A heat-insulating and energy-saving environmentally friendly exterior wall coating

By modifying acrylic acid and adding additives to form a chemical cross-linking network, the adhesion and hardness of the exterior wall coating are improved, solving the problems of weather resistance and stain resistance while maintaining the heat insulation effect.

CN122405091BActive Publication Date: 2026-11-17XINJIANG DINGHENG CONSTR ENG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610769312.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2026-05-21
Filing Date
2026-05-31
Publication Date
2026-11-17
Estimated Expiration
2046-05-31

AI Technical Summary

Technical Problem

Currently, exterior wall coatings have poor weather resistance and are prone to stain adhesion, leading to reduced heat insulation performance.

Method used

Modified acrylic acid, modified additives, modified glass microspheres, rutile titanium dioxide, leveling agent, defoamer and dispersant are used to improve the adhesion and hardness of the coating through a chemical cross-linking network. The fluorinated polysiloxane structure on the modified additive reduces surface energy and prevents dust accumulation.

Benefits of technology

It improves the coating's impact resistance and stain resistance, and the dense cross-linked structure resists the erosion of moisture, ultraviolet rays and pollutants, while maintaining its heat insulation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a heat-insulating and energy-saving environmentally friendly exterior wall coating, comprising the following raw materials by weight: 100-120 parts modified acrylic acid, 10-20 parts modified additives, 20-30 parts modified glass microspheres, 15-25 parts rutile titanium dioxide, 0.2-0.8 parts leveling agent, 0.3-0.6 parts defoamer, 0.5-1 parts dispersant, and 40-50 parts water. During the mixing and coating process, the amino groups on the modified additives can react with the epoxy groups on the modified acrylic acid and the epoxy groups on the modified glass microspheres to form a chemical cross-linking network. The dense cross-linking structure can effectively resist the erosion of moisture, ultraviolet rays, and pollutants, and slow down chalking, discoloration, and peeling. The fluorinated polysiloxane structure on the modified additives, with fluorinated segments, will accumulate on the coating surface, significantly reducing surface energy and fundamentally solving the problem of easy dust accumulation in heat-insulating coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat-insulating coating preparation technology, specifically to a heat-insulating and energy-saving environmentally friendly exterior wall coating. Background Technology

[0002] Building energy consumption accounts for a significant proportion of global energy consumption, and heat loss through building envelopes is one of the key factors contributing to persistently high energy consumption. As the outermost protective and decorative layer of a building, exterior wall coatings have evolved from simple protection and aesthetics to proactive energy conservation and environmental friendliness. Developing exterior wall coatings with excellent thermal insulation properties is of great significance for reducing building heating and cooling energy consumption and promoting the achievement of "dual-carbon" goals in the building sector. Currently, most mainstream exterior wall insulation coatings on the market use polyacrylate resins as the main film-forming material. Traditional acrylic emulsions rely on physical drying to form a film; polymer particles deform and fuse to form a coating after moisture evaporates, lacking chemical cross-linking between molecular chains. This purely physical film-forming method results in low coating cohesive strength, poor hydrophobicity, and easy adhesion of dust from the air. Once the surface becomes dirty, the reflectivity drops sharply, affecting the thermal insulation effect. Summary of the Invention

[0003] The purpose of this invention is to provide a heat-insulating and energy-saving environmentally friendly exterior wall coating, which solves the problems of poor weather resistance and easy adhesion of stains to the current exterior wall coatings, which leads to a reduction in heat insulation effect.

[0004] The objective of this invention can be achieved through the following technical solutions: A heat-insulating and energy-saving environmentally friendly exterior wall coating is made by the following steps: Step A1: Mix acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and toluene, and react for 6-8 hours at a speed of 150-200 r / min and a temperature of 70-80℃ to obtain modified polyacrylic acid. Step A2: Place hollow glass microspheres in sodium hydroxide solution and stir for 3-5 hours at a speed of 200-300 r / min and a temperature of 60-65℃. Filter to remove the filtrate to obtain pretreated glass microspheres. Mix ethanol, deionized water, and 3-glycidoxypropyltrimethoxysilane and stir at a speed of 150-200 r / min, a temperature of 60-65℃, and a pH of 4-4.5. Add the pretreated glass microspheres and react for 3-5 hours to obtain modified glass microspheres. Step A3: Weigh the following raw materials by weight: 100-120 parts modified acrylic acid, 10-20 parts modified additives, 20-30 parts modified glass microspheres, 15-25 parts rutile titanium dioxide, 0.2-0.8 parts leveling agent, 0.3-0.6 parts defoamer, 0.5-1 parts dispersant, and 40-50 parts water. Mix the raw materials evenly to obtain a heat-insulating and energy-saving environmentally friendly exterior wall coating.

[0005] Furthermore, the mass ratio of acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, and azobisisobutyronitrile in step A1 is 5:60:30:5:1.

[0006] Furthermore, the concentration of the sodium hydroxide solution in step A2 is 0.3 mol / L, and the mass ratio of ethanol, deionized water, 3-glycidoxypropyltrimethoxysilane, and pretreated glass microspheres is 300:10:2:100.

[0007] Furthermore, the modified additive is prepared by the following steps: Step B1: Dissolve lithium trimethylsilanolate in tetrahydrofuran, purge with nitrogen, and stir at 200-300 r / min and 0°C while adding trifluoropropylmethylcyclotrisiloxane. Heat to 20-25°C and react for 6-8 hours. Then add methyldichlorosilane and continue the reaction for 3-5 hours to obtain the modifier. Mix castor oil, the modifier, the cassiterite catalyst, and toluene evenly, purge with nitrogen, and react at 150-200 r / min and 80-85°C for 6-8 hours to obtain modified castor oil. Step B2: Mix octamethylcyclotetrasiloxane, tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide, and purge with nitrogen. React at 150-200 r / min and 90-95℃ for 10-12 h, then raise the temperature to 105-110℃ and continue the reaction for 2-3 h to obtain dihydropolysiloxane. Mix dihydropolysiloxane, acrylic acid, caster catalyst and toluene evenly, purge with nitrogen, and react at 150-200 r / min and 80-85℃ for 6-8 h to obtain carboxylated polysiloxane. Step B3: Mix carboxylated polysiloxane, modified castor oil, p-toluenesulfonic acid, and xylene, and react them for 10-15 hours at a speed of 120-150 r / min and a temperature of 100-110℃ to obtain hyperbranched polysiloxane. Mix hyperbranched polysiloxane, ethylenediamine, dicyclohexylcarbodiimide, and xylene, and react them for 3-5 hours at a speed of 120-150 r / min and a temperature of 20-25℃ to obtain modified additive.

[0008] Furthermore, in step B1, the molar ratio of Si-Cl bonds on lithium trimethylsilanolate, trifluoropropylmethylcyclotrisiloxane, and methyldichlorosilane is 1:5:1, the molar ratio of castor oil to modifier is 1:3, and the amount of castor catalyst is 0.01% of the mass of modifier.

[0009] Furthermore, in step B2, the molar ratio of octamethylcyclotetrasiloxane, tetramethyldisiloxane, and tetramethylammonium hydroxide is 1.2:1:1.5, the molar ratio of dihydropolysiloxane and acrylic acid is 1:2, and the amount of caster catalyst is 0.01% of the mass of acrylic acid.

[0010] Furthermore, in step B3, the ratio of carboxylated polysiloxane to modified castor oil is 2n+1:n, where n is a natural number greater than 0. The amount of p-toluenesulfonic acid is 1% of the mass of the carboxylated polysiloxane, and the molar ratio of carboxyl groups, ethylenediamine, and dicyclohexylcarbodiimide on the hyperbranched polysiloxane is 1:1:1.1.

[0011] The beneficial effects of the present invention are as follows: The present application discloses a heat-insulating and energy-saving environmentally friendly exterior wall coating, which includes the following raw materials: modified acrylic acid, modified additives, modified glass microspheres, rutile titanium dioxide, leveling agent, defoamer, dispersant and water. The modified acrylic acid is prepared by free radical polymerization of acrylic acid, butyl acrylate, methyl methacrylate and glycidyl methacrylate to obtain modified polyacrylic acid.

[0012] Modified glass microspheres are prepared by treating hollow glass microspheres with sodium hydroxide solution to activate the surface hydroxyl groups, and then treating the pretreated glass microspheres with 3-glycidyl etheroxypropyltrimethoxysilane to graft epoxy groups onto the surface, thus obtaining modified glass microspheres.

[0013] The modifying additive uses trimethylsilyllithium as an initiator and trifluoropropylmethylcyclotrisiloxane as a polymerization monomer to form a polysiloxane with lithium silanolate at one end. Methyldichlorosilane is added, causing the Si-Cl bonds on the methyldichlorosilane to react with the lithium silanolate, thus obtaining the modifier. Castor oil is reacted with the modifier, causing the double bonds on the castor oil to react with the Si-H bonds on the modifier, thus obtaining modified castor oil. Octamethylcyclotetrasiloxane is ring-opened polymerized, and tetramethyldisiloxane is used for end-capping, thus obtaining a double-ended polysiloxane. Hydrogen-modified polysiloxanes are prepared by reacting dihydropolysiloxane with acrylic acid, causing the Si-H bonds on the dihydropolysiloxane to react with the double bonds on the acrylic acid, thus obtaining carboxylated polysiloxanes. The carboxylated polysiloxanes are then reacted with modified castor oil, causing the carboxyl groups on the carboxylated polysiloxanes and the hydroxyl groups on the modified castor oil to esterify, thus obtaining hyperbranched polysiloxanes. Finally, the hyperbranched polysiloxanes are reacted with ethylenediamine, causing the carboxyl groups on the hyperbranched polysiloxanes and the amino groups on the ethylenediamine to dehydrate, thus obtaining a modified additive.

[0014] During the raw material mixing and coating process, the amino groups on the modified additives can react with the epoxy groups on the modified acrylic acid and the modified glass microspheres to form a chemical cross-linking network, which improves the adhesion and hardness of the coating, giving the coating film good impact resistance. The dense cross-linked structure can effectively resist the erosion of moisture, ultraviolet rays and pollutants, and slow down chalking, discoloration and peeling. The fluorinated polysiloxane structure on the modified additives, with fluorinated segments, will accumulate on the coating surface, significantly reducing surface energy and solving the problem of easy dust accumulation in heat insulation coatings from the root. Detailed Implementation

[0015] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0016] Example 1: A heat-insulating and energy-saving environmentally friendly exterior wall coating is prepared by the following steps: Step A1: Acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and toluene are mixed and reacted at 150 r / min and 70℃ for 6 h to obtain modified polyacrylic acid. Step A2: Hollow glass microspheres were placed in sodium hydroxide solution and stirred for 3 hours at a speed of 200 r / min and a temperature of 60℃. The filtrate was then filtered to obtain pretreated glass microspheres. Ethanol, deionized water and 3-glycidoxypropyltrimethoxysilane were mixed and stirred at a speed of 150 r / min, a temperature of 60℃ and a pH of 4. The pretreated glass microspheres were added and the mixture was reacted for 3 hours to obtain modified glass microspheres. Step A3: Weigh the following raw materials by weight: 100 parts modified acrylic acid, 10 parts modified additive, 20 parts modified glass microspheres, 15 parts rutile titanium dioxide, 0.2 parts leveling agent, 0.3 parts defoamer, 0.5 parts dispersant, and 40 parts water. Mix the raw materials evenly to obtain a heat-insulating and energy-saving environmentally friendly exterior wall coating.

[0017] The mass ratio of acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate and azobisisobutyronitrile in step A1 is 5:60:30:5:1.

[0018] The concentration of the sodium hydroxide solution in step A2 is 0.3 mol / L, and the mass ratio of ethanol, deionized water, 3-glycidoxypropyltrimethoxysilane and pretreated glass microspheres is 300:10:2:100.

[0019] The leveling agent mentioned in step A3 is BYK-333, the defoamer is BYK-054, and the dispersant is DISPERBYK-140.

[0020] The modified additive is prepared by the following steps: Step B1: Lithium trimethylsilanolate was dissolved in tetrahydrofuran under nitrogen protection. The mixture was stirred at 200 r / min and 0°C, and trifluoropropylmethylcyclotrisiloxane was added. The mixture was heated to 20°C and reacted for 6 hours. Then, methyldichlorosilane was added, and the reaction continued for 3 hours to obtain the modifier. Castor oil, the modifier, the castor catalyst, and toluene were mixed evenly under nitrogen protection. The mixture was reacted at 150 r / min and 80°C for 6 hours to obtain modified castor oil. Step B2: Octamethylcyclotetrasiloxane, tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed and purged with nitrogen. The mixture is reacted at 150 r / min and 90 °C for 10 h. The temperature is then raised to 105 °C and the reaction is continued for 2 h to obtain dihydropolysiloxane. Dihydropolysiloxane, acrylic acid, caster catalyst and toluene are mixed evenly and purged with nitrogen. The mixture is reacted at 150 r / min and 80 °C for 6 h to obtain carboxylated polysiloxane. Step B3: Carboxylated polysiloxane, modified castor oil, p-toluenesulfonic acid and xylene are mixed and reacted at 120 r / min and 100 °C for 10 h to obtain hyperbranched polysiloxane. Hyperbranched polysiloxane, ethylenediamine, dicyclohexylcarbodiimide and xylene are mixed and reacted at 120 r / min and 20 °C for 3 h to obtain modified additive.

[0021] The molar ratio of Si-Cl bonds on lithium trimethylsilanolate, trifluoropropylmethylcyclotrisiloxane and methyldichlorosilane in step B1 is 1:5:1, the molar ratio of castor oil and modifier is 1:3, and the amount of cassette catalyst is 0.01% of the mass of modifier.

[0022] In step B2, the molar ratio of octamethylcyclotetrasiloxane, tetramethyldisiloxane, and tetramethylammonium hydroxide is 1.2:1:1.5, the molar ratio of dihydropolysiloxane and acrylic acid is 1:2, and the amount of caster catalyst is 0.01% of the mass of acrylic acid.

[0023] The ratio of carboxylated polysiloxane to modified castor oil in step B3 is 3:1, the amount of p-toluenesulfonic acid is 1% of the mass of carboxylated polysiloxane, and the molar ratio of carboxyl groups, ethylenediamine and dicyclohexylcarbodiimide on the hyperbranched polysiloxane is 1:1:1.1.

[0024] Example 2: A heat-insulating and energy-saving environmentally friendly exterior wall coating is prepared by the following steps: Step A1: Acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and toluene are mixed and reacted for 7 hours at a speed of 150 r / min and a temperature of 75℃ to obtain modified polyacrylic acid. Step A2: Hollow glass microspheres were placed in sodium hydroxide solution and stirred for 4 hours at a speed of 200 r / min and a temperature of 65℃. The filtrate was then filtered to obtain pretreated glass microspheres. Ethanol, deionized water and 3-glycidoxypropyltrimethoxysilane were mixed and stirred at a speed of 150 r / min, a temperature of 65℃ and a pH of 4. The pretreated glass microspheres were added and the mixture was reacted for 4 hours to obtain modified glass microspheres. Step A3: Weigh the following raw materials by weight: 110 parts modified acrylic acid, 15 parts modified additives, 25 parts modified glass microspheres, 20 parts rutile titanium dioxide, 0.5 parts leveling agent, 0.4 parts defoamer, 0.8 parts dispersant, and 45 parts water. Mix the raw materials evenly to obtain a heat-insulating and energy-saving environmentally friendly exterior wall coating.

[0025] The mass ratio of acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate and azobisisobutyronitrile in step A1 is 5:60:30:5:1.

[0026] The concentration of the sodium hydroxide solution in step A2 is 0.3 mol / L, and the mass ratio of ethanol, deionized water, 3-glycidoxypropyltrimethoxysilane and pretreated glass microspheres is 300:10:2:100.

[0027] The leveling agent mentioned in step A3 is BYK-306, the defoamer is BYK-066N, and the dispersant is DISPERBYK-182.

[0028] The modified additive is prepared by the following steps: Step B1: Lithium trimethylsilanolate was dissolved in tetrahydrofuran under nitrogen protection. The mixture was stirred at 300 r / min and 0°C, and trifluoropropylmethylcyclotrisiloxane was added. The mixture was heated to 20°C and reacted for 7 hours. Then, methyldichlorosilane was added, and the reaction continued for 4 hours to obtain the modifier. Castor oil, the modifier, the castor catalyst, and toluene were mixed evenly under nitrogen protection. The mixture was reacted at 150 r / min and 85°C for 7 hours to obtain modified castor oil. Step B2: Octamethylcyclotetrasiloxane, tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed and purged with nitrogen. The mixture is reacted at 200 r / min and 90 °C for 11 h. The temperature is then raised to 108 °C and the reaction is continued for 2.5 h to obtain dihydropolysiloxane. Dihydropolysiloxane, acrylic acid, caster catalyst and toluene are mixed evenly and purged with nitrogen. The mixture is reacted at 150 r / min and 85 °C for 7 h to obtain carboxylated polysiloxane. Step B3: Carboxylated polysiloxane, modified castor oil, p-toluenesulfonic acid and xylene are mixed and reacted at 120 r / min and 105 °C for 13 h to obtain hyperbranched polysiloxane. Hyperbranched polysiloxane, ethylenediamine, dicyclohexylcarbodiimide and xylene are mixed and reacted at 120 r / min and 25 °C for 4 h to obtain modified additive.

[0029] The molar ratio of Si-Cl bonds on lithium trimethylsilanolate, trifluoropropylmethylcyclotrisiloxane and methyldichlorosilane in step B1 is 1:5:1, the molar ratio of castor oil and modifier is 1:3, and the amount of cassette catalyst is 0.01% of the mass of modifier.

[0030] In step B2, the molar ratio of octamethylcyclotetrasiloxane, tetramethyldisiloxane, and tetramethylammonium hydroxide is 1.2:1:1.5, the molar ratio of dihydropolysiloxane and acrylic acid is 1:2, and the amount of caster catalyst is 0.01% of the mass of acrylic acid.

[0031] The ratio of carboxylated polysiloxane to modified castor oil in step B3 is 5:2, the amount of p-toluenesulfonic acid is 1% of the mass of carboxylated polysiloxane, and the molar ratio of carboxyl groups, ethylenediamine and dicyclohexylcarbodiimide on the hyperbranched polysiloxane is 1:1:1.1.

[0032] Example 3: A heat-insulating and energy-saving environmentally friendly exterior wall coating, prepared by the following steps: Step A1: Acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and toluene are mixed and reacted for 8 hours at a speed of 200 r / min and a temperature of 80℃ to obtain modified polyacrylic acid. Step A2: Hollow glass microspheres were placed in sodium hydroxide solution and stirred for 5 hours at 300 r / min and 65°C. The filtrate was then filtered to obtain pretreated glass microspheres. Ethanol, deionized water and 3-glycidoxypropyltrimethoxysilane were mixed and stirred at 200 r / min, 65°C and pH 4.5. The pretreated glass microspheres were added and the mixture was reacted for 5 hours to obtain modified glass microspheres. Step A3: Weigh the following raw materials by weight: 120 parts modified acrylic acid, 20 parts modified additives, 30 parts modified glass microspheres, 25 parts rutile titanium dioxide, 0.8 parts leveling agent, 0.6 parts defoamer, 1 part dispersant and 50 parts water. Mix the raw materials evenly to obtain a heat-insulating and energy-saving environmentally friendly exterior wall coating.

[0033] The mass ratio of acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate and azobisisobutyronitrile in step A1 is 5:60:30:5:1.

[0034] The concentration of the sodium hydroxide solution in step A2 is 0.3 mol / L, and the mass ratio of ethanol, deionized water, 3-glycidoxypropyltrimethoxysilane and pretreated glass microspheres is 300:10:2:100.

[0035] The leveling agent mentioned in step A3 is BYK-358N, the defoamer is BYK-065, and the dispersant is DISPERBYK-2013.

[0036] The modified additive is prepared by the following steps: Step B1: Lithium trimethylsilanolate was dissolved in tetrahydrofuran under nitrogen protection. The mixture was stirred at 300 r / min and 0°C, and trifluoropropylmethylcyclotrisiloxane was added. The mixture was heated to 25°C and reacted for 8 hours. Then, methyldichlorosilane was added, and the reaction continued for 5 hours to obtain the modifier. Castor oil, the modifier, the castor catalyst, and toluene were mixed evenly under nitrogen protection. The mixture was reacted at 200 r / min and 85°C for 8 hours to obtain modified castor oil. Step B2: Octamethylcyclotetrasiloxane, tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed and purged with nitrogen. The mixture is reacted at 200 r / min and 95 °C for 12 h. The temperature is then raised to 110 °C and the reaction is continued for 3 h to obtain dihydropolysiloxane. Dihydropolysiloxane, acrylic acid, caster catalyst and toluene are mixed evenly and purged with nitrogen. The mixture is reacted at 200 r / min and 85 °C for 8 h to obtain carboxylated polysiloxane. Step B3: Carboxylated polysiloxane, modified castor oil, p-toluenesulfonic acid and xylene are mixed and reacted at 150 r / min and 110 °C for 15 h to obtain hyperbranched polysiloxane. Hyperbranched polysiloxane, ethylenediamine, dicyclohexylcarbodiimide and xylene are mixed and reacted at 150 r / min and 25 °C for 5 h to obtain modified additive.

[0037] The molar ratio of Si-Cl bonds on lithium trimethylsilanolate, trifluoropropylmethylcyclotrisiloxane and methyldichlorosilane in step B1 is 1:5:1, the molar ratio of castor oil and modifier is 1:3, and the amount of cassette catalyst is 0.01% of the mass of modifier.

[0038] In step B2, the molar ratio of octamethylcyclotetrasiloxane, tetramethyldisiloxane, and tetramethylammonium hydroxide is 1.2:1:1.5, the molar ratio of dihydropolysiloxane and acrylic acid is 1:2, and the amount of caster catalyst is 0.01% of the mass of acrylic acid.

[0039] The ratio of carboxylated polysiloxane to modified castor oil in step B3 is 7:3, the amount of p-toluenesulfonic acid is 1% of the mass of carboxylated polysiloxane, and the molar ratio of carboxyl groups, ethylenediamine and dicyclohexylcarbodiimide on the hyperbranched polysiloxane is 1:1:1.1.

[0040] Comparative Example 1: This comparative example did not include glycidyl methacrylate compared to Example 1, but the remaining steps were the same.

[0041] Comparative Example 2: In this comparative example, hollow glass microspheres were used instead of modified glass microspheres, while the other steps were the same as in Example 1.

[0042] Comparative Example 3: This comparative example uses glycerol instead of modified castor oil, but the other steps are the same as in Example 1.

[0043] The coatings prepared in Examples 1-3 and Comparative Examples 1-3 were sprayed onto standard tinplate and cured to obtain corresponding samples. The tests were conducted according to GB / T9780-2013 standards, using a mixture of petrolatum and carbon black as the stain. The tests used five levels (0-4) to evaluate the results, corresponding to levels 5, 4, 3, 2, and 1 of the basic gray card GB / T250. The colorimetric evaluation level was determined according to the color difference between the conventional colorimetric box and the basic gray card, as per item 8.2b of GB / T9761-2008. Water resistance was tested according to GB / T1733-1993 standards, with the samples immersed in water for 360 hours. Alkali resistance was tested according to GB / T9265-2009 standards, with the samples immersed in a saturated calcium hydroxide solution for 360 hours. Aging resistance was tested according to GB / T1865-2009 standards, with irradiation for 1000 hours. Results were determined according to GB / T1766-2008 standards. The test results are shown in Table 1 below.

[0044] Table 1 As shown in Table 1, this application has excellent stain resistance and weather resistance.

[0045] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.

Claims

1. A heat-insulating and energy-saving environmentally friendly exterior wall coating, characterized in that: It is made by the following steps: Step A1: Mix acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and toluene, and react them to obtain modified polyacrylic acid; Step A2: Place hollow glass microspheres in sodium hydroxide solution, stir and treat, filter to remove filtrate to obtain pretreated glass microspheres. Mix ethanol, deionized water and 3-glycidoxypropyltrimethoxysilane, stir and add the pretreated glass microspheres to react and obtain modified glass microspheres. Step A3: Weigh the following raw materials in parts by weight: 100-120 parts modified polyacrylic acid, 10-20 parts modified additives, 20-30 parts modified glass microspheres, 15-25 parts rutile titanium dioxide, 0.2-0.8 parts leveling agent, 0.3-0.6 parts defoamer, 0.5-1 parts dispersant, and 40-50 parts water. Mix the raw materials evenly to obtain a heat-insulating and energy-saving environmentally friendly exterior wall coating. The modified additive is prepared by the following steps: Step B1: Dissolve lithium trimethylsilanolate in tetrahydrofuran, purge with nitrogen, stir and add trifluoropropylmethylcyclotrisiloxane, heat and react, then add methyldichlorosilane and continue the reaction to obtain the modifier. Mix castor oil, modifier, castor catalyst and toluene evenly, purge with nitrogen and react to obtain modified castor oil. Step B2: Mix octamethylcyclotetrasiloxane, tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide, and react under nitrogen protection to obtain dihydropolysiloxane. Mix dihydropolysiloxane, acrylic acid, castor catalyst and toluene evenly, and react under nitrogen protection to obtain carboxylated polysiloxane. Step B3: Mix carboxylated polysiloxane, modified castor oil, p-toluenesulfonic acid and xylene, and react to obtain hyperbranched polysiloxane. Mix hyperbranched polysiloxane, ethylenediamine, dicyclohexylcarbodiimide and xylene, and react to obtain modified additive.

2. The heat-insulating and energy-saving environmentally friendly exterior wall coating according to claim 1, characterized in that: The mass ratio of acrylic acid, butyl acrylate, methyl methacrylate, glycidyl methacrylate and azobisisobutyronitrile in step A1 is 5:60:30:5:

1.

3. The heat-insulating and energy-saving environmentally friendly exterior wall coating according to claim 1, characterized in that: The concentration of the sodium hydroxide solution in step A2 is 0.3 mol / L, and the mass ratio of ethanol, deionized water, 3-glycidoxypropyltrimethoxysilane and pretreated glass microspheres is 300:10:2:

100.

4. The heat-insulating and energy-saving environmentally friendly exterior wall coating according to claim 1, characterized in that: The molar ratio of Si-Cl bonds on lithium trimethylsilanolate, trifluoropropylmethylcyclotrisiloxane and methyldichlorosilane in step B1 is 1:5:1, and the molar ratio of castor oil and modifier is 1:

3.

5. The heat-insulating and energy-saving environmentally friendly exterior wall coating according to claim 1, characterized in that: The molar ratio of octamethylcyclotetrasiloxane, tetramethyldisiloxane and tetramethylammonium hydroxide in step B2 is 1.2:1:1.5, and the molar ratio of dihydropolysiloxane and acrylic acid is 1:

2.

6. The heat-insulating and energy-saving environmentally friendly exterior wall coating according to claim 1, characterized in that: The ratio of carboxylated polysiloxane to modified castor oil in step B3 is 2n+1:n, where n is a natural number greater than 0, and the molar ratio of carboxyl groups, ethylenediamine, and dicyclohexylcarbodiimide on the hyperbranched polysiloxane is 1:1:1.1.

Citation Information

Patent Citations

  • Yellowing-resistant organic silicon modified epoxy sealant and preparation method thereof