A method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings

By constructing a green composite modification system and a multi-source solid waste collaborative design, the problems of dispersion and interfacial bonding of siderite tailings in polypropylene matrix were solved, and high-performance iron tailings-filled polypropylene-based environmentally friendly stone paperboard was prepared. It has excellent processing rheology and mechanical properties, achieving a balance between environmental protection and high performance.

CN122323498BActive Publication Date: 2026-11-17青岛佳晟德高分子材料有限公司 +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610328546.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-03-18
Publication Date
2026-11-17
Estimated Expiration
2046-03-18

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve uniform dispersion and strong interfacial bonding when introducing complex inorganic powders such as siderite tailings into a high proportion of polypropylene matrix. This leads to interfacial defects, stress concentration, and processing rheology issues. Furthermore, traditional coupling agents pose environmental risks and are insufficient to meet the requirements of high-end packaging materials.

Method used

Using multi-source solid waste such as siderite tailings, coal gangue and phosphogypsum as fillers, a green composite modification system is constructed by stearic acid and epoxidized soybean oil. Combined with grafted compatibilizer and elastomer, and using a three-layer co-extrusion process of graded grinding, in-situ activation, intensive mixing and granulation and gradient cooling, polypropylene-based environmentally friendly stone paperboard filled with iron tailings is prepared.

Benefits of technology

It achieves uniform dispersion of materials with high filler content, excellent processing rheology, high edge compressive strength and burst strength, and also has waterproof and moisture-proof, flexural and fatigue resistance and controllable photo-oxidative degradation characteristics, thus meeting the requirements of environmental protection and high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122323498B_ABST
    Figure CN122323498B_ABST
Patent Text Reader

Abstract

This invention relates to the field of high-performance polypropylene technology, specifically a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings. This invention improves upon the problems of poor processing performance and difficulty in achieving optimal finished product performance in stone paperboard. By using multi-source solid waste such as siderite tailings, coal gangue, and phosphogypsum as fillers, and employing a green composite modification system constructed with stearic acid and epoxidized soybean oil to replace traditional coupling agents, combined with grafted compatibilizers and elastomers, the paperboard is produced through a three-layer co-extrusion process involving graded grinding, in-situ activation, intensive mixing and granulation, and gradient cooling. The resulting paperboard, with a solid waste content ≥50%, exhibits excellent processing rheology, high edge crush strength, and burst strength, while also possessing waterproof and moisture-proof properties, folding resistance, fatigue resistance, and controllable photo-oxidative degradation characteristics, achieving a balance between green environmental protection and high performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-performance polypropylene technology, specifically to a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings. Background Technology

[0002] Polypropylene, a general-purpose thermoplastic resin, is widely used in packaging, automotive, and home appliance industries due to its advantages such as low density, balanced mechanical properties, good chemical resistance, and ease of processing and molding. With the global advocacy for replacing wood and steel with plastics and promoting a green circular economy, the development of high-performance, low-cost, and environmentally friendly modified polypropylene composites has become a research hotspot in the field of polymer materials. Among these efforts, using inorganic powders to modify polypropylene and prepare novel stoneboard-like packaging materials with waterproof, moisture-proof, and durable properties has shown great application potential in the logistics and cold chain packaging market because it can significantly reduce resin usage, improve material rigidity, and impart a certain degree of biodegradability.

[0003] Among numerous inorganic fillers, compared to traditional industrial minerals such as calcium carbonate and talc, utilizing industrial by-product powders with complex chemical compositions and crystal structures, such as siderite tailings and coal gangue, as functional fillers is not only an effective way to reduce the cost of composite materials, but also an important direction for realizing the functionalization and ecologization of high-performance polypropylene composite materials. However, introducing these high-hardness, high-polarity complex inorganic powders into a high proportion of non-polar polypropylene matrices faces severe challenges in interface science and processing rheology.

[0004] First, fillers such as siderite tailings have extremely poor interfacial compatibility with the non-polar polypropylene matrix. High filler content easily leads to agglomeration, causing severe interfacial defects and stress concentration in the composite material under stress. This results in a significant decrease in the burst strength and elongation at break of the finished product, exhibiting significant brittleness. Second, ultrafine, high-filler-content rigid particles cause a sharp increase in the viscosity of the polypropylene melt, narrowing the processing rheological window. This easily leads to process problems such as extruder torque overload, melt fracture, and die wear, severely limiting continuous industrial production. Furthermore, traditional small-molecule chemical coupling agents such as aluminates and titanates, used to improve inorganic / organic interfaces, while improving compatibility to some extent, pose a risk of volatile organic compound (VOC) residues, making it difficult to meet the stringent environmental standards of high-end packaging fields such as food contact packaging.

[0005] Therefore, how to construct a novel, efficient, and green interface modification system to achieve high-proportion uniform dispersion and strong interfacial bonding of complex inorganic functional fillers such as siderite tailings in a polypropylene matrix, while simultaneously solving the processing rheological challenges and the contradiction between rigidity and toughness in highly filled systems, and preparing high-performance polypropylene-based environmentally friendly composite materials, is a key technical problem that urgently needs to be solved in the field of polymer material modification. Based on this, this application proposes a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings. Using multi-source solid waste such as siderite tailings, coal gangue, and phosphogypsum as fillers, a green composite modification system constructed with stearic acid and epoxidized soybean oil is used to replace traditional coupling agents. Combined with grafted compatibilizers and elastomers, the paperboard is produced through a three-layer co-extrusion process involving graded grinding, in-situ activation, intensive mixing and granulation, and gradient cooling. The resulting paperboard, with a solid waste content ≥50%, exhibits excellent processing rheology, high edge crush strength, and burst strength, while also possessing waterproof and moisture-proof properties, folding resistance, fatigue resistance, and controllable photo-oxidative degradation characteristics, achieving a balance between green environmental protection and high performance.

[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings. The preparation method is as follows: the middle core material, the upper layer material and the lower layer material are melted and plasticized separately, co-extruded together by a die head, shaped by a three-roll calender, heated and cooled, corona treated, die-cut, printed and dried to obtain the final product. The intermediate core layer material is high-filled iron tailings masterbatch; Both the upper and lower layers are composed of homopolymer polypropylene and copolymer polypropylene.

[0008] Preferably, the high-filled iron tailings plastic masterbatch is obtained by mixing green modified composite filler and resin matrix premix, followed by extrusion plasticization and air-cooled die surface hot cutting.

[0009] Preferably, the resin matrix premix is ​​obtained by mixing homopolymer polypropylene, copolymer polypropylene, ethylene-octene copolymer and maleic anhydride grafted polypropylene.

[0010] The melt flow rate (MFR) of the homopolymer polypropylene was 2.0-4.0 g / 10 min, determined according to GB / T 3682 at 230℃ and 2.16 kg load; the weight-average molecular weight (Mw) was 3.5 × 10⁻⁶. 5 -4.5×10 5 g / mol; isotacticity ≥ 96.0%. Within this molecular weight and isotacticity range, polypropylene has high molecular chain regularity and strong crystallinity, which can impart extremely high modulus and compressive strength to paperboard, preventing deformation under heavy loads.

[0011] The copolymer polypropylene was selected from ethylene-propylene block copolymers, with an ethylene monomer copolymer content of 7.0 wt% - 15.0 wt%; MFR of 8.0-12.0 g / 10min, determined according to GB / T 3682 at 230℃ and 2.16 kg load; Mw of 2.2 × 10⁻⁶. 5 -2.8×10 5 g / mol. The high MFR ensures the resin's ability to wet highly filled mineral powder; the ethylene segments in the block copolymer structure break the continuous crystalline region, providing impact toughness at low temperatures.

[0012] The ethylene-octene copolymer is a metallocene-catalyzed polyolefin elastomer, wherein the octene (C8) comonomer content is 20.0 wt%-38.0 wt%; and the density is 0.860-0.875 g / cm³. 3 The molecular weight distribution index (MFR) is 0.5-2.0 g / 10 min, determined according to GB / T 3682 at 190℃ and 2.16 kg load; the molecular weight distribution index (MWD) is ≤2.5. High octene content and low density mean the material has more significant rubber elasticity, effectively absorbing energy during cardboard folding or impact; the narrower molecular weight distribution helps form a uniform dispersion structure within the polypropylene matrix.

[0013] Maleic anhydride-grafted polypropylene uses homopolymer polypropylene as the grafting matrix, with a maleic anhydride (MAH) grafting rate of 0.8wt%-1.5wt%; MFR ≥ 40.0 g / 10 min, determined according to GB / T 3682 at 230℃ and 2.16 kg load. The high grafting rate provides ample reactive sites for bonding with the mineral powder; the ultra-high fluidity ensures that the compatibilizer preferentially wets and coats the mineral powder surface before the high-viscosity matrix resin, forming an effective interfacial layer.

[0014] Preferably, the green modified composite filler is obtained by in-situ coating of multi-source composite inorganic mineral powder with lubricant and plasticizer, followed by cooling and discharge. The surface coating is completed by utilizing the reaction between the carboxyl groups of stearic acid and the hydroxyl groups on the surface of the mineral powder, and the capture effect of the epoxy groups of epoxidized soybean oil on the acidic sites of phosphogypsum. The preparation method of the green modified composite filler is as follows: siderite tailings, coal gangue and phosphogypsum are mixed, and after ultrasonic cleaning with water to remove surface soil and soluble salts, the mixture is dried, screened to remove impurities and then sent to a ring roller mill for grinding. The particle size is selected by sieving to obtain multi-source composite inorganic mineral powder. The ultrasonic cleaning power is 1.5kW, the frequency is 28kHz, and the mixture is cleaned for 30min at a solid-liquid ratio of 1:5.

[0015] Preferably, the lubricant is one of stearic acid, oleic acid, oxidized polyethylene wax, and erucamide; the plasticizer is one of epoxidized soybean oil, tributyl acetylacetonate, calcium lignosulfonate, and modified soybean lecithin. Stearic acid is added in a liquefied form, heated to 80℃-90℃ to completely transform it into a transparent liquid fluid with a significantly reduced viscosity. It is then transported through an insulated pipe to the nozzle of a high-speed mixer, where high-pressure air atomizes it into micron-sized droplets, which are sprayed onto the surface of the rapidly tumbling mineral powder at 110℃. The oxidized polyethylene wax has an acid value of 15-20 mgKOH / g.

[0016] The preferred method for preparing modified soybean lecithin is as follows: 1000g of concentrated soybean lecithin is added to a three-necked flask equipped with a stirrer, thermometer, and reflux condenser. The water bath is turned on to raise the temperature to 65°C, and the mixture is stirred at 300 rpm until it is completely melted and fluid. Then, 20g of water is added, and stirring is continued for 20 minutes to allow the phospholipid micelles to fully swell and expose the reaction sites. The acetone-insoluble matter (total phospholipids) of the concentrated soybean lecithin is ≥60%, and the soybean oil content is 38.4%.

[0017] Maintain the temperature at 70℃, adjust the stirring speed to 500 rpm, and slowly add 25g of acetic anhydride to the flask using a constant pressure dropping funnel, controlling the dropping rate and completing the addition within 30 minutes. After the addition is complete, raise the temperature to 80℃ and maintain the temperature for 60 minutes. Acetic anhydride undergoes an acylation reaction with the amino group in the phospholipid molecule to generate N-acetylphosphatidylethanolamine. The acylation reaction passivates the chemical activity of the amino group, thereby inhibiting the thermal browning reaction during processing and significantly improving the heat resistance.

[0018] After the reaction is complete, the temperature is lowered to 60℃, and 20% sodium hydroxide aqueous solution is slowly added dropwise to adjust the pH of the system to 7.0-7.5. Then, 15g of 30% hydrogen peroxide is added, and the mixture is stirred and bleached at 60℃ for 40 minutes. The above is to remove the original dark yellow / brown color of soybean lecithin to prevent it from affecting the whiteness of the final stone cardboard. Vacuum dehydration and drying were carried out for 90 minutes at a vacuum of -0.09 MPa and a temperature of 90°C, and the moisture content of the system was measured by Karl Fischer method until it was less than 0.5%. Heating was stopped, the vacuum was released, and the material was discharged at 50°C to obtain a light yellow paste or viscous liquid acetylated modified soybean lecithin. It is a yellow viscous fluid with an acid value ≤25 mgKOH / g. The heat resistance is good; no obvious carbonization is observed after heating at 210°C for 1 hour, and the color deepening is <2 levels. The HLB value is 8-10, and the hydrophilic-lipophilic balance is moderate, which is suitable for both inorganic mineral powder and polypropylene resin.

[0019] This invention does not simply involve physically mixing various solid wastes. Instead, it constructs a three-dimensional synergistic system based on the mineralogical properties of siderite tailings, coal gangue, and phosphogypsum, achieving a balance between rigidity and toughness, chemical activity, and processing rheology. The structural synergy of the multi-source solid wastes achieves this balance: siderite tailings serve as the main framework, with its high-hardness iron / silicon oxides providing excellent rigidity and photodegradation catalytic activity centers; coal gangue, rich in layered silicates such as kaolinite, acts as a sheet-like reinforcement in the composite material, and the trace amounts of unburned residual carbon provide a self-lubricating effect, effectively improving the material's toughness; the calcium sulfate whiskers in phosphogypsum fill the microscopic voids in the tailings and resin, not only providing flame retardancy and smoke suppression but also adjusting the packing density of the filling system.

[0020] To address the complex surface polarities of the three components mentioned above, this invention abandons the traditional aluminate / titanium esters and designs a two-component system of stearic acid and epoxidized soybean oil. The carboxyl groups of stearic acid preferentially undergo chemical adsorption with metal ions on the surface of siderite tailings and phosphogypsum, forming a hydrophobic monolayer and significantly reducing surface energy. Epoxidized soybean oil utilizes its epoxy groups to act as an acid scavenger to neutralize trace acidic substances remaining in phosphogypsum and prevent polypropylene resin degradation. Furthermore, it acts as a plasticizer, penetrating the interlayer structure of coal gangue and the resin molecular chains, significantly reducing the melt viscosity of the highly filled system.

[0021] The aforementioned synergistic effect keeps the melt flow rate of the high-filled masterbatch within a suitable processing range. Combined with the chemical bridging effect of PP-g-MAH and the gradient cooling process, the internal stress between heterogeneous materials is eliminated, ultimately achieving excellent performance with high burst strength, high flexural strength and controllable degradation at high doping levels.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. By introducing bio-based epoxidized soybean oil and stearic acid to construct a green composite modification system, combined with a high-flowability copolymer polypropylene matrix, the problems of easy agglomeration of multi-source solid waste and excessively high melt viscosity under high filler content are effectively solved. This modification system utilizes the steric hindrance and internal lubrication effect of long-chain molecules to significantly reduce the interfacial frictional resistance between inorganic powder and resin, greatly improve the processing rheological properties of composite materials, ensure smooth melt flow during high-speed extrusion granulation and sheet forming, avoid mold blockage, and improve production efficiency.

[0023] 2. By employing maleic anhydride grafts as a chemical bridge, combined with multi-stage particle size distribution and gradient cooling and shaping processes, the technical bottlenecks of weak interfacial bonding and high internal stress in stoneboard were overcome. A robust interfacial layer was established between the inorganic filler and the organic matrix through chemical bonding, effectively transferring stress. Simultaneously, the dense packing of particles of varying sizes and slow heat release eliminated microscopic defects and residual stress, achieving an excellent balance between high edge crush strength and high burst strength in the finished paperboard. This significantly improved the structural load-bearing capacity and impact resistance of the packaging material.

[0024] 3. Utilizing the natural photocatalytic properties of transition metal elements in siderite tailings, synergistically with the photoinitiation effect of bio-based additives, and supplemented with an elastomer toughening formula, the material is endowed with excellent weather resistance and controllable degradation capabilities. The hydrophobic modified layer effectively blocks moisture penetration, and combined with the flexible network of the toughening phase, significantly improves the cardboard's waterproof, moisture-proof, and folding fatigue resistance. Furthermore, after disposal, it can decompose and break through photo-oxidation reactions, achieving an ecological closed loop for logistics packaging, from long-term durability to green degradation. Attached Figure Description

[0025] Figure 1 The graph shows the edge crush strength and bursting strength test results of Examples 1-3, Example 11, Comparative Examples 1-4 and Comparative Example 7 of the present invention. Detailed Implementation

[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] Please see Figure 1 This invention provides a method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings, the technical solution of which is as follows: Example 1: Both siderite tailings and coal gangue were collected from the Daxigou tailings pond. The siderite tailings contained 35.0%-55.0% silica, 12.0%-25.0% total iron (Fe2O3), 10.0%-20.0% calcium oxide and magnesium oxide, ≤8.0% aluminum oxide, and 15.0%-28.0% loss on ignition. The siderite tailings, coal gangue, and phosphogypsum were mixed in a mass ratio of 6:2:2. After ultrasonic cleaning with water to remove surface soil and soluble salts, the mixture was dried at 105°C until the moisture content was below 0.5%. After screening to remove impurities, the mixture was sent to a ring roller mill for grinding. The mill pressure was adjusted to 12MPa and the classifier speed was adjusted. The mineral powder with a particle size distribution D97 of 1000 mesh was selected by screening, which is a multi-source composite inorganic mineral powder.

[0028] 100 parts of multi-source composite inorganic mineral powder were added to a high-speed mixer with a heating jacket and stirred and dried at 1500 rpm at 110°C for 15 minutes to remove microporous moisture using frictional heat and external heating. Then, 1.5 parts of liquefied stearic acid and 2.5 parts of epoxidized soybean oil were sprayed into the high-speed rotating mineral powder. The mixture was kept at 110°C and the speed was adjusted to 2000 rpm for 10 minutes of continuous stirring. After cooling to 45°C, the mixture was discharged to obtain the green modified composite filler.

[0029] 35 parts of homopolymer polypropylene with a melt index of 3.0 g / 10 min, 10 parts of copolymer polypropylene with a melt index of 10.0 g / 10 min, 4 parts of ethylene-octene copolymer, and 2.5 parts of maleic anhydride grafted polypropylene (PP-g-MAH) were added to a low-speed mixer and premixed at 300 rpm for 5 min at 25°C to obtain a resin matrix premix. 60 parts of green modified composite filler and 45 parts of the resin matrix premix were fed into a twin-screw extruder with an L / D ratio of 48:1. The feeding section temperature was set to 175°C, the plasticizing and dispersing section temperature to 205°C, and the die head temperature to 190°C. The mixture was degassed and vented under a vacuum of -0.08 MPa, and then hot-cut by an air-cooled die. The granulation speed was controlled at 0.8 tons / h to obtain a high-filled iron tailings plastic masterbatch.

[0030] Stone paperboard is prepared using a three-layer co-extrusion casting process. The middle core layer consists of 100% high-filled iron tailings masterbatch, while the upper and lower surface layers consist of a mixture of 80% homopolymer polypropylene and 20% copolymer polypropylene, forming an A / B / A structure. The core layer material is extruded at an extrusion pressure of 15 MPa and a melting temperature of 200°C, while the surface layer material is extruded at 190°C. After co-extrusion through a T-die, the materials are shaped using a three-roll calender. The temperatures of the three rolls are set sequentially: upper roll 80°C, middle roll 60°C, and lower roll 40°C, utilizing gradient cooling to eliminate internal stress. Subsequently, the board is introduced into a heating and leveling chamber via a six-roll traction device and undergoes thermal relaxation and leveling at 100°C to eliminate waviness. After leveling, it is naturally cooled to room temperature. The board is then pulled at a speed of 0.6 tons / h, and the surface is subjected to high-frequency corona treatment to achieve a surface tension of 38 dyne / cm. After longitudinal edge trimming and transverse length cutting, a smooth semi-finished stone paperboard is obtained.

[0031] The semi-finished stone cardboard is fed into a flat roller die-cutting machine for die-cutting. The die-cutting blade is installed according to the box design requirements. The gauge pressure of the die-cutting hydraulic system is set to 18MPa and the die-cutting speed is 25 times / min. Folding lines with a depth of 50% of the cardboard thickness are pressed on the surface of the cardboard, and excess edge waste is removed. The die-cut cardboard is then pushed out, ensuring that the cut edges are free of burrs and the crease lines are clear and unbroken.

[0032] The fixed mold cardboard is positioned and transferred to a high-definition color screen printing machine. Water-based environmentally friendly ink is used for printing. The printing squeegee angle is set to 75 degrees and the printing speed is 1200 sheets / h. After printing, it is treated in a 60℃ UV curing drying channel for 30 seconds to allow the ink to instantly cure and adhere, resulting in a beautifully printed cardboard with a color fastness of level 4.

[0033] The printed cardboard is automatically folded along the mold line and fed into an ultrasonic welding and binding machine. The ultrasonic frequency is set to 20kHz and the welding time is 0.8 seconds. This replaces the traditional metal nails or glue. The high-frequency vibration causes the polypropylene matrix at the cardboard overlap to melt and interlock instantly, completing the environmentally friendly hot melt binding and obtaining the finished stone-plastic box.

[0034] The prepared high-iron tailings environmentally friendly stone cardboard (stone-plastic box) has the following parameters: thickness 3.0 mm; density 1.28 g / cm³; edge crush strength = 4.21 kN / m; burst strength = 680 kPa; total content of siderite tailings and solid waste = 57.1%; natural light oxygen degradation cycle 7.2 months; folding resistance = 5235 times; 24-hour water absorption rate = 0.12%; VOC emission < 5 mg / kg; peel strength at binding ≥ 120 N / 5 cm.

[0035] The preparation methods of the iron tailings-filled polypropylene-based environmentally friendly stone paperboard prepared in Examples 2-6 are different from those in Example 1. The specific parameters are summarized in Table 1.

[0036] Table 1 Key Process Parameters for Iron Tailings Filled Polypropylene-Based Environmentally Friendly Stone Paperboard Example 7: The basic formulation is the same as in Example 1, except that the modifier is adjusted to 1.5 parts oleic acid and 2.5 parts tributyl acetylic acid.

[0037] Example 8: The basic formulation is the same as in Example 1, except that the modifier is adjusted to 1.5 parts of oxidized polyethylene wax and 2.5 parts of calcium lignosulfonate.

[0038] Example 9: The basic formulation is the same as in Example 1, except that the modifier is adjusted to 1.5 parts modified soybean lecithin and 1.0 part erucamide. Note: The total amount is kept balanced and finely adjusted.

[0039] Example 10: The basic formula is the same as in Example 1, with the mixing mass ratio of siderite tailings, coal gangue and phosphogypsum being 6.2:2.3:1.5.

[0040] Example 11: The basic formula is the same as in Example 1, with the mixing mass ratio of siderite tailings, coal gangue and phosphogypsum being 5.8:1.7:2.5.

[0041] Based on Example 1, the following five comparative examples were set up. Except for the differences below, the other steps and parameters are completely consistent with Example 1. Each comparative example specifically changes the key influencing factors to demonstrate the synergistic effect and necessity of each component and process in the technical solution of this application.

[0042] Comparative Example 1: In the powder processing step, no stearic acid and epoxidized soybean oil were added; only physical heating and mixing were performed.

[0043] Comparative Example 2: In the resin matrix premix of the internal mixing and granulation step, PP-g-MAH was removed, and its mass fraction was made up by homopolymer polypropylene.

[0044] Comparative Example 3: In the powder processing step, the grinding particle size D97 was adjusted to 400 mesh (coarse powder).

[0045] Comparative Example 4: In the molding process, the gradient temperature setting was canceled, and the three-roll forming temperature was uniformly set to 25℃ to simulate rapid cooling with cooling water.

[0046] Comparative Example 5: In the resin matrix formulation, the copolymer polypropylene and ethylene-octene copolymer toughening agents were removed and replaced entirely with homopolymer polypropylene with a melt index of 3.0 g / 10 min.

[0047] Comparative Example 6: The basic formula is the same as in Example 1, except that a single type of siderite tailings is added.

[0048] Comparative Example 7: The basic formula is the same as in Example 1, except that coal gangue is removed and phosphogypsum is added to make up the difference. The ratio of iron tailings to phosphogypsum is 3:2. Comparative Example 8 uses the same basic formula as Example 1, except that phosphogypsum is removed and siderite tailings are added to make up the difference, with a ratio of iron tailings to coal gangue of 4:1.

[0049] Test Example 1 The granulation masterbatches prepared in Examples 1-11, Comparative Examples 1, and Comparative Examples 5-8 were subjected to melt flow rate tests in accordance with the national standard GB / T 3682.1-2018. The masterbatch sample to be tested was dried in an 80℃ forced-air drying oven for 4 hours to remove surface moisture. A melt flow rate meter was used, with the test temperature set to 230℃ and the nominal load to 2.16 kg. After the temperature stabilized, the sample was added to the barrel, compacted and preheated for 4 minutes. The sample strip was automatically cut, and the extrusion mass (g / 10min) within 10 minutes was calculated. The final test results are summarized in Table 2.

[0050] Table 2. Test results of melt flow rate of masterbatch in Examples 1-11 and comparative examples As shown in Table 2, the melt flow rate data of Examples 1-11 all demonstrate significant advantages over Comparative Examples 1 and 5 in terms of processing fluidity of high-dosage solid waste filling systems, and all are within the range suitable for processing.

[0051] Comparative Example 1, due to the removal of the green modification system composed of stearic acid and epoxidized soybean oil during powder processing, had the lowest MFR value among all groups, almost losing its fluidity. This is because inorganic mineral powders such as siderite tailings and coal gangue have extremely high surface energy and polarity. Without organic coating, the mineral powder particles easily agglomerate, and the interfacial friction with the non-polar polypropylene matrix is ​​extremely high. Lacking the internal lubrication of epoxidized soybean oil and the surface passivation effect of stearic acid, the melt generates huge viscous resistance during extrusion, making processing extremely difficult. Comparative Example 5, although retaining the filler modification treatment, replaced all the matrix resin with homopolymer polypropylene with a low fluidity (MFR 3.0), removing the high fluidity copolymer polypropylene. The test results showed that its MFR dropped to 1.8 g / 10 min, indicating that in a high-filler system, the basic fluidity of the matrix resin plays a decisive supporting role in the rheological properties of the final masterbatch. High-rigidity homopolymer polypropylene alone cannot effectively support the high filler content of 57%, resulting in a dry system and a lack of sufficient carrier resin to wet and drive the flow of mineral powder. Comparative Example 6, containing only iron tailings, has high particle hardness and lacks lubrication from residual coal gangue and filling with phosphogypsum, leading to high friction and a significant decrease in MFR. Comparative Example 7, lacking coal gangue, shows a slight decrease in fluidity. Comparative Example 8, lacking phosphogypsum, has a weakened anchoring-plasticizing effect of epoxidized soybean oil on acidic sites, resulting in slightly poorer dispersibility.

[0052] Internal comparisons within the example groups showed that Example 3, due to its lower filler content and relatively coarser particle size, had the smallest specific surface area of ​​mineral powder, resulting in the weakest adsorption and hindrance effect on the resin, thus exhibiting the highest MFR and best flowability. Example 4, although increasing the amount of lubricant, used 1500-mesh ultrafine powder, leading to a sharp increase in specific surface area and increased resin coating of filler, resulting in increased internal melt friction and a relatively lower MFR. Example 2, despite its high filler content, maintained excellent flowability of 3.7 g / 10 min by increasing the amount of epoxidized soybean oil and using a high melt index copolymer polypropylene. Example 7 showed a significantly increased MFR. ATBC, a highly efficient plasticizer, can penetrate between polypropylene molecular chains to increase free volume, and the unsaturated double bonds in oleic acid molecules create significant steric hindrance, greatly reducing the friction coefficient between molecular chains and resulting in excellent melt flowability.

[0053] In summary, the green modification system is primarily responsible for reducing the interfacial energy between inorganic powders and resins and providing intermolecular lubrication, which is the core key to solving the problem of high-filler flowability. The compounding strategy of the matrix resin is mainly responsible for providing a rheological carrier and adjusting the basic viscosity of the system. Both are indispensable in the formulation, and the lubricant ratio needs to be dynamically adjusted according to the particle size (specific surface area) and filler content. A single resin selection or the absence of surface modification cannot meet the rheological requirements of high-volume environmentally friendly stoneboard for high-speed extrusion and sheet-forming processes.

[0054] Test Example 2 Density, edge crush strength, and bursting strength were tested on the iron tailings-filled polypropylene-based environmentally friendly stone paperboard prepared in the examples and comparative examples.

[0055] Density was tested according to the impregnation method in GB / T 1033.1-2008. Standard samples were cut, and their mass in air and in the impregnation solution ethanol were measured at 23℃. The apparent density (g / cm³) of the material was calculated. This index directly reflects the filling density and lightweight level under high doping levels. Edge crush strength is tested according to GB / T 6546-2021; a rectangular specimen is placed between the two pressure plates of a compression tester, with the corrugated direction perpendicular to the pressure plates, and pressure is applied at a speed of 12.5 mm / min until the specimen crushes. The maximum compressive force is recorded, and the unit is kN / m. This index is a core parameter for measuring the stacking load-bearing capacity of packaging boxes. Bursting strength was determined according to GB / T 1539-2007. A Mullen-type hydraulic bursting strength tester was used. The sample was clamped between upper and lower jaws, and a uniformly increasing hydraulic pressure was applied to the sample through a diaphragm until the sample broke. The maximum pressure value was recorded, and the unit was kPa. This index reflects the toughness of the material against localized impacts and fractures during transportation. The test results are summarized in Table 3 and... Figure 1 middle.

[0056] Table 3 Summary of test results of physical and mechanical properties of finished paperboards from Examples 1-11 and comparative examples According to the density, edge crush strength and bursting strength data shown in Table 3, Examples 1-11 show significant advantages over Comparative Examples 1-8 in terms of overall mechanical properties and structural stability of environmentally friendly stone paperboard made from siderite tailings.

[0057] Comparative Example 2, due to the removal of PP-g-MAH from the matrix formulation, exhibited significantly lower edge crush strength and burst strength compared to Example 1. This indicates that physical coating with stearic acid and epoxidized soybean oil alone can only solve the dispersion problem and cannot provide high-strength interfacial transfer. Lacking the chemical anchoring provided by PP-g-MAH, the inorganic mineral powder and organic matrix rapidly debonded under stress, creating interfacial voids and leading to structural failure of the material even at relatively low stress. Comparative Example 3 used 400-mesh coarse-grained, ungraded mineral powder, resulting in significantly lower burst strength than the Example group. The large mineral powder particles became huge stress concentration points in the thin-walled plate, easily triggering crack propagation under external impact. Furthermore, the single particle size could not form a dense packing, resulting in numerous internal voids and low mechanical transfer efficiency. Comparative Example 4 eliminated the gradient cooling step in the molding process and adopted rapid cooling for shaping. Although the density was the same as in Example 1, the burst strength dropped significantly to 489 kPa. This is mainly because polypropylene is a crystalline polymer, and the thermal conductivity of the high-filler system differs from that of pure resin. Rapid cooling leads to inconsistent shrinkage rates between the core layer and the surface layer of the board, resulting in the accumulation of huge residual thermal stress inside. These internal stresses are released when subjected to external impact, and when superimposed on the external force, the board exhibits a brittle pre-damaged state. Comparative Example 5 used a single homopolymer polypropylene as the matrix, and its edge crush strength was even higher than some examples, but its burst strength was extremely poor, exhibiting typical high rigidity and low toughness characteristics. Homopolymer polypropylene has high molecular chain regularity and strong rigidity, which is beneficial for resisting static compression (edge ​​crush), but it lacks the flexible amorphous regions provided by copolymer polypropylene and ethylene-octene copolymer to absorb impact energy. For logistics packaging boxes, having only high edge crush strength but no high burst strength means that the box is very easy to break during drops or collisions, which cannot meet the actual use requirements. Comparative Example 1 performed the worst in mechanical testing, confirming that the lack of surface modification leads to complete separation of the matrix and filler, and the material essentially becomes a loose sand pile, unable to bear any effective load.

[0058] In Comparative Example 6, the main component of siderite tailings is high-hardness iron / silicon oxide. While this provides the cardboard with a very high rigidity skeleton, it lacks flexible components for cushioning. Without the layered toughening provided by coal gangue and the filling of phosphogypsum powder, the single high-hardness particles form severe stress concentration points under stress, resulting in extreme brittleness and an inability to withstand dynamic folding and localized bursting forces. Furthermore, the high density of pure tailings leads to a finished product density of 1.38 g / cm³, which is detrimental to lightweighting. Comparative Examples 7 and 8 show a decline in the performance of the stone slabs due to the absence of coal gangue and phosphogypsum. Only when siderite tailings, coal gangue, and phosphogypsum work synergistically in a specific ratio can a balance between rigidity and toughness be achieved.

[0059] In summary, green chemical modification provides a solid foundation for interfacial bonding, the optimized particle size distribution of multi-source solid waste improves stress distribution, the rigidity-toughness balance design of the matrix resin endows the material with comprehensive mechanical properties, and the gradient cooling process ensures the stability of the material's microstructure. The results show that these four dimensions of technological improvement are indispensable in the preparation of siderite tailings stone paperboard; the absence of any single factor will lead to the collapse of key performance indicators, failing to meet the needs of industrial packaging.

[0060] Test Example 3 The iron tailings-filled polypropylene-based environmentally friendly stone paperboard prepared in the examples and comparative examples was tested for folding tolerance, 24-hour water absorption, and elongation at break. The specific test methods are as follows: The folding endurance test is based on GB / T 2679.5-2002. Since stoneboard combines the properties of paper and plastic, this standard is commonly used in the industry to evaluate folding endurance. The cut sample is fixed between the upper and lower jaws of the MIT folding endurance tester, a tension of 9.8 N is applied, and the sample is folded 135° repeatedly at a frequency of 175 times / min until it breaks. The number of folds is recorded (double folds count as one). This indicator simulates the scenario of repeated opening and closing of a carton lid.

[0061] The 24-hour water absorption rate is determined according to GB / T 1034-2008. The dried sample is completely immersed in distilled water at 23°C for 24 hours. After removing the sample and wiping off the surface moisture, it is weighed immediately and the percentage increase in mass is calculated. This index mainly examines the stability and waterproof performance of the material in a humid environment.

[0062] The elongation at break was determined according to GB / T 1040.2-2006. A universal testing machine was used to tensile dumbbell-shaped specimens at a tensile speed of 50 mm / min. The ratio of the increase in the distance between gauge marks at fracture to the initial gauge length was recorded. This index reflects the ductility and flexibility of the material. The test results are shown in Table 4.

[0063] Table 4 Summary of test results for the toughness and weather resistance of finished paperboards from Examples 1-11 and comparative examples According to the folding tolerance, 24-hour water absorption rate, and elongation at break data shown in Table 4, Examples 1-11 showed significant advantages over Comparative Examples 1-8 in terms of flexibility, water resistance, and ductility of the iron tailings environmentally friendly stone cardboard. Example 7 showed the best toughness. The synergistic plasticizing effect of acid and ATBC greatly increased the chain segment mobility of the amorphous region of polypropylene, making the molecular chains less prone to breakage when the material is repeatedly folded and stretched, exhibiting excellent fatigue resistance and ductility.

[0064] Comparative Example 1, lacking any green modification system composed of stearic acid and epoxidized soybean oil during the powder processing stage, exhibited a high 24-hour water absorption rate, significantly inferior to other groups, and a folding tolerance of only 125 cycles. This is because inorganic mineral powders such as siderite tailings and coal gangue are inherently hydrophilic, and the uncoated powder surfaces are directly exposed, forming numerous water adsorption sites and seepage channels. Simultaneously, the lack of lubrication and dispersing effects from the modifier led to severe filler agglomeration. These agglomerates became significant defects during stretching and folding, resulting in instantaneous brittle fracture. Comparative Example 2, by removing the PP-g-MAH compatibilizer from its formulation, although the water absorption rate was controlled at 0.25% due to the physical coverage of stearic acid, showed a significant decrease in folding tolerance and elongation at break. This indicates that physical lubrication alone cannot resist dynamic fatigue; under the stress of repeated folding, the weak interfacial bonds rapidly failed, triggering microcrack propagation along the interface. Comparative Example 3 used coarse mineral powder with a 400-mesh single-peak distribution, resulting in a water absorption rate of 0.48% and a low elongation at break. This is because the coarse particles could not achieve close packing, and the large gaps between the particles created a capillary effect, accelerating water penetration. Simultaneously, the large particles acted as stress concentration points, severely hindering the axial stretching of the polymer molecular chains. Comparative Example 4 used a rapid cooling and shaping process, and its water absorption rate was the same as the example group, indicating that the chemical hydrophobicity was not affected. However, the folding tolerance and elongation at break were significantly impaired. The residual internal stress caused by rapid cooling was equivalent to applying a preload to the material. This internal stress accelerated the fatigue failure process under the action of external folding forces, making the material exhibit hard and brittle characteristics. Comparative Example 5 used a single homopolymer polypropylene as the matrix, with an elongation at break of only 15.5% and a folding tolerance of 550 cycles. In the absence of flexible amorphous regions provided by copolymer polypropylene and ethylene-octene copolymer, the highly crystalline homopolymer polypropylene could not effectively dissipate deformation energy, leading to brittle fracture of the highly filled system under low strain. The results of Comparative Examples 6-8 show that the absence of one of the following—siderite tailings, coal gangue, and phosphogypsum—results in a deterioration in overall toughness and weather resistance.

[0065] In summary, the hydrophobic long chains in the green modification system are primarily responsible for imparting excellent waterproof and moisture-proof properties to the material and assisting in dispersion, preventing the formation of agglomeration defects. The toughening formulation and compatibilizer of the matrix resin are mainly responsible for providing the flexibility of the continuous phase and the interfacial transfer capability, determining the material's elongation limit. The gradient cooling process, by eliminating internal stress, ensures the long-term stability of the material structure. The results show that surface modification, interfacial reinforcement, matrix toughening, and stress relief are all indispensable in the preparation of stoneboard; only through synergistic effects can high toughness and high weather resistance be achieved while ensuring high filler content.

[0066] Test Example 4 The iron tailings-filled polypropylene-based environmentally friendly stone paperboard prepared in the examples and comparative examples were subjected to natural photo-oxidative degradation performance tests. The natural photo-oxidative degradation cycle test was conducted according to GB / T 20197-2006 and GB / T 16422.2-2014, using an accelerated aging extrapolation method. The paperboard was cut into dumbbell-shaped standard samples, and the aging conditions were as follows: placed in a xenon lamp aging test chamber, with a blackboard temperature of 63℃ and an irradiance of 0.51 W / (m²·nm)@340nm, simulating outdoor sunlight exposure; samples were taken every 100 hours to test the elongation at break. When the elongation at break retention rate of the sample decreased to 50%, the accelerated aging time was recorded; based on the average daily sunshine in Xi'an, the accelerated aging time was converted into a degradation cycle (months) under natural conditions. The test results are shown in Table 5.

[0067] Note: This test uses an industry-standard empirical formula. Accelerated aging for 100 hours is roughly equivalent to one month of exposure to strong natural light.

[0068] Table 5 Summary of test results for the natural light-induced oxidation degradation performance of finished paperboards from Examples 1-11 and the comparative examples According to the natural light-induced degradation cycle data shown in Table 5, Examples 1-11 show significant advantages in terms of environmentally friendly and controllable degradation performance compared to Comparative Examples 1, 3 and 5, achieving an ideal degradation cycle of 6-9 months, which meets both the service life of logistics packaging and the requirements for rapid environmental degradation.

[0069] Comparative Example 1, which did not add epoxidized soybean oil during preparation, had a natural photo-oxidation degradation period of 11.5 months, significantly slower than the Example group. This is because epoxidized soybean oil, as a bio-based unsaturated fatty acid ester, has double bonds and epoxy groups in its molecular chain that are sensitive to photothermal activity and easily generate free radicals under light, acting as photoinitiators. The absence of epoxidized soybean oil resulted in a lack of active centers to induce polymer chain breakage, and the unmodified mineral powder could not effectively exert its catalytic effect. Comparative Example 3 used 400-mesh coarse-grained mineral powder, extending the degradation period to 9.2 months. Iron in siderite tailings is a natural photodegradation catalyst, but the small specific surface area of ​​the coarse powder greatly reduces the contact area and catalytic active sites between the iron and the polypropylene matrix, leading to a decrease in the efficiency of the photo-oxidation reaction. Comparative Example 5 used a single highly crystalline homopolymer polypropylene as the matrix, with a degradation period of 10.3 months. Homopolymer polypropylene molecules are tightly packed, making it difficult for oxygen to diffuse into the crystalline region. Furthermore, it lacks the amorphous regions provided by the comonomers to act as entry points for the oxidation reaction, thus delaying the oxidative fracture process of the matrix resin. Comparative Example 6, with its excessively high iron content (entirely tailings), exhibited excessively strong photocatalytic performance and a too-rapid degradation rate, leading to unstable performance during storage.

[0070] In summary, the transition metal elements in siderite tailings primarily provide active centers for photocatalytic degradation, serving as the intrinsic driving force for the material's self-degradation. The green modifier, epoxidized soybean oil, mainly provides easily oxidized initiation sites, accelerating the generation and transport of free radicals. Furthermore, the ultrafine powder processing and the compounding with the matrix resin further enhance oxygen diffusion and contact efficiency. The results indicate that the catalytic effect of siderite tailings and the initiating effect of bio-based additives are both indispensable in the degradation mechanism of environmentally friendly stone cardboard. Their synergistic effect enables a qualitative change in the material from recalcitrant to controllable degradation; the absence of any single component will result in the product failing to meet environmental protection standards.

[0071] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings, characterized in that, The preparation method is as follows: the middle core material, the upper layer material and the lower layer material are melted and plasticized separately, co-extruded together through a die head, shaped by a three-roll calender, heated and cooled, corona treated, die-cut, printed and dried to obtain the final product; The intermediate core material is a high-filled iron tailings plastic masterbatch; the high-filled iron tailings plastic masterbatch is obtained by mixing green modified composite filler and resin matrix premix, followed by extrusion plasticization and air-cooled die surface hot cutting. The green modified composite filler is obtained by in-situ coating of multi-source composite inorganic mineral powder with lubricant and plasticizer, followed by cooling and discharge. Both the upper and lower materials are composed of homopolymer polypropylene and copolymer polypropylene; The preparation method of the multi-source composite inorganic mineral powder is as follows: siderite tailings, coal gangue and phosphogypsum are mixed, and after ultrasonic cleaning with water to remove surface soil and water-soluble impurities, the mixture is dried, screened to remove impurities, and then sent to a ring roller mill for grinding. The multi-source composite inorganic mineral powder is obtained by screening. The mixing mass ratio of the siderite tailings, the coal gangue, and the phosphogypsum is 2.8-6.2:1.7-2.3:1.5-2.5; the mixing ratio of the green modified composite filler and the resin matrix premix is ​​55-65:40-50.

2. The method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings according to claim 1, characterized in that, The resin matrix premix is ​​obtained by mixing homopolymer polypropylene, copolymer polypropylene, ethylene-octene copolymer and maleic anhydride grafted polypropylene.

3. The method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings according to claim 1, characterized in that, The lubricant is one of stearic acid, oleic acid, oxidized polyethylene wax, and erucamide; the plasticizer is one of epoxidized soybean oil, tributyl acetylacetonate, calcium lignosulfonate, and modified soybean lecithin.

4. The method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings according to claim 3, characterized in that, Modified soybean lecithin is obtained by melting and hydration pretreatment of soybean lecithin, acetylation reaction, neutralization and oxidative bleaching, and vacuum dehydration and discharge.

5. The method for preparing polypropylene-based environmentally friendly stone paperboard filled with iron tailings according to claim 4, characterized in that, The acetylation reaction is carried out by adding acetic anhydride dropwise into the product of the hydration pretreatment and reacting at a constant temperature; the neutralization is carried out by adding sodium hydroxide solution to adjust the pH to neutral; the oxidative bleaching is carried out by adding hydrogen peroxide solution and stirring.

Citation Information

Patent Citations

  • Polypropylene-based film with improved mechanical and sealing properties and method of making same

    CN104379100A

  • Reinforced thermoplastic polymer resin composite material and preparation method thereof

    CN113045839A

  • A wood plastic composite

    WO2020036591A1