A thermal insulation nano-ceramic coating and its preparation method
By using phenylboronic acid-modified acrylate emulsion, o-diol-grafted silica aerogel, and slow-release composite microspheres in nano-ceramic thermal insulation coatings to construct a dynamic cross-linking network, the problem of insufficient interfacial bonding strength between inorganic fillers and organic resin matrix is solved, achieving long-lasting thermal insulation and self-healing properties.
Patent Information
- Application Number
- CN202611192087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-08-07
AI Technical Summary
Existing nano-ceramic thermal insulation coatings have limited interfacial bonding strength between inorganic thermal insulation fillers and organic resin matrix under long-term hot and cold alternating service conditions. This makes them prone to microcracks that lead to performance degradation, thus limiting their long-term service performance and large-scale application.
Using phenylboronic acid-modified acrylate emulsion as the film-forming matrix, combined with vicinal glycol-grafted silica aerogel, modified nanocellulose, and slow-release composite microspheres, the interfacial bonding strength is enhanced through the Knudsen effect and dynamic cross-linking network to construct a multi-level thermal insulation network, achieving long-term thermal insulation.
It effectively improves the interfacial bonding strength and thermal insulation performance of the coating, and has long-term thermal insulation and active self-healing capabilities, adapting to the needs of long-term service conditions.
Smart Images

Figure CN122686193B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating technology, and in particular to a heat-insulating nano-ceramic coating and its preparation method. Background Technology
[0002] With the continuous increase in demand for building energy conservation and industrial equipment insulation, high-efficiency thermal insulation materials have become one of the core technological paths to reduce building operating energy consumption and industrial equipment heat loss. Thermal insulation coatings, with their outstanding advantages such as convenient construction, compatibility with irregularly shaped substrates, no splicing thermal bridges, and controllable overall costs, are gradually replacing some traditional block insulation materials and are widely used in diverse scenarios such as building exterior walls, petrochemical storage tanks, thermal pipelines, and cold chain warehousing. Among them, nano-ceramic thermal insulation coatings, by introducing nano-scale ceramic functional fillers, hollow thermal insulation microspheres, and other components to construct a multi-level thermal barrier structure, combined with the film-forming protective properties of organic film-forming resins, possess characteristics such as lightweight and ultra-thinness, fire resistance, and UV aging resistance, making them a research hotspot in the field of thermal insulation coatings in recent years. The industry typically optimizes the heat conduction path by compounding hollow fillers and aerogels of different sizes, or by surface modification of fillers to improve their dispersibility in the resin matrix, thereby further improving the thermal insulation efficiency and mechanical properties of the coating. However, the interfacial bonding strength between inorganic thermal insulation fillers and organic resin matrix is limited. Under long-term hot and cold alternating service, microcracks are easily generated and performance degradation is caused, which restricts the long-term service performance and large-scale application of the coating. Summary of the Invention
[0003] To address the shortcomings of existing technologies, the present invention aims to provide a thermally insulating nano-ceramic coating and its preparation method. Using a phenylboronic acid-modified acrylate emulsion as the film-forming matrix, and vicinal diol-grafted silica aerogel and slow-release composite microspheres as fillers, combined with modified nanocellulose, a thermally insulating nano-ceramic coating is prepared. The aerogel nanopores achieve basic thermal insulation through the Knudsen effect, with the vicinal diol on the surface forming reversible borate ester bonds with the phenylboronic acid groups in the matrix to construct a dynamic cross-linked network. The modified nanocellulose forms a suspended mesh through hydrogen bonds to support lightweight fillers, and its phenylboronic acid groups participate in cross-linking, ensuring the network is fully interconnected. The slow-release composite microspheres construct a multi-level thermal insulation network with hollow cavities and aerogel nanopores. A mesoporous silica coating layer protects the integrity of the cavities. The phenylboronic acid pinacol ester loaded within the pores hydrolyzes and releases phenylboronic acid during crack seepage, acting as a supplementary boron source to promote coordination balance and repair micro-damage, thus meeting the requirements of long-term service conditions.
[0004] To achieve the above objectives, the present invention employs the following technical solution:
[0005] In a first aspect, the present invention provides a thermal insulation nano-ceramic coating, the coating comprising phenylboronic acid modified acrylate emulsion, vicinal glycol grafted silica aerogel, modified nanocellulose, slow-release composite microspheres, rutile titanium dioxide, and additives.
[0006] The phenylboronic acid modified acrylate emulsion is obtained by emulsion polymerization of acrylate monomers and 3-acrylamidophenylboronic acid; the acrylate monomers include butyl acrylate, methyl methacrylate, acrylic acid and dimethylaminoethyl methacrylate.
[0007] The vicinal diol-grafted silica aerogel is obtained by grafting hydrophobic silica aerogel with KH560 and then performing ring-opening hydrolysis under acidic conditions to generate vicinal diol groups.
[0008] The modified nanocellulose is obtained by grafting nanocellulose with a methyltrimethoxysilane hydrophobically modified intermediate and a phenylboronic acid silane intermediate; the phenylboronic acid silane intermediate is obtained by reacting 3-aminophenylboronic acid and KH560 in the dark.
[0009] The sustained-release composite microspheres are obtained by coating a mesoporous silica layer with hollow glass microspheres as the core, CTAB as the template and TEOS as the silicon source, using a sol-gel method, followed by hydrophobic modification with dimethyltrimethoxysilane and vacuum impregnation in an impregnation solution; the impregnation solution includes pinacol phenylboronic acid ester and anhydrous ethanol.
[0010] The additives include dispersants, wetting agents, defoamers, bactericides, film-forming aids, and pH buffers.
[0011] Further, the dispersant includes sodium polyacrylate and polycarboxylate; the wetting agent is acetylenic diol; the defoamer is organosilicon; the bactericide is isothiazolinone; the film-forming aid is dodecyl alcohol ester; the pH buffer includes sodium bicarbonate and sodium carbonate; the mass ratio of the phenylboronic acid modified acrylate emulsion, vicinal diol grafted silica aerogel, modified nanocellulose, sustained-release composite microspheres, rutile titanium dioxide and the additives is (30-50):(3-6):(1.0-2.5):(4.0-8.0):(3.0-8.0):(1.18-3.03).
[0012] Furthermore, the nanocellulose is cellulose nanofiber with a diameter of 20-50 nm, a length of 2-10 μm, and an aspect ratio ≥100; the 3-aminophenylboronic acid is in free acid form; and the hydrophobic silica aerogel has a particle size of 50-200 μm and a BET specific surface area of 600-800 m². 2 / g, water contact angle >150°; the hollow glass microspheres are borosilicate hollow glass microspheres with a particle size of 20-60μm and a true density of 0.3-0.5g / cm³. 3The rutile titanium dioxide is KRONOS R-2220 rutile titanium dioxide produced by the chloride process. The inorganic coating is made of aluminum and silicon composite coating, and the surface is treated with hydrophobic organic polysiloxane. The average particle size is 200-300nm. The polycarboxylate is SN-5040. The organosilicon is BYK-024.
[0013] Secondly, the present invention provides a method for preparing a thermal insulation nano-ceramic coating, comprising the following steps:
[0014] S1. 3-Aminophenylboronic acid and KH560 were reacted in anhydrous ethanol in the dark to obtain a phenylboronic acid silane intermediate; nanocellulose was dispersed in an aqueous ethanol solution, the pH was adjusted, and monomethyltrimethoxysilane was added dropwise. The reaction was carried out under heat, and after centrifugation and washing, the nanocellulose was redispersed, the pH was adjusted, and the phenylboronic acid silane intermediate was added dropwise. The reaction was carried out, and after centrifugation, washing, and drying, modified nanocellulose was obtained.
[0015] S2. Prepare silane prehydrolysis solution; Dissolve Pluronic F127 in deionized water, add hydrophobic silica aerogel and dilute ammonia in sequence, add the silane prehydrolysis solution dropwise, heat and react, filter, wash, adjust pH, react, filter under reduced pressure, rinse and dry to obtain 1,4-diol grafted silica aerogel.
[0016] S3. Prepare the modification solution and impregnation solution; add hollow glass microspheres to dilute hydrochloric acid, wash, dry to obtain pretreated microspheres, add ethanol aqueous solution, adjust pH, add CTAB, add anhydrous ethanol solution of TEOS dropwise, react, extract, modify with the modification solution, drain, rinse, place in the impregnation solution for vacuum impregnation, filter, wash, and dry to obtain sustained-release composite microspheres;
[0017] S4. Ammonium persulfate is added to deionized water to obtain initiator A, and sodium bisulfite is added to deionized water to obtain initiator B; acrylate monomer, 3-acrylamidophenylboronic acid, n-dodecyl mercaptan, sodium dodecyl sulfate, OP-10 and deionized water are mixed to obtain a pre-emulsion; a portion of the pre-emulsion, initiator A and initiator B are mixed, heated, the remaining pre-emulsion is added dropwise, matured, cooled, sodium bicarbonate and sodium carbonate are added, and filtered to obtain a phenylboronic acid modified acrylate emulsion;
[0018] S5. Dissolve sodium bicarbonate, sodium carbonate, sodium polyacrylate and acetylacetonate in deionized water, add phenylboronic acid modified acrylate emulsion, add aerogel suspension dropwise, add polycarboxylate, dodecyl alcohol ester, organosilicon and isothiazolinone in sequence, add cellulose suspension, add slow-release composite microspheres and rutile titanium dioxide in batches, adjust pH, measure viscosity and filter to obtain thermal insulation nano-ceramic coating.
[0019] In one feasible implementation, in S1, the mass-to-volume ratio of 3-aminophenylboronic acid, KH560, and anhydrous ethanol is (8-12) g:(13-20) g:(80-120) mL; the temperature of the light-protected reaction is 45-55℃, and the time of the light-protected reaction is 2-4 h; the mass-to-volume ratio of nanocellulose, monomethyltrimethoxysilane, phenylboronic acid silane intermediate, and ethanol aqueous solution is (1.5-2.5) g:(0) mL. 0.3-0.8)g : (0.4-0.8)g : (350-450)mL; the volume ratio of anhydrous ethanol to deionized water in the ethanol aqueous solution is 7:3; the pH adjustment reagent is 0.5mol / L glacial acetic acid, and the pH is adjusted to 4.5-5.0; the rate of adding methyltrimethoxysilane is 0.15-0.25g / min; the temperature of the heat preservation reaction is 35-45℃, and the heat preservation reaction time is 2-4h.
[0020] In one feasible implementation, in step S1, the centrifugal washing step is as follows: centrifugation at 7000-9000 rpm for 15-25 min, followed by resuspending the precipitate in anhydrous ethanol and washing three times, with 80-120 mL of anhydrous ethanol used each time; the redispersing medium is 400-600 mL of an ethanol-water solution, wherein the volume ratio of anhydrous ethanol to deionized water in the ethanol-water solution is 95:5; after redispersing, the pH-adjusting reagent is 0.5 mol / L glacial acetic acid, and the pH is adjusted to 4.8-5.2. The addition of the phenylboronic acid silane intermediate takes 10-30 minutes; after the addition of the phenylboronic acid silane intermediate, the reaction temperature is 25-35°C, and the reaction time is 3-5 hours; the centrifugation speed is 7000-9000 rpm, and the centrifugation time is 15-25 minutes; the washing step is as follows: the precipitate is washed three times with anhydrous ethanol, 150-250 mL each time; the drying is vacuum drying, the drying temperature is 35-45°C, and the drying time is 10-15 hours.
[0021] The primary amino nitrogen atom on the benzene ring of 3-aminophenylboronic acid has a lone pair of electrons, exhibiting nucleophilicity, while the terminal epoxy group of the KH560 molecule has a three-membered ring structure with a carbon-oxygen bond angle of approximately 60°, much lower than sp. 3 The ideal bond angle of the hybrid carbon atom is 109.5°. Significant angle strain puts the three-membered ring in a high-energy unstable state. Furthermore, carbon-oxygen bond polarization causes the carbon atom to carry a partial positive charge. Under heating conditions, the lone pair electrons of the amino nitrogen atom launch a nucleophilic attack on the carbon atom with less steric hindrance in the epoxy group, causing the carbon-oxygen bond to break and the three-membered ring to open via an SN2 mechanism. This generates a bifunctional phenylboronic acid silane intermediate that carries both phenylboronic acid reaction sites and a hydrolyzable trimethoxysilane group. This intermediate allows the phenylboronic acid group to be covalently grafted onto the surface of an inorganic support via a silane condensation reaction.
[0022] Nanocellulose possesses a high aspect ratio and abundant surface hydroxyl groups. Its cellulose chains can interlock to form a suspended network through intermolecular hydrogen bonds. However, its strong hydrophilicity makes it prone to aggregation and instability in weakly alkaline emulsion systems, requiring prior hydrophobic modification. Under acidic conditions provided by glacial acetic acid, the methoxy group of methyltrimethoxysilane is protonated and activated. Water molecules nucleophilically replace the methoxy group to generate a silanol intermediate. The silanol further undergoes a condensation reaction with the hydroxyl groups on the surface of cellulose nanofibers to form a siloxane covalent bond, introducing a methyl hydrophobic layer on the fiber surface. This acidic condition simultaneously regulates the silanol condensation rate to a moderate range, preventing excessive self-condensation of methyltrimethoxysilane to form oligomers and reduce the effective grafting rate on the fiber surface. The hydrophobically modified fiber surface still retains some incompletely condensed silanol groups. This is because the grafted methyltrimethoxysilane molecules form a dense hydrophobic layer on the fiber surface, creating steric hindrance, making it difficult for adjacent silanol groups to approach and condense further. This provides active reaction sites for the subsequent covalent grafting of phenylboronic acid silane intermediates. The trimethoxysilane group of the phenylboronic acid silane intermediate hydrolyzes under the same acidic conditions to generate silanol, which undergoes intermolecular condensation with silanol, covalently grafting the phenylboronic acid group onto the nanocellulose.
[0023] The modified nanocellulose thus prepared plays a triple role in the coating system: the intermolecular hydrogen bonds of the cellulose chains form a continuous suspended network that effectively supports both aerogel and composite microspheres, two types of lightweight fillers, preventing storage sedimentation; the surface methyl hydrophobic layer ensures its uniform dispersion in weakly alkaline emulsions to maintain the integrity of the hydrogen bond network; and the grafted phenylboronic acid groups simultaneously participate in the coordination crosslinking of borate esters, connecting the polymer segments between the rigid nodes of the aerogel, enabling the dynamic crosslinking network to achieve full connectivity from the molecular scale to the micrometer scale.
[0024] In one feasible implementation, the step of preparing the silane pre-hydrolyzed solution in S2 is as follows: 0.3-0.8g KH560, 1-3mL deionized water and 5-12mL anhydrous ethanol are mixed, and the pH is adjusted to 8.5 with 0.1mol / L dilute ammonia. The mixture is pre-hydrolyzed at room temperature for 10-30min. The mass-volume ratio of Pluronic F127, hydrophobic silica aerogel, dilute ammonia and deionized water is (0.05-0.15)g:(3-5)g:(3-8)mL:(350-450)mL. The concentration of the dilute ammonia is 0.1mol / L. The time for adding the silane pre-hydrolyzed solution is 0.5-1.5h. The target temperature for the heating reaction is 45-55℃, and the heating reaction time is 2-4h.
[0025] In one feasible implementation, in step S2, the filtration condition is a vacuum of -0.08 to -0.09 MPa; the washing step is as follows: the filter cake is rinsed twice with deionized water and redispersed in 350-450 mL of deionized water; the pH adjustment reagent is 0.5 mol / L glacial acetic acid, and the pH is adjusted to 4.0; after pH adjustment, the reaction temperature is 45-55℃, and the reaction time is 1.5-3 h; the vacuum filtration condition is a vacuum of -0.08 to -0.09 MPa; the rinsing step is as follows: the filter cake is rinsed three times with deionized water and once with anhydrous ethanol, each time using 80-120 mL; the drying is vacuum drying, the drying temperature is 35-45℃, and the drying time is 10-15 h.
[0026] Hydrophobic silica aerogels have a nanoporous framework, and the pore size of the internal nanopores is smaller than the mean free path of air molecules under normal pressure. The movement of gas molecules in the pores is restricted, and collisions mainly occur between molecules and pore walls rather than between molecules, i.e., the Knudsen effect. Gas thermal conduction is effectively suppressed, providing basic thermal insulation for the coating. However, aerogels without surface functionalization are only dispersed in the matrix as inert fillers. They lack chemical bonding with the polymer matrix, resulting in weak interfacial adhesion. During long-term service, interfacial debonding is prone to occur, leading to performance degradation. KH560 undergoes hydrolysis under weakly alkaline conditions provided by dilute ammonia, converting the trimethoxysilyl group into silanol, which then condenses with the silanol on the aerogel surface to form a siloxane bond, covalently grafting the epoxy group onto the aerogel surface. Subsequently, under the catalysis of glacial acetic acid, the epoxy oxygen atom is protonated, activating the three-membered ring. Water molecules nucleophilically attack the epoxy ring, causing it to open, generating a vicinal diol structure. This transforms the inert epoxy group into a coordinatingly active vicinal diol crosslinking anchor. The glacial acetic acid catalytic pathway is mild, with a low risk of corrosion to the aerogel nanoporous framework, which is beneficial for maintaining the integrity of the pore structure.
[0027] In a weakly alkaline system, the vicinal diol grafted onto the aerogel surface acts as a bidentate ligand, chelating with the phenylboronic acid groups of the emulsion matrix. The boron atom of phenylboronic acid coordinates with the two hydroxyl oxygen atoms of the vicinal diol to form a five-membered ring borate ester bond. The aerogel particles act as rigid nodes, connecting the polymer chains into a dynamic cross-linked network, which significantly improves the interfacial bonding strength between the inorganic filler and the organic matrix. When the coating is subjected to thermal cycling or external deformation and microcracks are generated, the mechanical stress at the crack tip causes the local borate ester bonds to preferentially dissociate. The exposed free phenylboronic acid and the vicinal diol groups rechelate in a weakly alkaline environment through reversible coordination equilibrium, providing active chemical protection for the coating against the accumulation of micro-damage during long-term service.
[0028] In one feasible implementation, in step S3, the step of preparing the modified solution is as follows: dissolving 0.005g of glacial acetic acid and 0.8-1.5g of methyltrimethoxysilane in 80-120mL of anhydrous ethanol; the step of preparing the impregnation solution is as follows: dispersing 1-2g of pinacol phenylboronic acid in 80-120mL of anhydrous ethanol and stirring at 250-350rpm for 5-15min; the mass-to-volume ratio of the hollow glass microspheres to dilute hydrochloric acid is (25-35)g:( 250-350) mL; the concentration of the dilute hydrochloric acid is 0.1 mol / L; the washing step is: washing with deionized water until pH=7; the drying temperature is 50-70℃, and the drying time is 1.5-3h; the mass-volume ratio of the pretreated microbeads, CTAB, ethanol aqueous solution and TEOS anhydrous ethanol solution is (25-35) g : (0.8-1.5) g : (250-350) mL : (30-50) mL.
[0029] In one feasible implementation, in step S3, the volume ratio of anhydrous ethanol to deionized water in the ethanol-water solution is 30:70; the pH adjustment reagent is 0.1 mol / L dilute ammonia water, and the pH is adjusted to 8.2-8.5; the mass-volume ratio of TEOS to anhydrous ethanol in the anhydrous ethanol solution of TEOS is (1.8-3.0) g: (30-50) mL; the time for adding the anhydrous ethanol solution of TEOS is 0.5-1.5 h; the reaction temperature is 35-45℃, and the reaction time is 2-4 h; the extraction step is as follows: transfer to an ethanol-hydrochloric acid mixture and reflux extract twice at 50-70℃, wherein the volume ratio of anhydrous ethanol to concentrated hydrochloric acid in the ethanol-hydrochloric acid mixture is 95:5, wherein the mass fraction of concentrated hydrochloric acid is 36-38%, 250-350 mL each time, 0.5-1.5 h each time, and wash with deionized water until the pH is 7.
[0030] In one feasible implementation, in step S3, the modification time of the modified liquid is 10-20 min; the rinsing reagent is anhydrous ethanol; the vacuum impregnation step is as follows: vacuuming to -0.09 MPa and maintaining for 20-40 min, restoring to normal pressure within 10-20 min, and then continuing to stand for impregnation for 0.5-1.5 h; the vacuum filtration and washing step is as follows: vacuum filtration under vacuum conditions of -0.05~-0.06 MPa, followed by rinsing twice with anhydrous ethanol, 40-60 mL each time; the drying is vacuum drying, the drying temperature is 20-30℃, and the drying time is 4-8 h.
[0031] Borosilicate hollow glass microspheres, with their internal low-pressure cavities, block heat conduction paths and suppress gas convection heat transfer within the cavities. Together with the nanoporous structure of aerogel, they form a multi-level thermal insulation network from nanopores to micron-sized cavities, enhancing the thermal insulation effect of the coating. However, borosilicate glass microspheres are susceptible to slow erosion in alkaline media; once the microspheres break and the cavity structure is destroyed, the thermal insulation performance is lost. Using CTAB as a template agent, its long-chain cations self-assemble into micellar structures in an aqueous solution on the surface of the microspheres. TEOS undergoes hydrolysis under dilute ammonia alkaline catalysis to generate silica monomers. These silica monomers condense and grow around the micelles, depositing on the surface of the microspheres to form a mesoporous silica coating layer with micelles as templates. Subsequently, reflux extraction is performed in an ethanol-hydrochloric acid mixture. Hydrochloric acid protons replace the electrostatic binding between the hydrophilic head groups of the template agent and the silanol groups, while ethanol dissolves the free template agent molecules from the pores, forming an ordered mesoporous structure. This mesoporous structure provides a carrying space for subsequent loading of active materials.
[0032] Methyltrimethoxysilane undergoes hydrophobic modification of the mesoporous inner surface through hydrolysis and condensation under acidic conditions, introducing a methyl hydrophobic layer into the pore walls. Subsequently, pinacol phenylboronic acid ester is loaded into the mesopores via vacuum-assisted impregnation. The vacuum condition forces the removal of residual air from the mesopores, allowing the pinacol phenylboronic acid ester solution to fully wet the pores. Due to the confinement effect of the hydrophobic pores, the methyl hydrophobic layer on the mesopore inner walls effectively reduces the wetting rate of water molecules in the pores, significantly reducing the hydrolysis rate of pinacol ester in the weakly alkaline storage environment of the coating. It delays the formation of microcracks in the coating and maintains sufficient chemical inertness during normal storage. When moisture seeps into the coating and microcracks develop, the moisture gradually breaks through the hydrophobic mesoporous barrier and enters the pores. The pinacol ester of phenylboronic acid undergoes hydrolysis, releasing phenylboronic acid and pinacol. The released phenylboronic acid acts as a supplementary boron source and directly combines with vicinal diol to form cycloboronic ester bonds, increasing the concentration of phenylboronic acid in the crack area. This promotes the dynamic coordination equilibrium of the boronic ester to shift towards the bonding direction, further enhancing the repair efficiency of the dynamic cross-linked network at the crack and meeting the requirements of long-term service conditions.
[0033] In one feasible implementation, in step S4, the mass-to-volume ratio of ammonium persulfate to deionized water in initiator A is (0.3-0.8) g:(20-40) mL, and the mass-to-volume ratio of sodium bisulfite to deionized water in initiator B is (0.1-0.3) g:(20-40) mL; the mass-to-volume ratio of acrylate monomer, 3-acrylamidophenylboronic acid, n-dodecyl mercaptan, sodium dodecyl sulfate, OP-10, and deionized water is... The volume ratio is (156.8-228.8) g : (6-10) g : (0.1-0.3) g : (1.5-3.0) g : (0.5-1.5) g : (150-200) mL; the mass ratio of butyl acrylate, methyl methacrylate, acrylic acid and dimethylaminoethyl methacrylate in the acrylate monomer is (100-140 : (55-85 : (1.5-3.0 : (0.3-0.8)).
[0034] In one feasible implementation, in step S4, the mass-to-volume ratio of the partial pre-emulsion, the remaining pre-emulsion, sodium bicarbonate, sodium carbonate, initiator A, and initiator B is (30-45) g : (284-398) g : (0.2-0.5) g : (0.05-0.12) g : (20-40) mL : (20-40) mL; the target temperature for heating is 55-65℃; the aging temperature is 55-65℃, and the aging time is 1-2 h; the target temperature for cooling is 35-45℃; and the filtration medium is a 100-mesh filter.
[0035] 3-Acrylamidophenylboronic acid is a bifunctional monomer that carries both acrylamide polymerization sites (carbon-carbon double bonds) and phenylboronic acid reaction sites. In emulsion polymerization, its acrylamide double bonds undergo free radical copolymerization with main monomers such as butyl acrylate and methyl methacrylate, chemically bonding the phenylboronic acid groups to the polymer backbone. This gives the film-forming matrix its own crosslinking reaction sites, avoiding storage instability problems caused by external crosslinking agents. Acrylic acid provides carboxyl groups to enhance the adhesion of the coating to the substrate, while dimethylaminoethyl methacrylate introduces amino functional sites. A redox initiation system composed of ammonium persulfate and sodium bisulfite is used. Persulfate ions and bisulfite ions undergo a single-electron transfer reaction to generate sulfate radical anions. The activation energy of this redox reaction is much lower than that of the thermal decomposition of ammonium persulfate alone. Therefore, sufficient free radicals can be generated to initiate polymerization at a lower temperature, effectively avoiding the thermal degradation or self-condensation side reaction of 3-acrylamidophenylboronic acid under high temperature conditions. This ensures the structural integrity and coordination reactivity of the phenylboronic acid groups. Dodecyl mercaptan, as a chain transfer agent, regulates the polymer molecular weight through chain transfer reaction, avoiding gelation caused by the interaction between phenylboronic acid groups during polymerization. Sodium dodecyl sulfate and OP-10 compound emulsifier provide a suitable micellar environment, ensuring the uniform emulsification and dispersion of monomers, including polar phenylboronic acid monomers.
[0036] As a film-forming matrix for coatings, phenylboronic acid modified acrylate emulsion has phenylboronic acid groups uniformly distributed on its polymer chains, which are the core boron source providers for the dynamic cross-linking network. After the emulsion forms a film, the phenylboronic acid groups on the polymer chains, together with the vicinal diol on the aerogel surface, the phenylboronic acid groups on the modified nanocellulose, and the phenylboronic acid released by the microspheres, constitute the cross-linking reaction system.
[0037] In one feasible implementation, in step S5, the mass ratio of the pH buffer, sodium polyacrylate, wetting agent, polycarboxylate, film-forming aid, defoamer, and bactericide is (0.13-0.33):(0.2-0.5):(0.1-0.3):(0.1-0.25):(0.5-1.2):(0.1-0.3):(0.05-0.15); the mass ratio of sodium bicarbonate to sodium carbonate in the pH buffer is (0.1-0.25):(0.03-0.08); and the mass-to-volume ratio of deionized water, aerogel suspension, and cellulose suspension is (2... 5-40)g: (15-25)mL: (8-12)mL; The preparation steps of the aerogel suspension are as follows: 3.0-6.0g of o-diol-grafted silica aerogel is dispersed in 15-25mL of deionized water to form a suspension; The preparation steps of the cellulose suspension are as follows: 1.0-2.5g of modified nanocellulose is dispersed in 8-12mL of deionized water to form a suspension; The pH adjustment reagent is 0.5mol / L glacial acetic acid, and the pH is adjusted to 7.2-7.5; The viscosity measurement parameters are: 25℃ Fort-4 viscosity is 60-80s; The filtration medium is an 80-mesh nylon sieve.
[0038] The pH of the coating is controlled within a weakly alkaline range using a buffer system composed of sodium bicarbonate and sodium carbonate. Under these conditions, phenylboronic acid mainly exists in the form of triangular boric acid molecules, with its boron atoms arranged in sp... 2 The hybrid planar configuration, with its coordination reaction with vicinal diol in a weak equilibrium state, makes it difficult to form a large number of borate ester bonds, resulting in insufficient construction of the crosslinking network. This ensures the stability of the coating during storage in the can. During film formation, water evaporation causes local enrichment of the alkaline buffer component in the coating, increasing the pH of the system. Phenylboronic acid transforms from a triangular boric acid molecule to a tetrahedral borate ester anion, and boron atoms are converted to sp... 3 The hybrid configuration, with its tetrahedral shape, can directly and rapidly chelate with the two hydroxyl oxygen atoms of the vicinal diol to form a five-membered ring borate bond, promoting the establishment of a crosslinking network in the coating. This pH-controlled delayed crosslinking design achieves an orderly transition from storage stability to film-forming crosslinking, giving the coating both application adaptability and post-film network density.
[0039] During coating formulation, the high refractive index of rutile titanium dioxide effectively reflects near-infrared radiation from the solar spectrum. Combined with the nanoporous barrier of aerogel and the cavity barrier of hollow microspheres, it forms a synergistic heat insulation mechanism of reflection and barrier, reducing the coating's heat conduction and radiation from both reflection and barrier perspectives. Sodium polyacrylate dispersant and acetylacetonate wetting agent successively ensure the initial dispersion and wetting of inorganic fillers in the aqueous phase. Polycarboxylate dispersant further stabilizes the filler suspension system after the addition of aerogel. Modified nanocellulose is added with low-speed stirring to avoid high shear damage to its hydrogen bond network structure. Slow-release composite microspheres and titanium dioxide are added in batches to avoid agglomeration caused by local overload. Dodecyl alcohol ester is used as a film-forming aid to lower the minimum film-forming temperature. Organosilicon defoamer eliminates the encapsulation of air bubbles during the preparation process. Isothiazolinone bactericide ensures the coating's in-tank corrosion protection. In the final system, the phenylboronic acid groups of the emulsion matrix, the vicinal diol anchors of the aerogel, the phenylboronic acid groups of the nanocellulose, and the phenylboronic acid released by the microspheres work together to construct a dynamic cross-linked network that runs from the molecular scale to the micron scale after film formation, giving the coating long-lasting thermal insulation and active self-healing dual service performance.
[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0041] This scheme uses phenylboronic acid-modified acrylate emulsion as the film-forming matrix. By preparing vicinal glycol-grafted silica aerogel and slow-release composite microspheres as fillers, combined with modified nanocellulose, a thermally insulating nano-ceramic coating is obtained, exhibiting both long-lasting thermal insulation and excellent aging resistance. The vicinal glycol-grafted silica aerogel possesses a nanoporous framework. Its internal nanopores, relying on the Knudsen effect, confine air movement within the pore size range, effectively suppressing convective heat transfer and providing basic thermal insulation capabilities for the coating. Simultaneously, the vicinal glycol grafted onto the aerogel surface acts as crosslinking anchors, undergoing bidentate chelate coordination with the phenylboronic acid groups of the matrix in a weakly alkaline system to generate reversible borate ester bonds with a five-membered ring structure. This constructs a dynamic crosslinking network with the aerogel as rigid nodes, enhancing the interfacial bonding strength between the inorganic filler and the matrix. After hydrophobic modification, nanocellulose is grafted with phenylboronic acid groups. The hydroxyl groups of the cellulose chains interlock through intermolecular hydrogen bonds to form a continuous suspended network, which effectively supports both aerogel and composite microspheres, preventing sedimentation during storage. Simultaneously, the phenylboronic acid groups participate in the coordination crosslinking of borate esters, further connecting the polymer segments between aerogel nodes. This allows the dynamic crosslinking network to achieve full connectivity from the molecular to the micrometer scale within the coating. When the coating is subjected to thermal cycling or external deformation, microcracks develop. The mechanical stress at the crack tip causes the local borate ester bonds to preferentially dissociate. The exposed free phenylboronic acid and vicinal diol groups re-chelate under a weakly alkaline environment through reversible coordination equilibrium to form borate ester bonds, providing an active chemical protection mechanism for the coating to resist the accumulation of micro-damage during long-term service.
[0042] The slow-release composite microspheres utilize the low-pressure cavity inside the borosilicate hollow glass microspheres to block the heat conduction path and inhibit the convective heat transfer of gas within the cavity. Together with the nanoporous structure of the aerogel, they form a multi-scale, multi-level thermal insulation network spanning from nanopores to micron cavities, synergistically enhancing the thermal insulation effect of the coating. The mesoporous silica coating layer acts as a physical barrier, preventing direct contact between the weakly alkaline medium of the coating and the glass core material, ensuring the long-term integrity of the hollow cavity structure. Furthermore, the pinacol phenylboronic acid ester loaded within the mesopores is confined by the hydrophobic channels, effectively reducing the amount of water molecules. The coating maintains sufficient chemical inertness to wet the pores during normal storage. When microcracks form in the coating and moisture seeps in, the moisture breaks through the barrier of the hydrophobic mesoporous structure and enters the pores. The pinacol ester of phenylboronic acid undergoes hydrolysis, releasing phenylboronic acid and pinacol. Benzylboronic acid can act as a supplementary boron source and directly combine with vicinal diol to form cycloboronic acid ester bonds, increasing the local concentration of phenylboronic acid in the cracks and promoting the dynamic coordination equilibrium of the boronic acid ester to shift towards the bonding direction. This further enhances the repair efficiency of the dynamic cross-linked network at the cracks, meeting the requirements of long-term service conditions. Attached Figure Description
[0043] Figure 1 This is a physical image of the thermal insulation nano-ceramic coating prepared in Example 1 of the present invention. Detailed Implementation
[0044] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the application will be further described in detail below with reference to embodiments. However, this should not be construed as limiting the scope of this application to the following examples. All other embodiments obtained by those skilled in the art without creative effort without departing from the above-described methodological spirit of this application are within the scope of protection of this application.
[0045] The singular forms “for,” “or,” “a,” “any,” and “described” used in this application are intended to include the plural forms unless the context clearly indicates otherwise. Furthermore, the terms “first” and “second” are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0046] The specifications of the substances involved in the embodiments and comparative examples of this application are as follows:
[0047] Nanocellulose consists of cellulose nanofibers with a diameter of 20-50 nm, a length of 2-10 μm, and an aspect ratio ≥100; 3-aminophenylboronic acid is in free acid form; the hydrophobic silica aerogel has a particle size of 50-200 μm and a BET specific surface area of 600-800 m². 2 / g, water contact angle >150°; the rutile titanium dioxide is KRONOS R-2220 type chloride process rutile titanium dioxide, the inorganic coating is aluminum and silicon composite coating, and the surface is treated with polysiloxane hydrophobic organic treatment; the polycarboxylate is SN-5040; the organosilicon is BYK-024.
[0048] Example 1
[0049] A method for preparing a thermal insulation nano-ceramic coating includes the following steps:
[0050] S1. Mix 10g of 3-aminophenylboronic acid, 16.5g of KH560, and 100mL of anhydrous ethanol, stir at 300rpm, and react at 50℃ in the dark for 3h to obtain a phenylboronic acid silane intermediate. Disperse 2.0g of nanocellulose in 400mL of an ethanol-water solution, wherein the volume ratio of ethanol to deionized water in the ethanol-water solution is 7:3. Shear at 1800rpm for 20min to obtain a nanocellulose suspension. Adjust the pH of the system to 4.7 with 0.5mol / L glacial acetic acid. Add 0.5g of methyltrimethoxysilane dropwise at 0.20g / min at 40℃, keep the reaction at this temperature for 3h, centrifuge at 8000rpm for 20min, discard the supernatant, and use the precipitate for... The precipitate was resuspended and washed three times with 100 mL of anhydrous ethanol each time, and then redispersed in 500 mL of an ethanol-water solution with a volume ratio of anhydrous ethanol to deionized water of 95:5. After shearing at 1800 rpm for 20 min, the mixture was cooled to 30 °C, and the pH was adjusted to 5.0 with 0.5 mol / L glacial acetic acid. 0.6 g of phenylboronic acid silane intermediate was added dropwise over 20 min. The mixture was stirred at 30 °C and 300 rpm for 4 h, centrifuged at 8000 rpm for 20 min, and the supernatant was discarded. The precipitate was washed three times with 200 mL of anhydrous ethanol each time and then vacuum dried at 40 °C for 12 h to obtain modified nanocellulose.
[0051] S2. Mix 0.5g KH560, 2mL deionized water, and 8mL anhydrous ethanol. Adjust the pH to 8.5 with 0.1mol / L dilute ammonia and pre-hydrolyze at room temperature for 20min to obtain a silane pre-hydrolyzed solution. Dissolve 0.1g Pluronic F127 in 400mL deionized water, add 4g hydrophobic silica aerogel, shear and disperse at 800rpm for 10min, and add 5mL... 0.1 mol / L dilute ammonia water was stirred at 40℃ for 1.0 h to obtain an aerogel suspension. The silane pre-hydrolyzed solution was added dropwise over 1.0 h. The temperature was raised to 50℃ and kept at that temperature for 3 h. The mixture was then filtered under reduced pressure at -0.08 MPa. The filter cake was rinsed twice with deionized water and redispersed in 400 mL of deionized water. The pH of the system was adjusted to 4.0 with 0.5 mol / L glacial acetic acid. The mixture was stirred at 50℃ for 2.25 h and then filtered under reduced pressure at -0.08 MPa. The filter cake was rinsed three times with deionized water and once with anhydrous ethanol, 100 mL each time. The mixture was then vacuum dried at 40℃ for 12 h to obtain 1 / 2-diol-grafted silica aerogel.
[0052] S3. Dissolve 0.005 g glacial acetic acid and 1.15 g methyltrimethoxysilane in 100 mL anhydrous ethanol to obtain a modified solution; disperse 1.5 g pinacol phenylboronic acid in 100 mL anhydrous ethanol and stir at 300 rpm for 10 min to obtain an impregnation solution; add 30 g of particles with a diameter of 40 μm and a true density of 0.4 g / cm³. 3 Borosilicate hollow glass microspheres were added to 300 mL of 0.1 mol / L dilute hydrochloric acid and stirred at 300 rpm for 30 min. After washing with deionized water to pH=7, the microspheres were dried at 60℃ for 2.25 h to obtain pretreated microspheres. The pretreated microspheres were then added to 300 mL of an ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water was 30:70), stirred at 80 rpm to disperse, and the pH of the system was adjusted to 8.2 with 0.1 mol / L dilute ammonia. 1.15 g of the pretreated microspheres were then added. After stirring with CTAB for 15 min, 2.4 g of TEOS was dissolved in 40 mL of anhydrous ethanol and added dropwise to the system for a total addition time of 1 h. The mixture was stirred at 40 °C and 80 rpm for 3 h. The mixture was then transferred to an ethanol-hydrochloric acid mixture and refluxed twice at 60 °C. The volume ratio of anhydrous ethanol to concentrated hydrochloric acid (37% by mass) in the ethanol-hydrochloric acid mixture was 95:5, with 300 mL added each time for 1 h. The mixture was washed with deionized water until pH=7, and then placed in the modified solution for 15 min at room temperature. After draining, the mixture was quickly rinsed once with anhydrous ethanol and then transferred to the impregnation solution. The solution was evacuated to -0.09 MPa and held for 30 min. After restoring to normal pressure within 15 min, the mixture was allowed to stand for 1 h. The mixture was then filtered under reduced pressure at -0.05 MPa, and washed twice with 50 mL of anhydrous ethanol each time. The mixture was then vacuum dried at 25 °C for 6 h to obtain sustained-release composite microbeads.
[0053] S4. Dissolve 0.55g ammonium persulfate in 30mL of deionized water to obtain initiator A, and dissolve 0.2g sodium bisulfite in 30mL of deionized water to obtain initiator B; 120g butyl acrylate, 70g methyl methacrylate, 2.25g acrylic acid, 0.55g dimethylaminoethyl methacrylate, 8g 3-acrylamidophenylboronic acid, 0.2g n-dodecyl mercaptan, 2.25g sodium dodecyl sulfate, 1.0g... OP-10 emulsifier was mixed with 175 mL of deionized water and stirred at 900 rpm for 30 min to obtain a pre-emulsion. 38 g of the pre-emulsion, initiator A, and initiator B were added to the polymerization reactor, and the temperature was raised to 60 °C. 341 g of the remaining pre-emulsion was added dropwise at a rate of 4 g / min. After aging at 60 °C for 1.5 h, the temperature was lowered to 40 °C, and 0.35 g of sodium bicarbonate and 0.085 g of sodium carbonate were added to stabilize the pH of the system at 8.4. The mixture was then filtered through a 100-mesh filter to obtain a phenylboronic acid modified acrylate emulsion.
[0054] S5. Add 32g of deionized water to a stirred tank, then add 0.18g of sodium bicarbonate, 0.05g of sodium carbonate, 0.3g of sodium polyacrylate dispersant, and 0.2g of acetylation diol wetting agent. Stir at 300rpm until dissolved. Add 30g of phenylboronic acid modified acrylate emulsion. Pre-disperse 4.5g of o-diol-grafted silica aerogel in 20mL of deionized water to form a uniform suspension. Slowly add the suspension dropwise to the tank while stirring at 600rpm for 10 minutes. Continue stirring for another 10 minutes. Add 0.175g of polycarboxylate dispersant and stir for 5.5 minutes. Then add 0.85g of alcohol ester dodecyl, 0... 0.2g of silicone defoamer and 0.10g of isothiazolinone bactericide were stirred for 5.5 minutes. The stirring speed was reduced to 350 rpm. 1.75g of modified nanocellulose, which had been pre-dispersed in 10mL of deionized water, was slowly added and stirred for 10 minutes. 6.0g of slow-release composite microspheres and 5.5g of rutile titanium dioxide with an average particle size of 250nm were added in three equal batches at 5-minute intervals. The mixture was stirred at 350 rpm for 22 minutes. The pH was adjusted to 7.4 with 0.5mol / L glacial acetic acid. The viscosity at 25℃ was 70s. After filtration through an 80-mesh nylon sieve, a thermal insulation nano-ceramic coating was obtained.
[0055] The actual product of the thermal insulation nano-ceramic coating prepared in this embodiment is shown below. Figure 1 As shown, the coating is a uniform, fine, milky-white paste with a consistent gloss.
[0056] Example 2
[0057] A method for preparing a thermal insulation nano-ceramic coating includes the following steps:
[0058] S1. Mix 8g of 3-aminophenylboronic acid, 13g of KH560, and 80mL of anhydrous ethanol, stir at 250rpm, and react at 45℃ in the dark for 2h to obtain a phenylboronic acid silane intermediate. Disperse 1.5g of nanocellulose in 350mL of an ethanol-water solution, wherein the volume ratio of ethanol to deionized water in the ethanol-water solution is 7:3. Shear at 1500rpm for 15min to obtain a nanocellulose suspension. Adjust the pH of the system to 4.5 using 0.5mol / L glacial acetic acid. Add 0.3g of methyltrimethoxysilane dropwise at 0.15g / min at 35℃, keep the reaction at this temperature for 2h, centrifuge at 7000rpm for 15min, discard the supernatant, and use the precipitate for... The precipitate was resuspended and washed three times with 80 mL of anhydrous ethanol each time, and then redispersed in 400 mL of an ethanol-water solution with a volume ratio of anhydrous ethanol to deionized water of 95:5. After shearing at 1500 rpm for 15 min, the mixture was cooled to 25 °C, and the pH was adjusted to 4.8 with 0.5 mol / L glacial acetic acid. 0.4 g of phenylboronic acid silane intermediate was added dropwise over 10 min. The mixture was stirred at 25 °C and 250 rpm for 3 h, centrifuged at 7000 rpm for 15 min, and the supernatant was discarded. The precipitate was washed three times with 150 mL of anhydrous ethanol each time and then vacuum dried at 35 °C for 10 h to obtain modified nanocellulose.
[0059] S2. Mix 0.3g KH560, 1mL deionized water, and 5mL anhydrous ethanol. Adjust the pH to 8.5 with 0.1mol / L dilute ammonia and pre-hydrolyze at room temperature for 10min to obtain a silane pre-hydrolyzed solution. Dissolve 0.05g Pluronic F127 in 350mL deionized water, add 3g hydrophobic silica aerogel, shear and disperse at 600rpm for 5min, and add 3mL... 0.1 mol / L dilute ammonia water was stirred at 35°C for 0.5 h to obtain an aerogel suspension. The silane pre-hydrolyzed solution was added dropwise over 0.5 h. The temperature was raised to 45°C and maintained for 2 h. The mixture was then filtered under reduced pressure at -0.08 MPa. The filter cake was rinsed twice with deionized water and redispersed in 350 mL of deionized water. The pH of the system was adjusted to 4.0 with 0.5 mol / L glacial acetic acid. The mixture was stirred at 45°C for 1.5 h and then filtered under reduced pressure at -0.08 MPa. The filter cake was rinsed three times with deionized water and once with anhydrous ethanol, each time using 80 mL. The mixture was then vacuum dried at 35°C for 10 h to obtain 1,000-diol-grafted silica aerogel.
[0060] S3. Dissolve 0.005 g glacial acetic acid and 0.8 g methyltrimethoxysilane in 80 mL anhydrous ethanol to obtain a modified solution; disperse 1 g pinacol phenylboronic acid ester in 80 mL anhydrous ethanol and stir at 250 rpm for 5 min to obtain an impregnation solution; add 25 g of particles with a particle size of 20 μm and a true density of 0.3 g / cm³. 3Borosilicate hollow glass microspheres were added to 250 mL of 0.1 mol / L dilute hydrochloric acid and stirred at 250 rpm for 20 min. After washing with deionized water to pH=7, the microspheres were dried at 50℃ for 1.5 h to obtain pretreated microspheres. The pretreated microspheres were then added to 250 mL of an ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water was 30:70), and dispersed by stirring at 60 rpm. The pH of the system was adjusted to 8.2 with 0.1 mol / L dilute ammonia, and 0.8 g of CTAB was added and stirred for 10 min. 1.8 g of... TEOS was dissolved in 30 mL of anhydrous ethanol and added dropwise to the system over a total of 0.5 h. The mixture was stirred at 35 °C and 60 rpm for 2 h. The mixture was then transferred to an ethanol-hydrochloric acid mixture and refluxed twice at 50 °C. The volume ratio of anhydrous ethanol to concentrated hydrochloric acid (36% by mass) in the ethanol-hydrochloric acid mixture was 95:5, with 250 mL added each time for 0.5 h. The mixture was washed with deionized water until neutral and then placed in the modified solution for 10 min at room temperature. After draining, the mixture was quickly rinsed once with anhydrous ethanol and then transferred to the impregnation solution. The solution was evacuated to -0.09 MPa and maintained at this pressure for 20 min. After restoring to normal pressure within 10 min, the mixture was allowed to stand for another 0.5 h. The mixture was then filtered under reduced pressure at -0.05 MPa, slurried and rinsed twice with 40 mL of anhydrous ethanol each time, and then vacuum dried at 20 °C for 4 h to obtain sustained-release composite microbeads.
[0061] S4. Dissolve 0.3g of ammonium persulfate in 20mL of deionized water to obtain initiator A, and dissolve 0.1g of sodium bisulfite in 20mL of deionized water to obtain initiator B; 100g of butyl acrylate, 55g of methyl methacrylate, 1.5g of acrylic acid, 0.3g of dimethylaminoethyl methacrylate, and 6g of... 3-Acrylamidophenylboronic acid, 0.1 g n-dodecyl mercaptan, 1.5 g sodium dodecyl sulfate, 0.5 g OP-10 emulsifier, and 150 mL deionized water were mixed and stirred at 800 rpm for 20 min to obtain a pre-emulsion. 30 g of the pre-emulsion, initiator A, and initiator B were added to a polymerization reactor, and the temperature was raised to 55 °C. 284 g of the remaining pre-emulsion was added dropwise at a rate of 3 g / min. After aging at 55 °C for 1 h, the temperature was lowered to 35 °C, and 0.2 g sodium bicarbonate and 0.05 g sodium carbonate were added to stabilize the pH of the system at 8.3. The mixture was then filtered through a 100-mesh filter to obtain a phenylboronic acid-modified acrylate emulsion.
[0062] S5. Add 25g of deionized water to a stirred tank, add 0.1g of sodium bicarbonate, 0.03g of sodium carbonate, 0.2g of sodium polyacrylate dispersant, and 0.1g of acetylacetonate diol wetting agent. Stir at 250rpm until dissolved. Add 33g of phenylboronic acid modified acrylate emulsion. Disperse 3.0g of 1 / 2-diol-grafted silica aerogel in 15mL of deionized water to form a uniform suspension. Slowly add the suspension dropwise to the tank while stirring at 400rpm for 5 minutes. Continue stirring for 5 minutes. Add 0.1g of polycarboxylate dispersant and stir for 3 minutes. Then add 0.5g of alcohol ester dodecyl and 0. 1g of silicone defoamer and 0.05g of isothiazolinone bactericide were stirred for 3 minutes. The stirring speed was reduced to 250 rpm. 1.0g of modified nanocellulose, which had been pre-dispersed in 8mL of deionized water, was slowly added and stirred for 5 minutes. 4.0g of slow-release composite microspheres and 3.0g of rutile titanium dioxide with an average particle size of 200nm were added in three equal batches at 5-minute intervals. The mixture was stirred at 250 rpm for 15 minutes. The pH was adjusted to 7.2 with 0.5mol / L glacial acetic acid. The viscosity at 25℃-4 was 60s. The mixture was filtered through an 80-mesh nylon sieve to obtain a thermal insulation nano-ceramic coating.
[0063] Example 3
[0064] A method for preparing a thermal insulation nano-ceramic coating includes the following steps:
[0065] S1. Mix 12g of 3-aminophenylboronic acid, 20g of KH560, and 120mL of anhydrous ethanol, stir at 350rpm, and react at 55℃ in the dark for 4h to obtain a phenylboronic acid silane intermediate. Disperse 2.5g of nanocellulose in 450mL of ethanol-water solution, wherein the volume ratio of ethanol to deionized water in the ethanol-water solution is 7:3. Shear at 2000rpm for 25min to obtain a nanocellulose suspension. Adjust the pH of the system to 5.0 with 0.5mol / L glacial acetic acid. Add 0.8g of methyltrimethoxysilane dropwise at 0.25g / min at 45℃, keep the reaction at this temperature for 4h, centrifuge at 9000rpm for 25min, discard the supernatant, and use the precipitate for... The precipitate was resuspended and washed three times with 120 mL of anhydrous ethanol each time, and then redispersed in 600 mL of an ethanol-water solution with a volume ratio of anhydrous ethanol to deionized water of 95:5. After shearing at 2000 rpm for 25 min, the mixture was cooled to 35 °C, and the pH was adjusted to 5.2 with 0.5 mol / L glacial acetic acid. 0.8 g of phenylboronic acid silane intermediate was added dropwise over 30 min. The mixture was stirred at 35 °C and 350 rpm for 5 h, centrifuged at 9000 rpm for 25 min, and the supernatant was discarded. The precipitate was washed three times with 250 mL of anhydrous ethanol each time and then vacuum dried at 45 °C for 15 h to obtain modified nanocellulose.
[0066] S2. Mix 0.8g KH560, 3mL deionized water, and 12mL anhydrous ethanol. Adjust the pH to 8.5 with 0.1mol / L dilute ammonia and pre-hydrolyze at room temperature for 30min to obtain a silane pre-hydrolyzed solution. Dissolve 0.15g Pluronic F127 in 450mL deionized water, add 5g hydrophobic silica aerogel, shear and disperse at 1000rpm for 15min, and add 8mL... 0.1 mol / L dilute ammonia water was stirred at 45℃ for 1.5 h to obtain an aerogel suspension. The silane pre-hydrolyzed solution was added dropwise over 1.5 h. The temperature was raised to 55℃ and kept at that temperature for 4 h. The mixture was then filtered under reduced pressure at a vacuum of -0.09 MPa. The filter cake was rinsed twice with deionized water and redispersed in 450 mL of deionized water. The pH of the system was adjusted to 4.0 with 0.5 mol / L glacial acetic acid. The mixture was stirred at 55℃ for 3 h and then filtered under reduced pressure at a vacuum of -0.09 MPa. The filter cake was rinsed three times with deionized water and once with anhydrous ethanol, each time using 120 mL. The mixture was then vacuum dried at 45℃ for 15 h to obtain 1 / 2-diol-grafted silica aerogel.
[0067] S3. Dissolve 0.005g glacial acetic acid and 1.5g methyltrimethoxysilane in 120mL anhydrous ethanol to obtain a modified solution; disperse 2g pinacol phenylboronic acid in 120mL anhydrous ethanol and stir at 350rpm for 15min to obtain an impregnation solution; add 35g of particles with a diameter of 60μm and a true density of 0.5g / cm³. 3 Borosilicate hollow glass microspheres were added to 350 mL of 0.1 mol / L dilute hydrochloric acid and stirred at 350 rpm for 40 min. After washing with deionized water to pH=7, the microspheres were dried at 70 °C for 3 h to obtain pretreated microspheres. The pretreated microspheres were added to 350 mL of an ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water was 30:70) and dispersed by stirring at 100 rpm. The pH of the system was adjusted to 8.5 with 0.1 mol / L dilute ammonia. 1.5 g of CTAB was added and stirred for 20 min. 3.0 g of TEOS was dissolved in 50 mL of anhydrous ethanol and added dropwise to the system over a total dropwise addition time of 1.5 h. The reaction was carried out at 45 °C and 100 rpm for 4 h. The mixture was refluxed twice at 70°C in an ethanol-hydrochloric acid mixture, with an anhydrous ethanol to concentrated hydrochloric acid (38% by mass) volume ratio of 95:5. 350 mL was used each time, and the mixture was left to stand for 1.5 h each time. The mixture was washed with deionized water until pH=7, then placed in the modified solution for 20 min at room temperature. After draining, it was quickly rinsed once with anhydrous ethanol and transferred to the impregnation solution. The solution was then evacuated to -0.09 MPa and held at this pressure for 40 min. After restoring to normal pressure within 20 min, the mixture was allowed to stand for another 1.5 h. The mixture was then filtered under reduced pressure at -0.06 MPa, slurried and rinsed twice with 60 mL of anhydrous ethanol each time, and dried under vacuum at 30°C for 8 h to obtain sustained-release composite microspheres.
[0068] S4. Dissolve 0.8g ammonium persulfate in 40mL of deionized water to obtain initiator A, and dissolve 0.3g sodium bisulfite in 40mL of deionized water to obtain initiator B; 140g butyl acrylate, 85g methyl methacrylate, 3.0g acrylic acid, 0.8g dimethylaminoethyl methacrylate, and 10g... 3-Acrylamidophenylboronic acid, 0.3g n-dodecyl mercaptan, 3.0g sodium dodecyl sulfate, 1.5g OP-10 emulsifier, and 200mL deionized water were mixed and stirred at 1000rpm for 40min to obtain a pre-emulsion. 45g of the pre-emulsion, initiator A, and initiator B were added to a polymerization reactor, and the temperature was raised to 65℃. 398g of the remaining pre-emulsion was added dropwise at a rate of 5g / min. After aging at 65℃ for 2h, the temperature was lowered to 45℃, and 0.5g sodium bicarbonate and 0.12g sodium carbonate were added to stabilize the pH of the system at 8.6. The mixture was then filtered through a 100-mesh filter to obtain a phenylboronic acid-modified acrylate emulsion.
[0069] S5. Add 40g of deionized water to a stirred tank, then add 0.25g of sodium bicarbonate, 0.08g of sodium carbonate, 0.5g of sodium polyacrylate dispersant, and 0.3g of acetylation diol wetting agent. Stir at 350rpm until dissolved. Add 50g of phenylboronic acid modified acrylate emulsion. Pre-disperse 6.0g of o-diol-grafted silica aerogel in 25mL of deionized water to form a uniform suspension. Slowly add the suspension dropwise to the tank while stirring at 800rpm for 15 minutes. Continue stirring for another 15 minutes. Add 0.25g of polycarboxylate dispersant and stir for 8 minutes. Then add 1.2g of alcohol ester dodecyl, 0... 0.3g of silicone defoamer and 0.15g of isothiazolinone bactericide were stirred for 8 minutes. The stirring speed was reduced to 450 rpm. 2.5g of modified nanocellulose, which had been pre-dispersed in 12mL of deionized water, was slowly added and stirred for 15 minutes. 8.0g of slow-release composite microspheres and 8.0g of rutile titanium dioxide with an average particle size of 300nm were added in three equal batches at 5-minute intervals. The mixture was stirred at 450 rpm for 30 minutes. The pH was adjusted to 7.5 with 0.5mol / L glacial acetic acid. The viscosity at 25℃ was 80s. The mixture was filtered through an 80-mesh nylon sieve to obtain a thermal insulation nano-ceramic coating.
[0070] Comparative Example 1
[0071] A method for preparing a thermal insulation nano-ceramic coating differs from Example 1 in that the o-diol-grafted silica aerogel is not prepared, and in step S5, an equal amount of hydrophobic silica aerogel is used instead of o-diol-grafted silica aerogel. The remaining steps and parameters are the same.
[0072] Comparative Example 2
[0073] A method for preparing a thermal insulation nano-ceramic coating differs from Example 1 in that the slow-release composite microspheres are not prepared. In step S5, an equal amount of borosilicate hollow glass microspheres are used instead of the slow-release composite microspheres. The remaining steps and parameters are the same.
[0074] Comparative Example 3
[0075] A method for preparing a thermal insulation nano-ceramic coating differs from Example 1 in that no modified cellulose is prepared, and in step S5, an equal amount of unmodified nano-cellulose is used to replace the modified cellulose. The remaining steps and parameters are the same.
[0076] Comparative Example 4
[0077] A method for preparing a thermal insulation nano-ceramic coating differs from Example 1 in that 3-acrylamidophenylboronic acid is not added in step S4, while the remaining steps and parameters are the same.
[0078] Performance testing:
[0079] Thermal conductivity test: The thermal insulation nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4 were respectively applied to a 150mm×150mm glass plate. The total dry film thickness was controlled to be 8.0mm by applying the coating layer by layer. After curing at room temperature for 7 days, the coating was removed from the glass plate and a 100mm diameter disc was cut as a test sample. The thermal conductivity of the coating was measured using a heat flow meter under the conditions of an average temperature of 25℃ and a temperature difference of 10℃ between the hot and cold surfaces. Three parallel samples were prepared for each group of samples, and the arithmetic mean was taken as the test result.
[0080] Storage stability test: The heat-insulating nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4 were respectively placed in 250mL sealed containers with lids and stored in a 50℃ constant temperature blower box for 30 days. After being taken out, they were naturally cooled to room temperature. First, it was observed whether the coatings exhibited phenomena such as gelation, clumping, sedimentation, stratification, or skin formation. Then, the viscosity at 25℃ before and after storage was measured using a Coat-4 viscometer (a viscosity change rate not exceeding 15% and without any visible abnormalities was considered passing; a small amount of sedimentation layer appeared at the bottom of the coating after storage, and the viscosity change rate at 25℃ exceeded 15% but did not exceed 30%, which was considered slight sedimentation; a significant sedimentation layer or stratification appeared at the bottom of the coating after storage, and the viscosity change rate at 25℃ exceeded 30%).
[0081] Self-healing performance test: The thermal insulation nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4 were respectively applied to glass slides with a dry film thickness of 1.0 mm and cured at room temperature for 7 days. A diamond scratch tool equipped with a micro-scratch instrument was used to scratch a 50 μm wide and 20 μm deep mark on the coating surface. The initial morphology and depth of the scratch were recorded using an optical microscope and a surface profilometer. The sample was placed in a constant temperature and humidity chamber at 25°C and 75% relative humidity for 48 hours. After removal, the depth of the scratch at the same position was measured again using a surface profilometer. The percentage of the reduction in scratch depth relative to the initial scratch depth was used as the self-healing rate. Three scratches were tested for each group of samples and the average value was taken.
[0082] Adhesion test: The thermal insulation nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4 were applied to 70mm×70mm mortar boards with a dry film thickness of 1.5mm. After curing at room temperature for 7 days, a 20mm diameter aluminum alloy test cylinder was bonded to the coating surface with epoxy structural adhesive. After curing at room temperature for 24 hours, the pull-off adhesion between the coating and the substrate was measured using an adhesion tester at a pull-out speed of 20mm / min. Five points were tested for each sample. The maximum and minimum values were removed, and the arithmetic mean of the remaining three data points was taken.
[0083] Artificial weathering test: The thermal insulation nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4 were used to prepare two sets of samples: Group A was coated on a 70mm×70mm mortar board with a dry film thickness of 1.5mm; Group B was coated on a 150mm×150mm glass plate, with the total dry film thickness controlled to be 8.0mm through layer-by-layer construction. After curing at room temperature for 7 days, all samples were subjected to an aging test chamber using a xenon lamp, with the irradiation intensity controlled at 0.50W / m² (340nm), blackboard temperature at 65℃, and relative humidity at 50%. Continuous irradiation for 102 minutes was followed by spraying for 18 minutes as one cycle, with a cumulative irradiation time of 1000h. After aging, the samples were removed. The adhesion of Group A samples after aging was tested under the same conditions as the initial adhesion test; for Group B samples, the coating was removed from the glass plate, and a 100mm diameter disc was cut to determine the thermal conductivity after aging under the same conditions as the initial thermal conductivity test.
[0084] Table 1. Performance test results of the thermal insulation nano-ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-4
[0085]
[0086] As shown in Table 1, the thermal conductivity and thermal conductivity after aging of the heat-insulating nano-ceramic coatings prepared in Examples 1-3 are generally lower than those of Comparative Examples 1-4, and the self-healing rate, adhesion, and adhesion after aging are generally higher than those of Comparative Examples 1-4. This indicates that the heat-insulating nano-ceramic coatings prepared in Examples 1-3 have better heat-insulating durability, self-healing ability, and interfacial mechanical properties than those of Comparative Examples 1-4.
[0087] In Comparative Example 1, hydrophobic silica aerogel was used instead of vicinal diol-grafted silica aerogel. The nanoporous framework and Knudsen effect insulation capacity of the aerogel remained unaffected. However, the vicinal diol on the aerogel surface was the only source of ligands for constructing the dynamic cross-linked network. The phenylboronic acid in the emulsion matrix, the modified nanocellulose, and the phenylboronic acid released by the microspheres all required bidentate chelation with the vicinal diol to form borate ester bonds. Without the vicinal diol anchor point, these three types of phenylboronic acid groups lost their coordination reaction targets, making it impossible to achieve a dynamic cross-linked network with aerogel as a rigid node. The self-repair rate was significantly reduced. The only remaining weak repair capability stemmed from the weak coordination between the emulsion phenylboronic acid and the residual vicinal diol on the cellulose framework of the nanocellulose that had not been modified and consumed. However, this interaction density was extremely low and disordered, failing to constitute an effective repair network. The breakage of the cross-linked network leads to a lack of chemical bonding between the aerogel and the polymer matrix, resulting in a significant reduction in interfacial adhesion. During aging, the weak interfaces continue to degrade under thermal cycling and spray impact, leading to a substantial decrease in adhesion after aging. Furthermore, the ungrafted hydrophobic aerogel surface lacks chemically compatible anchor points with the emulsion system, resulting in slow phase separation from the matrix during accelerated storage, manifested as slight sedimentation.
[0088] Comparative Example 2 used borosilicate hollow glass microspheres instead of the slow-release composite microspheres. The low-pressure cavity structure of the microspheres remained intact, and the initial thermal conductivity was close to that of Example 1. Furthermore, the microspheres had small particle size and limited density difference from the emulsion system, and no sedimentation occurred during storage. At this time, the dynamic cross-linking network of the coating remained intact. However, the exposed borosilicate glass microspheres lacked the physical barrier protection of the mesoporous silica coating layer in the weakly alkaline coating system. During aging, they were continuously eroded by the alkaline medium, gradually thinning and eventually causing local perforation. The cavity structure was destroyed, leading to a significant increase in thermal conductivity after aging. Simultaneously, due to the lack of pinacol phenylboronic acid ester, the coating lacked a repair mechanism for the slow-release replenishment of boron at microcracks, resulting in a self-repair rate significantly lower than that of Example 1, but still higher than that of Comparative Examples 1 and 4, where the cross-linking network was completely broken. This indicates that the basic cross-linking network still possesses a certain repair capability even without slow-release reinforcement.
[0089] Comparative Example 3 used unmodified nanocellulose instead of modified nanocellulose. The strong hydrophilicity of the unmodified nanocellulose surface led to its agglomeration and instability in the weakly alkaline emulsion system. The cellulose chains could not form an effective suspended network, and both the aerogel and composite microspheres, being lightweight fillers, lost their suspension support and settled during storage, resulting in a significant sedimentation assessment of storage stability. After the filler settled, the filler distribution within the coating became severely uneven, and localized enrichment areas formed thermal bridges, leading to an increase in the equivalent thermal conductivity. More importantly, the unmodified nanocellulose was not grafted with a phenylboronic acid silane intermediate, and therefore lacked phenylboronic acid functional groups, making it impossible to form borate ester coordination with the o-diol of the aerogel. The crosslinked network lost the bridging channels mediated by nanocellulose that connected the polymer segments between aerogel nodes. Although the coordination crosslinking between the emulsion phenylboronic acid and the o-diol of the aerogel still existed, and the phenylboronic acid released by the microspheres could also coordinate with the o-diol of the aerogel, the spatial coverage and continuity of the network were significantly reduced due to the lack of nanocellulose bridging channels, resulting in a significant decrease in the self-healing rate. The decrease in thermal conductivity and adhesion after aging was greater than that in Example 1. This is because the uneven distribution of filler resulted in a lack of dual protection of thermal insulation filler and cross-linking network in some areas of the coating. These weak areas degraded first during the aging process.
[0090] Comparative Example 4 did not contain 3-acrylamidophenylboronic acid, and therefore lacked phenylboronic acid reaction sites on the polymer backbone. The emulsion matrix is the continuous phase of the coating, and the phenylboronic acid groups on the polymer chains are the core link that chemically anchors the filler to the matrix. Without this group, although boronic acid from the modified nanocellulose can still form boronic ester coordination with the aerogel diol, and phenylboronic acid from the microspheres can still form boronic ester coordination with the aerogel diol, these crosslinks only occur between discrete fillers and cannot extend to the continuous phase of the polymer matrix. The coating essentially becomes a physically filled polymer composite film, with no chemical bonding between the filler and the matrix, resulting in a significant decrease in self-healing rate. Micro-damage at scratches cannot be effectively repaired through the reversible coordination of boronic ester bonds. Due to the lack of a crosslinked network constraint in the matrix, the polymer chains rely solely on physical entanglement to maintain cohesion, leading to insufficient coating density and mechanical strength. Both initial adhesion and post-aging adhesion are significantly reduced, posing a serious risk of mechanical property degradation during long-term service.
[0091] Comparative Examples 1-4 lacked o-diol-grafted silica aerogel, slow-release composite microspheres, modified nanocellulose, and 3-acrylamidophenylboronic acid, respectively. This resulted in the inability to construct a dynamic cross-linking network, failure of the filler's suspended mesh and loss of bridging channels, erosion and damage of the microsphere cavities during weak alkaline aging, lack of local boron source replenishment at microcracks, and no chemical bonding between the filler and the matrix. All of these factors contributed to varying degrees of deterioration in thermal insulation durability, self-healing ability, and interfacial mechanical properties.
[0092] The above results demonstrate and describe the basic principles and main features of this application, as well as its advantages.
[0093] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of the present invention without departing from the spirit and scope of the claims. All of these forms are within the protection scope of the present invention.
Claims
1. A thermal insulation nano-ceramic coating, characterized in that, The coating comprises phenylboronic acid modified acrylic emulsion, vicinal glycol grafted silica aerogel, modified nanocellulose, slow-release composite microspheres, rutile titanium dioxide, and additives. The phenylboronic acid modified acrylate emulsion is obtained by emulsion polymerization of acrylate monomers and 3-acrylamidophenylboronic acid; the acrylate monomers include butyl acrylate, methyl methacrylate, acrylic acid and dimethylaminoethyl methacrylate. The vicinal diol-grafted silica aerogel is obtained by grafting hydrophobic silica aerogel with KH560 and then performing ring-opening hydrolysis under acidic conditions to generate vicinal diol groups. The modified nanocellulose is obtained by grafting nanocellulose with a methyltrimethoxysilane hydrophobically modified intermediate and a phenylboronic acid silane intermediate; the phenylboronic acid silane intermediate is obtained by reacting 3-aminophenylboronic acid and KH560 in the dark. The sustained-release composite microspheres are obtained by coating a mesoporous silica layer with hollow glass microspheres as the core, CTAB as the template and TEOS as the silicon source, using a sol-gel method, followed by hydrophobic modification with dimethyltrimethoxysilane and vacuum impregnation in an impregnation solution; the impregnation solution includes pinacol phenylboronic acid ester and anhydrous ethanol. The additives include dispersants, wetting agents, defoamers, bactericides, film-forming aids, and pH buffers.
2. The thermal insulation nano-ceramic coating according to claim 1, characterized in that, The dispersant is sodium polyacrylate and polycarboxylate; the wetting agent is alkynyl glycol; the defoamer is organosilicon; the bactericide is isothiazolinone; the film-forming aid is dodecyl alcohol ester; the pH buffer includes sodium bicarbonate and sodium carbonate; the mass ratio of the phenylboronic acid modified acrylate emulsion, vicinal diol grafted silica aerogel, modified nanocellulose, slow-release composite microspheres, rutile titanium dioxide and the additives is (30-50):(3-6):(1.0-2.5):(4.0-8.0):(3.0-8.0):(1.18-3.03).
3. A method for preparing a thermal insulation nano-ceramic coating as described in claim 1 or 2, characterized in that, Includes the following steps: S1. 3-Aminophenylboronic acid and KH560 were reacted in anhydrous ethanol in the dark to obtain a phenylboronic acid silane intermediate; nanocellulose was dispersed in an aqueous ethanol solution, the pH was adjusted, and monomethyltrimethoxysilane was added dropwise. The reaction was carried out under heat, and after centrifugation and washing, the nanocellulose was redispersed, the pH was adjusted, and the phenylboronic acid silane intermediate was added dropwise. The reaction was carried out, and after centrifugation, washing, and drying, modified nanocellulose was obtained. S2. Prepare silane prehydrolysis solution; Pluronic F127 was dissolved in deionized water, and hydrophobic silica aerogel, dilute ammonia and the silane prehydrolysis solution were added in sequence. The mixture was heated and reacted, filtered, washed, pH adjusted, reacted, filtered under reduced pressure and dried to obtain 1,2-diol-grafted silica aerogel. S3. Prepare the modified solution and impregnation solution; Hollow glass microspheres were added to dilute hydrochloric acid, washed, and dried to obtain pretreated microspheres. An aqueous ethanol solution was added to adjust the pH, and an anhydrous ethanol solution of CTAB and TEOS was added to react. After extraction and modification with the modified solution, the microspheres were placed in the impregnation solution for vacuum impregnation, filtered, washed, and dried to obtain sustained-release composite microspheres. S4. Ammonium persulfate is added to deionized water to obtain initiator A, and sodium bisulfite is added to deionized water to obtain initiator B; acrylate monomer, 3-acrylamidophenylboronic acid, n-dodecyl mercaptan, sodium dodecyl sulfate, OP-10 and deionized water are mixed to obtain a pre-emulsion; a portion of the pre-emulsion, initiator A and initiator B are mixed, heated, the remaining pre-emulsion is added dropwise, matured, cooled, and sodium bicarbonate and sodium carbonate are added to obtain a phenylboronic acid modified acrylate emulsion; S5. Dissolve pH buffer, sodium polyacrylate and wetting agent in deionized water, and then add phenylboronic acid modified acrylate emulsion, aerogel suspension, polycarboxylate, film-forming aid, defoamer and bactericide, cellulose suspension, slow-release composite microspheres and rutile titanium dioxide in sequence. Adjust the pH to obtain a thermal insulation nano-ceramic coating.
4. The method for preparing a thermal insulation nano-ceramic coating according to claim 3, characterized in that, In S1, the mass-to-volume ratio of 3-aminophenylboronic acid, KH560, and anhydrous ethanol is (8-12) g: (13-20) g: (80-120) mL; the temperature of the light-protected reaction is 45-55℃, and the time of the light-protected reaction is 2-4 h; the mass-to-volume ratio of nanocellulose, first methyltrimethoxysilane, phenylboronic acid silane intermediate, and ethanol aqueous solution is (1.5-2.5) g: (0.3-0.8) g: (0.4-0.8) g: (350-450) mL.
5. The method for preparing a thermal insulation nano-ceramic coating according to claim 4, characterized in that, In step S1, the volume ratio of anhydrous ethanol to deionized water in the ethanol-water solution is 7:3; the pH is adjusted to 4.5-5.0; the temperature of the heat preservation reaction is 35-45℃, and the heat preservation reaction time is 2-4 hours; the redispersing medium is 400-600 mL of ethanol-water solution, wherein the volume ratio of anhydrous ethanol to deionized water in the ethanol-water solution is 95:5; after redispersing, the pH is adjusted to 4.8-5.2; after adding the silane phenylboronic acid intermediate, the reaction temperature is 25-35℃, and the reaction time is 3-5 hours.
6. The method for preparing a thermal insulation nano-ceramic coating according to claim 3, characterized in that, In step S2, the step of preparing the silane pre-hydrolyzed solution is as follows: 0.3-0.8g KH560, 1-3mL deionized water, and 5-12mL anhydrous ethanol are mixed, and the pH is adjusted to 8.5; the mass-to-volume ratio of Pluronic F127, hydrophobic silica aerogel, dilute ammonia, and deionized water is (0.05-0.15)g:(3-5)g:(3-8)mL:(350-450)mL; the concentration of the dilute ammonia is 0.1mol / L; the target temperature for the heating reaction is 45-55℃, and the heating reaction time is 2-4h; the pH is adjusted to 4.0; after pH adjustment, the reaction temperature is 45-55℃, and the reaction time is 1.5-3h.
7. The method for preparing a thermal insulation nano-ceramic coating according to claim 3, characterized in that, In step S3, the steps for preparing the modified solution are as follows: dissolving 0.005g of glacial acetic acid and 0.8-1.5g of methyltrimethoxysilane in 80-120mL of anhydrous ethanol; the steps for preparing the impregnation solution are as follows: dispersing 1-2g of pinacol phenylboronic acid in 80-120mL of anhydrous ethanol; the mass-to-volume ratio of the hollow glass microspheres to dilute hydrochloric acid is (25-35)g:(250-350)mL; the concentration of the dilute hydrochloric acid is 0.1mol / L; the mass-to-volume ratio of the pretreated microspheres, CTAB, ethanol aqueous solution and TEOS anhydrous ethanol solution is (25-35)g:(0.8-1.5)g:(250-350)mL:(30-50)mL.
8. The method for preparing a thermal insulation nano-ceramic coating according to claim 7, characterized in that, In step S3, the volume ratio of anhydrous ethanol to deionized water in the ethanol-water solution is 30:70; the pH is adjusted to 8.2-8.5; the mass-to-volume ratio of TEOS to anhydrous ethanol in the TEOS anhydrous ethanol solution is (1.8-3.0) g: (30-50) mL; the reaction temperature is 35-45℃; the reaction time is 2-4 h; the modification time of the modified solution is 10-20 min; the vacuum impregnation step is as follows: vacuum to -0.09 MPa and maintain for 20-40 min, restore normal pressure within 10-20 min, and continue to stand for impregnation for 0.5-1.5 h.
9. The method for preparing a thermal insulation nano-ceramic coating according to claim 3, characterized in that, In step S4, the mass-to-volume ratio of ammonium persulfate to deionized water in initiator A is (0.3-0.8) g: (20-40) mL, and the mass-to-volume ratio of sodium bisulfite to deionized water in initiator B is (0.1-0.3) g: (20-40) mL; the mass-to-volume ratio of acrylate monomers, 3-acrylamidophenylboronic acid, n-dodecyl mercaptan, sodium dodecyl sulfate, OP-10 to deionized water is (156.8-228.8) g: (6-10) g: (0.1-0.3) g: (1.5-3.0) g: (0.5-1.5) g: (150-200) mL; and the mass ratio of butyl acrylate, methyl methacrylate, acrylic acid and dimethylaminoethyl methacrylate in acrylate monomers is (100-140): (55-85): (1.5-3.0): (0.3-0.8).
10. The method for preparing a thermal insulation nano-ceramic coating according to claim 9, characterized in that, In step S4, the mass-to-volume ratio of the partial pre-emulsion, the remaining pre-emulsion, sodium bicarbonate, sodium carbonate, initiator A, and initiator B is (30-45) g : (284-398) g : (0.2-0.5) g : (0.05-0.12) g : (20-40) mL : (20-40) mL; the target temperature for heating is 55-65℃; the ripening temperature is 55-65℃, and the ripening time is 1-2 h; the target temperature for cooling is 35-45℃.
11. The method for preparing a thermal insulation nano-ceramic coating according to claim 3, characterized in that, In step S5, the mass ratio of the pH buffer, sodium polyacrylate, wetting agent, polycarboxylate, film-forming aid, defoamer, and bactericide is (0.13-0.33):(0.2-0.5):(0.1-0.3):(0.1-0.25):(0.5-1.2):(0.1-0.3):(0.05-0.15); the mass ratio of sodium bicarbonate to sodium carbonate in the pH buffer is (0.1-0.25):(0.03-0.08).
12. The method for preparing a thermal insulation nano-ceramic coating according to claim 11, characterized in that, In step S5, the mass-to-volume ratio of the deionized water, aerogel suspension, and cellulose suspension is (25-40) g : (15-25) mL : (8-12) mL; the preparation step of the aerogel suspension is as follows: 3.0-6.0 g of o-diol-grafted silica aerogel is dispersed in 15-25 mL of deionized water to form a suspension; the preparation step of the cellulose suspension is as follows: 1.0-2.5 g of modified nanocellulose is dispersed in 8-12 mL of deionized water to form a suspension; the pH is adjusted to 7.2-7.5.
Citation Information
Patent Citations
Phenylboronic acid ester dynamic crosslinking nanogel material as well as preparation method and application thereof
CN121588277A
Water-based inorganic nano ceramic heat-insulating coating and preparation method thereof
CN122127818A