A light high-strength silver-plated copper alloy conductor for new-generation aerospace and marine equipment

By introducing lightweight reinforcing components and rare earth elements into copper alloy conductors, combined with nano-silicon carbide particles and specific processing techniques, the problem of synergistic improvement of lightweight, high strength, and conductivity of copper alloy conductors in aerospace and marine engineering equipment has been solved, achieving high performance stability in extreme environments.

CN122279311BActive Publication Date: 2026-11-10YANGZHOU YAGUANG CABLE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610528512.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-04-21
Publication Date
2026-11-10
Estimated Expiration
2046-04-21

AI Technical Summary

Technical Problem

Existing copper alloy conductors face the challenge of simultaneously improving lightweight, high strength, and conductivity in aerospace and marine engineering equipment. The addition of traditional alloying elements leads to lattice distortion, affecting conductivity. The interfacial bonding between the coating and the substrate is unstable, making it prone to corrosion and causing performance degradation in extreme environments.

Method used

Lightweight reinforcing components aluminum, magnesium, and rare earth elements yttrium and cerium are used to form a diffusely distributed intermetallic compound through solid solution and precipitated phases. Combined with nano-silicon carbide particles, a multi-scale strengthening system is formed. A gradient diffusion interface is constructed through vacuum melting, multi-pass cold drawing, electrochemical deposition, and synergistic heat treatment processes.

Benefits of technology

A lightweight, high-strength, and highly conductive copper alloy conductor has been developed, which can maintain structural stability in extreme environments, reduce signal transmission loss, and improve overall reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122279311B_ABST
    Figure CN122279311B_ABST
Patent Text Reader

Abstract

The application relates to the alloy material processing technical field and discloses a preparation process of a light high-strength silver-plated copper alloy conductor for a new-generation aerospace and marine equipment, which comprises the following steps: vacuum smelting raw materials containing copper, a light strengthening component and a structure stabilizing aid, obtaining a wire through multi-pass cold drawing, sequentially depositing a transition layer and a silver plating layer after pretreatment and carrying out synergic heat treatment; the application reduces the density through the light strengthening component, locks the grain boundary through the structure stabilizing aid, combines cold drawing and heat treatment to construct a multi-scale strengthening system, and significantly improves the tensile strength of the conductor. Through the transition layer and the precise silver plating process, the interface bonding force is enhanced, and atomic diffusion is inhibited, so that the deep coupling of light weight, high strength, high conductivity and excellent environmental adaptability of the conductor is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy material processing technology, specifically to a lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment. Background Technology

[0002] As next-generation aerospace equipment develops towards lightweight, high integration, and adaptability to extreme environments, the demand for high-performance conductive materials is becoming increasingly urgent. Signal transmission and power distribution systems in aerospace vehicles require conductors with excellent conductivity while also meeting stringent weight reduction targets and high-strength support performance. Simultaneously, next-generation marine engineering equipment, such as deep-sea exploration, seabed observation networks, and ship integrated power systems, places even more stringent service requirements on conductive materials. Conductors must not only withstand the coupled corrosion environment of high salt spray, high humidity, and seawater pressure, but also endure continuous alternating stress and impact loads under long-term mooring or towing conditions. Traditional copper alloy conductors are prone to problems such as plating peeling, interface corrosion, and stress fatigue failure in marine environments. Currently, silver-plated copper alloy wires are widely used in the aerospace field due to their good conductivity, oxidation resistance, and weldability. Traditional copper alloys often employ solid solution strengthening or deformation strengthening methods, adding alloying elements to enhance the matrix strength and thus adapt to complex mechanical environments.

[0003] In pursuing high strength, existing copper alloy systems face the challenge of balancing increased density with decreased conductivity. The addition of conventional alloying elements can easily induce lattice distortion, leading to increased electron scattering and thus weakening the material's conductivity advantage. Furthermore, under extreme temperature differences and vibration coupling, the microstructure stability of traditional alloys has room for optimization, and the interfacial bonding force between the substrate and the coating may fluctuate during service, affecting the overall reliability of the conductor. The long-term underwater service environment of marine engineering equipment further exacerbates the electrochemical corrosion tendency between the coating and the substrate, and the low-frequency fatigue load introduced by the dynamic movement of the equipment poses a synergistic optimization requirement for the conductor's lightweight, high strength, and environmental corrosion resistance. Therefore, how to achieve a synergistic improvement in strength and conductivity while maintaining lightweighting through precise alloying design and microstructure control is a direction that urgently needs optimization in the field of aerospace conductive materials. Summary of the Invention

[0004] In order to solve the technical problems in the prior art, this application provides a lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment.

[0005] The first inventive objective of this invention is achieved through the following technical solution: A lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment includes a base alloy, a transition layer disposed on the surface of the base alloy, and a silver plating layer disposed on the surface of the transition layer. The base alloy comprises the following components in parts by weight: copper; The lightweight reinforcing component is at least two of aluminum, magnesium, and lithium; A tissue stabilizing agent, wherein the tissue stabilizing agent is at least one selected from yttrium, cerium, and lanthanum.

[0006] By adopting the above technical solution, the matrix alloy uses copper as the main conductive phase. By introducing lightweight reinforcing components, solid solutions or precipitates are formed in the copper lattice. The aluminum, magnesium, and lithium elements in the lightweight reinforcing components have low atomic masses. After entering the copper matrix, they occupy lattice sites through substitution or interstitial solid solution, changing the lattice constant. During deformation processing, these elements induce lattice distortion, generating a stress field that interacts with dislocations and hinders dislocation movement. At the same time, through a specific combination, the lightweight reinforcing components precipitate from the supersaturated solid solution during subsequent heat treatment, forming dispersed intermetallic compound particles. These particles produce a pinning effect within the grains. The rare earth elements in the structure stabilizing agent have large atomic radii, easily accumulate at grain boundaries, occupy grain boundary vacancies, reduce grain boundary energy, and inhibit grain growth under high temperature or extreme environments. The rare earth elements react chemically with impurity elements in the matrix to form high-melting-point spherical compounds, purifying grain boundaries, reducing the electron scattering cross section at grain boundaries, and maintaining the mean free path of electrons.

[0007] Optionally, the total mass of the lightweight reinforcing component accounts for 1 wt% to 3 wt% of the total mass of the matrix alloy; the lightweight reinforcing component comprises aluminum and magnesium, and the mass ratio of aluminum to magnesium is 1:1 to 3:1.

[0008] By adopting the above technical solution, aluminum and magnesium form a composite precipitate with a specific structure in a copper matrix. The lattice constant of the composite precipitate matches that of the copper matrix, which reduces the phase transition strain energy at the phase interface and forms a semi-coherent interface. While maintaining a high density of dislocation pinning sites, it reduces the interference to coherent electron waves.

[0009] Optionally, the tissue stabilizing agent further includes nano-silicon carbide particles with an average particle size of 40 nm to 60 nm.

[0010] By adopting the above technical solution, nano-silicon carbide particles are distributed in the grain gaps of the matrix alloy to form a dispersed strengthening phase; the nano-silicon carbide particles have high modulus and thermal stability, can bear part of the load under stress, and limit the creep behavior of the matrix structure under temperature fluctuation.

[0011] The second objective of this invention is achieved through the following technical solution: A manufacturing process for a lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment includes the following steps: Step 1, Melting and Casting: The components of the base alloy are put into a vacuum induction melting furnace and melted under vacuum conditions to obtain an alloy melt; the alloy melt is injected into a mold for continuous casting to obtain an alloy billet; Step 2, Deformation processing: The alloy billet is subjected to multiple cold drawing processes to obtain an alloy wire with a specific diameter; between adjacent cold drawing processes, the alloy billet or wire is subjected to short-time flash annealing. Step 3, Surface pretreatment: The alloy wire is subjected to degreasing, pickling and activation, and rinsing in sequence to remove the surface oxide layer and deposits; Step 4, Transition layer deposition: A transition layer is formed on the surface of the alloy wire after surface pretreatment by electrochemical deposition; Step 5, silver plating: Electroplating silver is performed on the surface of the transition layer to form a silver plating layer, thus obtaining the initial composite conductor product; Step 6, Synergistic heat treatment: The composite conductor sample is placed in a protective atmosphere furnace, heated to a first predetermined temperature and held at that temperature for a specific time, and then cooled to ambient temperature along with the furnace.

[0012] By adopting the above technical solutions, the vacuum melting environment in step one reduces the probability of gaseous impurities such as oxygen and hydrogen entering the melt, avoiding the formation of oxide inclusions; the continuous casting process controls the cooling rate, allowing alloying elements to form fine dendritic structures during crystallization, reducing macroscopic segregation; the multi-pass cold drawing process in step two generates high-density dislocations, stacking faults, and deformation twins inside the wire, and the grains are elongated along the drawing direction to form a fibrous structure, increasing the axial tensile strength of the material; the surface pretreatment in step three presents a highly active layer of fresh metal atoms on the alloy surface, providing a physical basis for the subsequent coating bonding; and the transition process in step four... In step five, the transition layer atoms diffuse simultaneously toward both the base alloy and the silver plating, forming a gradient transition region to alleviate the thermal stress caused by the difference in thermal expansion coefficients between the base and the plating. In step six, the synergistic heat treatment induces recovery and recrystallization within the base, releasing the excessive internal stress accumulated during deformation processing. Simultaneously, it promotes the precipitation of supersaturated solid solution strengthening elements in the form of dispersed phases, restoring conductivity while maintaining strength through a precipitation strengthening mechanism.

[0013] Optionally, in step four, the transition layer is a nickel transition layer, and its deposition process includes: The surface-pretreated alloy wire was immersed in a solution containing 300 g·L -1 Nickel aminosulfonate and 30 g·L-1 In the electrolyte of boric acid, using the alloy wire as the cathode, the current density is controlled at 2 A·dm³. -2 Deposition for 5 minutes.

[0014] By adopting the above technical solution, nickel atoms form a dense coating layer on the alloy surface. The nickel layer acts as a barrier layer, inhibiting the long-range diffusion of copper atoms towards the silver plating layer, reducing the brittle intermetallic compounds formed by atomic interdiffusion during service, and maintaining the mechanical integrity of the interface.

[0015] Optionally, in step five, the electroplating solution used for the silver plating process comprises 35 g·L -1 Potassium silver cyanide, 100 g·L -1 Free potassium cyanide and 5 mL·L -1 Organic brightener; electroplating bath temperature controlled at 30℃, cathode current density at 0.5A·dm³ -2 .

[0016] By adopting the above technical solution, potassium silver cyanide is used as the main salt to provide silver ions, and free potassium cyanide is used as a complexing agent to adjust the polarization of the solution. The organic brightener is adsorbed on the high-energy sites on the cathode surface, which changes the double layer structure, inhibits grain coarsening, makes the silver coating exhibit a fine-grained structure, reduces surface roughness, and reduces skin effect loss during high-frequency signal transmission.

[0017] Optionally, in step two, the surface area reduction rate of each cold drawing process is 18%, and the total processing rate is 95%; the temperature of the short-time flash annealing is 450°C and the time is 2 seconds.

[0018] By adopting the above technical solution, short-time flash annealing causes partial recovery of the wire, eliminates excessive brittleness caused by work hardening, maintains the plastic processing performance of the material, and enables the wire to be continuously deformed to a predetermined fine diameter without breaking.

[0019] Optionally, the specific steps of the smelting and casting are as follows: The components of the matrix alloy were placed in a vacuum induction melting furnace and evacuated to a vacuum level of 1×10⁻⁶. -2 Pa to 1×10 -3 Pa was melted at 1250℃ to obtain an alloy melt; During the smelting process, the electromagnetic induction stirring device is activated, and the stirring frequency is controlled at 25Hz, the stirring current is 150A, and the stirring is continued for 15 minutes. After melting, the molten alloy is injected into a horizontal continuous casting machine mold equipped with a cooling water circulation system for continuous casting, with the traction speed controlled at 150 mm / min. -1 The cooling water flow rate is 20 L / min. -1 The alloy billet with a diameter of 15 mm was obtained.

[0020] By adopting the above technical solution, electromagnetic induction stirring generates Lorentz force, which drives the melt to generate forced convection, so that the lightweight reinforcing components and the structure stabilizing agents are evenly distributed in the copper matrix, eliminating the component stratification phenomenon caused by density differences and improving the composition uniformity of the billet.

[0021] Optionally, in step three, the pickling solution used for pickling activation is a mixed solution containing 15 wt% sulfuric acid and 5 wt% hydrogen peroxide.

[0022] By adopting the above technical solution, hydrogen peroxide is used as an oxidant to increase the pickling rate, dilute sulfuric acid dissolves the alkaline oxides on the surface, and the mixed solution forms a micro-rough structure on the wire surface, increasing the surface area and improving the mechanical interlocking force between the subsequent coating and the substrate.

[0023] Optionally, the specific steps of the synergistic heat treatment are as follows: The composite conductor precursor was placed in a furnace with a protective atmosphere containing 95 vol% argon and 5 vol% hydrogen, and heated at 5 °C / min. -1 Heat to 400℃ at a rising rate and hold for 2 hours; After the heat preservation is completed, first use 2℃·min -1 The temperature was reduced to 200°C at a cooling rate and held for 1 hour, and then cooled to room temperature with the furnace.

[0024] By adopting the above technical solution, the size and distribution density of the precipitated phase are controlled by segmented cooling, preventing the precipitated particles from growing excessively and keeping the reinforcing phase within the nanoscale range, thereby maximizing the pinning effect.

[0025] In summary, this application includes at least one of the following beneficial technical effects: 1. By designing alloy components and controlling the microstructure, the problem of synergistic lightweighting and high performance of conductive materials for aerospace environments was solved; the introduction of lightweight reinforcing components into the matrix alloy reduced the overall density of the conductor, meeting the weight reduction requirements of aerospace equipment; the addition of microstructure stabilizing agents effectively locked the grain boundaries and improved the microstructure stability of the material under extreme temperature differences.

[0026] 2. The preparation process uses a logical combination of vacuum melting, multi-pass cold drawing and synergistic heat treatment to construct a multi-scale strengthening system consisting of dislocation strengthening, solid solution strengthening and dispersion strengthening inside the matrix, thereby obtaining extremely high tensile strength. At the same time, by setting a transition layer and silver plating process, the interfacial bonding force between the matrix and the plating layer is enhanced, forming a gradient diffusion interface, which effectively suppresses atomic diffusion and interfacial cracking during service.

[0027] 3. The fine-grained structure and low-roughness surface of the silver coating reduce signal transmission loss; the overall process achieves deep coupling between the material's microstructure and macroscopic properties, resulting in a conductive material state that combines lightweight, high strength, high conductivity, and excellent environmental adaptability. Attached Figure Description

[0028] Figure 1 This is a flowchart of the overall preparation process of the present invention.

[0029] Figure 2 This is a flowchart of the preparation example 1 of the present invention.

[0030] Figure 3 The flowchart is for Example 7 of the present invention.

[0031] Figure 4 This is a flowchart of Embodiment 1 of the present invention. Detailed Implementation

[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. In addition, the forms of the various structures described in the following embodiments are merely illustrative. The preparation process of a lightweight, high-strength silver-plated copper alloy conductor for a new generation of aerospace and marine engineering equipment involved in the present invention is not limited to the structures described in the following embodiments. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0033] Please see Figures 1-4 The process for manufacturing a lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment, as shown, includes the following raw materials: Electrolytic copper, 99.98 wt% purity, purchased from Jiangsu Boaote Steel Co., Ltd. High-purity aluminum, 99.95 wt% purity, purchased from Tianjin Yuhengxiang Metal Products Co., Ltd. Magnesium metal, 99.9 wt% purity, purchased from Suzhou Haichuan Rare Metals Products Co., Ltd. Lithium metal, 99.9 wt% purity, purchased from Guangdong Daxiao Chemical Co., Ltd. Metallic yttrium, 99.9 wt% purity, purchased from Ganzhou Liantuo New Materials Co., Ltd. The nano-silicon carbide particles, with an average particle size of 40-60 nm, are spherical and have a purity of 99.9 wt%, and were purchased from Guangzhou Hongwu Materials Technology Co., Ltd. Nickel aminosulfonate, purity 99.5 wt%, purchased from Jinan Kaichuang Chemical Co., Ltd. Potassium silver cyanide, purity 99.9 wt%, purchased from Jinjiang Jinshun Chemical Trading Co., Ltd. Organic brightener, model Ag-102, purchased from Greenlink (Jining) Chemical Technology Co., Ltd.; Hydrogen peroxide and sulfuric acid were both purchased from Anhui Huertai Chemical Co., Ltd. Free potassium cyanide was purchased from Xinjiang Huaxing Youbang Trading Co., Ltd. Acetone was purchased from Maoming Xiongda Chemical Co., Ltd.

[0034] Preparation Example 1 A matrix alloy billet, the preparation method of which is as follows: 100 kg of electrolytic copper was added to a vacuum induction melting furnace, and the vacuum system was turned on to evacuate to a vacuum level of 1 × 10⁻⁶. -2 Pa to 1×10 -3 Pa, set the melting temperature to 1250℃, and after the copper is completely melted, 1.5 kg of high-purity aluminum, 0.5 kg of metallic magnesium and 0.1 kg of metallic yttrium are sequentially added through the feeding hopper to obtain the alloy melt; Start the electromagnetic induction stirring device, control the stirring frequency at 25Hz and the stirring current at 150A, and continue stirring for 15 minutes. Then, inject the alloy melt into the mold of a horizontal continuous casting machine equipped with a cooling water circulation system, and control the traction speed at 150 mm / min. -1 The cooling water flow rate is 20 L / min. -1 This yields an alloy billet with a diameter of 15 mm.

[0035] Preparation Example 2 A base alloy billet, which differs from Preparation Example 1 in that: the high-purity aluminum is 0.5 kg; the rest is the same as Preparation Example 1.

[0036] Preparation Example 3 A base alloy billet, which differs from Preparation Example 1 in that: the high-purity aluminum is 3.0 kg; the rest is the same as Preparation Example 1.

[0037] Preparation Example 4 A base alloy billet, which differs from Preparation Example 1 in that: the high-purity aluminum is 0.3 kg; the rest is the same as Preparation Example 1.

[0038] Preparation Example 5 A base alloy billet, which differs from Preparation Example 1 in that: the high-purity aluminum is 3.5 kg; the rest is the same as Preparation Example 1.

[0039] Preparation Example 6 A matrix alloy billet, which differs from Preparation Example 1 in that: an equal mass of metallic lithium is used instead of metallic magnesium; the rest is the same as Preparation Example 1.

[0040] Preparation Example 7 A surface treatment process is described below: an alloy billet is placed on a multi-pass cold drawing machine for deformation processing, with a reduction rate of 18% per pass and a total processing rate of 95% to obtain alloy wire. Short-time flash annealing is performed between adjacent passes using an induction heating device at a temperature of 450°C for 2 seconds. The alloy wire was immersed in a pickling solution containing 15 wt% sulfuric acid and 5 wt% hydrogen peroxide for 3 minutes at room temperature (25°C), then rinsed with deionized water for 2 minutes, and subsequently immersed in a solution containing 300 g·L⁻¹ sulfuric acid and 5 wt% hydrogen peroxide. -1 Nickel aminosulfonate and 30 g·L -1 In the electrolyte of boric acid, using alloy wire as the cathode, the current density is controlled at 2 A·dm³. -2 After deposition for 5 minutes, a wire with a nickel transition layer is obtained.

[0041] Preparation Example 8 A surface treatment process differs from Preparation Example 7 in that: short-time flash annealing is not performed, and hydrogen peroxide is not added to the pickling solution; the rest is the same as Preparation Example 7.

[0042] Preparation Example 9 A surface treatment process, which differs from Preparation Example 7 in that: no transition layer electrodeposition is performed; the rest is the same as Preparation Example 7.

[0043] Preparation Example 10 A surface treatment process differs from Preparation Example 7 in that: metal cerium of equal mass is used instead of metal yttrium; the rest is the same as Preparation Example 7.

[0044] Preparation Example 11 A surface treatment process differs from Preparation Example 7 in that: lanthanum is used in place of yttrium by mass; the rest is the same as Preparation Example 7.

[0045] Preparation Example 12 A surface treatment process differs from Preparation Example 7 in that: 0.033 kg each of yttrium, cerium, and lanthanum are added simultaneously; the rest of the process is the same as Preparation Example 7.

[0046] Preparation Example 13 A surface treatment process, which differs from Preparation Example 7 in that: 1.0 kg of high-purity aluminum and 1.0 kg of metallic magnesium are used; the rest are the same as Preparation Example 7.

[0047] Preparation Example 14 A surface treatment process differs from Preparation Example 7 in that: 0.5 kg of high-purity aluminum and 1.5 kg of metallic magnesium are used; the rest are the same as in Preparation Example 7.

[0048] Preparation Example 15 A surface treatment process, which differs from Preparation Example 7 in that: 1.5 kg of high-purity aluminum and 0.5 kg of metallic magnesium are used; the rest are the same as Preparation Example 7.

[0049] Preparation Example 16 A surface treatment process, which differs from Preparation Example 7 in that: 0.4 kg of high-purity aluminum and 1.6 kg of metallic magnesium are used; the rest are the same as Preparation Example 7.

[0050] Preparation Example 17 A surface treatment process, which differs from Preparation Example 7 in that: no nano-silicon carbide particles are added to the matrix alloy; the rest is the same as Preparation Example 7.

[0051] Preparation Example 18 A surface treatment process differs from Preparation Example 7 in that: 50 kg of electrolytic copper, 0.75 kg of high-purity aluminum, 0.25 kg of metallic magnesium, and 0.05 kg of metallic yttrium are used; the rest are the same as in Preparation Example 7.

[0052] Preparation Example 19 A surface treatment process differs from Preparation Example 7 in that: the amount of electrolytic copper is 150 kg, the amount of high-purity aluminum is 2.25 kg, the amount of metallic magnesium is 0.75 kg, and the amount of metallic yttrium is 0.15 kg; the rest is the same as Preparation Example 7.

[0053] Example 1 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor includes the following steps: The base alloy billet from Preparation Example 1 was obtained, and cold drawing, pickling and nickel transition layer deposition were performed according to the operating procedure described in Preparation Example 7 to obtain pretreated alloy wire. The pretreated alloy wire was immersed in a silver plating bath. The plating solution consisted of 35 g / L potassium silver cyanide. -1 100 g·L⁻¹ of free potassium cyanide -1 Organic brightener 5 mL·L -1 The electroplating solution temperature was controlled at 30℃, and the cathode current density was 0.5 A·dm³. -2 Electroplating for 15 minutes yields a preliminary composite conductor product; The raw composite conductor was placed in a resistance furnace filled with a protective atmosphere of 95 vol% Ar + 5 vol% H2 and heated at 5 °C / min. -1 The temperature was increased to 400℃ at a heating rate of 100℃, held for 2 hours, and then increased at a rate of 2℃·min. -1 The temperature was lowered to 200℃ and held for 1 hour. Finally, the furnace was cooled to room temperature to obtain a lightweight, high-strength silver-plated copper alloy conductor.

[0054] Comparative Example 1 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 8; the rest is the same as in Example 1.

[0055] Comparative Example 2 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 9; the rest is the same as in Example 1.

[0056] Comparative Example 3 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that: after silver plating in step five, the synergistic heat treatment described in step six is ​​not performed, and the product is directly used as the finished product; the rest of the process is the same as in Example 1.

[0057] Example 2 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 10; the rest is the same as in Example 1.

[0058] Example 3 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 11; the rest is the same as in Example 1.

[0059] Example 4 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 12; the rest is the same as Example 1.

[0060] Example 5 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 13; the rest is the same as in Example 1.

[0061] Example 6 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 14; the rest is the same as in Example 1.

[0062] Example 7 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 15; the rest is the same as in Example 1.

[0063] Example 8 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 16; the rest is the same as in Example 1.

[0064] Example 9 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 17; the rest is the same as in Example 1.

[0065] Example 10 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that an electromagnetic induction stirring device is not used during the smelting process; the rest is the same as in Example 1.

[0066] Example 11 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the synergistic heat treatment temperature is set to 350°C; the rest is the same as in Example 1.

[0067] Example 12 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the synergistic heat treatment temperature is set to 450°C; the rest is the same as in Example 1.

[0068] Example 13 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the synergistic heat treatment holding time is 1 hour; the rest is the same as in Example 1.

[0069] Example 14 The preparation process of a lightweight, high-strength silver-plated copper alloy conductor differs from that of Example 1 in that the synergistic heat treatment holding time is 4 hours; the rest is the same as that of Example 1.

[0070] Example 15 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the base alloy blank is derived from Preparation Example 2; the rest is the same as in Example 1.

[0071] Example 16 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the base alloy blank is derived from Preparation Example 3; the rest is the same as in Example 1.

[0072] Example 17 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the base alloy blank is derived from Preparation Example 4; the rest is the same as in Example 1.

[0073] Example 18 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the base alloy blank is derived from Preparation Example 5; the rest is the same as in Example 1.

[0074] Example 19 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the base alloy blank is derived from Preparation Example 6; the rest is the same as in Example 1.

[0075] Example 20 A preparation process for a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 18, and the heat treatment temperature is 380°C; the rest of the process is the same as in Example 1.

[0076] Example 21 A process for preparing a lightweight, high-strength silver-plated copper alloy conductor differs from Example 1 in that the surface treatment process is derived from Preparation Example 19, and the heat treatment temperature is 420°C; the rest of the process is the same as in Example 1.

[0077] The following tests were conducted on Examples 1-21 and Comparative Examples 1-3: Tensile strength was tested using an electronic universal testing machine. Conductivity was measured using an eddy current conductivity meter. (In IACS%); Material density was determined using the Archimedes displacement method. The test results are shown in Table 1.

[0078] Table 1. Detection results of Examples 1-21 and Comparative Examples 1-2:

[0079] Based on Table 1, the test results are analyzed as follows: Compared with Comparative Examples 1 and 1-2, the overall mechanical and electrical properties of Example 1 are superior to those of Comparative Examples 1-2. The difference between Example 1 and Comparative Examples 1-2 is that Example 1 underwent short-time flash annealing, acid pickling activation, and nickel transition layer deposition during the preparation process. The nickel transition layer, as a diffusion barrier layer, effectively inhibited the long-range migration between copper and silver atoms, reduced the formation of brittle intermetallic compounds, and maintained the structural integrity of the interface. At the same time, acid pickling activation improved the mechanical interlocking strength between the coating and the substrate. It can be seen that complete surface treatment and transition layer deposition are beneficial to improving the overall performance of the conductor.

[0080] Comparing Example 1 and Comparative Example 3, the electrical conductivity of Example 1 was significantly higher than that of Comparative Example 3, while the tensile strength only decreased slightly. Comparative Example 3 did not undergo synergistic heat treatment, and its interior retained the high-density dislocations and work-hardened structure introduced by cold drawing. Although it achieved the highest tensile strength, the lattice distortion was severe, and electron scattering was intensified, resulting in a significant decrease in electrical conductivity to 85.8%. Example 1, through synergistic heat treatment, caused the matrix to recover and recrystallize, releasing the excessive internal stress. At the same time, it promoted the precipitation of strengthening elements in the form of nano-dispersed phases, increasing the electrical conductivity by nearly 8% while only losing about 4% of the tensile strength. It can be seen that the synergistic heat treatment step is a key process step to achieve synergistic optimization of strength and electrical conductivity.

[0081] Comparing Examples 1 and 5-8, the tensile strength and conductivity matching degree of Example 1 is better than that of Examples 5-8. The difference between Example 1 and Examples 5-8 is that the mass ratio of aluminum to magnesium in the matrix alloy of Example 1 is within a specific range. Under this ratio, aluminum and magnesium form a composite precipitate with a semi-coherent interface in the copper matrix. While generating dislocation pinning effect, the precipitate has a low lattice distortion energy, which reduces the scattering effect on electron waves. It can be seen that the precise control of the aluminum-magnesium mass ratio is conducive to achieving a synergistic improvement in strength and conductivity.

[0082] Comparing Example 1 and Example 9, the tensile strength of Example 1 is significantly higher than that of Example 9. The difference between Example 1 and Example 9 is that nano-silicon carbide particles were added to the matrix alloy of Example 1. The nano-silicon carbide particles, as a high-modulus second phase, are distributed at the grain boundaries and within the grains. They share the load through a dispersion strengthening mechanism and limit the recovery rate of the matrix structure during heat treatment, thus maintaining a high-density deformation-strengthened structure. It can be seen that the addition of nano-silicon carbide particles is beneficial to improving the strength of the material.

[0083] Comparing Example 1 and Example 10, Example 1 exhibits better performance stability and uniformity than Example 10. The difference between Example 1 and Example 10 lies in the fact that Example 1 employed an electromagnetic induction stirring device during the smelting process. The Lorentz force generated by the electromagnetic stirring drives the melt to produce strong convection motion, which ensures that lightweight components such as aluminum, magnesium, and lithium, as well as rare earth elements with density differences, are evenly distributed in the copper melt, eliminating component segregation. It can be seen that performing electromagnetic stirring is beneficial to improving the microstructure uniformity of the alloy billet.

[0084] Comparing Examples 1 and 11-14, Example 1 achieved an optimal balance between tensile strength and electrical conductivity. The difference between Example 1 and Examples 11-14 lies in the fact that Example 1 employed a specific synergistic heat treatment temperature and time. Under these conditions, work hardening within the matrix was moderately eliminated, while reinforcing elements in the supersaturated solid solution precipitated as nanoscale dispersed phases. The size and distribution density of the precipitated phases achieved a balance between pinning dislocations and maintaining the mean free path. It can be seen that reasonable synergistic heat treatment parameters are beneficial for optimizing the overall performance of the conductor.

[0085] Compared with Examples 1 and 15-18, Example 1 shows a better trade-off between density and strength than Examples 15-18. The difference between Example 1 and Examples 15-18 is that the loading of the lightweight reinforcing component in Example 1 is in the range of 1-3 wt%. Within this range, the alloy achieves significant weight reduction while avoiding severe lattice distortion and a significant decrease in conductivity caused by excessive alloying elements, thus maintaining the lightweight and high-strength characteristics required for aerospace equipment. It can be seen that controlling the content of the lightweight reinforcing component within a reasonable range is beneficial to improving the applicability of the material.

[0086] Comparing Example 1 and Example 19, the density of Example 1 is lower than that of Example 19. The difference between Example 1 and Example 19 is that Example 1 uses a combination of aluminum and magnesium as a strengthening method. Magnesium atoms and lithium atoms have smaller atomic masses, and their effect on reducing the overall density is more significant after entering the copper lattice. Moreover, the precipitated strengthening phase formed has higher thermal stability. It can be seen that selecting a specific combination of lightweight strengthening components is beneficial to achieving lightweight design of conductors.

[0087] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of protection claimed in this application.

[0088] All contents not described in detail in the specification are existing technologies known to those skilled in the art, and the model parameters of each raw material and equipment are not specifically limited; conventional equipment can be used. Control elements and auxiliary systems not mentioned in this technical solution are not shown in the figures because they are existing technologies, and will not be described here.

[0089] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment, characterized in that... include: A base alloy, a transition layer disposed on the surface of the base alloy, and a silver plating layer disposed on the surface of the transition layer; The base alloy comprises the following components in parts by weight: copper; The lightweight reinforcing component is at least two of aluminum, magnesium, and lithium; Tissue stabilizing agent, wherein the tissue stabilizing agent is at least one selected from yttrium, cerium, and lanthanum; The total mass of the lightweight reinforcing component accounts for 1 wt% to 3 wt% of the total mass of the matrix alloy; the lightweight reinforcing component comprises aluminum and magnesium, and the mass ratio of aluminum to magnesium is 1:1 to 3:1; The tissue stabilizing agent also includes nano-silicon carbide particles, the average particle size of which is 40 nm to 60 nm. The preparation process of the copper alloy conductor includes the following steps: Step 1, Melting and Casting: The components of the base alloy are put into a vacuum induction melting furnace and melted under vacuum conditions to obtain an alloy melt; the alloy melt is injected into a mold for continuous casting to obtain an alloy billet; Step 2, Deformation processing: The alloy billet is subjected to multiple cold drawing processes to obtain alloy wire; between adjacent cold drawing processes, the alloy billet or wire is subjected to short-time flash annealing. Step 3, Surface pretreatment: The alloy wire is subjected to degreasing, pickling and activation, and rinsing in sequence to remove the surface oxide layer and deposits; Step 4, Transition layer deposition: A transition layer is formed on the surface of the alloy wire after surface pretreatment by electrochemical deposition; Step 5, silver plating: electroplating silver is performed on the surface of the transition layer to form a silver plating layer, thus obtaining the initial composite conductor product; Step 6, Synergistic heat treatment: The composite conductor sample is placed in a protective atmosphere furnace, heated to a first predetermined temperature and held at that temperature, and then cooled to ambient temperature with the furnace. In step three, the pickling solution used for pickling activation is a mixed solution containing 15 wt% sulfuric acid and 5 wt% hydrogen peroxide; In step four, the transition layer is a nickel transition layer, and its deposition process includes: The pretreated alloy wire was immersed in an electrolyte containing 300 g·L⁻¹ nickel aminosulfonate and 30 g·L⁻¹ boric acid. The alloy wire was used as the cathode, and the current density was controlled at 2 A·dm⁻² for 5 min. The specific steps of the synergistic heat treatment are as follows: The composite conductor sample was placed in a furnace with a protective atmosphere containing 95 vol% argon and 5 vol% hydrogen, and heated to 400°C at a heating rate of 5°C·min⁻¹, and held at that temperature for 2 hours. After the heat preservation is completed, the temperature is first reduced to 200℃ at a cooling rate of 2℃·min-1 and kept at that temperature for 1 hour, and then cooled to room temperature with the furnace.

2. The lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment according to claim 1, characterized in that, The specific steps of the smelting and casting are as follows: The components of the matrix alloy were placed in a vacuum induction melting furnace and evacuated to a vacuum level of 1×10⁻⁶. -2 Pa to 1×10 - 3 Pa was melted at 1250℃ to obtain an alloy melt; During the smelting process, the electromagnetic induction stirring device is activated, and the stirring frequency is controlled at 25Hz, the stirring current is 150A, and the stirring is continued for 15 minutes. After melting, the molten alloy is injected into a horizontal continuous casting machine mold equipped with a cooling water circulation system for continuous casting, with the traction speed controlled at 150 mm / min. -1 The cooling water flow rate is 20 L / min. -1 The alloy billet with a diameter of 15 mm was obtained.

3. The lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment according to claim 1, characterized in that, In step two, the surface area reduction rate of each cold drawing process is 18%, and the total processing rate is 95%; the temperature of the short flash annealing is 450℃ and the time is 2s.

4. The lightweight, high-strength silver-plated copper alloy conductor for next-generation aerospace and marine engineering equipment according to claim 1, characterized in that, In step five, the electroplating solution used for the silver plating process comprises 35 g·L -1 Potassium silver cyanide, 100 g·L -1 Free potassium cyanide and 5 mL·L -1 Organic brightener; electroplating bath temperature controlled at 30℃, cathode current density at 0.5A·dm³ -2 .

Citation Information

Patent Citations

  • An Aluminum Hybrid Metal Matrix Composite And Method Of Preparation Thereof

    AU2021104792A4

  • High-temperature abrasion resistant composite material and preparation method thereof

    CN107747070A