 1.

[0066] Table 1: Electrochemical Performance Test Results

[0067]

[0068] As can be seen from Table 1, the silicon-based anode solid-state battery prepared by this invention not only has high rate performance, but also excellent cycle stability.

[0069] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0070] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-rate silicon-based solid-state anode battery, characterized in that: Includes the following steps: Step S1: Use a homogenizer to thoroughly mix lithium polyacrylate@nano silicon / N-doped porous carbon, sulfide solid electrolyte and conductive agent to obtain silicon-based anode material; Step S2: Press the sulfide solid electrolyte to form a solid electrolyte layer, then press a silicon-based anode material on one side of the solid electrolyte layer to form a silicon-based anode, and press a cathode material on the other side to form a cathode, thus obtaining a high-rate silicon-based anode solid battery.

2. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of lithium polyacrylate@nano-silicon / N-doped porous carbon, sulfide solid electrolyte, and conductive agent is 60:35:

5.

3. The preparation method according to claim 1, characterized in that: In step S1, the preparation method of lithium polyacrylate@nano-silicon / N-doped porous carbon includes the following steps: Step A1: Disperse nano-silicon / N-doped porous carbon in an ethanol aqueous solution by ultrasonication for 1 h, adjust the pH to 4.2, add KH570, then heat to 60℃ and stir for 5 h, wash with ethanol and deionized water three times alternately, and vacuum dry to obtain grafted modified nano-silicon / N-doped porous carbon. Step A2: Disperse the grafted modified nano-silicon / N-doped porous carbon evenly in deionized water, add isobutanol, adjust the pH to 9.5, sonicate for 1 hour, add emulsifier OP-10 and stir for 12 hours, purge with nitrogen, add sodium bicarbonate and potassium persulfate and stir evenly, then slowly add acrylic acid dropwise and heat to 75℃ for polymerization reaction for 5.5-6.5 hours, wash with water until neutral, adjust the pH to 6-7, then add 0.8-1.2 mol / L lithium hydroxide aqueous solution and stir for 5-8 hours, wash until neutral, and dry to obtain lithium polyacrylate@nano-silicon / N-doped porous carbon.

4. The preparation method according to claim 3, characterized in that: In step A1, the preparation method of nano-silicon / N-doped porous carbon is as follows: N-doped porous carbon and nano-silicon powder are uniformly mixed, anhydrous ethanol is added and mixed evenly, and then transferred to a ball milling jar filled with argon gas for ball milling treatment. After vacuum drying, nano-silicon / N-doped porous carbon is obtained.

5. The preparation method according to claim 3, characterized in that: In step A1, the ratio of nano-silicon / N-doped porous carbon, ethanol aqueous solution and KH570 is 1g:100mL:0.05-0.15g.

6. The preparation method according to claim 3, characterized in that: In step A1, the method for preparing N-doped porous carbon includes the following steps: Step B1: Add citric acid monohydrate and magnesium nitrate hexahydrate to deionized water, then transfer to a 90°C water bath and stir until the solvent evaporates. Then place at 180°C for 2 hours to foam and obtain carbon precursor. Step B2: Mix the carbon precursor, urea and potassium oxalate and grind them. Then transfer the mixture to a tube furnace and heat it to 750-850℃ at a heating rate of 3℃ / min under a nitrogen atmosphere. Hold the temperature for 2 hours. Then wash the product with 3mol / L hydrochloric acid for 8-10 hours. After washing the product to neutrality, dry it to obtain N-doped porous carbon.

7. The preparation method according to claim 6, characterized in that: In step B1, the ratio of citric acid monohydrate, magnesium nitrate hexahydrate, and deionized water is 0.8-1.2g:2-2.5g:20mL.

8. The preparation method according to claim 6, characterized in that: In step B2, the mass ratio of carbon precursor, urea, and potassium oxalate is 1:2:

2.

9. The preparation method according to claim 3, characterized in that: The ratio of the amount of grafted modified nano-silicon / N-doped porous carbon, deionized water, isobutanol, emulsifier OP-10, sodium bicarbonate, potassium persulfate, acrylic acid and lithium hydroxide aqueous solution in step A2 is 0.5-1.5g:100mL:0.4-1mL:0.2-0.6g:0.3-0.9g:0.04-0.12g:2-6g:50mL.

10. A high-rate silicon-based solid-state anode battery prepared by the method described in any one of claims 1-9.

Citation Information

Patent Citations

  • Preparation method of nitrogen-doped porous silicon-carbon negative electrode

    CN114824232A