Separators for energy storage devices, separator reels and energy storage devices

CN122580760APending Publication Date: 2026-08-14ASAHI KASEI BATTERY SEPARATOR CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580010589.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-29
Filing Date
2025-03-28
Publication Date
2026-08-14

AI Technical Summary

Benefits of technology

[0054]根据本发明,能够提供一种通过抑制分隔件送出时的静电的产生而能够抑制针孔的产生的分隔件。另外,根据本发明,通过抑制静电的产生,能够提供操作性优异的分隔件。进而,包含本发明的分隔件的电池的循环特性和倍率特性优异。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A separator for an energy storage device is provided, comprising: a porous substrate, a layer containing inorganic filler disposed on a first main surface of the porous substrate, and a layer containing a thermoplastic polymer disposed on the surface of the layer containing inorganic filler and on a second main surface of the porous substrate, wherein the coverage area S of the layer containing thermoplastic polymer on the surface of the layer containing inorganic filler is provided. c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate is between 30% and 100%. p The thickness t of the thermoplastic polymer layer on the inorganic filler layer exceeds 0% and is less than 30%. c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy t c / t p The relationship is >1.00.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to separators for energy storage devices, separator reels, and energy storage devices. Background Technology

[0002] In recent years, the development of energy storage devices, represented by non-aqueous electrolyte batteries, has been actively underway. Typically, in non-aqueous electrolyte batteries such as lithium-ion batteries, a microporous membrane is placed between the positive and negative electrodes as a separator. This separator prevents direct contact between the positive and negative electrodes and allows ions to permeate through the electrolyte held within the microporous membrane.

[0003] For separators, the requirements include characteristics such as the ability to quickly stop the battery reaction under abnormal heating (fusible characteristic) and the ability to maintain shape even at high temperatures to prevent dangerous situations where the positive and negative electrode materials react directly (short-circuit characteristic), which are related to the safety requirements of the past.

[0004] In addition to safety, in order to endow the separator with various functions, the coating of functional layers of microporous membranes, the layer composition of functional layers, and the coating patterns such as dots were studied.

[0005] For example, Patent Document 1 discloses a separator for an energy storage device, which has: a polyolefin microporous membrane and a thermoplastic polymer covering layer covering at least a portion of at least one surface of the polyolefin microporous membrane, the thermoplastic polymer covering layer being disposed in a dotted manner on the polyolefin microporous membrane.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: International Publication No. 2014 / 017651 Summary of the Invention

[0009] The problem the invention aims to solve

[0010] As a potential problem with separators, one example is that static electricity (easily charged) can be generated when the separator is fed out of a winding body such as a spool or when it begins to travel from the spool. If the separator has a high charge, electrostatic discharge can occur, resulting in pinholes, which can cause short circuits in the battery.

[0011] In addition, the separation components attract each other or adhere to surrounding rollers, which deteriorates the operability of the separation components and reduces process efficiency, and this is also a problem.

[0012] In view of the above, the object of the present invention is to provide a separator that suppresses the generation of pinholes and reduces operability by suppressing the generation of static electricity when the separator is fed from the roll.

[0013] Solution for solving the problem

[0014] Through repeated and in-depth research, the inventors discovered that the above-mentioned problems could be solved by using a separator for an energy storage device having the following configuration, thus completing the present invention.

[0015] That is, the present invention is as follows.

[0016] [Project 1]

[0017] A separator for an energy storage device, comprising: a porous substrate,

[0018] A layer containing inorganic filler disposed on the first main surface of the porous substrate, and

[0019] A layer containing a thermoplastic polymer disposed on the surface of the layer containing inorganic fillers and on the second main surface of the porous substrate.

[0020] The coverage area S of the thermoplastic polymer-containing layer on the surface of the inorganic filler-containing layer c Between 30% and 100%,

[0021] The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p More than 0% and less than 30%,

[0022] The thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy t c / t p The relationship is >1.00.

[0023] [Project 2]

[0024] According to the separator for the energy storage device described in Project 1, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy S c / S p Relationship ≥2.00.

[0025] [Project 3]

[0026] According to the separator for the energy storage device described in Project 1 or 2, the coverage area S of the layer containing the thermoplastic polymer on the surface of the layer containing the inorganic filler is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substratep Satisfying 55%≤S c +S p A relationship of ≤75%.

[0027] [Project 4]

[0028] According to any one of items 1 to 3, the separator for an energy storage device, wherein the inorganic filler particle size contained in the layer containing inorganic filler satisfies 1.0 ≤ D90 / D10 ≤ 5.0.

[0029] The thermoplastic polymer contained in the layer on the second main surface of the porous substrate has a particle size that satisfies the relationship 1.0≤D90 / D10≤5.0.

[0030] [Project 5]

[0031] The separator for the energy storage device according to any one of items 1 to 4, wherein the stripped charge when discharged from the drum is above -15kV and below +15kV.

[0032] [Project 6]

[0033] A reel formed by winding the energy storage device described in any one of items 1 to 5 with a separator, wherein the surface pressure applied to the innermost layer is less than 5 MPa.

[0034] [Project 7]

[0035] The separator for an energy storage device according to any one of items 1 to 5 is obtained by coating the surface of the porous substrate or the layer containing inorganic filler disposed on the porous substrate with an aqueous slurry containing a thermoplastic polymer.

[0036] [Project 8]

[0037] A separator for an energy storage device according to any one of items 1 to 5 and 7, wherein the thermoplastic polymer-containing layer is arranged in a dotted pattern.

[0038] [Project 9]

[0039] A separator for an energy storage device according to any one of items 1 to 5 and 7 to 8, wherein the layer containing the thermoplastic polymer comprises: a copolymer of monomer units containing (meth)acrylate monomers.

[0040] [Project 10]

[0041] An energy storage device comprising, as described in any one of items 1-5 and 7-9, a separator for energy storage, a positive electrode, a negative electrode, and a non-aqueous electrolyte.

[0042] [Project 11]

[0043] A separator for an energy storage device according to any one of items 1-5 and 7-9, wherein the thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c Standard deviation s tc The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Standard deviation s tp Satisfy s tc / s tp The relationship is greater than 1.0.

[0044] [Project 12]

[0045] A method for manufacturing a separator for an energy storage device according to any one of items 1 to 5 and 7 to 9, comprising:

[0046] The process of preparing porous substrates;

[0047] The process of forming an inorganic filler-containing layer by coating a slurry containing inorganic fillers onto the first main surface of the porous substrate; and

[0048] The process of forming a thermoplastic polymer layer by coating a slurry containing a thermoplastic polymer onto the surface of the inorganic filler layer and the second main surface of the porous substrate.

[0049] The viscosity of the slurry containing the thermoplastic polymer is at a shear rate of 60,000 sec. -1 The values ​​are above 1 mPa·s and below 20 mPa·s.

[0050] The shear rate v when the slurry containing the thermoplastic polymer is coated on the surface of the layer containing inorganic fillers. c The shear rate v when the slurry containing the thermoplastic polymer is coated on the second main surface of the porous substrate p The relationship between equations (2) and (3) is satisfied.

[0051] 30000sec -1 ≤v c ≤200000sec -1 …Formula (2)

[0052] 5000sec -1 ≤v c -v p ≤40000sec -1 …Formula (3)

[0053] The effects of the invention

[0054] According to the present invention, a separator can be provided that can suppress the generation of pinholes by suppressing the generation of static electricity during separator delivery. Furthermore, according to the present invention, by suppressing the generation of static electricity, a separator with excellent operability can be provided. Consequently, batteries incorporating the separator of the present invention exhibit excellent cycle characteristics and rate performance. Detailed Implementation

[0055] The following is a detailed description of the method for implementing the present invention (hereinafter referred to as "this embodiment"). It should be noted that the present invention is not limited to the following embodiment, and can be implemented in various modifications within its scope.

[0056] In addition, unless otherwise specified, the characteristic values ​​described in this embodiment refer to values ​​measured by the methods described in the [Example] item or by methods that can be understood by those skilled in the art as equivalent to them.

[0057] In the following description, the upper or lower limit of the numerical range recorded in stages can be replaced with the upper or lower limit of other numerical ranges recorded in stages. Furthermore, in the following description, the upper or lower limit of a certain numerical range can be replaced with the value described in the embodiment. Moreover, regarding the term "process" in the following description, an independent process is naturally included in this terminology; however, if it cannot be clearly distinguished from other processes, it can also be included in this terminology as long as it achieves the function of the "process".

[0058] <Separator for energy storage devices>

[0059] The separator for the energy storage device in this embodiment (hereinafter, sometimes simply referred to as "separator") has: a porous substrate,

[0060] A layer containing inorganic fillers disposed on the first main surface of a porous substrate, and

[0061] A layer containing a thermoplastic polymer disposed on the surface of a layer containing inorganic fillers and on the second main surface of a porous substrate.

[0062] The coverage area S of the thermoplastic polymer layer on the surface of the layer containing inorganic fillers c Between 30% and 100%,

[0063] The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p More than 0% and less than 30%,

[0064] The thickness t of the thermoplastic polymer layer on the surface of the layer containing inorganic fillers. c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy tc / t p The relationship is >1.00.

[0065] The factors that determine the charge on a separator are generally "contact area", "friction", "humidity", "pressure", and "temperature". In the manufacturing process of separators and batteries, moisture is preferably eliminated and temperature and humidity are managed to be constant. Therefore, it is difficult to arbitrarily change the environmental factors of "temperature" and "humidity". It can be said that the manufacturing process of separators and batteries is an environment in which static electricity can easily become a problem.

[0066] Therefore, the inventors conducted in-depth research focusing on "contact area", "friction", and "pressure".

[0067] The separator is mainly composed of a substrate, a layer containing inorganic fillers, and a layer containing thermoplastic polymers.

[0068] The inventors conducted research and found that the contact between the inorganic filler layer and the thermoplastic polymer layer has a significant impact on the generation of static electricity. It is speculated that this is because, compared to the substrate, the inorganic filler layer, with its higher surface roughness and insulation, contacts the thermoplastic polymer layer, thus causing not only peeling charge but also triboelectric charging when the separator is fed from the roll.

[0069] Therefore, while considering the balance with battery performance, the inventors set the coverage area and thickness of the thermoplastic polymer layer, as well as the particle size distribution of the inorganic filler and the thermoplastic polymer, to a certain level or above, thereby completing the separator of this embodiment in which the contact area between the inorganic filler layer and the thermoplastic polymer layer is reduced.

[0070] The separator in this embodiment has a porous substrate, a layer containing inorganic filler disposed on a first main surface of the porous substrate, and a layer containing thermoplastic polymer disposed on the surface of the layer containing inorganic filler and on a second main surface of the porous substrate.

[0071] In this disclosure, the first principal surface of the porous substrate refers to at least one surface of the porous substrate (in one embodiment, a single surface of the porous substrate). Additionally, in this disclosure, the second principal surface of the porous substrate refers to the surface located opposite the first principal surface of the porous substrate.

[0072] The separator in this embodiment has a layer containing inorganic filler disposed on a first main surface of a porous substrate, thereby exhibiting excellent heat resistance.

[0073] Furthermore, the separator of this embodiment has a thermoplastic polymer layer disposed on the surface of the layer containing inorganic filler and on the second main surface of the porous substrate, thereby improving the adhesion to the electrode and thus providing excellent cycle characteristics.

[0074] In this embodiment, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c Preferably, the coverage area is between 30% and 100%, with a coverage rate S. c More preferably, the coverage area ratio is 35% or more and 80% or less, S c Further preferred is 40% or more and 70% or less.

[0075] In this embodiment, the coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate is... p Preferably, the coverage rate is greater than 0% and less than 30%, more preferably, the coverage area ratio S p For coverage areas between 5% and 25%, the preferred coverage rate S is further optimized. p It is between 5% and 20%.

[0076] From the viewpoints of reducing the contact area between the inorganic filler layer and the thermoplastic polymer layer, suppressing the generation of static electricity, and improving the adhesion to the electrode while maintaining ion permeability, it is preferable that the coverage area of ​​the thermoplastic polymer layer on the surface of the inorganic filler layer and on the second main surface of the porous substrate is within the range described above.

[0077] Here, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Calculated using the following formulas respectively.

[0078] S c (%) = (Area of ​​thermoplastic polymer-containing layer covering the surface of the inorganic filler layer / Surface area of ​​the inorganic filler layer) × 100

[0079] S p (%) = Coverage area of ​​the thermoplastic polymer-containing layer on the second main surface of the porous substrate / Surface area of ​​the porous substrate × 100

[0080] It should be noted that the coverage area S of the layer containing the thermoplastic polymer on the surface of the layer containing the inorganic filler is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p The determination can be performed using the methods described in the examples.

[0081] In this embodiment, the thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Preferred to satisfy t c / tp A relationship greater than 1.00 is preferred, and t is more preferably satisfied. c / t p For a relationship ≥1.40, further optimization is performed to satisfy t. c / t p A relationship ≥2.00 is preferred, especially if t is satisfied. c / t p For a relationship ≥ 3.00, the optimal choice satisfies t. c / t p Relationships ≥4.00.

[0082] From the viewpoint of reducing the contact area between the inorganic filler layer and the thermoplastic polymer layer and suppressing the generation of static electricity, it is preferable that the ratio of the thickness of the inorganic filler layer on the surface of the inorganic filler layer to the thickness of the thermoplastic polymer layer on the second main surface of the porous substrate is within the range described above.

[0083] The effect of this embodiment can be achieved by setting the ratio of the coverage area ratio and the thickness ratio of the layer containing the inorganic filler on the surface of the layer and the second main surface of the porous substrate containing the thermoplastic polymer to a specified range.

[0084] The thickness t of the thermoplastic polymer layer on the surface of the layer containing inorganic fillers. c Preferably, the micrometer is 0.1 μm or more and 5.0 μm or less, more preferably 0.5 μm or more and 4.0 μm or less, and even more preferably 1.0 μm or more and 3.0 μm or less.

[0085] The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Preferably, the micrometer is 0.1 μm or more and 3.0 μm or less, more preferably 0.1 μm or more and 2.0 μm or less, and even more preferably 0.1 μm or more and 1.0 μm or less.

[0086] It should be noted that the thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p The determination can be performed using the methods described in the examples.

[0087] In this embodiment, the thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c Standard deviation s tc The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Standard deviation s tp Preferred to satisfy s tc / s tp The relationship is >1.0. The thickness t of the thermoplastic polymer layer on the surface of the layer containing inorganic fillers.c Standard deviation s tc The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Standard deviation s tp Ratio: s tc / s tp Preferably more than 1, more preferably more than 3, further preferably more than 5, and especially preferably more than 7.

[0088] From the viewpoint of reducing the contact area between the inorganic filler-containing layer and the thermoplastic polymer on the second main surface of the porous substrate when overlapping separators are used, and suppressing the generation of static electricity, it is preferable to adjust the surface roughness of the thermoplastic polymer on the surface of the inorganic filler-containing layer and the surface roughness of the thermoplastic polymer on the second main surface of the porous substrate, respectively, so that the ratio of the standard deviation of the thickness of the thermoplastic polymer-containing layer is: s tc / s tp The above range applies.

[0089] It should be noted that the thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c Standard deviation s tc The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Standard deviation s tp The determination can be performed using the methods described in the examples.

[0090] Regarding the thickness t of the thermoplastic polymer layer on the surface of the layer containing inorganic fillers. c Standard deviation s tc At thickness t c Given the same numerical values, from the viewpoint of ensuring the gap (preventing contact) between the surface of the inorganic filler-containing layer and the surface of the thermoplastic polymer-containing layer on the second main surface of the porous substrate when overlapping separators are used, the standard deviation s is preferred. tc The value is large.

[0091] Standard deviation s tc Preferably, the distance is 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.10 μm or more, and particularly preferably 0.30 μm or more. Furthermore, from the viewpoint of maintaining a constant distance between the electrode and the separator inside the battery, the standard deviation s tc Preferably, it is 1.50 μm or less, more preferably 1.00 μm or less, and even more preferably 0.70 μm or less.

[0092] Standard deviation s tcThe shear rate and particle size of the thermoplastic polymer particles during coating can be adjusted when a thermoplastic polymer-containing slurry (described later) is coated onto the surface of a layer containing inorganic fillers to form a thermoplastic polymer-containing layer. For example, if the shear rate during coating of the thermoplastic polymer-containing slurry is increased, the standard deviation s will be adjusted. tc If the shear rate during coating is reduced, the standard deviation s increases. tc The size decreases. Additionally, by increasing the particle size of the thermoplastic polymer particles, the standard deviation s... tc It gets bigger.

[0093] Regarding the thickness t of the thermoplastic polymer-containing layer on the second principal surface of the porous substrate p Standard deviation s tp At thickness t p Given the same numerical value, if the standard deviation s tp As the value increases, the layer containing thermoplastic polymer on the second principal surface of the porous substrate may locally contact the surface of the layer containing inorganic filler when overlapping separators. Therefore, from the viewpoint of suppressing static electricity generation, a standard deviation s is preferred. tp The value is small.

[0094] Standard deviation s tp Preferably, the micrometer is 1.00 μm or less, more preferably 0.50 μm or less, even more preferably 0.30 μm or less, and particularly preferably 0.10 μm or less. Furthermore, from the viewpoint of improving adhesion to the electrode, the standard deviation s tp Preferably, it is 0.01 μm or more, more preferably 0.02 μm or more, even more preferably 0.03 μm or more, and particularly preferably 0.05 μm or more.

[0095] Standard deviation s tp The shear rate during coating can be adjusted when a layer containing a thermoplastic polymer is formed by coating a slurry containing a thermoplastic polymer (described later) onto the surface of a porous substrate. For example, if the shear rate during coating of the slurry containing the thermoplastic polymer is increased, the standard deviation s will be adjusted. tp If the shear rate during coating is reduced, the standard deviation s increases. tp It gets smaller.

[0096] In this embodiment, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Preferred to satisfy S c / S p A relationship ≥2.00 is preferred, especially one satisfying S. c / S p Relationships ≥3.00.

[0097] From the viewpoint of reducing the contact area between the inorganic filler layer and the thermoplastic polymer layer and suppressing the generation of static electricity, it is preferable that the area ratio of the inorganic filler layer on the surface and the thermoplastic polymer layer on the second main surface of the porous substrate is within the range described above.

[0098] In this embodiment, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is... c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Preferably, 55% ≤ S c +S p A relationship of ≤75% is preferred, and 60%≤S is even more desirable. c +S p The relationship is ≤70%.

[0099] When the combined coverage area of ​​the layer containing the inorganic filler and the layer containing the thermoplastic polymer on the second main surface of the porous substrate is 55% or more, the adhesion to the electrode is improved and the cycle characteristics are excellent, therefore this is preferred. Furthermore, if the combined coverage area of ​​the layer containing the inorganic filler and the layer containing the thermoplastic polymer on the second main surface of the porous substrate is 75% or less, the ion permeability does not decrease and the rate capability is excellent, therefore this is also preferred.

[0100] In the separator of this embodiment, it is preferable that the particle size of the inorganic filler in the layer containing inorganic filler satisfies the relationship 1.0≤D90 / D10≤5.0, and the particle size of the thermoplastic polymer in the layer containing thermoplastic polymer on the surface of the layer containing inorganic filler and on the second main surface of the porous substrate satisfies the relationship 1.0≤D90 / D10≤5.0.

[0101] From the viewpoint of suppressing the generation of static electricity, it is preferable that the thickness of the layer containing the thermoplastic polymer on the surface of the layer containing the inorganic filler and on the second main surface of the porous substrate, as well as the particle size of the inorganic filler and the thermoplastic polymer, are within a specified range.

[0102] The effects of this embodiment can be achieved by setting the thickness of the layer containing the inorganic filler and the layer containing the thermoplastic polymer on the surface of the porous substrate, as well as the particle size of the inorganic filler and the thermoplastic polymer, to a specified range.

[0103] The separator of this embodiment achieves excellent circulation characteristics by disposing a layer containing thermoplastic polymer on the surface of a layer containing inorganic filler disposed on a first main surface of a porous substrate and on a second main surface of the porous substrate (or, in one embodiment, on both sides of the separator). Furthermore, by controlling the coverage area ratio and thickness of the two layers containing thermoplastic polymer respectively, the generation of static electricity caused by the contact between the layer containing inorganic filler and the layer containing thermoplastic polymer can be suppressed.

[0104] (A dotted pattern of layers containing thermoplastic polymers)

[0105] In this embodiment, the thermoplastic polymer-containing layer can be configured in a dotted pattern.

[0106] Dots indicate that a substrate contains portions of thermoplastic polymer and portions that do not; the portions containing thermoplastic polymer exist as islands. A dot pattern represents a regular arrangement of dots.

[0107] It should be noted that the portion of the thermoplastic polymer-containing layer can be independent.

[0108] In this embodiment, when the thermoplastic polymer layer of the separator is arranged in a dotted pattern, it is preferable to have a reduction in resistance due to the presence of Li ion channels (regions where there is no thermoplastic polymer on the substrate but where the permeability of Li ions is particularly excellent) and an increase in electrolyte permeability (injection capability) during the battery manufacturing process.

[0109] In one approach, the dotted pattern of the thermoplastic polymer layer functions as an adhesive layer that bonds the electrodes to the spacers.

[0110] The separator in this embodiment can suppress the generation of static electricity when the separator is fed from the roll by reducing the contact area between the inorganic filler layer and the thermoplastic polymer layer. To reduce the contact area between the adhesive layer and the inorganic filler layer, the coverage area S of the thermoplastic polymer layer on the surface of the inorganic filler layer is increased. c Alternatively, reduce the coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate. p Or it can be achieved by satisfying both of these conditions.

[0111] <Diameter of the point>

[0112] From the viewpoints of reducing battery resistance, facilitating venting, improving electrolyte permeability (injection capability), reducing heat accumulation and thus improving safety, and suppressing static electricity generation or pinhole generation, the diameter of the dots in the thermoplastic polymer layer is preferably 50 μm or more and 1000 μm or less, more preferably 100 μm or more and 500 μm or less, particularly preferably 150 μm or more and 300 μm or less, and most preferably 200 μm or more and 300 μm or less.

[0113] The point diameter of the thermoplastic polymer-containing layer was measured using a microscope (model: VHX-7000, manufactured by KEYENCE). The separator used as the sample was photographed at 100x (coaxial incidence), and the diameter of each of the five points was measured in measurement mode. The average value of these measurements was calculated as the point diameter.

[0114] <Distance between points>

[0115] From the viewpoint of ensuring sufficient gaps between multiple points to ensure the permeation flow path of the electrolyte and good venting, and from the viewpoint of suppressing static electricity generation, the inter-point distance of the layer containing the thermoplastic polymer is preferably 50 μm or more and 3000 μm or less, more preferably 100 μm or more and 2500 μm or less, even more preferably 150 μm or more and 2000 μm or less, and even more preferably 200 μm or more and 500 μm or less.

[0116] The inter-point distance of the thermoplastic polymer-containing layer was measured using a microscope (model: VHX-7000, manufactured by KEYENCE). The separator used as the sample was photographed at 100x (coaxial projection). In measurement mode, any point was selected, and the distances from its center to the centers of points located longitudinally, laterally, and diagonally at that point were measured. The average of these distances was taken as the inter-point distance.

[0117] From the viewpoint of maintaining an excellent balance between adhesion to the electrode and fluidity to the electrolyte, the inter-point distance / diameter of the thermoplastic polymer-containing layer is preferably 0.3 or more and 5 or less, more preferably 0.5 or more and 4 or less, even more preferably 0.7 or more and 3.8 or less, and particularly preferably 1 or more and 3.5 or less.

[0118] From the viewpoint of ensuring good venting, the arrangement angle of the points of the thermoplastic polymer-containing layer is preferably less than 40°, and there is no lower limit to the arrangement angle, for example, it can be 0° or more.

[0119] (Uniformly dispersed coating of a layer containing thermoplastic polymer)

[0120] When forming the thermoplastic polymer-containing layer of this embodiment, the thermoplastic polymer can also be coated on the layer containing inorganic fillers and the porous substrate in a manner that the thermoplastic polymer is uniformly dispersed (in one embodiment, uniform dispersion coating).

[0121] In one approach, uniform dispersion coating can be performed in a manner where the coating surface (e.g., the surface of a polyolefin microporous membrane or a layer containing inorganic fillers) is completely covered by a layer containing a thermoplastic polymer, or in a manner where a portion of the coating surface is exposed.

[0122] The constituent elements of the separator in this embodiment will be described below.

[0123] [Layer containing thermoplastic polymer]

[0124] The thermoplastic polymer-containing layer in this embodiment comprises a thermoplastic polymer.

[0125] (Thermoplastic polymer)

[0126] The thermoplastic polymers used in this embodiment are not particularly limited, and examples include: polyolefin resins such as polyethylene, polypropylene, and α-polyolefins; fluorinated resins such as polyvinylidene fluoride and polytetrafluoroethylene and copolymers containing them; diene polymers containing conjugated dienes such as butadiene and isoprene as monomer units, or copolymers containing them and their hydrogenates; acrylic polymers containing acrylates and methacrylates as monomer units, or copolymers containing them and their hydrogenates; rubbers such as ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate; cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; resins with melting points and / or glass transition temperatures of 180°C or higher, such as polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamide imide, polyamide, and polyester, and mixtures thereof. Furthermore, monomers having hydroxyl, sulfonic acid, carboxyl, amide, or cyano groups can also be used as monomers for synthesizing thermoplastic polymers.

[0127] Among these thermoplastic polymers, diene polymers, acrylic polymers, or fluoropolymers are preferred in terms of their excellent adhesion to electrode active materials, strength, and flexibility.

[0128] (Diene polymers)

[0129] Diene polymers are not particularly limited, and can be, for example, polymers comprising monomer units formed by polymerizing conjugated dienes such as butadiene and isoprene, which have two conjugated double bonds. Conjugated diene monomers are not particularly limited, and examples include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. They can be polymerized individually or copolymerized.

[0130] The proportion of monomer units formed by polymerizing conjugated dienes in diene polymers is not particularly limited, but is, for example, 40% or more by mass in all diene polymers, preferably 50% or more by mass, and more preferably 60% or more by mass.

[0131] The term "dien polymer" is not particularly limited, and examples include homopolymers of conjugated dienes such as polybutadiene and polyisoprene, and copolymers of conjugated dienes with monomers that can be copolymerized. The monomers that can be copolymerized are not particularly limited, and examples include (meth)acrylate monomers described later, and the following monomers (hereinafter also referred to as "other monomers").

[0132] As for "other monomers," there are no specific limitations. Examples include: α,β-unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), itaconic acid, and fumaric acid; styrene monomers such as styrene, chlorostyrene, vinyltoluene, tert-butylstyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylnaphthalene, chloromethylstyrene, hydroxymethylstyrene, α-methylstyrene, and divinylbenzene; olefins such as ethylene and propylene; halogen-containing monomers such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; and so on. Vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether; vinyl ketones such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, and isopropylene vinyl ketone; heterocyclic vinyl compounds such as N-vinylpyrrolidone, vinylpyridine, and vinylimidazolium; acrylate and / or methacrylate compounds such as methyl acrylate and methyl methacrylate; hydroxyalkyl compounds such as β-hydroxyethyl acrylate and β-hydroxyethyl methacrylate; and amide monomers such as acrylamide, N-hydroxymethylacrylamide, and acrylamide-2-methylpropanesulfonic acid, etc., can be used in combination of one or more of these compounds.

[0133] (Acrylic polymer)

[0134] There are no particular limitations on acrylic polymers, but polymers containing monomer units formed by polymerizing (meth)acrylate monomers are preferred.

[0135] When the layer containing the thermoplastic polymer includes an acrylic polymer as the thermoplastic polymer, it is preferably a copolymer containing monomer units of (meth)acrylate monomers.

[0136] If the thermoplastic polymer in the layer containing the thermoplastic polymer comprises a copolymer of monomer units containing (meth)acrylate monomers, the adhesive strength of the separator is improved with low unit area weight, and is therefore preferred.

[0137] It should be noted that in this specification, "(meth)acrylic acid" means "acrylic acid or methacrylic acid", and "(meth)acrylate" means "acrylate or methacrylate".

[0138] As monomers of (meth)acrylates, there are no particular limitations. Examples include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, tetradecyl methacrylate, stearyl methacrylate, and other alkyl methacrylates; hydroxyl-containing (meth)acrylates such as hydroxyl-containing (meth)acrylate, hydroxyl-containing (meth)acrylate, and hydroxyl-containing (meth)acrylate; amino-containing (meth)acrylates such as aminoethyl methacrylate; and epoxy-containing (meth)acrylates such as glycidyl methacrylate (GMA).

[0139] The proportion of monomer units polymerized from (meth)acrylate monomers is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more of the total acrylic polymer. Examples of acrylic polymers include homopolymers of (meth)acrylate monomers and copolymers thereof with monomers that can be copolymerized.

[0140] As copolymerizable monomers, the “other monomers” listed in the above diene polymers can be used, and one or more of them can be used in combination.

[0141] (Fluoropolymers)

[0142] There are no particular limitations on fluorinated polymers; examples include homopolymers of vinylidene fluoride and copolymers thereof with monomers that can be copolymerized. From the viewpoint of electrochemical stability, fluorinated polymers are preferred.

[0143] The proportion of monomer units polymerized from vinylidene fluoride is not particularly limited, but for example, it is 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more.

[0144] There are no particular limitations on the monomers that can copolymerize with vinylidene fluoride. Examples include fluorinated olefin unsaturated compounds such as vinyl fluoride, tetrafluoroethylene, trifluorochloroethylene, hexafluoropropylene, hexafluoroisobutylene, perfluoroacrylic acid, perfluoromethacrylic acid, and fluoroalkyl esters of acrylic acid or methacrylic acid; non-fluorinated olefin unsaturated compounds such as cyclohexyl vinyl ether and hydroxyethyl vinyl ether; and non-fluorinated diene compounds such as butadiene, isoprene, and chloroprene.

[0145] Among fluoropolymers, homopolymers of vinylidene fluoride, vinylidene fluoride / tetrafluoroethylene copolymers, and vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers are preferred. Particularly preferred fluoropolymers are vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers, whose monomer composition typically comprises 30–90% by mass of vinylidene fluoride, 9–50% by mass of tetrafluoroethylene, and 1–20% by mass of hexafluoropropylene. These fluoropolymer particles can be used alone or in mixtures of two or more.

[0146] In addition, monomers having hydroxyl, carboxyl, amino, sulfonic acid, amide, or cyano groups can also be used as monomers for synthesizing the above-mentioned thermoplastic polymers.

[0147] Monomers containing hydroxyl groups are not particularly limited; examples include vinyl monomers such as pentenol.

[0148] Monomers with carboxyl groups are not particularly limited; examples include (meth)acrylic acid, itaconic acid, and other unsaturated carboxylic acids with olefinic double bonds, as well as vinyl monomers such as pentenoic acid.

[0149] There are no particular limitations on monomers containing amino groups; examples include 2-aminoethyl methacrylate.

[0150] Monomers with sulfonic acid groups are not particularly limited, and examples include: vinyl sulfonic acid, methyl vinyl sulfonic acid, (methyl)propane sulfonic acid, styrene sulfonic acid, ethyl (meth)acrylate-2-sulfonate, 2-acrylamide-2-methylpropane sulfonic acid, 3-allyloxy-2-hydroxypropane sulfonic acid, etc.

[0151] Monomers with amide groups are not particularly limited; examples include acrylamide (AM), methacrylamide, N-hydroxymethylacrylamide, and N-hydroxymethylmethacrylamide.

[0152] Monomers containing cyano groups are not particularly limited; examples include acrylonitrile (AN), methacrylonitrile, α-chloroacrylonitrile, and α-cyanoethyl acrylate.

[0153] The thermoplastic polymer used in this embodiment can be used alone or in combination with two or more polymers, but it is preferred to include two or more polymers. The thermoplastic polymer can be used with a solvent, which can uniformly and stably disperse the thermoplastic polymer. Examples of solvents include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, dichloromethane, hexane, etc., with aqueous solvents such as water being preferred. Furthermore, the thermoplastic polymer can be used in latex form.

[0154] (Glass transition temperature of thermoplastic polymers)

[0155] From the viewpoint that the thermoplastic polymer constituting the layer of thermoplastic polymer exhibits good adhesion to the substrate and inhibits adhesion, as well as adhesion between the separator and the electrode, and can ensure the distance between the electrode and the separator in the energy storage device, and shorten the electrolyte injection time, the thermoplastic polymer preferably has the following thermal properties: having at least two glass transition temperatures, at least one of which is located in the region below 20°C, and at least one of which is located in the region above 30°C and below 150°C.

[0156] Here, the glass transition temperature is determined by the DSC curve obtained by differential scanning calorimetry (DSC). It should be noted that, in this disclosure, the glass transition temperature is sometimes expressed as Tg.

[0157] Specifically, the value is determined by the intersection of the straight line extending from the low-temperature side of the DSC curve towards the high-temperature side and the tangent at the inflection point of the step-like change portion of the glass transition. More specifically, refer to the method described in the embodiments.

[0158] Here, "glass transition" refers to the endothermic transition that occurs during DSC, accompanied by a change in the state of the polymer used as a test piece, due to a change in heat. Such a change in heat is observed in the DSC curve as a step-like shape or a combination of a step-like shape and a peak.

[0159] "Step-like variation" refers to the portion of a DSC curve where the curve deviates from the previous baseline and shifts to a new baseline. It should be noted that this also includes shapes formed by a combination of peaks and step-like variations.

[0160] The "inflection point" represents the point where the gradient of the DSC curve is greatest in the step-like change section. Alternatively, it can also be represented as the point where the upward-convex curve in the step-like change section changes to a downward-convex curve.

[0161] A "peak" refers to the portion of a DSC curve that deviates from the baseline and then returns to the baseline.

[0162] The “baseline” represents the DSC curve of the temperature range in which the test piece does not undergo transformation or reaction.

[0163] In this embodiment, by ensuring that at least one of the glass transition temperatures of the thermoplastic polymer used is in the region below 20°C, excellent adhesion to the porous substrate or the layer containing inorganic fillers is achieved, and adhesion is suppressed, resulting in excellent adhesion between the separator and the electrode.

[0164] From the viewpoint of operability and anti-adhesion, the glass transition temperature is preferably -100°C or higher, more preferably -50°C or higher, even more preferably -40°C or higher, or particularly preferably -6°C or higher. From the viewpoint of adhesion to porous substrates or layers containing inorganic fillers, it is preferably 20°C or lower, more preferably 10°C or lower, or particularly preferably 0°C or lower.

[0165] In this embodiment, by using a thermoplastic polymer in which at least one of the glass transition temperatures is in the region of 30°C or higher and 150°C or lower, the adhesion and operability of the separator to the electrode are excellent, thereby maintaining the distance between the electrode surface and the separator substrate surface in the energy storage device and shortening the electrolyte injection time.

[0166] From the viewpoint of operability and anti-adhesion, the glass transition temperature is preferably 30°C or higher, more preferably 40°C or higher, even more preferably 60°C or higher, or particularly preferably 85°C or higher. From the viewpoint of adhesive strength, it is preferably 150°C or lower, more preferably 130°C or lower, or particularly preferably 120°C or lower.

[0167] Thermoplastic polymers can have two glass transition temperatures, for example, by mixing two or more thermoplastic polymers, but are not limited to this method.

[0168] In particular, by combining polymers with high and low glass transition temperatures, the overall glass transition temperature of the thermoplastic polymer can be controlled. Furthermore, various functions can be imparted to the thermoplastic polymer as a whole. For example, in the case of blending, especially by blending two or more polymers with glass transition temperatures above 30°C and below 20°C, both adhesion resistance and coatability for polyolefin microporous membranes can be achieved.

[0169] As for the mixing ratio during blending, the ratio of the polymer having a glass transition temperature in the region above 30°C to the polymer having a glass transition temperature in the region below 20°C is preferably in the range of 0.1:99.9 to 99.9:0.1, more preferably 5:95 to 95:5, even more preferably 50:50 to 95:5, and even more preferably 60:40 to 90:10. Alternatively, a combination of polymers with high viscosity and polymers with high elasticity can be used to control viscoelasticity.

[0170] In this embodiment, the glass transition temperature (Tg) of the thermoplastic polymer can be appropriately adjusted, for example, by changing the monomer composition and the proportion of each monomer used in manufacturing the thermoplastic polymer. That is, it can be roughly estimated from the Tg of the homopolymer of each monomer typically used in the manufacture of the thermoplastic polymer (e.g., as described in a "Polymer Handbook") and the mixing ratio of the monomers. A copolymer with a high ratio of monomers such as styrene, methyl methacrylate, and acrylonitrile, which provide a polymer with a Tg of approximately 100°C, can be obtained; a copolymer with a low Tg can be obtained by high ratios of monomers such as butadiene, which provides a polymer with a Tg of approximately -80°C, and n-butyl acrylate and 2-ethylhexyl acrylate, which provide a polymer with a Tg of approximately -50°C.

[0171] Furthermore, the glass transition temperature (Tg) of the polymer can be estimated using the FOX formula (Formula (1) below). It should be noted that the glass transition temperature of the thermoplastic polymer in this embodiment is the glass transition temperature measured by the DSC method described above.

[0172] 1 / Tg = W1 / Tg1 + W2 / Tg2 + ... + W i / Tg i +···W n / Tg n (1)

[0173] In equation (1), Tg(K) represents the Tg of the copolymer, Tg i (K) represents the Tg of the homopolymer of each monomer i, W i This indicates the mass fraction of each monomer.

[0174] The glass transition temperature of thermoplastic polymers is determined by the following method.

[0175] Take an appropriate amount of the thermoplastic polymer coating solution in an aluminum pan and dry it in a hot air dryer at 130°C for 30 minutes. Place approximately 5 mg of the dried film into an aluminum container for testing, and obtain the DSC and DDSC curves under a nitrogen atmosphere using a DSC measuring apparatus (TA Instruments, DSC Q2000). The testing conditions are as follows.

[0176] (Phase 1 heating process)

[0177] Start at 40°C and increase the temperature at a rate of 50°C per minute. Once it reaches 200°C, maintain this temperature for 5 minutes.

[0178] (Phase 2 cooling procedure)

[0179] Cool from 200°C at a rate of 20°C per minute. Maintain the temperature at -50°C for 5 minutes.

[0180] (Stage 3 warming process)

[0181] The temperature was increased from -50°C to 200°C at a rate of 20°C per minute. DSC and DDSC data were obtained during this third stage of heating.

[0182] According to the method described in JIS-K7121, the intersection of the baseline (the straight line obtained by extending the baseline of the obtained DSC curve towards the high temperature side) and the tangent at the inflection point (the point where the upward convex curve becomes the downward convex curve) is taken as the glass transition temperature (Tg).

[0183] (Structure of layers containing thermoplastic polymers)

[0184] In the layer containing thermoplastic polymer, it is preferable that a thermoplastic resin with a glass transition temperature of 30°C or higher and 150°C or lower is present on the outermost surface side of the separator for the energy storage device, and a thermoplastic resin with a glass transition temperature of 20°C or lower is present on the interface side between the polyolefin microporous membrane and the layer containing thermoplastic polymer. It should be noted that "outermost surface" refers to the surface of the layer containing thermoplastic polymer that contacts the electrode when the separator for the energy storage device is laminated with the electrode. Furthermore, "interface" refers to the surface of the layer containing thermoplastic polymer that contacts the polyolefin microporous membrane.

[0185] In layers containing thermoplastic polymers, the presence of a thermoplastic polymer with a glass transition temperature of 30°C or higher and 150°C or lower on the outermost surface of the separator for energy storage devices results in superior adhesion to the microporous membrane, leading to excellent adhesion between the separator and the electrode. Furthermore, the presence of a thermoplastic polymer with a glass transition temperature of 20°C or lower at the interface between the polyolefin microporous membrane and the thermoplastic polymer-containing layer further enhances the adhesion and operability between the separator and the electrode. Therefore, separators with such thermoplastic polymer-containing layers tend to exhibit even improved adhesion and operability between the separator and the electrode.

[0186] The aforementioned structure can be achieved in the following ways: (a) the thermoplastic polymer comprises particulate thermoplastic polymer and an adhesive polymer that bonds the particulate thermoplastic polymer to the polyolefin microporous membrane while the particulate thermoplastic polymer is exposed on the surface, wherein the glass transition temperature of the particulate thermoplastic polymer is in the region of 30°C or higher and 150°C or lower, and a thermoplastic polymer with a glass transition temperature of 20°C or lower is present at the interface between the polyolefin microporous membrane and the layer containing the thermoplastic polymer; (b) the thermoplastic polymer is a laminated structure, wherein the thermoplastic polymer that forms the outermost layer when the separator is made has a glass transition temperature in the region of 30°C or higher and 150°C or lower, and a thermoplastic polymer with a glass transition temperature of 20°C or lower is present at the interface between the polyolefin microporous membrane and the layer containing the thermoplastic polymer, etc. It should be noted that (b) the thermoplastic polymer can be a laminated structure of each polymer with a different Tg.

[0187] (Particle size of thermoplastic polymers)

[0188] The structure of the thermoplastic polymer in this embodiment is not particularly limited; for example, it can be configured as granules. Having such a structure tends to improve the adhesion between the separator and the electrode, as well as the operability of the separator. Here, "granular" refers to the state in which each thermoplastic polymer has an outline during scanning electron microscopy (SEM) measurements; it can be elongated, spherical, polygonal, etc.

[0189] The particle size distribution and D10, D50, and D90 of the granular thermoplastic polymer were obtained by measuring the thermoplastic polymer particle dispersion using a laser particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Corporation). The particle size distribution of the thermoplastic polymer particle dispersion can be adjusted as needed, using the particle size distribution of the dispersion solvent or binder polymer as a baseline. The particle sizes with cumulative frequencies of 10%, 50%, and 90% were set as the average volumetric particle size D10, D50, and D90 of the thermoplastic polymer particles, respectively.

[0190] In this embodiment, the particle size of the thermoplastic polymer contained in the layer containing the thermoplastic polymer preferably satisfies the relationship 1.0≤D90 / D10≤5.0, more preferably satisfies the relationship 1.0≤D90 / D10≤3.0, and even more preferably satisfies the relationship 1.0≤D90 / D10≤2.0.

[0191] When the particle size ratio of the thermoplastic polymer particles in the layer containing the thermoplastic polymer is set within a specified range, the particle size distribution of the thermoplastic polymer can be kept constant, the friction and contact area between the thermoplastic polymer and the inorganic filler can be controlled, and the generation of static electricity can be suppressed, which is therefore preferred.

[0192] In the particle size distribution of the slurry containing thermoplastic polymers, the average particle size D90 of the thermoplastic polymer particles is preferably 0.5 μm or more and 1.5 μm or less, more preferably 0.5 μm or more and 1.0 μm or less. From the viewpoint of ensuring good ion permeability of the separator, D90 is preferably 0.5 μm or more, and from the viewpoint of preventing the sedimentation of thermoplastic polymer particles when the slurry is left to stand, D90 is preferably 1.5 μm or less.

[0193] In the particle size distribution of the slurry containing the thermoplastic polymer, the average particle size D50 of the thermoplastic polymer particles is preferably 0.3 μm or more and 1.5 μm or less, more preferably 0.5 μm or more and 1.0 μm or less, and even more preferably 0.5 μm or more and 0.7 μm or less. From the viewpoint of improving the anchoring strength with the electrode surface and exhibiting high adhesion, a D50 of 0.3 μm or more is preferred, and from the viewpoint of improving the tightness with the electrode surface and exhibiting high adhesion, a D50 of 1.5 μm or less is preferred.

[0194] In the particle size distribution of the slurry containing the thermoplastic polymer, the average particle size D10 of the thermoplastic polymer particles is preferably 0.2 μm or more and 1.0 μm or less, more preferably 0.3 μm or more and 0.5 μm or less. From the viewpoint of preventing thermoplastic polymer particles from entering the pores of the porous substrate and thus hindering ion permeation, D10 is preferably 0.2 μm or more, and from the viewpoint of improving the dot-forming properties of the thermoplastic polymer particles, D10 is preferably 1.0 μm or less.

[0195] (Weight per unit area of ​​each single side of the layer containing the thermoplastic polymer)

[0196] In the separator of this embodiment, from the viewpoint of balancing adhesion to the electrode and ion permeability, the unit area weight of the thermoplastic polymer-containing layer is preferably 0.03 g / m² per single side. 2 Above and 0.50g / m 2 The following is more preferably 0.04 g / m 2 Above and 0.45g / m 2 The optimal value is 0.06 g / m³. 2 Above and 0.40g / m 2 the following.

[0197] The weight per unit area of ​​the layer containing the thermoplastic polymer can be adjusted by changing the polymer concentration of the coating liquid and the coating amount of the polymer solution. From the viewpoint of suppressing battery shape deformation accompanying electrode expansion and contraction and thus improving battery cycle characteristics, a weight of 0.06 g / m² is preferred without impairing the effectiveness of this embodiment. 2 The above range.

[0198] [Substrate]

[0199] The separator requires both insulation and ion permeability; therefore, the separator substrate (hereinafter referred to as porous substrate or substrate) is typically formed from insulating materials such as paper, nonwoven fabric made of polyolefin, or microporous membrane made of resin, which are porous insulating materials. In particular, for separator substrates used in energy storage devices such as non-aqueous secondary batteries that have positive and negative electrodes capable of absorbing and releasing lithium, and non-aqueous electrolytes formed by dissolving electrolytes in non-aqueous solvents, polyolefin microporous membranes with redox resistance and the ability to form a dense and uniform porous structure are preferred.

[0200] (Polyolefin microporous membrane)

[0201] The polyolefin microporous membrane used in this embodiment is not particularly limited. For example, a microporous membrane composed of a polyolefin resin composition containing polyolefin can be cited, but a microporous membrane with polyolefin resin as the main component is preferred. The content of polyolefin resin in the polyolefin microporous membrane of this embodiment is not particularly limited. From the perspective of closing performance when used as a separator in an energy storage device, a microporous membrane formed of a polyolefin resin composition in which polyolefin resin accounts for 50% or more and 100% or less of the total mass fraction of the components constituting the microporous membrane is preferred. The proportion of polyolefin resin is more preferably 60% or more and 100% or less, and even more preferably 70% or more and 100% or less.

[0202] Polyolefin resin is not particularly limited and refers to polyolefin resins commonly used in extrusion, injection, blow molding, and blow molding processes. Homopolymers and copolymers, as well as multi-stage polymers, of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene can be used. In addition, polyolefins selected from the group consisting of these homopolymers, copolymers, and multi-stage polymers can be used alone or in combination.

[0203] Examples of polyolefin resins are not specifically limited to these types; for example, low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, ultra-high molecular weight polyethylene, etc.; isotactic polypropylene, atactic polypropylene, etc.; ethylene-propylene atactic copolymer; polybutene; ethylene propylene rubber, etc.

[0204] When the separator of this embodiment is used as a battery separator, it is preferable to use polyethylene as the main component due to its low melting point and high strength, and it is particularly preferable to use a resin with high-density polyethylene as the main component.

[0205] Furthermore, from the viewpoint of improving the heat resistance of microporous membranes, it is more preferable to use microporous membranes formed from resin compositions comprising polypropylene and polyolefin resins other than polypropylene. Here, the stereostructure of the polypropylene is not limited, and it can be any of isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene.

[0206] The proportion of polypropylene relative to the total polyolefins in the polyolefin resin composition is not particularly limited, but from the viewpoint of balancing heat resistance and good shut-off function, it is preferably 1 to 35% by mass, more preferably 3 to 20% by mass, and even more preferably 4 to 10% by mass. In this case, there is no limitation on the polyolefin resin other than polypropylene; examples include homopolymers or copolymers of olefin hydrocarbons such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Specifically, examples include polyethylene, polybutene, and ethylene-propylene random copolymers.

[0207] From the viewpoint of the pore-closing properties through hot melting, polyethylene other than polypropylene is preferably used, including low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, and ultra-high molecular weight polyethylene. From the viewpoint of strength, polyethylene with a density of 0.93 g / cm³ as measured according to JIS K 7112 is more preferred. 3 Above and 0.97 g / cm 3 The following polyethylene.

[0208] The viscosity-average molecular weight of the polyolefin resin constituting the polyolefin microporous membrane is not particularly limited, but is preferably 30,000 or more and 12 million or less, more preferably 50,000 or more and less than 2 million, further preferably 100,000 or more and less than 1.2 million, and most preferably 500,000 or more and less than 1 million. If the viscosity-average molecular weight of the polyolefin resin is 30,000 or more, the melt tension during melt molding increases, resulting in better formability, and the polymers tend to have high strength due to entanglement, making it preferred. On the other hand, when the viscosity-average molecular weight of the polyolefin resin is 12 million or less, it is easy to uniformly melt-mix, and it tends to have excellent sheet formability, especially thickness stability, making it preferred. Furthermore, when the viscosity-average molecular weight of the polyolefin resin is less than 1 million, it tends to easily clog pores when the temperature rises, resulting in good pore-closing function, making it preferred. It should be noted that, for example, a mixture of a polyolefin with a viscosity-average molecular weight of 2 million and a polyolefin with a viscosity-average molecular weight of 270,000 can be used, with the viscosity-average molecular weight of the mixture being less than 1 million, instead of using a polyolefin with a viscosity-average molecular weight of less than 1 million alone.

[0209] The polyolefin microporous membrane in this embodiment may contain optional additives. Such additives are not particularly limited, and examples include polymers other than polyolefins; inorganic particles; antioxidants such as phenolic, phosphorus-based, and sulfur-based agents; metallic soaps such as calcium stearate and zinc stearate; ultraviolet absorbers; light stabilizers; antistatic agents; antifogging agents; and coloring pigments. The total content of these additives relative to 100 parts by weight of the polyolefin resin composition is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less.

[0210] (Physical properties of polyolefin microporous membranes)

[0211] The conversion of polyolefin microporous membranes (in one case, PO microporous membranes) to weight per unit area (g / m²) 2 The preferred puncture strength (hereinafter referred to as the puncture strength converted to unit area weight) is 50 gf / (g / m²). 2 ) or above or 60gf / (g / m 2 ) or above. It has 50gf / (g / m³) 2) or above or 60gf / (g / m 2 PO microporous membranes with a puncture strength per unit area weight of 70 gf / (g / m²) tend to be less prone to breakage in impact tests of energy storage devices. From the viewpoint of improving the safety of energy storage devices, such as impact resistance, while maintaining the strength of the PO microporous membrane, a puncture strength per unit area weight of 70 gf / (g / m²) is more preferable. 2 ) or higher, and more preferably 80 gf / (g / m 2 The above is not limited to the conversion of puncture intensity per unit area weight; for example, it can be 200 gf / (g / m²). 2 Below ) or 150gf / (g / m 2 Below ) or 140gf / (g / m 2 )the following.

[0212] Regarding the puncture strength (hereinafter referred to as puncture strength) of the PO microporous membrane, which is not converted to a unit area weight, the lower limit is preferably 100 gf or more (preferably 0.98 N or more), more preferably 200 gf or more, and even more preferably 300 gf or more. From the viewpoint of suppressing the breakage of the PO microporous membrane in impact tests, a puncture strength of 100 gf or more is preferred. In addition, from the viewpoint of stability during membrane formation, the upper limit of the puncture strength of the PO microporous membrane is preferably 1000 gf or less, more preferably 800 gf or less, and even more preferably 700 gf or less. The lower limit can be used as long as it is a value that can achieve stable production of membrane formation and battery manufacturing. The upper limit is set according to the balance with other characteristics. The puncture strength can be increased by the shear force applied to the molded article during extrusion or by the increase in molecular chain orientation caused by stretching, but with the increase of strength, the thermal stability deteriorates with the increase of residual stress, so it is controlled according to the purpose.

[0213] The weight per unit area of ​​the polyolefin microporous membrane in this embodiment is not particularly limited, but is preferably 2.8 g / m³. 2 The above, and more preferably 3.5g / m 2 The above, and more preferably 4.0 g / m 2 The preferred value is 6.4 g / m³. 2 The following, or more preferably, is 5.4 g / m 2 The following, and more preferably, is 4.8 g / m 2 the following.

[0214] The porosity of the polyolefin microporous membrane in this embodiment is not particularly limited, but is preferably 20% or more, more preferably 35% or more, even more preferably 40% or more, particularly preferably 45% or more, preferably 80% or less, more preferably 60% or less, and even more preferably 55% or less.

[0215] From the viewpoint of ensuring the permeability of the separator, it is preferable to set the porosity of the polyolefin microporous membrane to 20% or more. On the other hand, from the viewpoint of ensuring puncture strength, it is preferable to set the porosity of the polyolefin microporous membrane to 80% or less. It should be noted that the porosity of the polyolefin microporous membrane can be adjusted by changing the stretch ratio, etc.

[0216] The thickness of the polyolefin microporous membrane in this embodiment is not particularly limited, but is preferably 2 μm or more, more preferably 4.5 μm or more, even more preferably 5.5 μm or more, and particularly preferably 6 μm or more. The thickness of the polyolefin microporous membrane is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 16 μm or less, particularly preferably 12 μm or less, and most preferably 9 μm or less.

[0217] From the viewpoint of improving mechanical strength, it is preferable to set the thickness of the polyolefin microporous membrane to 2 μm or more. On the other hand, when the thickness of the polyolefin microporous membrane is set to 30 μm or less, the volume occupied by the separator is reduced, which tends to be advantageous in terms of increasing battery capacity, and is therefore preferred.

[0218] The air permeability of the polyolefin microporous membrane in this embodiment is not particularly limited, but is preferably 10 sec / 100cm. 3 The above, and more preferably, is 20 sec / 100cm 3 The above, and more preferably 30 sec / 100cm 3 The above, and more preferably, is 90 sec / 100 cm. 3 The above, and the optimal value, is 100 sec / 100 cm. 3 The above. The preferred air permeability of the polyolefin microporous membrane is 300 sec / 100 cm. 3 The following is more preferably 200 sec / 100 cm 3 The following is a further preferred value: 180 sec / 100 cm 3 The following is particularly preferred: 140 sec / 100 cm 3 the following.

[0219] From the perspective of suppressing the self-discharge of the energy storage device, it is preferable to set the air permeability of the polyolefin microporous membrane to 10 sec / 100 cm. 3 That's all. On the other hand, from the viewpoint of obtaining good charge-discharge characteristics, it is preferable to have the air permeability of the polyolefin microporous membrane be 300 sec / 100 cm. 3 It should be noted that the above-mentioned air permeability can be adjusted by changing the stretching temperature and stretch ratio.

[0220] In this embodiment, the average pore size of the polyolefin microporous membrane is preferably 0.15 μm or less, more preferably 0.1 μm or less. The average pore size of the polyolefin microporous membrane is preferably 0.01 μm or more.

[0221] When manufacturing a separator for an energy storage device, from the viewpoint of suppressing self-discharge of the energy storage device and suppressing capacity reduction, it is preferable to set the average pore size of the polyolefin microporous membrane to 0.15 μm or less.

[0222] Furthermore, when the average pore size of the polyolefin microporous membrane is within the aforementioned range, the contact angle of the adhesive coating liquid with the surface of the substrate containing the thermoplastic polymer layer or the surface of the layer containing the inorganic filler (in one embodiment, the coating surface of the thermoplastic polymer) can be controlled within the range specified in this application, which is therefore preferable. The average pore size can be adjusted by changing the stretch ratio during the manufacture of the polyolefin microporous membrane, etc.

[0223] The short-circuit temperature, which serves as an indicator of the heat resistance of the polyolefin microporous membrane in this embodiment, is preferably 140°C or higher, more preferably 150°C or higher, and even more preferably 160°C or higher. When manufacturing a separator for an energy storage device, from the viewpoint of the safety of the energy storage device, it is preferable to set the short-circuit temperature to 140°C or higher.

[0224] The viscosity-average molecular weight of the polyolefin microporous membrane in this embodiment is not particularly limited, but is preferably 100,000 or more and 5,000,000 or less, more preferably 300,000 or more and 1,500,000 or less, and even more preferably 500,000 or more and 1,000,000 or less. When the viscosity-average molecular weight of the polyolefin microporous membrane is 100,000 or more and 5,000,000 or less, it is preferred from the viewpoint of the polyolefin microporous membrane's puncture strength, permeability, thermal shrinkage, and shut-off function.

[0225] (Manufacturing method of polyolefin microporous membrane)

[0226] The method for manufacturing the polyolefin microporous membrane of this embodiment is not particularly limited, and known manufacturing methods can be used. Examples include: a method in which a polyolefin resin composition and a plasticizer are melt-blended and formed into a sheet, then stretched as needed, and the plasticizer is extracted to achieve porosity; a method in which a polyolefin resin composition is melt-blended and extruded at a high draw ratio, and the polyolefin crystal interface is peeled off by heat treatment and stretching, thereby achieving porosity; a method in which a polyolefin resin composition and an inorganic filler are melt-blended and formed onto a sheet, and the interface between the polyolefin and the inorganic filler is peeled off by stretching, thereby achieving porosity; and a method in which a polyolefin resin composition is dissolved, impregnated in a solvent unsuitable for polyolefins, the polyolefin is solidified, and the solvent is removed, thereby achieving porosity, etc.

[0227] The following is an example of a method for manufacturing microporous membranes: a method for extracting plasticizer after melt-blending a polyolefin resin composition and a plasticizer to form a sheet.

[0228] First, the polyolefin resin composition and plasticizer are melt-blended. Examples of melt-blending methods include: feeding the polyolefin resin and other desired additives into a resin mixing apparatus such as an extruder, kneader, LABO PLASTOMILL, mixing roller, or Banbury mixer; and mixing by introducing the plasticizer at an arbitrary ratio while heating and melting the resin components. Preferably, the polyolefin resin, other additives, and plasticizer are pre-blended at a predetermined ratio using a Henschel mixer or similar equipment before being fed into the resin mixing apparatus. More preferably, only a portion of the plasticizer is added during pre-blending, while the remaining plasticizer is fed into the resin mixing apparatus. This improves the dispersibility of the plasticizer, allowing for high-ratio stretching without film breakage when stretching the sheet-like shape of the melt-blended mixture of resin composition and plasticizer in subsequent processes.

[0229] As a plasticizer, a non-volatile solvent capable of forming a homogeneous solution above the melting point of the polyolefin can be used. Specific examples of such non-volatile solvents include hydrocarbons such as liquid paraffin and paraffin wax; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol. Among these, liquid paraffin has high compatibility with polyethylene and polypropylene, and even when the melt-blended compound is stretched, interfacial delamination between the polyolefin resin composition and the plasticizer is less likely to occur, thus it tends to facilitate uniform stretching and is therefore preferred.

[0230] The ratio of the polyolefin resin composition to the plasticizer is not particularly limited as long as it allows for uniform melt mixing and molding into sheets. For example, in a composition containing both the polyolefin resin composition and the plasticizer, the mass fraction of the plasticizer is preferably 30 to 80% by mass, more preferably 40 to 70% by mass. When the mass fraction of the plasticizer is 80% by mass or less, there is a tendency for insufficient melt tension during melt molding and improved formability. On the other hand, when the mass fraction of the plasticizer is 30% by mass or more, even when the mixture of the polyolefin resin composition and the plasticizer is stretched at a high ratio, the polyolefin chains are not cleaved, resulting in a uniform and fine porous structure and increased strength.

[0231] Next, the molten compound is formed into a sheet. One method for manufacturing the sheet is to extrude the molten compound into a sheet using a T-die, bring it into contact with a heat conductor, and cool it to a temperature sufficiently lower than the crystallization temperature of the resin component to solidify it. The heat conductor used for cooling and solidification can be metal, water, air, or the plasticizer itself; metal rollers are preferred due to their high thermal conductivity. Furthermore, when in contact with a metal roller, if the sheet is sandwiched between the rollers, the efficiency of heat transfer is further improved, the sheet becomes oriented, the film strength increases, and the surface smoothness of the sheet is also improved; therefore, this is even more preferable. The die lip spacing during sheet extrusion from the T-die is preferably 400 μm or more and 3000 μm or less, more preferably 500 μm or more and 2500 μm or less. When the die lip spacing is 400 μm or more, die buildup is reduced, the impact of streaks and defects on film quality is less, and the tendency for film breakage can be prevented during subsequent stretching processes. On the other hand, if the die lip spacing is less than 3000μm, there is a tendency for rapid cooling, prevention of uneven cooling, and maintenance of sheet thickness stability.

[0232] It is preferable to stretch the sheet-like material thus obtained. As a stretching process, uniaxial stretching or biaxial stretching can be used appropriately; from the viewpoint of the strength of the resulting microporous membrane, biaxial stretching is preferred. If the sheet-like material is stretched at a high ratio along the biaxial direction, the molecules are oriented along the planar direction, resulting in a microporous membrane that is less prone to rupture and has high puncture strength. Examples of stretching methods include simultaneous biaxial stretching, successive biaxial stretching, multi-segment stretching, and multiple stretching. From the viewpoints of improved puncture strength, uniform stretching, and closure properties, simultaneous biaxial stretching is preferred.

[0233] It should be noted that, in this context, simultaneous biaxial stretching refers to a stretching method that simultaneously performs stretching in the MD direction (the mechanical direction of the microporous membrane) and the TD direction (the direction that crosses the MD of the microporous membrane at a 90° angle), and the stretching ratios in each direction can be different. Successive biaxial stretching refers to a stretching method that independently performs stretching in the MD direction or the TD direction, where, while stretching in the MD or TD direction, the other direction is either unrestrained or fixed to a fixed length.

[0234] The stretching ratio, measured in terms of area ratio, is preferably in the range of 20 times or more and 100 times or less, and more preferably in the range of 25 times or more and 50 times or less. The stretching ratio in each axial direction is preferably in the range of 4 times or more and 10 times or less in the MD direction and 4 times or more and 10 times or less in the TD direction, and more preferably in the range of 5 times or more and 8 times or less in the MD direction and 5 times or more and 8 times or less in the TD direction. When the total area ratio is 20 times or more, there is a tendency to impart sufficient strength to the obtained microporous membrane; on the other hand, when the total area ratio is 100 times or less, there is a tendency to prevent membrane breakage during the stretching process and obtain high productivity.

[0235] Alternatively, the sheet-shaped body can be calendered. Calendering can be performed, for example, by using a pressure method employing a dual-belt press. Calendering, in particular, can increase the orientation of the surface portion. The calendering ratio is preferably greater than 1 and less than 3, more preferably greater than 1 and less than 2. When the calendering ratio is greater than 1, there is a tendency for increased surface orientation and increased film strength of the resulting microporous film. On the other hand, if the calendering ratio is less than 3, the orientation difference between the surface portion and the central interior is small, and there is a tendency to form a uniform porous structure in the thickness direction of the film, which is therefore preferred.

[0236] Next, the plasticizer is removed from the sheet-shaped body to form a microporous membrane. One method for removing the plasticizer is, for example, immersing the sheet-shaped body in an extraction solvent to extract the plasticizer and then thoroughly drying it. The method for extracting the plasticizer can be either batch or continuous. To suppress shrinkage of the microporous membrane, it is preferable to constrain the ends of the sheet-shaped body during the immersion and drying process. Furthermore, the residual amount of plasticizer in the microporous membrane is preferably less than 1% by mass.

[0237] As the extraction solvent, it is preferable to use a solvent that is a poor solvent for the polyolefin resin composition but a good solvent for the plasticizer, and whose boiling point is lower than the melting point of the polyolefin resin. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as dichloromethane and 1,1,1-trichloroethane; non-chlorinated halogenated solvents such as hydrofluoroethers and hydrofluorocarbons; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. It should be noted that these extraction solvents can be recovered and reused through operations such as distillation.

[0238] To suppress the shrinkage of the microporous membrane, heat treatments such as heat setting or heat relaxation can be performed after the stretching process or after the microporous membrane is formed. Additionally, post-treatments such as hydrophilization using surfactants or cross-linking using ionizing radiation can be applied to the microporous membrane.

[0239] [Layer containing inorganic fillers]

[0240] Furthermore, the separator for the energy storage device in this embodiment may include a layer containing inorganic filler and a resin-based binder (in this embodiment, the layer containing inorganic filler is sometimes referred to as a porous layer). The location of the layer containing inorganic filler may include at least a portion of the surface of the polyolefin microporous membrane, at least a portion of the surface of the layer containing a thermoplastic polymer, and / or between the polyolefin microporous membrane and the layer containing a thermoplastic polymer.

[0241] In one embodiment, the inorganic filler-containing layer is located between the polyolefin microporous membrane and the thermoplastic polymer-containing layer. The separator in this embodiment may have an inorganic filler-containing layer on one and / or both sides of the polyolefin microporous membrane.

[0242] (Inorganic packing)

[0243] The inorganic filler used in the above-mentioned inorganic filler-containing layer is not particularly limited, but preferably has a melting point of over 200°C, high electrical insulation, and electrochemical stability within the operating range of lithium-ion secondary batteries.

[0244] Materials used as inorganic fillers include, for example, oxide ceramics such as alumina, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, cerium dioxide, yttrium oxide, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, barium sulfate, aluminum hydroxide, aluminum hydroxide, boehmite, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, magnesia chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers. From the viewpoint of stability within lithium-ion secondary batteries, at least one material from the group consisting of alumina, boehmite, and barium sulfate is preferred. Furthermore, as the boehmite, a synthetic boehmite that can reduce ionic impurities that adversely affect the characteristics of electrochemical elements is preferred.

[0245] Examples of inorganic filler shapes include plate-like, scaly, polyhedral, needle-like, columnar, granular, spherical, spindle-shaped, and block-like shapes. Multiple inorganic fillers with these shapes can also be used in combination. From the viewpoint of balancing permeability and heat resistance, block-like shapes are preferred.

[0246] The aspect ratio of the inorganic filler is preferably 1.0 or higher and 5.0 or lower, more preferably 1.1 or higher and 3.0 or lower. Setting the aspect ratio of the inorganic filler to 5.0 or lower is preferable from the viewpoints of suppressing the amount of moisture adsorbed by the multilayer porous membrane (in one embodiment, a layer containing the inorganic filler and a polyolefin microporous membrane), suppressing capacity degradation during repeated cycles, and suppressing deformation of the polyolefin microporous membrane at temperatures exceeding its melting point.

[0247] The preferred specific surface area for inorganic fillers is 3.0 m². 2 / g or more and 17m 2 / g or less, preferably 5.0m 2 / g or more and 15m 2 / g or less, more preferably 6.5m 2 / g or more and 13m 2 / g or less.

[0248] From the perspective of suppressing the water adsorption of multilayer porous membranes and inhibiting capacity degradation during repeated cycles, an inorganic filler with a specific surface area of ​​17 m² is preferred. 2 / g or less. This is achieved by making the specific surface area of ​​the inorganic filler 3.0m². 2 The specific surface area of ​​the inorganic filler is preferred from the viewpoint of suppressing deformation of the polyolefin microporous membrane at temperatures exceeding its melting point. The specific surface area of ​​the inorganic filler was determined using the BET adsorption method.

[0249] In this embodiment, the particle size of the inorganic filler in the layer containing inorganic filler preferably satisfies the relationship 1.0≤D90 / D10≤5.0, and more preferably satisfies the relationship 2.0≤D90 / D10≤4.0.

[0250] When the particle size ratio of the inorganic filler in the layer containing inorganic filler is set to a specified range, the friction and contact area between the thermoplastic polymer and the inorganic filler can be controlled by keeping the particle size distribution of the inorganic filler constant, thereby suppressing the generation of static electricity, which is therefore preferred.

[0251] Methods for adjusting the particle size distribution of inorganic fillers to the above-mentioned range include, for example, pulverizing the inorganic fillers using a ball mill, bead mill, air jet mill, etc., to obtain the desired particle size distribution; and preparing fillers with multiple particle size distributions and then blending them.

[0252] In the particle size distribution of the slurry containing inorganic fillers, the average particle size D90 of the inorganic filler particles is preferably 0.1 μm or more and 2.5 μm or less, more preferably 0.3 μm or more and 1.5 μm or less, and even more preferably 0.50 μm or more and 1.0 μm or less. From the viewpoint of ensuring good ion permeability of the separator, it is preferable that the average particle size D90 of the inorganic filler particles is 0.1 μm or more, and from the viewpoint of ensuring good heat resistance of the separator, it is preferable that D90 is 2.5 μm or less.

[0253] In the particle size distribution of the slurry containing inorganic fillers, the average particle size D50 of the inorganic filler particles is preferably 0.10 μm or more and 1.50 μm or less, more preferably 0.20 μm or more and 1.0 μm or less, and even more preferably 0.40 μm or more and 0.70 μm or less.

[0254] From the viewpoint of improving battery resistance by suppressing the intrusion of inorganic fillers into the pores of the substrate and suppressing capacity degradation during repeated cycles, it is preferred that the average particle size D50 of the inorganic filler particles is 0.10 μm or more. From the viewpoint of easily forming a thin layer containing inorganic fillers, increasing battery capacity and suppressing the deterioration of rate characteristics, it is preferred that the average particle size D50 of the inorganic filler particles is 1.50 μm or less.

[0255] In the particle size distribution of the slurry containing inorganic fillers, the average particle size D10 of the inorganic filler particles is preferably 0.08 μm or more and 0.80 μm or less, more preferably 0.09 μm or more and 0.50 μm or less, and even more preferably 0.20 μm or more and 0.35 μm or less. Having an average particle size D10 of 0.08 μm or more is preferred from the viewpoint of suppressing the amount of water adsorption in the multilayer porous membrane and suppressing capacity degradation during repeated cycles. Having an average particle size D10 of 0.80 μm or less is preferred from the viewpoint of suppressing the deformation of the polyolefin microporous membrane at temperatures exceeding its melting point.

[0256] The particle size distribution and D10, D50, and D90 of the inorganic filler particles were obtained by measuring the inorganic filler particle dispersion using a laser particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Corporation). As needed, the particle size distribution of the inorganic filler particle dispersion can be adjusted using the particle size distribution of the solvent or binder polymer in the inorganic filler particle dispersion as a baseline. The particle size at a cumulative frequency of 10% was defined as the average volumetric particle size D10 of the inorganic filler particles, the particle size at a cumulative frequency of 50% was defined as the average volumetric particle size D50, and the particle size at a cumulative frequency of 90% was defined as the average volumetric particle size D90.

[0257] The proportion of inorganic filler in the inorganic filler layer can be appropriately determined from the perspectives of the inorganic filler's tightness, the permeability of the multilayer porous membrane, and its heat resistance. It is preferably 50% by mass or more and less than 100% by mass, more preferably 70% by mass or more and less than 99.99% by mass, further preferably 80% by mass or more and less than 99.9% by mass, and particularly preferably 90% by mass or more and less than 99% by mass.

[0258] (Resin-based adhesives)

[0259] There is no particular limitation on the type of resin-based adhesive. When using the multilayer porous membrane in this embodiment as a separator for lithium-ion secondary batteries, it is preferable to use an adhesive that is insoluble in the electrolyte of lithium-ion secondary batteries and is electrochemically stable within the operating range of lithium-ion secondary batteries.

[0260] Specific examples of resin-based adhesives include the following 1) to 7).

[0261] 1) Polyolefins: such as polyethylene, polypropylene, ethylene propylene rubber, and their modifiers;

[0262] 2) Conjugated diene polymers: such as styrene-butadiene copolymers and their hydrides, acrylonitrile-butadiene copolymers and their hydrides, acrylonitrile-butadiene-styrene copolymers and their hydrides;

[0263] 3) Acrylic polymers: such as methacrylate-acrylate copolymers, styrene-acrylate copolymers, and acrylonitrile-acrylate copolymers;

[0264] 4) Polyvinyl alcohol-based resins: such as polyvinyl alcohol and polyvinyl acetate;

[0265] 5) Fluorinated resins: such as polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer;

[0266] 6) Cellulose derivatives: such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose;

[0267] 7) Resins with a melting point and / or glass transition temperature of 180°C or higher, or polymers that do not have a melting point but have a decomposition temperature of 200°C or higher: for example, polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, polyester.

[0268] From the viewpoint of further improving safety during short circuits, 3) acrylic polymers, 5) fluorinated resins, and 7) polyamides as polymers are preferred. As polyamides, from the viewpoint of durability, fully aromatic polyamides are preferred, with poly(m-phenylene isophthalamide) being the most preferred.

[0269] From the viewpoint of suitability of resin-based binders and electrodes, the above-mentioned 2) conjugated diene polymer is preferred, and from the viewpoint of voltage resistance, the above-mentioned 3) acrylic polymer and 5) fluorinated resin are preferred.

[0270] The conjugated diene polymers mentioned above (2) are polymers that contain conjugated diene compounds as monomer units.

[0271] Examples of the aforementioned conjugated diene compounds include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadienes, and substituted and side-chain conjugated hexadienes. One type may be used alone, or two or more may be used in combination. 1,3-butadiene is particularly preferred.

[0272] The acrylic polymer described in 3) above is a polymer containing a (meth)acrylic acid compound as a monomer unit. The (meth)acrylic acid compound described above represents at least one selected from the group consisting of (meth)acrylic acid and (meth)acrylates.

[0273] Examples of (meth)acrylates used in the acrylic polymers described in section 3) above include alkyl (meth)acrylates, such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate; epoxy-containing (meth)acrylates, such as glycidyl acrylate and glycidyl methacrylate, may be used alone or in combination of two or more. Among these, 2-ethylhexyl acrylate (EHA) and butyl acrylate (BA) are particularly preferred.

[0274] From a safety perspective in crash testing, acrylic polymers are preferably polymers containing EHA or BA as major structural units. The major structural unit refers to the polymer fraction corresponding to monomers comprising at least 40 mol% of all raw materials used to form the polymer.

[0275] The conjugated diene polymers (2) and acrylic polymers (3) mentioned above can also be polymers obtained by copolymerizing with other monomers that can copolymerize with them. Examples of other copolymerizable monomers include: unsaturated alkyl carboxylic acid esters, aromatic vinyl monomers, cyanide vinyl monomers, unsaturated monomers containing hydroxyl alkyl groups, unsaturated carboxylic acid amide monomers, crotonic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, etc. These can be used individually or in combination of two or more. Among the above, unsaturated alkyl carboxylic acid ester monomers are particularly preferred. Examples of unsaturated alkyl carboxylic acid ester monomers include dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconic acid, monomethyl fumarate, monoethyl fumarate, etc. These can be used individually or in combination of two or more.

[0276] It should be noted that the above-mentioned 2) conjugated diene polymer can also be a polymer obtained by copolymerizing the above-mentioned (meth)acrylic acid compound as other monomers.

[0277] From the viewpoint that the cohesive force between multiple inorganic particles is strong even at high temperatures above room temperature and that thermal shrinkage is suppressed, resin-based adhesives are preferably in the form of latex, and more preferably latex of acrylic polymers.

[0278] The average particle size of the resin-based binder is preferably 50 nm or more and 500 nm or less, more preferably 60 nm or more and 460 nm or less, and even more preferably 80 nm or more and 250 nm or less. When the average particle size of the resin-based binder is 50 nm or more, when layers containing inorganic fillers and resin-based binders are stacked on at least one side of a polyolefin microporous membrane, ion permeability is not easily reduced, and high output characteristics are easily obtained. In addition, even under conditions of rapid temperature rise during abnormal heating, smooth shut-off characteristics are exhibited, and high safety is easily obtained. When the average particle size of the resin-based binder is 500 nm or less, good adhesion is exhibited, and when multilayer porous membranes are formed, there is a tendency for good thermal shrinkage and excellent safety.

[0279] The average particle size of resin-based binders can be controlled by adjusting polymerization time, polymerization temperature, raw material composition ratio, raw material input sequence, pH, etc.

[0280] To improve dispersion stabilization or coating properties, dispersants such as surfactants can be added to the inorganic filler coating solution. The dispersant adsorbs onto the surface of the inorganic filler particles in the slurry, stabilizing the particles through electrostatic repulsion, etc. Examples of dispersants include polycarboxylates, sulfonates, and polyoxyethers. The amount of dispersant added is preferably 0.2 parts by weight or more and 5.0 parts by weight or less, and more preferably 0.3 parts by weight or more and 1.0 parts by weight or less, based on solid content, relative to 100 parts by weight of the inorganic filler.

[0281] (Physical properties, structure, and formation methods of layers containing inorganic fillers)

[0282] The thickness of the layer containing inorganic filler is preferably 0.1 μm or more and 4.0 μm or less, more preferably 0.2 μm or more and 3.0 μm or less, even more preferably 0.5 μm or more and 2.0 μm or less, and particularly preferably 1.0 μm or more and 1.5 μm or less. From the viewpoint of preventing performance and safety deterioration due to micro-short circuits caused by the inability to resist the shrinkage stress of the substrate during storage tests, and from the viewpoint of suppressing the deformation of the microporous membrane at temperatures exceeding the melting point, a thickness of 0.1 μm or more for the layer containing inorganic filler is preferred. From the viewpoint of increasing battery capacity and suppressing the deterioration of rate characteristics, and from the viewpoint of suppressing the amount of moisture adsorbed by the multilayer porous membrane, a thickness of 4.0 μm or less for the layer containing inorganic filler is preferred.

[0283] It should be noted that the thickness of the layer containing inorganic filler was measured using the method described in the examples.

[0284] The preferred layer density in the inorganic filler layer is 1.10 g / (m³). 2 ·μm) or higher and 3.00g / (m 2 ·μm or less, more preferably 1.20 g / (m 2 ·μm) or higher and 2.90g / (m 2 Below 1.40 g / (m) μm, further preferably 1.40 g / (m 2 ·μm) or higher and 2.70g / (m 2 ·μm or less, particularly preferably 1.50 g / (m 2 ·μm) or higher and 2.50g / (m 2 • μm or less. From the viewpoint of suppressing the deformation of PO microporous membranes at temperatures exceeding their melting point, a layer density of 1.10 g / (m³) in the layer containing inorganic fillers is preferred. 2 • μm) or higher. From the viewpoint of maintaining the ion permeability of the inorganic filler layer and suppressing capacity degradation during repeated cycling, a layer density of 3.00 g / (m³) in the inorganic filler layer is preferred. 2 Below μm.

[0285] As a method for forming a layer containing inorganic fillers, one example is a method of forming a layer containing inorganic fillers by coating at least one side (e.g., the first main side of a porous substrate) of a microporous membrane mainly composed of a polyolefin resin with a coating liquid (in one manner, a slurry containing inorganic fillers) containing an inorganic filler, a resin-based binder, and a solvent.

[0286] As a solvent for a coating liquid containing inorganic fillers and resin-based binders, a solvent that can uniformly and stably disperse the inorganic fillers and resin-based binders is preferred. Examples include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, dichloromethane, hexane, etc.

[0287] To improve dispersion stabilization and coatability, various additives can be added to the coating solution containing inorganic fillers and resin-based binders, including: dispersants such as surfactants; thickeners; wetting agents; defoamers; and pH adjusters containing acids and bases. These additives are preferably those that can be removed during solvent removal; however, they may remain in the inorganic filler-containing layer as long as they are electrochemically stable within the operating range of lithium-ion secondary batteries, do not hinder battery reactions, and are stable up to approximately 200°C.

[0288] Regarding methods for dispersing inorganic fillers and resin-based binders in the solvent of a coating liquid, there are no particular limitations as long as the method can achieve the dispersion characteristics of the coating liquid required for the coating process. Examples include ball mills, bead mills, planetary ball mills, vibratory ball mills, sand mills, colloid mills, ultrafine grinding mills, roller mills, high-speed impeller dispersers, dispersers, homogenizers, high-speed impact mills, ultrasonic dispersion, and mechanical stirring based on stirring blades, etc.

[0289] Regarding methods for coating microporous membranes with a coating liquid containing inorganic fillers and resin-based binders, there are no particular limitations as long as the desired thickness and coverage area of ​​the inorganic filler-containing layer can be achieved. Examples include gravure coating, small-diameter gravure coating, reverse roller coating, transfer roller coating, mating coating, dip coating, doctor blade coating, air knife coating, scraper coating, rod coating, extrusion coating, cast coating, mold coating, screen printing, and spraying.

[0290] Furthermore, when the surface of the microporous membrane, which serves as the separator substrate, is surface-treated before applying the coating liquid containing inorganic fillers and resin-based binders, the coating liquid is easier to apply, and the adhesion between the coated inorganic filler-containing layer and the surface of the microporous membrane is improved, which is therefore preferred. The surface treatment method is not particularly limited as long as it does not significantly damage the porous structure of the microporous membrane; examples include corona discharge treatment, mechanical roughening, solvent treatment, acid treatment, and ultraviolet oxidation.

[0291] Regarding methods for removing solvent from a coating film after coating with a coating solution containing inorganic fillers and resin-based binders, there are no particular limitations as long as the method does not adversely affect the microporous membrane. Examples include methods such as drying the microporous membrane at a temperature below its melting point while it is being fixed, and methods such as low-temperature, reduced-pressure drying. From the viewpoint of ensuring the bonding between the binder polymer (the binder component of the resin-based binder) and the microporous membrane as a substrate, the layer containing inorganic fillers (in one case, a porous layer), and the bonding force between the particulate binders, while simultaneously preventing ion permeability obstruction of the separator, drying at atmospheric pressure is preferred. From the viewpoint of controlling the shrinkage stress in the MD direction of the microporous membrane and multilayer porous membranes, it is preferable to appropriately adjust the drying temperature, winding tension, etc.

[0292] [Properties and Structure of Separators]

[0293] From the viewpoint of excellent electrolyte injection properties, low air accumulation, and short injection time, the contact angle of the electrolyte in the separator of this embodiment is preferably 0° or more and 20° or less, more preferably 2° or more and 18° or less, and even more preferably 4° or more and 16° or less. The contact angle of the electrolyte is more preferably measured on the surface of the thermoplastic polymer-containing layer in the separator where a dotted pattern is formed.

[0294] The lower limit of the total thickness of the separator for the energy storage device in this embodiment is preferably 5 μm or more, more preferably 6 μm or more, and even more preferably 8 μm or more. The upper limit is preferably 20 μm or less, more preferably 17 μm or less, even more preferably 15 μm or less, and particularly preferably 11.5 μm or less. From the viewpoint of ensuring the strength and safety of the separator for the energy storage device, it is preferable to set the total thickness of the separator for the energy storage device to 5 μm or more. On the other hand, from the viewpoint of obtaining good charge-discharge characteristics by reducing battery resistance, it is preferable to set the total thickness of the separator for the energy storage device to 20 μm or less.

[0295] The total thickness of the separator for the energy storage device is preferably 5 μm or more and 20 μm or less, more preferably 6 μm or more and 17 μm or less, even more preferably 7 μm or more and 15 μm or less, and particularly preferably 8 μm or more and 11.5 μm or less.

[0296] The total thickness of the separator in this embodiment is determined by the following method.

[0297] The thickness of the separator was measured at room temperature (23±2℃) using a miniature thickness gauge "KBM (trademark)" manufactured by Toyo Seiki Co., Ltd.

[0298] The lower limit of the unit area weight of the separator for the energy storage device in this embodiment is preferably 5.0 g / m². 2The above, more preferably 6.1 g / m 2 The above is further preferred to be 7.5g / m 2 The upper limit is preferably 13.5 g / m 2 The preferred value is 12.0 g / m³. 2 The following is a further preferred value: 7.6 g / m 2 From the viewpoint of ensuring strength and safety, it is preferable that the weight per unit area of ​​the separator for the energy storage device in this embodiment is 5.0 g / m². 2 That's all. On the other hand, from the viewpoint of reducing battery resistance and obtaining good charge-discharge characteristics, it is preferable that the weight per unit area of ​​the separator for the energy storage device in this embodiment is 13.5 g / m². 2 the following.

[0299] In this embodiment, the lower limit of the air permeability of the separator for the energy storage device is preferably 10 sec / 100 cm. 3 The above is preferred, with 20 sec / 100cm being more ideal. 3 The above is further preferred to be 30 sec / 100cm. 3 The optimal value is 50 sec / 100 cm. 3 That's all. The upper limit of the air permeability of the separator for the energy storage device in this embodiment is preferably 200 sec / 100cm. 3 The following is more preferably 180 sec / 100 cm 3 Hereinafter, 150 sec / 100 cm is further preferred. 3 The optimal value is 120 sec / 100 cm. 3 the following.

[0300] In manufacturing a separator for an energy storage device, from the viewpoint of suppressing the occurrence of micro-short circuits, reducing performance and safety degradation during storage tests, and further suppressing self-discharge of the energy storage device, the air permeability of the separator for the energy storage device in this embodiment is set to 10 sec / 100 cm. 3 The above are preferred options. On the other hand, from the viewpoint of reducing battery resistance and obtaining good charge-discharge characteristics, it is preferable that the air permeability of the separator for the energy storage device in this embodiment is 200 sec / 100 cm. 3 The permeability of the separator in this embodiment of the energy storage device can be adjusted by changing the stretching temperature, stretching ratio, area ratio, and existing form of the thermoplastic polymer during the manufacturing of the polyolefin microporous membrane.

[0301] Regarding the puncture strength of the separator for the energy storage device according to this embodiment, its lower limit is preferably 200 gf or more, more preferably 300 gf or more, further preferably 400 gf or more, and particularly preferably 450 gf or more. From the viewpoints of suppressing film rupture caused by detached active material when the separator is wound together with the electrode, suppressing short circuits caused by the expansion and contraction of the electrode during charging and discharging, and improving the impact resistance of the energy storage device, a puncture strength of 200 gf or more for the separator for the energy storage device according to this embodiment is preferred. In addition, from the viewpoint of reducing width shrinkage caused by orientation relaxation during heating, the upper limit of the puncture strength of the separator for the energy storage device according to this embodiment is preferably 800 gf or less, more preferably 700 gf or less, and further preferably 600 gf or less.

[0302] Regarding the thermal shrinkage rate of the separator for the energy storage device in this embodiment, the thermal shrinkage rate of the TD at 150°C for 1 hour is preferably -3% or more and 10% or less, more preferably -1% or more and 8% or less, and even more preferably 0% or more and 5% or less. Here, if the thermal shrinkage rate of the TD at 150°C for 1 hour is -3% or more, the risk of short circuits between electrodes caused by separator distortion due to negative shrinkage (expansion) and the reduction in performance and safety are suppressed. If the thermal shrinkage rate of the TD at 150°C for 1 hour is 10% or less, the reduction in performance and safety caused by micro-short circuits during storage tests is suppressed.

[0303] The thermal shrinkage rate of the separator in this embodiment can be adjusted by appropriately combining the stretching operation and heat treatment of the substrate. While suppressing the thermal shrinkage rate of TD at 150°C for 1 hour, the thermal shrinkage rate of MD is preferably -3% to 10% or less, more preferably -1% or more and 8% or less, and even more preferably 0% or more and 5% or less.

[0304] In this disclosure, the length direction (MD) refers to the mechanical direction of the continuous forming of the microporous membrane, and the width direction (TD) refers to the direction of the MD that traverses the microporous membrane at an angle of 90°.

[0305] The closing temperature of the separator for the energy storage device in this embodiment, which serves as a safety indicator for the energy storage device, is preferably 160°C or less, more preferably 155°C or less, even more preferably 150°C or less, and most preferably 145°C or less.

[0306] The short-circuit temperature of the separator for the energy storage device in this embodiment, which is an indicator of heat resistance, is preferably 140°C or higher, more preferably 150°C or higher, and even more preferably 160°C or higher. When the separator in this embodiment is a separator for an energy storage device, from the viewpoint of the safety of the energy storage device, it is preferable to set the short-circuit temperature to 160°C or higher.

[0307] [Manufacturing method of the separator]

[0308] The method for manufacturing the separator for the energy storage device according to this embodiment includes:

[0309] The process of preparing porous substrates;

[0310] The process of forming a layer containing inorganic fillers on the first main surface of a porous substrate; and

[0311] The process of coating a slurry containing a thermoplastic polymer onto the surface of a layer containing an inorganic filler disposed on a first main surface of a porous substrate and onto a second main surface of the porous substrate to form a layer containing a thermoplastic polymer.

[0312] In one embodiment, the method for manufacturing the separator for the energy storage device includes:

[0313] The process of preparing porous substrates;

[0314] The process of forming an inorganic filler-containing layer by coating a slurry containing inorganic fillers onto the first main surface of a porous substrate; and

[0315] The process of forming a thermoplastic polymer layer by coating a slurry containing a thermoplastic polymer onto the surface of a layer containing inorganic fillers and the second main surface of a porous substrate.

[0316] The viscosity of the slurry containing thermoplastic polymers at a shear rate of 60,000 sec -1 The values ​​are above 1 mPa·s and below 20 mPa·s.

[0317] The shear rate v when a slurry containing a thermoplastic polymer is coated on the surface of a layer containing inorganic fillers. c The shear rate v when coating a slurry containing a thermoplastic polymer on the second main surface of a porous substrate p Satisfying the relationship between equations (2) and (3):

[0318] 30000sec -1 ≤v c ≤200000sec -1 …Formula (2)

[0319] 5000sec -1 ≤v c -v p ≤40000sec -1 …Formula (3).

[0320] <Process for preparing porous substrate>

[0321] The manufacturing method of this embodiment includes a step of preparing a porous substrate. This step may include, for example, the microporous membrane fabrication process described above and the surface treatment of the substrate described later.

[0322] <Process for forming a layer containing inorganic fillers>

[0323] The manufacturing method of this embodiment includes a step of forming a layer containing inorganic filler on a first main surface of a porous substrate. As a method for forming the layer containing inorganic filler, the method described in the above-described method for forming a layer containing inorganic filler can be implemented.

[0324] <Process for forming a layer containing thermoplastic polymer>

[0325] The manufacturing method of this embodiment includes the following steps: applying a slurry containing a thermoplastic polymer to the surface of a layer containing inorganic fillers disposed on a first main surface of a porous substrate and to a second main surface of the porous substrate, thereby forming a layer containing a thermoplastic polymer. The method of applying the slurry is not particularly limited; for example, a method of applying a slurry containing a thermoplastic polymer and a solvent (in one embodiment, a coating liquid containing a thermoplastic polymer) to a polyolefin microporous membrane (in one embodiment, a porous substrate) or a layer containing inorganic fillers can be described.

[0326] When a slurry containing a thermoplastic polymer is coated onto a polyolefin microporous membrane or a layer containing inorganic fillers, if the slurry penetrates into the interior of the polyolefin microporous membrane or the layer containing inorganic fillers, the thermoplastic polymer fills the surface and interior of the pores of the microporous membrane, reducing ion permeability. Therefore, a poor solvent for the thermoplastic polymer is preferred as the solvent for the slurry.

[0327] When a poor solvent for thermoplastic polymers is used as the solvent for a slurry containing thermoplastic polymers, the coating liquid does not penetrate into the interior of the polyolefin microporous membrane or the layer containing inorganic fillers. The thermoplastic polymers are mainly present on the surface of the microporous membrane, which is preferred from the viewpoint of suppressing the reduction of ion permeability.

[0328] For example, water is preferred as a solvent for thermoplastic polymers. Furthermore, there are no particular limitations on solvents that can be used with water; examples include ethanol and methanol. Defoamers (such as KM-73 from Shin-Etsu Chemical Co., Ltd., and SK-14 from Nissin Chemical Co., Ltd.) can be added to the slurry as needed.

[0329] In one method, the slurry is prepared by dispersing a thermoplastic polymer in a solvent. In another method, the solvent used to disperse the thermoplastic polymer can be any solvent that is unsuitable for the thermoplastic polymer. Organic solvents and water are preferred as unsuitable solvents for the thermoplastic polymer, and water is more preferred from the viewpoint of suppressing static electricity.

[0330] In one embodiment, the coating liquid containing the thermoplastic polymer (or, in one embodiment, a slurry containing the thermoplastic polymer) can be an aqueous slurry using water as a solvent.

[0331] From the viewpoint that the dot shape of the thermoplastic polymer-containing layer cannot be maintained due to the suppression of coating liquid flow, and from the viewpoint of controlling the thickness distribution of the coating layer, the solid content in 100% by mass of the thermoplastic polymer-containing slurry is preferably 6% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 35% by mass or less, even more preferably 15% by mass or more and 33% by mass or less, and particularly preferably 20% by mass or more and 31% by mass or less.

[0332] From the viewpoint that the dot shape of the thermoplastic polymer-containing layer cannot be maintained due to the suppression of coating liquid flow, and from the viewpoint of controlling the thickness distribution of the coating layer, the viscosity of the thermoplastic polymer-containing slurry at 20°C is preferably 5 mPa·s or more and 150 mPa·s or less, more preferably 10 mPa·s or more and 100 mPa·s or less, and even more preferably 25 mPa·s or more and 80 mPa·s or less.

[0333] It should be noted that the viscosity of the slurry containing thermoplastic polymer at 20°C was determined by the method described in the examples.

[0334] From the viewpoint that the dot shape of the thermoplastic polymer-containing layer cannot be maintained due to the suppression of coating liquid flow, and from the viewpoint of controlling the thickness distribution of the coating layer, the surface tension of the slurry containing thermoplastic polymer is preferably 10 mN / m or more and 70 mN / m or less, more preferably 20 mN / m or more and 60 mN / m or less, and even more preferably 25 mN / m or more and 50 mN / m or less.

[0335] From the viewpoint of preventing the aggregation of coating liquid, the pH of the slurry containing thermoplastic polymer is preferably 6 or higher and 10 or lower, more preferably 7 or higher and 9 or lower.

[0336] The viscosity of the slurry containing thermoplastic polymers at a shear rate of 60,000 sec -1 The preferred values ​​are 1 mPa·s or more and 20 mPa·s or less, more preferably 3 mPa·s or more and 15 mPa·s or less, and even more preferably 5 mPa·s or more and 10 mPa·s or less.

[0337] In addition, the viscosity of the slurry containing thermoplastic polymers at a shear rate of 90,000 sec -1The preferred values ​​are 3 mPa·s or more and 25 mPa·s or less, more preferably 4 mPa·s or more and 15 mPa·s or less, even more preferably 5 mPa·s or more and 12 mPa·s or less, and particularly preferably 8 mPa·s or more and 10 mPa·s or less.

[0338] From the perspective of suppressing the point shape of the thermoplastic polymer-containing layer due to the flow of the coating liquid, and from the perspective of controlling the thickness distribution of the coating layer, a shear rate of 60,000 seconds is used. -1 and 90000 seconds -1 The viscosity of the slurry containing the thermoplastic polymer (in one mode, high shear viscosity) is preferably controlled within a specified range, with a shear rate of 90,000 sec. -1 The high shear viscosity is preferably greater than a shear rate of 60,000 sec. -1 High shear viscosity.

[0339] It should be noted that the shear rate of the slurry containing thermoplastic polymers is 60,000 seconds. -1 and 90000 seconds -1 The high shear viscosity was determined using the method described in the examples.

[0340] The shear rate v when a slurry containing a thermoplastic polymer is coated on the surface of a layer containing inorganic fillers. c The shear rate v when coating a slurry containing a thermoplastic polymer on the second main surface of a porous substrate p It is preferable to satisfy the relationship between the following equations (2) and (3).

[0341] 30000sec -1 ≤v c ≤200000sec -1 …Formula (2)

[0342] 5000sec -1 ≤v c -v p ≤40000sec -1 …Formula (3)

[0343] By increasing the shear rate, the viscosity of the thermoplastic polymer-containing slurry is increased (in one method, the viscosity of the thermoplastic polymer-containing slurry under shear conditions during coating), thereby increasing the thickness t of the thermoplastic polymer-containing layer on the surface of the inorganic filler layer. c The deviation is denoted by the standard deviation s. tc As the value increases, it becomes easier to ensure the gap (preventing contact) between the surface of the inorganic filler layer and the surface of the thermoplastic polymer layer on the second main surface of the porous substrate when overlapping separators are used.

[0344] Based on the above reasons, the shear rate v when coating a slurry containing a thermoplastic polymer onto the surface of a layer containing inorganic fillers is... c Preferably 30000 sec -1 The above, more preferably 50000 seconds -1 The above is further optimized to 60,000 seconds. -1 The above is further optimized to 75000 seconds. -1 The above is particularly preferred, with 76000 seconds. -1 The optimal value is 90,000 seconds. -1 above.

[0345] In addition, from the perspective of preventing coating streaks and friction, the shear rate v c Preferably 200,000 sec -1 The following, more preferably, is 150,000 seconds. -1 The following, and more preferably 100,000 seconds -1 The following, particularly preferred, is 95000 seconds. -1 the following.

[0346] Furthermore, from the point-forming perspective, v c Preferably 30000 sec -1 Above and 200,000 seconds -1 Hereinafter, 50000 sec is preferred. -1 Above and 150,000 seconds -1 The following is particularly preferred: 60,000 seconds. -1 Above and 100,000 seconds -1 the following.

[0347] By reducing the shear rate, the viscosity of the thermoplastic polymer-containing slurry is reduced (in one embodiment, the viscosity of the thermoplastic polymer-containing slurry under shear conditions during coating), thereby increasing the thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate. p Become uniform, standard deviation s tp The value decreases, thus reducing the localized surface contact between the thermoplastic polymer layer and the inorganic filler layer on the second main surface of the porous substrate when overlapping separators are used.

[0348] Based on the above reasons, the shear rate v when coating a slurry containing a thermoplastic polymer on the second main surface of a porous substrate is... p Preferably 100000 sec -1 Hereinafter, 90000 sec is preferred. -1 The following is a further preferred value: 80,000 seconds. -1The following is particularly preferred: 60,000 seconds. -1 Below. Additionally, from the viewpoint of pattern formation, the shear rate v p Preferred time: 10000 seconds -1 The above, more preferably 20000 seconds -1 The above is further optimized to 30,000 seconds. -1 The above, especially preferred, is 50,000 seconds. -1 above.

[0349] The shear rate v when a slurry containing a thermoplastic polymer is applied to the surface of a layer containing inorganic fillers is measured. c The shear rate v when coating a slurry containing a thermoplastic polymer on the second main surface of a porous substrate p The difference is controlled within a certain range; the uneven thickness of the thermoplastic polymer-containing layer on both sides of the separator, i.e., the standard deviation s, is... tc and standard deviation s tp The balance becomes good, and when the separators are overlapped, the layer containing thermoplastic polymer on the second main surface of the porous substrate does not easily come into contact with the layer containing inorganic filler.

[0350] Based on the above reasons, the shear rate v when coating a slurry containing a thermoplastic polymer onto the surface of a layer containing inorganic fillers is... c The shear rate v when coating a slurry containing a thermoplastic polymer on the second main surface of a porous substrate p The difference: v c -v p Preferably 5000 sec -1 The above, more preferably 10000 seconds -1 The above is further optimized to 15000 seconds. -1 The above, especially preferred, is 30,000 seconds. -1 above.

[0351] v c -v p Preferably 40000 sec -1 Hereinafter, 35000 seconds is preferred. -1 The following is particularly preferred: 30,000 seconds -1 the following.

[0352] v c -v p Preferably 5000 sec -1 Above and 40,000 seconds -1 Hereinafter, 10000 sec is preferred. -1 Above and 35000 seconds -1 The following is particularly preferred: 15000 seconds-1 Above and 30,000 seconds -1 the following.

[0353] It should be noted that the shear rate when the slurry containing thermoplastic polymer is coated onto a porous substrate and a layer containing inorganic filler was measured using the method described in the examples.

[0354] It should be noted that in this disclosure, the shear rate v c and shear rate v p 70000 seconds -1 The above scenarios are assumed to have a high shearing rate.

[0355] Furthermore, although not bound by theory, when the shear rate is low when coating a slurry containing thermoplastic polymers onto a porous substrate and a layer containing inorganic fillers, there is a tendency for the viscosity of the slurry containing thermoplastic polymers to decrease and the thickness of the layer containing thermoplastic polymers to become more uniform. On the other hand, when the shear rate is high when coating a slurry containing thermoplastic polymers onto a porous substrate and a layer containing inorganic fillers, there is a tendency for the viscosity of the slurry containing thermoplastic polymers to increase and the thickness of the layer containing thermoplastic polymers to become uneven.

[0356] There are no particular limitations on the method of coating a coating liquid containing thermoplastic polymer onto a microporous membrane or a layer containing inorganic filler, as long as the method can achieve the desired coverage area ratio and thickness of the layer containing thermoplastic polymer.

[0357] Examples of coating methods include gravure coating, small-diameter gravure coating, reverse roller coating, transfer roller coating, conformal coating, dip coating, doctor blade coating, air knife coating, scraper coating, rod coating, extrusion coating, cast coating, mold coating, screen printing, spraying, spraying machine coating, and inkjet coating. Among these, gravure coating or spraying is preferred due to the high degree of freedom in coating shape for thermoplastic polymers and the ease of obtaining an optimal coverage area.

[0358] Furthermore, from the viewpoint of adjusting the dotted pattern of the thermoplastic polymer-containing layer as described above, gravure coating or inkjet coating is preferred, and coating methods that allow for easy adjustment of the printing plate are even more preferred.

[0359] From the viewpoint of adjusting the dot pattern of the layer containing the thermoplastic polymer as described above, it is preferable to use the thermoplastic polymer described above and its unsuitable solvents, etc., to optimize the coating liquid containing the thermoplastic polymer.

[0360] Regarding coating solutions containing thermoplastic polymers, considering both adhesion to the electrodes and ion permeability, the preferred coating amount per single side of the separator is 0.03 g / m. 2Above and 0.50g / m 2 The following is more preferably 0.04 g / m 2 Above and 0.45g / m 2 The optimal value is 0.06 g / m³. 2 Above and 0.40g / m 2 the following.

[0361] Furthermore, if the porous substrate serving as the separator substrate is surface-treated before applying the coating liquid containing the thermoplastic polymer, the coating liquid containing the thermoplastic polymer is easier to apply, and the adhesion between the porous substrate or the layer containing inorganic fillers and the thermoplastic (adhesive) polymer is improved, which is therefore preferred. The surface treatment method is not particularly limited as long as it does not significantly damage the porous structure of the porous substrate; examples include corona discharge treatment, plasma treatment, mechanical roughening, solvent treatment, acid treatment, and ultraviolet oxidation.

[0362] In the case of corona discharge treatment, from the viewpoint of adjusting the contact angle between the thermoplastic polymer-containing layer or separator and the electrolyte to the numerical range described above, the corona treatment intensity on the substrate surface is preferably 1 W / (m²). 2 / min) or higher and 40W / (m 2 More preferably, it is in the range of 3W / (m) or less. 2 / min) or higher and 32W / (m 2 Within the range of 5W / (m / min) or less, it is further preferred to be within the range of 5W / (m / min). 2 / min) or higher and 25W / (m 2 The corona treatment intensity is within the range of ( / min) or less. With a corona treatment intensity within the above range, there is a tendency to introduce hydrophilic groups onto the substrate surface, thereby improving affinity and wettability with the electrolyte. Furthermore, it is preferable to perform the corona discharge treatment after forming a dotted pattern of a layer containing a thermoplastic polymer.

[0363] There are no particular limitations on the method for removing solvent from the coating after applying a thermoplastic polymer, as long as it does not adversely affect the porous substrate. For example, methods such as drying the porous substrate at a temperature below its melting point while fixing it, drying under reduced pressure at low temperature, and immersing it in a solvent that is unfavorable to the adhesive polymer to allow the adhesive polymer to solidify while simultaneously extracting the solvent are all possible methods.

[0364] <Drying Process>

[0365] The manufacturing method of this embodiment may include a step of coating at least one surface of a porous substrate with a slurry containing a thermoplastic polymer and then drying the slurry.

[0366] In the drying of the slurry, the drying rate is preferably 0.03 g / (m²). 2 ·s) or more and 4.0 g / (m 2 More preferably, it is in the range of 0.05 g / (m) or less. 2 ·s) or more and 3.5g / (m 2 Within the range of ·s) or less, it is further preferred to be 0.08 g / (m 2 ·s) or more and 3.0g / (m 2 Within the range of ·s).

[0367] When the drying rate is within a certain range, a moderate drying rate inhibits leveling, introduces an uneven structure of thermoplastic polymer particles onto the surface, and tends to improve wettability. From the same point of view, in the drying of the coated film, it is also preferable to raise the temperature to a level that does not damage the particle shape of the thermoplastic polymer-containing layer.

[0368] [Separator Roll]

[0369] A device formed by winding separators onto a core material is called a separator roll (or, in one case, a roll). In recent years, there has been a trend towards longer separators wound on rolls to improve productivity. However, if the separators are made longer, the issue of static electricity generation is expected to become more significant.

[0370] The greater the "pressure" applied to the separator, the worse the static electricity becomes. The inner side of the separator is most susceptible to pressure when it is rolled into a roll; the closer to the innermost layer, the higher the risk of static electricity generation.

[0371] It should be noted that, in this disclosure, the innermost layer of the separator roll refers to the surface where the core and the separator are in direct contact.

[0372] The inventors discovered that, in actual delivery of the separator from the roll, the stripping charge increases as it approaches the innermost layer.

[0373] In addition, the thinning of separators for the purpose of increasing energy density (e.g., coating with a thickness of about 6 to 9 μm in polyolefin microporous membranes or about 1 to 1.5 μm in layers containing inorganic fillers) is also a trend. However, there is a tendency for the pressure applied to the inner layer to increase due to the thinning of separators, and the risk of static electricity can be expected to increase further.

[0374] Therefore, it is preferable to manufacture the roll by winding the separator while controlling the inner layer pressure below a certain level.

[0375] The roll can be made by winding the separator using any core (e.g., resin, paper, and glass) at any winding tension (e.g., 0.01~1.50 N / mm).

[0376] As indicators for evaluating the impact of electrostatics on separators, there are peel charge and electrostatic-based adhesion evaluations.

[0377] In this embodiment, the stripping charge of the separator when it is delivered from the drum is preferably -15kV or higher and +15kV or lower, more preferably -10kV or higher and +10kV or lower, and even more preferably -8kV or higher and +8kV or lower.

[0378] The separator in this embodiment can prevent pinholes from forming when the separator is ejected by suppressing static electricity and the associated sparks.

[0379] The stripping charge is obtained from the stripping charge of the separator roll of this embodiment, which is formed by winding the separator of this embodiment onto the core, when the separator is delivered from the separator by the following method.

[0380] On an acrylonitrile-butadiene-styrene (ABS) core with an outer diameter of 6 inches, the separator of the sample is wound 4000m so that the entire surface of the roll becomes the second main surface of the porous substrate, thus producing a separator roll sample for evaluation (hereinafter referred to as the roll).

[0381] After a 3000m separator is fed from a circular drum, a 50m separator is stretched along the tangential direction of the drum and fed out at a speed of 10m / min. The stripping charge at this point is measured, and the average value is taken as the stripping charge when the separator is fed out of the drum in this embodiment. At the point where the separator leaves the drum (hereinafter referred to as the stripping point), an electrostatic meter (model: FMA-004, manufactured by Simco Japan Co., Ltd.) is installed at a position 20mm in the direction in which the separator is fed out and 25mm in the direction perpendicular to the surface of the fed separator to measure the stripping charge. The measurement is performed at a temperature of 23°C and a humidity of 20%.

[0382] The electrostatic adhesion of the separator roll of this embodiment, which is formed by winding the separator of this embodiment onto the core, is determined by the following method.

[0383] On an acrylonitrile-butadiene-styrene (ABS) core with an outer diameter of 6 inches, the separator of the sample is wound 4000m so that the entire surface of the roll becomes the second main surface of the porous substrate, thus producing a separator roll sample for evaluation (hereinafter referred to as the roll).

[0384] After a 3000m section of separator is fed from a circular roll, the separator is stretched tangentially along the roll at a speed of 10m / min. The proportion of the separator pulled towards the roll after being cut with scissors at a point 20cm from the peel point is used as an indicator of electrostatic adhesion. The measurement was conducted at 23℃ and 20% humidity.

[0385] In this embodiment, the surface pressure applied to the innermost layer of the separator roll is preferably 5 MPa or less. Alternatively, in one embodiment, when the separator of this embodiment is wound to form a roll, the surface pressure applied to the innermost layer is preferably 5 MPa or less, more preferably 3 MPa or less, and even more preferably 2 MPa or less.

[0386] The separator roll of this embodiment can prevent the generation of static electricity by suppressing the surface pressure applied to the innermost layer within a specified range.

[0387] The surface pressure applied to the innermost layer of the separator roll of this embodiment, which is formed by winding the separator of this embodiment around the core, is determined by the following method.

[0388] A sensor sheet (Nitta Corporation FlexiForce A201-25) is attached to a 6-inch outer diameter core made of acrylonitrile-butadiene-styrene (ABS). The separator is wound 4000m onto the core in such a way that the entire surface of the roll becomes the second main surface of the porous substrate, thus creating an evaluation roll.

[0389] Using a digital multimeter (SANWA RD701), the resistance value applied to the sensor sheet is measured. The measured resistance value is then applied to a pre-prepared standard curve to calculate the surface pressure applied to the innermost layer.

[0390] It should be noted that the standard curve is created using the following method.

[0391] While applying a certain pressure to the pressure-sensitive part of the sensor plate, the resistance value measured by a digital multimeter is repeatedly recorded while the pressure applied to the sensor plate is changed. The pressure and resistance values ​​are plotted on a graph to create a standard curve. The standard curve is created by plotting data with a pressure of 0 MPa or higher and 5 MPa or lower at at least 5 points.

[0392] [Layered Body]

[0393] The laminate of this embodiment is formed by stacking a separator and an electrode. The separator in this embodiment can be used as a laminate by bonding it to the electrode. The laminate of this embodiment exhibits excellent operability during winding and superior cycle and rate characteristics of the energy storage device, thereby suppressing the generation of static electricity when the separator is ejected and thus suppressing pinhole formation. Therefore, its application as a laminate is not particularly limited; for example, it can be suitable for use in batteries such as non-aqueous electrolyte secondary batteries, energy storage devices such as capacitors, and capacitors.

[0394] The electrodes used in the laminated body of this embodiment can be the electrodes described in the section on energy storage devices described later. The method for manufacturing the laminated body using the separator of this embodiment is not particularly limited; for example, the separator of this embodiment can be overlapped with the electrodes, and then heated and / or pressurized as needed. Heating and / or pressurizing can be performed while the electrodes and separator are overlapped. Alternatively, it can be manufactured by heating and / or pressurizing a wound body obtained by overlapping the electrodes and separator and winding it into a circular or flat vortex shape.

[0395] Alternatively, the laminate can be stacked into a flat plate in the order of positive electrode-separator-negative electrode-separator, or negative electrode-separator-positive electrode-separator, and manufactured by heating and / or pressurizing as needed. In the laminate, from the viewpoint of effectively utilizing the effects of this embodiment, it is preferable that the side of the separator containing the inorganic filler layer described above is positioned opposite the positive electrode, with the separator substrate as a reference.

[0396] More specifically, the separator of this embodiment can be prepared as a longitudinally elongated separator with a width of 10-500 mm (preferably 50-500 mm) and a length of 200-4000 m (preferably 1000-4000 m). The separator is then stacked in the order of positive electrode-splitter-negative electrode-splitter, or negative electrode-splitter-positive electrode-splitter, and manufactured by heating and / or pressurizing as needed.

[0397] The preferred heating temperature is 40°C to 120°C. The preferred heating time is 5 seconds to 30 minutes. The preferred pressure during pressurization is 1 to 30 MPa. The preferred pressurization time is 5 seconds to 30 minutes. Furthermore, the order of heating and pressurization can be heating followed by pressurization, pressurization followed by heating, or simultaneous pressurization and heating. Simultaneous pressurization and heating are preferred.

[0398] <Electronic Storage Devices>

[0399] The separator of this embodiment can be used for separating components and materials in batteries, capacitors, capacitors, etc. Especially when used as a separator for an energy storage device, it can impart a tight seal between the electrodes and excellent battery performance. Hereinafter, a preferred embodiment for an energy storage device that is a non-aqueous electrolyte secondary battery will be described.

[0400] The energy storage device of this embodiment includes a positive electrode, a negative electrode, a separator for the energy storage device of this embodiment, and a non-aqueous electrolyte. When manufacturing a non-aqueous electrolyte secondary battery using the separator of this embodiment, the positive electrode, negative electrode, and non-aqueous electrolyte are not limited, and known positive electrodes, negative electrodes, and non-aqueous electrolytes can be used.

[0401] There are no particular limitations on the cathode material; examples include lithium-containing composite oxides such as LiCoO2, LiNiO2, spinel-type LiMnO4, and olivine-type LiFePO4.

[0402] There are no particular limitations on the anode material. Examples include graphitic, non-graphitized carbonaceous, easily graphitized carbonaceous, and composite carbonaceous materials; silicon, tin, metallic lithium, and various alloy materials.

[0403] There are no particular limitations on non-aqueous electrolytes; electrolytes made by dissolving electrolytes in organic solvents can be used. Examples of organic solvents include propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. Examples of electrolytes include lithium salts such as LiClO4, LiBF4, and LiPF6.

[0404] The method for manufacturing an energy storage device using the separator of this embodiment is not particularly limited. When the energy storage device is a secondary battery, for example, the separator of this embodiment is prepared into a longitudinally elongated shape with a width of 10 to 500 mm (preferably 50 to 500 mm) and a length of 200 to 4000 m (preferably 1000 to 4000 m). The separator is overlapped in the order of positive electrode-separator-negative electrode-separator or negative electrode-separator-positive electrode-separator, and wound into a circular or flat vortex shape to obtain a wound body. The wound body is placed in a battery canister and then electrolyte is injected, thereby manufacturing the device.

[0405] At this point, the aforementioned laminate can be formed by heating and / or pressurizing the wound body. Alternatively, a laminate formed by winding the aforementioned laminate into a circular or flat vortex shape can also be used as the wound body. Furthermore, the energy storage device can be manufactured through the following steps: a process of laminating a laminate obtained by stacking it into a flat plate shape in the order of positive electrode-separator-negative electrode-separator, or negative electrode-separator-positive electrode-separator, or laminating the aforementioned laminate using a bag-shaped film, followed by injecting electrolyte; and a process of heating and / or pressurizing as appropriate. The aforementioned heating and / or pressurizing process can be performed before and / or after the electrolyte injection process.

[0406] In an energy storage device comprising a positive electrode, a negative electrode, a separator as described in this embodiment, and a non-aqueous electrolyte, from the viewpoint of effectively utilizing the effects of this embodiment, the separator is preferably arranged such that one side of the layer containing the inorganic filler described above, based on a substrate, is opposite to the positive electrode.

[0407] The energy storage device of this embodiment can be manufactured using the same method as the battery used in the rate characteristic test, cycle characteristic test, etc., described in the embodiments described later.

[0408] It should be noted that, unless otherwise specified, the measured values ​​of the above parameters are those measured according to the measurement methods described in the examples below.

[0409] Example

[0410] The present invention will now be described in detail based on embodiments and comparative examples, but the present invention is not limited to the embodiments. The methods for measuring and evaluating various physical properties used in the following manufacturing examples, embodiments, and comparative examples are described below. It should be noted that, unless otherwise specified, all measurements and evaluations are performed at room temperature of 23°C, 1 atmosphere, and 50% relative humidity.

[0411] [Determination Method]

[0412] <Viscosity-average molecular weight (hereinafter also referred to as "Mv")>

[0413] Based on ASRM-D4020, the intrinsic viscosity [η] at 135°C in decahydronaphthalene solvent is determined, and the Mv of polyethylene is calculated using the following formula.

[0414] [η]=0.00068×Mv 0.67

[0415] In addition, the Mv of polypropylene is calculated by the following formula.

[0416] [η]=1.10×10 -4 Mv 0.80

[0417] <Volume average particle size of thermoplastic polymer particles and inorganic filler particles>

[0418] The particle size distribution and D10, D50, and D90 of the thermoplastic polymer particles and inorganic filler particles were obtained by measuring the dispersions of thermoplastic polymer particles and inorganic filler particles using a laser particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Corporation). If necessary, the particle size distribution of the thermoplastic polymer particle dispersion, the inorganic filler particle dispersion, or the binder polymer can be used as a baseline to adjust the particle size distribution of the thermoplastic polymer particles and the inorganic filler particle dispersion.

[0419] The average volumetric particle size D10 is defined as the particle size at which the cumulative frequency of the thermoplastic polymer particles and inorganic filler particles reaches 10%. The average volumetric particle size D50 is defined as the particle size at which the cumulative frequency of the thermoplastic polymer particles and inorganic filler particles reaches 50%. The average volumetric particle size D90 is defined as the particle size at which the cumulative frequency of the thermoplastic polymer particles and inorganic filler particles reaches 90%.

[0420] <Weight per unit area of ​​polyolefin microporous membranes and weight per unit area of ​​separators>

[0421] A 10cm x 10cm square sample was cut from a polyolefin microporous membrane (porous substrate), and its weight was determined using an AEL-200 electronic balance manufactured by Shimadzu Corporation. The weight was then multiplied by 100 to calculate the weight per cubic meter of membrane. 2 The unit area weight (g / m²) of polyolefin microporous membranes 2 ).

[0422] A 10cm × 10cm square sample was cut from the separator of this embodiment, and its weight was measured using an AEL-200 electronic balance. The weight was then multiplied by 100 to calculate the weight per 1m³. 2 Weight per unit area of ​​the separator (g / m²) 2 ).

[0423] <Porosity (%) of polyolefin microporous membranes>

[0424] A 10cm × 10cm square sample was cut from a polyolefin microporous membrane. Its volume (cm³) was calculated. 3 The membrane density was set to 0.95 (g / cm³) based on the mass (g) and mass (g). 3 ), use the following formula to calculate.

[0425] Porosity = (Volume - Mass / Film Density) / Volume × 100

[0426] Air permeability of polyolefin microporous membranes and separators (seconds / 100cm) 3 )>

[0427] According to JIS P-8117, the air permeability is defined as the air resistance of polyolefin microporous membranes and separators measured using a Gurley air permeability meter G-B2 (trademark) manufactured by Toyo Seiki Co., Ltd.

[0428] <Thickness of polyolefin microporous membranes and separators>

[0429] The thickness of polyolefin microporous membranes and separators was measured at room temperature (23±2℃) using a miniature thickness gauge "KBM (trademark)" manufactured by Toyo Seiki Co., Ltd.

[0430] <Glass transition temperature (°C) of thermoplastic polymers>

[0431] Take an appropriate amount of coating liquid containing thermoplastic polymer (non-volatile component = 30%) in an aluminum pan and dry it in a hot air dryer at 130°C for 30 minutes. Place approximately 5 mg of the dried film into an aluminum container for testing, and obtain the DSC and DDSC curves under a nitrogen atmosphere using a DSC measuring apparatus (TA Instruments, DSC Q2000). The testing conditions are as follows.

[0432] (Phase 1 heating process)

[0433] Start at 40°C and increase the temperature at a rate of 50°C per minute. Once it reaches 200°C, maintain this temperature for 5 minutes.

[0434] (Phase 2 cooling procedure)

[0435] Cool from 200°C at a rate of 20°C per minute. Maintain the temperature at -50°C for 5 minutes.

[0436] (Stage 3 warming process)

[0437] The temperature was increased from -50°C to 200°C at a rate of 20°C per minute. DSC and DDSC data were obtained during this third stage of heating.

[0438] According to the method described in JIS-K7121, the intersection of the baseline (the straight line obtained by extending the baseline of the obtained DSC curve towards the high temperature side) and the tangent at the inflection point (the point where the upward convex curve becomes the downward convex curve) is taken as the glass transition temperature (Tg).

[0439] <Coverage ratio (%) of the thermoplastic polymer-containing layer on the surface of the inorganic filler layer and on the second main surface of the porous substrate>

[0440] The coverage ratio of the thermoplastic polymer layer on the surface of the inorganic filler layer and on the second principal surface of the porous substrate is expressed as the ratio (area%) of the total coverage area of ​​the thermoplastic polymer layer to the surface area of ​​the inorganic filler layer or the surface area on the second principal surface of the porous substrate.

[0441] The coverage area ratio was measured using a microscope (model: VHX-7000, manufactured by KEYENCE).

[0442] The separator samples were photographed at 100x magnification (coaxial incident light). From the command "Measurement & Scale", "Automatic Area Measurement (Particle Count)", "Extraction Method Brightness (Standard)", and "Fill Hole" were selected. The total coverage area of ​​the thermoplastic polymer-containing layer was determined by binarization based on the Otsu method. Ten measurements were taken for each sample, and the arithmetic mean of all measurements was calculated.

[0443] If the contrast of the captured image is not clear, you can adjust the brightness of the light source appropriately, or use other light sources (model: PD2-1024, manufactured by CCS Corporation) for shooting.

[0444] <Determination of the thickness of layers containing inorganic fillers and layers containing thermoplastic polymers>

[0445] The cross-section of the separator used as the sample was processed using BIB (broad ion beam).

[0446] The processing conditions for the cross-section were as follows: An IM4000 laser from Hitachi High-Tech was used, with argon as the beam type, an accelerating voltage of 3kV, and a beam current of 25~35μA. During processing, to suppress thermal damage, the sample was cooled as needed until just before processing. Specifically, the sample was placed in a cooling device at -40°C for 24 hours. This resulted in a smooth cross-section for the separator.

[0447] The thickness t of the layer containing inorganic fillers and the layer containing thermoplastic polymers c and t p Measurements were performed using a scanning electron microscope (SEM) (model: S-4800, manufactured by HITACHI). Osmium deposition was applied to the samples, and observations were conducted at an accelerating voltage of 1.0 kV and 5000x to calculate the thicknesses of the layers containing inorganic fillers and thermoplastic polymers.

[0448] Regarding the thermoplastic polymer-containing layer, for both the thermoplastic polymer-containing layer on the surface of the inorganic filler layer and the thermoplastic polymer-containing layer on the second main surface of the porous substrate, 10 measurements were taken for each sample, and the arithmetic mean was calculated. The t value was then calculated. c and t p .

[0449] Standard deviation of coating thickness (including thermoplastic polymer layer): s tc and s tp >

[0450] For the separator used as a sample, the cross-section was processed in the same manner as described above in "Determination of the thickness of layers containing inorganic fillers and layers containing thermoplastic polymers".

[0451] Regarding the thickness of the thermoplastic polymer layer (dot) on the surface of the inorganic filler layer and the thickness of the thermoplastic polymer layer on the second main surface of the porous substrate, under the same conditions as in <Determination of the Thickness of Inorganic Filler Layer and Thermoplastic Polymer Layer>, SEM was used to measure the positions of 10 locations where more than one thermoplastic polymer particle exists in the cross-section of the sample after cross-section processing, and the arithmetic mean was calculated. The thickness of each coating layer (thermoplastic polymer layer) was then calculated.

[0452] Standard deviation of the thickness of each coating layer (including the thermoplastic polymer layer): s tc and s tp (In Equation 1, s is equivalent to ) and is expressed by Equation 1:

[0453] Formula 1:

[0454]

[0455] (In the formula, N is the number of measurement locations, x) i (The data is the measurement data, and x(-) is the average of the measurement data.)

[0456] As measured data: x i The thickness of each coating layer (the thickness of the thermoplastic polymer layer on the surface of the inorganic filler layer and the thickness of the thermoplastic polymer layer on the second main surface of the porous substrate) calculated above is obtained by applying Equation 1 above.

[0457] Shear rate when applying a slurry containing thermoplastic polymer: v c and v p >

[0458] Shear rate v during coating of slurry containing thermoplastic polymer c and v p (In Equation 2, γ is equivalent to γ) as expressed by Equation 2:

[0459] Formula 2:

[0460]

[0461] (In the formula, RPM is the rotational speed of the roller (revolutions per minute), R...) rollLet be the radius of the roller (m), and h be the gap between the roller and the scraper (m).

[0462] Apply the h obtained by the following method to Equation 2 above to calculate the result.

[0463] h is determined by setting a high-speed camera facing the axial surface of the gravure roller and photographing the gap between the gravure roller and the scraper during coating. It should be noted that the shutter speed of the high-speed camera can be adjusted appropriately as long as it does not produce motion blur.

[0464] When using a camera capable of displaying a scale, the gap between the gravure roller and the squeegee in the resulting image is calculated using the scale. When using a camera without a scale, a ruler is placed next to the object during shooting to calculate the gap. The gap h can be controlled by the type of squeegee (material and thickness), the squeegee's contact method (angle, pressure, and contact position), and the type of gravure roller (surface material and surface roughness).

[0465] Viscosity

[0466] The viscosity of a slurry containing thermoplastic polymers was measured using a TVB10M viscometer (manufactured by Toki Sangyo Co., Ltd.) at a temperature of 20°C.

[0467] High shear viscosity

[0468] The high-shear rotational viscometer PM9002HV (manufactured by Mitsui Electric Machinery Co., Ltd.) with E-type beads was used to measure the shear rate under the following conditions: rotation speed from 0 rpm to 12000 rpm, maximum rotation speed of 8800 rpm, room temperature, and acceleration time of 10 sec. The shear rate was calculated to be 60000 sec. -1 and 90000sec -1 The viscosity (high shear viscosity) of the slurry containing thermoplastic polymers.

[0469] <Inter-point distance of layers containing thermoplastic polymers>

[0470] The inter-point distance of the thermoplastic polymer-containing layer was measured using a microscope (model: VHX-7000, manufactured by KEYENCE). The separator used as the sample was photographed at 100x (coaxial incidence). In measurement mode, any point was selected, and the distances from its center to the centers of points located longitudinally, laterally, and obliquely at that point were measured. The average of these distances was taken as the inter-point distance.

[0471] <Diameter of the layer containing thermoplastic polymer>

[0472] The point diameter of the thermoplastic polymer-containing layer was measured using a microscope (model: VHX-7000, manufactured by KEYENCE). The separator used as the sample was photographed at 100x (coaxial incidence), and the diameter of each of the five points was measured in measurement mode. The average value of these measurements was calculated as the point diameter.

[0473] <Preparation of positive and negative electrodes for rate performance and cycle performance testing>

[0474] According to the nickel, manganese, and cobalt composite oxide (NMC) used as the positive electrode active material (Ni:Mn:Co=1:1:1 (elemental ratio), density is 4.70 g / cm³. 3 90.4% by mass of graphite powder (KS6) as a conductive additive (density 2.26 g / cm³) 3 1.6% by mass of acetylene black powder (AB) (with a number-average particle size of 6.5 μm) and acetylene black powder (AB) (with a density of 1.95 g / cm³). 3 The composition includes 3.8% by mass of polyvinylidene fluoride (PVdF) as a binder (with a density of 1.75 g / cm³), and polyvinylidene fluoride (PVdF) as a binder. 3 4.2% by mass were mixed and dispersed in N-methylpyrrolidone (NMP) to prepare a slurry. This slurry was then coated onto one side of a 20 μm thick aluminum foil, which would become the positive electrode current collector, using a die coater. After drying at 130°C for 3 minutes, the foil was compressed using a roller press to form the positive electrode. The coating weight of the positive electrode active material at this point was 109 g / m². 2 .

[0475] Graphite powder A (density 2.23 g / cm³) will be used as the negative electrode active material. 3 The number-average particle size (12.7 μm) was 87.6% by mass, and the graphite powder B (density 2.27 g / cm³) was also present. 3 A slurry was prepared by dispersing 9.7% by mass of a mixture of cellulose (6.5 μm number average particle size), 1.4% by mass of ammonium salt of carboxymethyl cellulose as a binder (solid content conversion) (solid content concentration 1.83% by mass aqueous solution), and 1.7% by mass of diene rubber latex (solid content conversion) (solid content concentration 40% by mass aqueous solution) in purified water. The slurry was then coated onto one side of a 12 μm thick copper foil, which would serve as the negative electrode current collector, using a die coater. After drying at 120°C for 3 minutes, the foil was compressed using a roller press to form the negative electrode. The coating amount of the negative electrode active material was 5.2 g / m³. 2 .

[0476] Preparation of non-aqueous electrolyte for rate performance and cycling performance testing

[0477] A non-aqueous electrolyte was prepared by dissolving LiPF6 as a solute at a concentration of 1.0 mol / L in a mixed solvent containing 1 wt% vinylene carbonate and ethyl methyl carbonate in a ratio of 1:2 (volume ratio).

[0478] <Battery Assembly>

[0479] Cut the separator or substrate into 24mm φ circles, and cut the positive and negative electrodes for rate and cycle performance testing into 16mm φ circles respectively. Stack the negative electrode, separator or substrate, and positive electrode in sequence with the active material surfaces of the positive and negative electrodes facing each other, and place them in a covered stainless steel container. The container and lid are insulated; the container is in contact with the copper foil of the negative electrode, and the lid is in contact with the aluminum foil of the positive electrode. Pour 0.4mL of non-aqueous electrolyte for rate and cycle performance testing into the container and seal it, thus assembling a simple battery (energy storage device).

[0480] <Evaluation of the production of the roll>

[0481] On an acrylonitrile-butadiene-styrene (ABS) core with an outer diameter of 6 inches, the separator of the sample is wound 4000m so that the entire surface of the roll becomes the second main surface of the porous substrate, thus producing a separator roll sample for evaluation.

[0482] Regarding the evaluation roll for the pressure evaluation test, the evaluation roll is manufactured in the same manner as described above, except that a sensor piece (Nitta Corporation FlexiForce A201-25) is attached to the core.

[0483] It should be noted that the winding tension when the separator is wound onto the spool is 0.10 N / mm in Example 15, 0.15 N / mm in Example 16, and 0.06 N / mm in other examples.

[0484] <Stripping charge when the separator is discharged from the separator drum>

[0485] After the separator is fed 3000m from the circular evaluation drum, a 50m separator is stretched along the tangent of the drum and fed out at a speed of 10m / min. The stripping charge at this time is measured and its average value is calculated.

[0486] For the point where the separator leaves the roll (hereinafter referred to as the peel point), an electrostatic discharge meter (model: FMA-004, manufactured by Simco Japan Co., Ltd.) is installed at a position 20 mm in the direction in which the separator is fed out and 25 mm in the direction perpendicular to the surface of the fed separator to measure the peel charge. The measurement is performed in an environment with a temperature of 23°C and a humidity of 20%.

[0487] Porous substrates are more likely to carry a negative charge than layers containing inorganic fillers. Therefore, when the porous substrate side is facing the electrostatic meter, the value is negative, while when the inorganic filler side is facing the electrostatic meter, the value is positive.

[0488] It should be noted that, in the embodiments, all measurements were performed on the surface of the porous substrate, so all measured values ​​are below 0.

[0489] <Electrostatic Adhesion>

[0490] After feeding a 3000m section of separator from a circular evaluation roll, the separator is stretched tangentially along the roll at a speed of 10m / min. The proportion of the separator pulled towards the roll after being cut with scissors at a distance of 20cm from the peel point is used as an indicator of electrostatic adhesion. Measurements were performed at 23°C and 20% humidity. If the evaluation is A to C, it is suitable for use as a separator in this embodiment.

[0491] A: In a roll of 100, electrostatic adhesion occurs in 15 or fewer rolls.

[0492] B: Of 100 rolls, more than 15 rolls but less than 30 rolls experienced electrostatic adhesion.

[0493] C: Out of 100 rolls, more than 30 rolls but less than 50 rolls are subject to electrostatic adhesion.

[0494] D: Out of 100 rolls, more than 50 rolls experienced electrostatic adhesion.

[0495] <Innermost pressure of the drum>

[0496] After fabricating the evaluation roll, the resistance applied to the sensor sheet was measured using a digital multimeter (SANWA RD701). The pressure of the innermost layer was calculated by applying the measured resistance value to a pre-prepared standard curve.

[0497] While applying a certain pressure to the pressure-sensitive part of the sensor plate, the resistance value measured by a digital multimeter is repeatedly recorded while the pressure applied to the sensor plate is changed. The pressure and resistance values ​​are then plotted on a graph to create a standard curve. It should be noted that the standard curve is created by plotting data with pressures above 0 MPa and below 5 MPa at least 5 points.

[0498] <Magnification Characteristics>

[0499] The initial charging (first charge) of the battery after assembly was performed for a total of approximately 6 hours using the following method: The assembled simple battery was charged at 25°C with a current of 3mA (approximately 0.5C) to a battery voltage of 4.2V, and then the current was gradually reduced from 3mA while maintaining the 4.2V voltage. Then, it was discharged at a current of 3mA to a battery voltage of 3.0V. Next, a total charging was performed for approximately 3 hours using the following method: The battery was charged at 25°C with a current of 6mA (approximately 1.0C) to a battery voltage of 4.2V, and then the current was gradually reduced from 6mA while maintaining the 4.2V voltage. Then, the discharge capacity when discharging at a current of 6mA to a battery voltage of 3.0V was taken as the 1C discharge capacity (mAh). Next, a total charging was performed for approximately 3 hours using the following method: The battery was charged at 25°C with a current of 6mA (approximately 1.0C) to a battery voltage of 4.2V, and then the current was gradually reduced from 6mA while maintaining the 4.2V voltage. Then, the discharge capacity when discharging to a battery voltage of 3.0V at a current of 12mA (approximately 2.0C) is taken as the 2C discharge capacity (mAh). Next, the ratio of the 2C discharge capacity to the 1C discharge capacity is calculated, and this value is used as the rate capability. It should be noted that in the charging and discharging of a simple battery at 25°C, a current of 6mA is approximately 1C.

[0500] If the rating is A to B, it can be used as a separator in this embodiment.

[0501] Rate capability (%) = (2C discharge capacity / 1C discharge capacity) × 100

[0502] Evaluation Criteria

[0503] A (Good): Rate capability exceeds 85%.

[0504] B (Acceptable): Ratio characteristics exceeding 80% but below 85%

[0505] C (Poor): Rate capability below 80%

[0506] <Cyclic Characteristics>

[0507] For the battery that has undergone the above-described rate characteristics, it is discharged at a discharge current of 1C to a discharge termination voltage of 3V at a temperature of 45°C, and then charged at a charging current of 1C to a charging termination voltage of 4.2V. This is considered one cycle, and the charge-discharge cycle is repeated. Then, the cycle characteristics are evaluated according to the following criteria using the capacity retention rate after 300 cycles relative to the initial capacity (capacity in the first cycle). If the evaluation is A to B, it can be used as a separator in this embodiment.

[0508] A (Good): Capacity maintenance rate of over 65%

[0509] B (Acceptable): Capacity maintenance rate of 60% or more but less than 65%

[0510] C (Poor): Volume maintenance rate less than 60%

[0511] <Preparation of Thermoplastic Polymers>

[0512] <Preparation of thermoplastic polymer a1>

[0513] In a reaction vessel equipped with a stirrer, reflux condenser, dropping tank, and thermometer, 70.4 parts by mass of ion-exchanged water, 0.5 parts by mass of "Aqualon KH1025", and 0.5 parts by mass of "ADEKA REASOAP SR1025" were added as initial feedstock, and the internal temperature of the reaction vessel was raised to 95°C. Then, while maintaining the internal temperature of the vessel at 95°C, 7.5 parts by mass of ammonium persulfate (2% aqueous solution) (referred to as "APS(aq)" in the table, the same below) were added.

[0514] On the other hand, an emulsion was prepared by homogenizing a mixture of 0.1 parts by weight of methacrylic acid (MAA), 0.1 parts by weight of acrylic acid (AA), 38.5 parts by weight of methyl methacrylate (MMA), 19.6 parts by weight of n-butyl acrylate (BA), 31.9 parts by weight of 2-ethylhexyl acrylate (EHA), 2 parts by weight of 2-hydroxyethyl methacrylate (HEMA), 5 parts by weight of acrylamide (AM), 2.8 parts by weight of glycidyl methacrylate (GMA), 0.7 parts by weight of trimethylolpropane triacrylate (A-TMPT) (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 0.3 parts by weight of γ-methacryloyloxypropyltrimethoxysilane (AcSi), 3.0 parts by weight of KH1025, 3.0 parts by weight of SR1025, 0.05 parts by weight of sodium p-styrene sulfonate (NaSS), 7.5 parts by weight of ammonium persulfate (2% aqueous solution), and 52 parts by weight of deionized water for 5 minutes. The obtained emulsion was added dropwise from the dropping tank to the above-mentioned reaction vessel. Dropping began 5 minutes after adding the ammonium persulfate aqueous solution to the reaction vessel, and the entire emulsion was added over 150 minutes. During the dropwise addition of the emulsion, the internal temperature of the vessel was maintained at 80°C. Meanwhile, the stir bar, which had been pre-placed in the reaction vessel, was continuously stirred using a magnetic stirrer.

[0515] After the emulsion was added dropwise, the internal temperature of the reaction vessel was maintained at 80°C for 90 minutes, and then cooled to room temperature to obtain the emulsion. The pH of the obtained emulsion was adjusted to 9.0 using an ammonium hydroxide aqueous solution (25% aqueous solution), yielding a 40% acrylic copolymer latex (thermoplastic polymer a1). The glass transition temperature (Tg) of the thermoplastic polymer a1 was evaluated using the method described above. The results are shown in Table 3-1 below.

[0516] <Preparation of thermoplastic polymers a2~a4>

[0517] As shown in Table 3-1, the composition of the emulsion was changed, and thermoplastic polymers a2 to a4 were obtained in the same manner as thermoplastic polymer a1. The glass transition temperature (Tg) was evaluated using the method described above. The results are shown in Table 3-1.

[0518] Thermoplastic polymers a1 to a4 were mixed in the combinations and proportions described in Table 3-2 to prepare coatings A1 to A3 containing thermoplastic polymers. The volume average particle sizes (D10, D50, and D90) of the obtained coatings A1 to A3 containing thermoplastic polymers were determined using the method described above. The results are shown in Table 3-2.

[0519] <Explanation of abbreviations in the table>

[0520] Emulsifier

[0521] KH1025: "AQUALON KH1025" registered trademark, manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd., 25% aqueous solution.

[0522] SR1025: A registered trademark of "ADEKA REASOAP SR1025", manufactured by ADEKA Co., Ltd., 25% aqueous solution.

[0523] NaSS: Sodium p-styrenesulfonate

[0524] Initiator

[0525] APS(aq): Ammonium persulfate (2% aqueous solution)

[0526] ·monomer

[0527] MAA: Methacrylic acid

[0528] AA: Acrylic acid

[0529] MMA: Methyl methacrylate

[0530] BA: n-Butyl acrylate

[0531] EHA: 2-Ethylhexyl acrylate

[0532] CHMA: Cyclohexyl methacrylate

[0533] St: Styrene

[0534] AN: Acrylonitrile

[0535] HEMA: 2-Hydroxyethyl methacrylate

[0536] AM: Acrylamide

[0537] GMA: Glycidyl methacrylate

[0538] A-TMPT: Trimethylolpropane triacrylate

[0539] AcSi: γ-methacryloyloxypropyltrimethoxysilane

[0540] <Preparation of slurries containing inorganic fillers>

[0541] The inorganic filler materials listed in Table 2 were dispersed in water to prepare slurries C1 to C4 containing inorganic fillers. The physical properties (average volume particle size D10, D50, and D90) of the inorganic fillers used in slurries C1 to C4 were determined using the method described above. The results are shown in Table 2.

[0542] <Example 1>

[0543] (Manufacturing of polyolefin microporous membrane B1)

[0544] 47 parts by mass of high-density polyethylene (HDPE) homopolymer with an Mv of 700,000, 46 parts by mass of HDPE homopolymer with an Mv of 300,000, and 7 parts by mass of polypropylene homopolymer with an Mv of 700,000 were dry-mixed using a drum mixer. One part by mass of tetramethylmethylene-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate was added as an antioxidant to 99 parts by mass of the resulting polyolefin mixture, and the mixture was dry-mixed again using a drum mixer to obtain a final mixture. The resulting mixture was fed to a twin-screw extruder under a nitrogen atmosphere via a feeder. Separately, liquid paraffin (kinematic viscosity 7.59 × 10⁻⁶ at 37.78°C) was pumped using a plunger pump. -5 m 2 / s) Inject into the extruder barrel. Adjust the feeder and pump operating conditions so that the proportion of liquid paraffin in the total extruded mixture is 68 parts by mass, i.e., the polymer concentration is 32 parts by mass.

[0545] Next, the materials were melt-blended in a twin-screw extruder while being heated to 160°C. The resulting melt-blended material was extruded through a T-die onto a cooling roller with a surface temperature controlled at 80°C, allowing the extrudate to contact the cooling roller and be cast. After cooling and solidification, a sheet-like material was obtained. This sheet was then stretched using a biaxial stretching machine under the specified ratio and temperature conditions for the properties of B1 as described in Table 1. After being immersed in dichloromethane to remove the liquid paraffin, the sheet was dried and stretched again using a tenter frame under the specified temperature and ratio conditions for the properties of B1 as described in Table 1. Finally, the stretched sheet was relaxed by approximately 10% in the width direction and then heat-treated to obtain the polyolefin microporous membrane B1.

[0546] For the obtained polyolefin microporous membrane B1, its physical properties (membrane weight per unit area, porosity, air permeability, and thickness, etc.) were determined as needed using the methods described above. The results are shown in Table 1.

[0547] (Manufacturing of polyolefin microporous membrane B2)

[0548] By appropriately modifying the manufacturing conditions to meet the physical properties shown in Table 1 (membrane weight per unit area, porosity, air permeability, and thickness, etc.), polyolefin microporous membrane B2 was obtained in the same manner as B1. The physical properties of the obtained polyolefin microporous membrane B2 were evaluated using the methods described above. The results are shown in Table 1.

[0549] <Example 1>

[0550] On one side of the polyolefin microporous membrane B1 (in one embodiment, the first main side of the substrate), a slurry C1 containing inorganic fillers, as shown in Table 2, is coated with a coating thickness of 1.5 μm to form a layer containing inorganic fillers. Then, on the surface of the layer containing inorganic fillers, a coating A1 containing thermoplastic polymers, as shown in Table 3-2, is applied by gravure coating to form a coating layer with a thickness t as shown in Table 4. c and coverage area ratio S c The layer containing thermoplastic polymer (layer 1 in the table).

[0551] Additionally, on the other side of the polyolefin microporous membrane B1 (in one embodiment, the second main surface of the substrate), a coating A1 containing a thermoplastic polymer is applied by gravure coating to form a coating layer with a thickness t as shown in Table 4. p and coverage area ratio S p The layer containing thermoplastic polymer (the second layer in the table).

[0552] Thus, a separator for an energy storage device is obtained, which has a layer containing a thermoplastic polymer in a dot pattern on the surface of a layer containing inorganic fillers and a polyolefin microporous membrane.

[0553] The properties of the obtained separators were evaluated using the methods described above, and the results are shown in Table 4.

[0554] (A layer containing thermoplastic polymer is uniformly dispersed and coated on a polyolefin microporous membrane or a layer containing inorganic fillers)

[0555] Uniform dispersion coating is performed by applying a coating containing thermoplastic polymers evenly to the entire surface of a polyolefin microporous membrane or a layer containing inorganic fillers using gravure coating or rod coating.

[0556] <Examples 2-21, Comparative Examples 1-8>

[0557] Except for changes to the polyolefin microporous membrane, the slurry containing inorganic fillers, the coating containing thermoplastic polymers, the coating shape of the thermoplastic polymer layer, the coverage area ratio of the thermoplastic polymer, and the coating thickness of the thermoplastic polymer layer, as shown in Table 4, a separator for an energy storage device was obtained similarly to Example 1, having a thermoplastic polymer layer (first layer) on the surface of the inorganic filler layer and a thermoplastic polymer layer (second layer) on the second main surface of the polyolefin microporous membrane. The physical properties of the obtained separator were evaluated using the methods described above. The results are also shown in Table 4.

[0558] [Table 1]

[0559]

[0560] [Table 2]

[0561]

[0562] [Table 3-1]

[0563]

[0564] [Table 3-2]

[0565]

[0566] [Table 4-1]

[0567]

[0568] [Table 4-2]

[0569]

[0570] [Table 4-3]

[0571]

[0572] [Table 4-4]

[0573]

[0574] [Table 4-5]

[0575]

[0576] [Table 4-6]

[0577]

[0578] [Table 4-7]

[0579]

[0580] [Table 4-8]

[0581]

Claims

1. A separator for an energy storage device, comprising: a porous substrate, A layer containing inorganic filler disposed on the first main surface of the porous substrate, and A layer containing a thermoplastic polymer disposed on the surface of the layer containing inorganic fillers and on the second main surface of the porous substrate. The coverage area S of the thermoplastic polymer-containing layer on the surface of the inorganic filler-containing layer c Between 30% and 100%, The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p More than 0% and less than 30%, The thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer c The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy t c / t p The relationship is >1.

00.

2. The separator for an energy storage device according to claim 1, wherein, The coverage area S of the thermoplastic polymer-containing layer on the surface of the inorganic filler-containing layer c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfy S c / S p Relationship ≥2.

00.

3. The separator for an energy storage device according to claim 1 or 2, wherein, The coverage area S of the thermoplastic polymer-containing layer on the surface of the inorganic filler-containing layer c The coverage area S of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Satisfying 55%≤S c +S p A relationship of ≤75%.

4. The separator for an energy storage device according to claim 1 or 2, wherein, The inorganic filler particle size contained in the layer satisfies 1.0 ≤ D90 / D10 ≤ 5.

0. The thermoplastic polymer contained in the layer on the second main surface of the porous substrate has a particle size that satisfies the relationship 1.0≤D90 / D10≤5.

0.

5. The separator for an energy storage device according to claim 1 or 2, wherein, The stripping charge when the coil is discharged from the drum is above -15kV and below +15kV.

6. A reel formed by winding the energy storage device according to claim 1 or 2 using a separator, wherein, The surface pressure applied to the innermost layer is below 5 MPa.

7. The separator for an energy storage device according to claim 1 or 2, which is obtained by coating the surface of the porous substrate or the layer containing the inorganic filler disposed on the porous substrate with an aqueous slurry comprising a thermoplastic polymer.

8. The separator for an energy storage device according to claim 1 or 2, wherein, The thermoplastic polymer-containing layer is arranged in a dotted pattern.

9. The separator for an energy storage device according to claim 1 or 2, wherein, The layer containing the thermoplastic polymer comprises a copolymer of monomer units containing (meth)acrylate monomers.

10. An energy storage device comprising a separator, a positive electrode, a negative electrode, and a non-aqueous electrolyte as described in claim 1 or 2.

11. The separator for an energy storage device according to claim 1 or 2, wherein, The thickness t of the thermoplastic polymer layer on the surface of the inorganic filler layer c Standard deviation s tc The thickness t of the thermoplastic polymer-containing layer on the second main surface of the porous substrate p Standard deviation s tp Satisfy s tc / s tp The relationship is greater than 1.

0.

12. A method for manufacturing a separator for an energy storage device according to claim 1 or 2, comprising: The process of preparing porous substrates; The process of forming an inorganic filler-containing layer by coating a slurry containing inorganic fillers onto the first main surface of the porous substrate; and The process of forming a thermoplastic polymer layer by coating a slurry containing a thermoplastic polymer onto the surface of the inorganic filler layer and the second main surface of the porous substrate. The viscosity of the slurry containing the thermoplastic polymer is at a shear rate of 60,000 sec. -1 The values ​​are above 1 mPa·s and below 20 mPa·s. The shear rate v when the slurry containing the thermoplastic polymer is coated on the surface of the layer containing inorganic fillers. c The shear rate v when the slurry containing the thermoplastic polymer is coated on the second main surface of the porous substrate p Satisfying the relationship between equations (2) and (3), 30000sec -1 ≤v c ≤200000sec -1 …Formula (2) 5000sec -1 ≤v c -v p ≤40000sec -1 …Formula (3).

Citation Information

Patent Citations

  • Separator for energy storage device, laminated body, and porous membrane

    WO2014017651A1