A plasma-based low-slag silicothermal magnesium smelting method

Magnesium smelting at high temperatures using a transferred arc plasma reactor, with control over the amount of calcium oxide added and the use of inert gas, has solved the problem of large tailings generation in magnesium smelting, achieving efficient and low-slag metallic magnesium production, and is suitable for near-atmospheric pressure continuous production.

CN122706975BActive Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611209715.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17
Estimated Expiration
2046-08-11

AI Technical Summary

Technical Problem

Existing magnesium smelting methods generate a large amount of tailings, resulting in low production efficiency of metallic magnesium. Furthermore, they rely on high vacuum conditions and long reaction times, making it difficult to achieve continuous production.

Method used

A transfer arc plasma reactor is used for reduction treatment at high temperature. By controlling the amount of calcium oxide added and the use of inert gas, a local ultra-high temperature reaction zone is established, which directly improves the reaction activity and reduces the amount of slag, thus achieving a rapid reduction reaction.

Benefits of technology

While reducing the amount of tailings generated, it significantly improved the production efficiency of metallic magnesium, simplified the equipment structure, reduced energy consumption, and achieved near-normal pressure continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122706975B_ABST
    Figure CN122706975B_ABST
Patent Text Reader

Abstract

This invention provides a plasma-based low-slag silicate smelting method for magnesium, comprising the following steps: S1, providing a mixture of magnesium-containing base material and flux; wherein the mass percentage of calcium oxide in the magnesium-containing base material is 10-30%; S2, placing the mixture in a transferred arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings; the reaction temperature of the reduction treatment is 2000-4000℃. This invention can improve the production efficiency of metallic magnesium while reducing the amount of tailings generated; this invention allows magnesium oxide, especially stable magnesium silicate phases such as Mg2SiO4, to reach decomposition and reduction temperatures that are difficult to reach with traditional heat sources, significantly weakening the Mg-O bond state, making magnesium oxide and magnesium silicates more likely to participate in reduction, and then utilizing the high-temperature reaction environment and the appropriate amount of calcium oxide added to reduce tailings generation and ensure the reduction rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of magnesium smelting, and particularly relates to a plasma-based low-slag silicothermal magnesium smelting method. Background Technology

[0002] The Pidgeon process is the most important industrial route for primary magnesium production. It typically uses calcined silica, ferrosilicon, and fluorite as main raw materials. After batching and briquetting, these materials undergo a thermal reduction reaction under high-temperature vacuum conditions to generate and recover magnesium vapor. In this system, CaO is usually introduced to promote the silyothermic reduction reaction, allowing it to combine with SiO2 to form a stable calcium silicate phase, thereby promoting the formation of metallic magnesium. However, the large-scale introduction of CaO leads to a significant amount of tailings.

[0003] Chinese invention patent CN101812599B describes a method for preparing metallic magnesium using dolomite as raw material. After obtaining calcined dolomite, the calcined dolomite is placed in a mixer and mixed with a reducing agent and flux to form a mixture. This mixture is then ground, pressed into pellets, and subjected to vacuum high-temperature thermal reduction for 4-6 hours. Although the calcium oxide in the calcined dolomite can promote magnesium formation, and the reduction rate of this patent can reach over 90%, the large amount of calcium oxide increases the slag volume, and the long thermal reduction time of 4-6 hours results in low production efficiency of metallic magnesium.

[0004] Therefore, it is necessary to provide a plasma-based low-slag silicothermal magnesium refining method to solve the technical problem of how to improve the production efficiency of metallic magnesium while reducing the amount of tailings generated. Summary of the Invention

[0005] The main objective of this invention is to provide a plasma-based low-slag silicothermal magnesium refining method, aiming to solve the technical problem of how to improve the production efficiency of metallic magnesium while reducing the amount of tailings generated.

[0006] To achieve the above objectives, the present invention provides a plasma-based low-slag silicothermal magnesium smelting method, comprising the following steps: S1 provides a mixture of magnesium-based material and flux; the magnesium-based material includes magnesium oxide, reducing agent, and calcium oxide; the mass percentage of calcium oxide in the magnesium-based material is 10-30%. S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings; the reaction temperature of the reduction treatment is 2000-4000℃.

[0007] Furthermore, during the reduction process, the transfer arc plasma reactor contains an inert gas; The transferred arc plasma reactor has an anode and a cathode, and the anode, the mixture, the inert gas, and the cathode form a conductive path during the reduction process; The inert gas is plasmaized under the action of the conductive path; The mixture reaches the reaction temperature under the action of the conductive path.

[0008] Furthermore, the reaction pressure of the mixture is 500-200000 Pa; The inert gas is in a state of inlet and outlet balance in the transfer arc plasma reactor; The inert gas includes at least one of argon and helium.

[0009] Furthermore, in the magnesium oxide material, the mass percentage of magnesium oxide is not less than 90%; In the magnesium-containing base material, the mass percentage of calcium oxide is 15-25%; the calcium oxide in the magnesium-containing base material is exogenous calcium oxide.

[0010] Furthermore, the mixture does not contain calcium carbonate.

[0011] Furthermore, the reducing agent includes ferrosilicon, and the molar ratio of magnesium oxide in the magnesium oxide material to silicon in the ferrosilicon is 2:1.1-1.5; in the ferrosilicon, the mass percentage of silicon is 50-90%.

[0012] Further, by percentage, the mass ratio of the flux to the magnesium-containing base material is no more than 5%; the flux includes metal fluorides; the metal fluorides include at least one of calcium fluoride, sodium fluoride, aluminum fluoride, potassium fluoride, and magnesium fluoride.

[0013] Furthermore, the method for obtaining the mixture includes: first preparing the mixture into powder, and then pressing it.

[0014] Furthermore, the method for obtaining the powder includes: ball milling the magnesium-containing base material and the flux together; the ball milling speed is 100-600 rpm, and the ball milling time is 10-80 min; The pressing pressure is 10-125 MPa, and the pressing holding time is not less than 3 minutes.

[0015] Furthermore, the reaction time of the reduction treatment is no more than 120 min; The mixture is conductive; the mixture forms a molten pool during the reduction process; The reaction current of the transferred arc plasma reactor during the reduction process is 20A-200kA.

[0016] Compared with the prior art, the present invention has at least the following advantages: This invention can improve the production efficiency of metallic magnesium while reducing the amount of tailings generated. This invention belongs to the plasma high-temperature driven low-slag magnesium smelting mode, which allows magnesium oxide materials, especially stable magnesium silicate phases such as Mg2SiO4, to enter the decomposition and reduction temperature range that is difficult to reach with traditional heat sources. At this time, the Mg-O bond state in the system is significantly weakened, and MgO and magnesium silicates are more likely to participate in the reduction.

[0017] This invention also utilizes the combination of a high-temperature reaction environment and a specific amount of calcium oxide added to reduce the generation of tailings and ensure the reduction rate. That is, in the high-temperature environment of this invention, one cannot rely on a high amount of calcium oxide added, nor can one reduce the amount of calcium oxide added indefinitely. Only by combining a specific amount of calcium oxide added with a high-temperature environment can a high reduction rate be maintained and the amount of tailings generated be kept at a low level.

[0018] Compared to the Pidgeon process for magnesium smelting, this invention establishes an ultra-high temperature reaction zone in a localized area using a transferred arc plasma reactor. This significantly improves the instantaneous thermal intensity and heating rate of the reaction zone, facilitating the rapid breaking down of the thermal stability of stable phases such as Mg2SiO4, increasing the activation degree of magnesium-containing phases, and enhancing the reduction process of MgO by Si. Furthermore, while the traditional Pidgeon process uses the reaction of CaO and SiO2 to form a stable calcium silicate phase, thus shifting the reaction equilibrium forward, this invention directly enhances the system's reactivity through the high-temperature environment created by the transferred arc plasma reactor. This allows magnesium-containing silicates to enter a higher-temperature decomposition and reduction range. Moreover, by controlling the amount of calcium oxide added within this high-temperature environment, the amount of slag is reduced, and the effective magnesium production capacity per unit reaction space and unit reaction time is increased. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0020] Figure 1 This is a thermodynamic analysis diagram of the high-temperature reduction principle in this invention; Figure 2 The XRD pattern of metallic magnesium in Example 1 of this invention; Figure 3 The image shows the XRD pattern of metallic magnesium in Comparative Example 2 of this invention.

[0021] The realization of the objective, functional characteristics and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.

[0024] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention, as well as the prior art known to those skilled in the art and the description of this invention, may be implemented using any prior art methods, devices, and materials similar to or equivalent to those described, used, or made of materials in the embodiments of this invention.

[0025] This invention provides a plasma-based low-slag silicothermal magnesium smelting method, comprising the following steps: S1 provides a mixture of magnesium-based material and flux; the magnesium-based material includes magnesium oxide, reducing agent, and calcium oxide.

[0026] In the magnesium-containing material of this invention, the mass percentage of calcium oxide is 10-30%. In this invention, the mass percentage of calcium oxide cannot be too high or too low; otherwise, it will be impossible to simultaneously maintain a high reduction rate and a low amount of tailings. It should be noted that the calcium oxide in the mixture originates solely from the magnesium-containing material, and the calcium oxide used in the subsequent reduction treatment also originates solely from the magnesium-containing material.

[0027] In some embodiments of the present invention, the purity (mass percentage) of magnesium oxide in the magnesium oxide material is not less than 90%; further, the purity of magnesium oxide in the magnesium oxide material is not less than 95%; further still, the purity of magnesium oxide in the magnesium oxide material is not less than 99%. The present invention, by controlling the purity of magnesium oxide in the magnesium oxide material, avoids an increase in the amount of tailings caused by other substances carried in the magnesium oxide material. In some preferred embodiments, the magnesium oxide material does not contain calcium carbonate.

[0028] In some embodiments of the present invention, the calcium oxide in the magnesium-containing base material is exogenous calcium oxide, and the exogenous calcium oxide and the magnesium oxide material are in a physically separated state. The exogenous calcium oxide refers to the calcium oxide in the magnesium-containing base material not originating from the magnesium oxide material, but rather requiring external addition. The present invention preferably uses exogenous calcium oxide in the magnesium-containing base material mainly because: in raw materials such as calcined white metal, calcium oxide and magnesium oxide are in a bound state, which leads to a reduction in their ability to fix silica. The present invention uses exogenous calcium oxide, which can improve its reactivity with silica and achieve magnesium oxide reduction with a lower calcium oxide content and lower tailings.

[0029] In some embodiments of the present invention, the mixture does not contain calcium carbonate; specifically, not only does the magnesium oxide material not carry calcium carbonate, but the mixture also does not contain calcium carbonate, thereby ensuring the normal progress of magnesium metal preparation.

[0030] In some embodiments of the present invention, the mixture comprises the magnesium oxide material, the reducing agent, the flux, and the calcium oxide; or, the mixture consists only of the magnesium oxide material, the reducing agent, the flux, and the calcium oxide. In some alternative embodiments, the mixture contains little or no other oxides besides magnesium oxide and calcium oxide.

[0031] In some embodiments of the present invention, the amount of calcium oxide added is kept within a specific range and combined with a specific reaction temperature. Compared with other addition amounts, this can ensure the reduction rate and significantly reduce the amount of slag. The mass percentage of calcium oxide in the magnesium-containing base material is further 10-25% or 15-30% or 20-30% or 25-30% or 15-25% or 14-26% or 15-20% or 14-21% or 20-25% or 18-22% or 13-17% or 14-16% or 22-25%.

[0032] In some embodiments of the present invention, the reducing agent comprises ferrosilicon; the molar ratio of magnesium oxide in the magnesium oxide material to silicon in the ferrosilicon is 2:1.1-1.5, more preferably 2:1.1-1.3; the mass percentage of silicon in the ferrosilicon is 50-90%, more preferably 70-80%, more preferably 74-76%; optionally, the ferrosilicon may be 75# ferrosilicon.

[0033] In some embodiments of the present invention, the mass ratio of the flux to the magnesium-containing base material is not greater than 5% by percentage, that is, the mass of the flux is not greater than 5% of the mass of the magnesium-containing base material, further being 1-5%, further being 1-3% or 3-5% or 1-2% or 2-4% or 4-5%; optionally, the flux comprises a metal fluoride; optionally, the metal fluoride comprises at least one of calcium fluoride, sodium fluoride, aluminum fluoride, potassium fluoride, and magnesium fluoride.

[0034] In some embodiments of the present invention, the method of obtaining the mixture includes: first preparing the mixture into powder, and then pressing it.

[0035] In some embodiments of the present invention, the powder is obtained by: ball milling the magnesium-containing base material and the flux together; the ball milling speed is 100-600 rpm, further 200-600 rpm, further 200-300 rpm; the ball milling time is 10-80 min, further 10-60 min or 50-70 min; in some cases, the ball-to-material ratio is 6-10:1, and the ball milling is carried out in a ball milling jar.

[0036] In some embodiments of the present invention, the pressing pressure is 10-125 MPa, more specifically 10-50 MPa; the pressing holding time is not less than 3 min, more specifically 5-30 min, more specifically 5-15 min; the pressing can be performed in a tablet press; optionally, the mixture obtained after pressing is cylindrical.

[0037] In some embodiments of the present invention, the powder is dried before the pressing is performed, and the drying method may be vacuum drying; optionally, the drying time is 3-24 hours, more preferably 6-24 hours or 5-7 hours; the drying pressure is 1-100 Pa, more preferably 90-100 Pa.

[0038] S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings.

[0039] In this invention, the reaction temperature of the reduction treatment is 2000-4000℃, further 2000-3300℃, further 2000-2500℃, or 2500-3000℃, or 2900-3100℃, or 2000-2100℃, or 2400-2600℃, or 2500-3300℃, or 2000-3000℃.

[0040] It should be noted that the reaction temperature is not arbitrarily selected. The present invention controls the reaction temperature through the transfer arc plasma reactor, which can ensure the reduction rate of magnesium oxide and the production efficiency of metallic magnesium under the condition of calcium oxide addition, and can quickly reduce the amount of tailings to obtain metallic magnesium.

[0041] In some embodiments of the present invention, the reaction time of the reduction treatment is no more than 120 min, further 10-120 min, further 10-60 min, further 15-30 min, 15-25 min, 20-50 min, 20-40 min, 20-30 min, or 20-25 min. Compared with existing magnesium smelting methods, the reduction treatment in the present invention has a shorter reaction time, which can effectively improve the production efficiency of metallic magnesium, thereby increasing the amount of metallic magnesium produced per unit time.

[0042] In some embodiments of the present invention, during the reduction process, the transferred arc plasma reactor contains an inert gas; the transferred arc plasma reactor has an anode and a cathode, and the anode, the mixture, the inert gas, and the cathode form a conductive path during the reduction process. The anode is presented in the form of an anode container for holding the mixture; the anode can be an anode crucible.

[0043] In this invention, the transferred arc plasma reactor operates in a transferred arc manner, rapidly heating and melting the material to enter the reaction state. This invention employs a transferred arc plasma method, directly constructing a conductive path so that the mixture undergoes a reduction reaction in a molten pool, simultaneously achieving material heating and electromagnetic stirring, overcoming the high reaction energy barrier of metallurgical reduction processes. The plasma arc in the transferred arc plasma reactor is generated between the cathode and anode; the transferred arc plasma reactor used in the various embodiments of this invention is specifically a transferred arc plasma reactor of a DC electric arc furnace.

[0044] In this invention, the reaction current of the transfer arc plasma reactor during the reduction process is 20A-200kA, further 100-500A, further 100-300A, or 200-300A, or 250-300A, or 280-320A, or 180-220A, or 230-270A, or 100-200A, or 200-250A, or 100-250A.

[0045] After the conductive path is formed, the inert gas is plasmaized under the action of the conductive path. By plasmaizing the inert gas in the conductive path, the molten pool of the mixture can be stirred in situ by jet, which enhances the heat and mass transfer of the reduction reaction and promotes the rapid occurrence of the reaction.

[0046] After the conductive path is formed, the mixture reaches the reaction temperature required for the reduction process under the action of the conductive path. In specific implementation, the transferred arc plasma reactor establishes a high-energy-density, high-temperature zone locally, thereby ensuring that the temperature of the reduction process meets the requirements and improving thermal efficiency. In this invention, the mixture is conductive; the mixture forms a molten pool during the reduction process.

[0047] In some embodiments of the present invention, the reaction pressure of the mixture is 500-200000 Pa, further 1000-90000 Pa, further 40000-90000 Pa, further 45000-55000 Pa, or 55000-65000 Pa, or 75000-85000 Pa, or 85000-90000 Pa, or 50000-90000 Pa, or 50000-80000 Pa, or 50000-60000 Pa, or 60000-80000 Pa, or 80000-90000 Pa, or 60000-90000 Pa; the inert gas is in a state of inlet and outlet balance in the transferred arc plasma reactor to ensure the control of the reaction pressure and to ensure the formation of the conductive path.

[0048] In some embodiments of the present invention, the inert gas includes at least one of argon and helium; further, the inert gas is argon.

[0049] In some embodiments of the present invention, after the mixture is placed in the transfer arc plasma reactor, the reaction area of ​​the transfer arc plasma reactor is evacuated to a vacuum using a vacuum pump, and inert gas is added. An inlet and outlet gas balance system is used to maintain the set pressure. Subsequently, the plasma power supply arc ignition device is started to heat and reduce MgO under a certain current, and finally volatilized and condensed metallic magnesium and a small amount of residual tailings are obtained.

[0050] In some embodiments of the present invention, the generated metallic magnesium rapidly escapes from the reaction zone of the transferred arc plasma reactor in vapor form and is introduced into the condensation unit for recovery, thereby reducing the residence time of magnesium vapor in the reaction zone and promoting the continuous forward reaction; optionally, the collection temperature of condensed magnesium is 30-60°C.

[0051] In some embodiments of the present invention, the reduction rate of the reduction treatment is 75-96%, further 80-96% or 87-96% or 90-96% or 90-91% or 92-96% or 92-93% or 95-96% or 77-96% or 93-96%.

[0052] In some embodiments of the present invention, the amount of slag produced per ton of magnesium in the reduction treatment is 2.3-3.2 tons, further 2.3-3.0 tons, 2.3-2.6 tons, 2.3-2.5 tons, 2.3-2.4 tons, 2.45-2.55 tons, 2.9-3.0 tons, 2.3-3.1 tons, 2.3-3.01 tons, or 2.3-2.8 tons.

[0053] As a further detailed explanation of the traditional Pidgeon process for magnesium smelting, the Pidgeon process generally suffers from problems such as complex vacuum systems, long reaction times, large slag production, high labor intensity, and low degree of continuous operation; for example: Firstly, the Pidgeon process for magnesium refining typically relies on a high vacuum to reduce the partial pressure of magnesium vapor and drive the reduction reaction forward. This results in the need for a vacuum pump set, a sealed reactor, and a matching condensation structure, making the equipment complex and the operating and maintenance costs high, which is not conducive to continuous and large-scale processes.

[0054] Secondly, the Pidgeon process for magnesium smelting adds a large amount of CaO to combine with the SiO2 produced in the reaction to form a calcium silicate slag phase, thereby weakening the adverse effect of SiO2 on the reaction equilibrium. However, this method is essentially a slag-making process to drive the reaction, which will lead to a significant increase in the amount of slag, high slag treatment pressure, and a heavy solid waste load on the magnesium recovery system.

[0055] Third, the Pidgeon process for magnesium smelting mostly uses external heating, which results in a long heat transfer path and limited thermal efficiency.

[0056] Fourth, the Pidgeon process for magnesium smelting is mostly an intermittent operation, with long cycles for processes such as charging, vacuuming, heating, holding, cooling and slag removal, making it difficult to achieve near-atmospheric pressure continuous production, which is not conducive to improving magnesium production efficiency per unit time.

[0057] Based on the above, this invention optimizes the Pidgeon process for magnesium smelting, thereby reducing the amount of tailings slag while ensuring the magnesium oxide reduction rate. Furthermore, this invention also solves the problems of external heating and intermittent operation. Overall, this invention solves various technical challenges of the Pidgeon process for magnesium smelting, including reliance on large amounts of CaO for slag formation, limitations imposed by high vacuum conditions, large slag volume, difficulty in continuous production, low thermal efficiency, and long reaction time. It achieves a rapid magnesium smelting method under near-atmospheric pressure, continuous operation, and low or even reduced slag conditions.

[0058] This invention proposes a rapid, low-slag magnesium smelting pathway by introducing a transferred arc plasma reactor. Based on efficient, centralized, and localized heating, it significantly increases the reduction reaction rate and reduces magnesium slag emissions. Furthermore, this invention eliminates the need for external heating; instead, it directly heats the mixture through a conductive path, resulting in a more thorough reduction reaction, increased magnesium yield, shorter reaction time, and reduced energy consumption. It also offers advantages such as rapid start-up, quick response, and strong adaptability. In addition, the reduction process of this invention can be carried out under near-atmospheric or slightly negative pressure conditions, which is beneficial for the continuous and automated production of magnesium.

[0059] To address the various problems existing in the traditional Pidgeon process for magnesium smelting, some of the ideas in this invention include: Firstly, a high-temperature heat source is provided by a transferred arc plasma reactor, replacing external heating.

[0060] Compared to the Pidgeon process for magnesium smelting, which relies on furnace wall heat transfer and long-term heat preservation, this invention establishes an ultra-high temperature reaction zone in a local area, which can significantly improve the instantaneous heat intensity and heating rate. This is beneficial for rapidly breaking the thermal stability of stable phases such as Mg2SiO4, increasing the activation degree of magnesium-containing phases, and strengthening the reduction process of Si to MgO.

[0061] Secondly, by utilizing the high-temperature reaction environment provided by the transferred arc plasma reactor and controlling the amount of CaO added, a high reduction rate and a low slag volume can be achieved simultaneously.

[0062] The Pidgeon process for magnesium smelting involves the reaction of CaO and SiO2 to form a stable calcium silicate phase, thereby shifting the reaction equilibrium in the forward direction. This invention, on the other hand, directly enhances the system's reactivity by utilizing the high temperature provided by the transferred arc plasma reactor, allowing magnesium silicates to enter a higher temperature decomposition and reduction range. Furthermore, by controlling the amount of CaO added, the amount of slag is reduced, the burden of slag formation is lessened, and the effective magnesium production capacity per unit reaction space and per unit reaction time is increased.

[0063] For an explanation of the principle of high-temperature reduction, see [link to relevant documentation]. Figure 1 The thermodynamic analysis results show that the reaction raw materials reach a high temperature of over 2500K, at which point the silicothermic reduction of MgO without CaO can occur under normal pressure. However, in actual processes, in order to simultaneously ensure a high reduction rate and a low slag amount, in addition to a high-temperature environment, it is also necessary to control the amount of CaO added.

[0064] Third, it breaks the strong dependence of Pijang magnesium smelting on high vacuum conditions.

[0065] This invention provides a high-temperature enhanced reaction through a transferred arc plasma reactor, and combined with the balanced control of the incoming and outgoing gases, the reaction can be carried out under near-normal pressure or slightly negative pressure conditions, thereby reducing the configuration requirements of the vacuum system, simplifying the equipment structure, reducing operating energy consumption and maintenance difficulty, and creating conditions for continuous operation.

[0066] The following are specific examples of the present invention: Example 1 A method for smelting magnesium, comprising the following steps: S1, magnesium oxide (99% purity), 75# ferrosilicon, calcium fluoride, and calcium oxide are ball-milled together in a ball mill jar to obtain a mixed powder; wherein, magnesium oxide, 75# ferrosilicon, and calcium oxide are magnesium-containing base materials.

[0067] The molar ratio of silicon in magnesium oxide and 75# ferrosilicon is 2:1.1, the mass percentage of calcium oxide in the magnesium-containing base material is 15%, and the amount of calcium fluoride added is 5% of the mass of the magnesium-containing base material; the ball milling speed is 200 rpm, the ball milling time is 60 min, and the ball-to-material ratio is 8:1.

[0068] The mixed powder was vacuum dried for 6 hours at a pressure of 100 Pa. After vacuum drying, the mixed powder was pressed using a tablet press at a pressure of 25 MPa for 5 minutes to obtain a cylindrical mixture.

[0069] S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings.

[0070] The transfer arc plasma reactor has an anode crucible and a cathode tungsten needle. The anode crucible is located below the cathode tungsten needle, and a transfer arc plasma is formed between the two during the reduction process.

[0071] The reduction process is as follows: the mixture is placed in the anode crucible, the transfer arc plasma reactor is evacuated to a vacuum using a vacuum pump and then argon is added. The inlet and outlet gas balance system is used to maintain the reaction pressure of the mixture at 50000Pa. The plasma power supply arc ignition device is activated with a reaction current of 250A. The anode crucible, mixture, argon gas, and cathode tungsten needle form a conductive path, creating an ultra-high temperature reaction zone in the anode crucible. The mixture undergoes a reduction reaction at around 3000℃ and forms a molten pool. The generated metallic magnesium escapes rapidly in the form of vapor and is introduced into the condensation unit for recovery. The condensed magnesium is collected at a temperature of 60℃.

[0072] In this embodiment, the XRD analysis of the obtained metallic magnesium is described in [reference needed]. Figure 2 As shown, the reduction rate after 20 minutes of reduction reaction was 95.16%, and the slag production per ton of magnesium was 2.33 tons. In this invention, the reduction rate refers to the demagnesification rate of the material, and the slag production per ton of magnesium refers to the slag yield per ton of metallic magnesium after conversion.

[0073] Example 2 A method for smelting magnesium, comprising the following steps: S1, magnesium oxide (99% purity), 75# ferrosilicon, calcium fluoride, and calcium oxide are ball-milled together in a ball mill jar to obtain a mixed powder; wherein, magnesium oxide, 75# ferrosilicon, and calcium oxide are magnesium-containing base materials.

[0074] The molar ratio of silicon in magnesium oxide and 75# ferrosilicon is 2:1.3, the mass percentage of calcium oxide in the magnesium-containing base material is 15%, and the amount of calcium fluoride added is 3% of the mass of the magnesium-containing base material; the ball milling speed is 200 rpm, the ball milling time is 60 min, and the ball-to-material ratio is 8:1.

[0075] The mixed powder was vacuum dried for 6 hours at a pressure of 100 Pa. After vacuum drying, the mixed powder was pressed using a tablet press at a pressure of 25 MPa for 5 minutes to obtain a cylindrical mixture.

[0076] S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings.

[0077] The transfer arc plasma reactor has an anode crucible and a cathode tungsten needle. The anode crucible is located below the cathode tungsten needle, and a transfer arc plasma is formed between the two during the reduction process.

[0078] The reduction process is as follows: the mixture is placed in the anode crucible, the transfer arc plasma reactor is evacuated to a vacuum using a vacuum pump and then argon is added. The inlet and outlet gas balance system is used to maintain the reaction pressure of the mixture at 80000Pa. The plasma power supply arc ignition device is activated with a reaction current of 250A. The anode crucible, mixture, argon gas, and cathode tungsten needle form a conductive path, creating an ultra-high temperature reaction zone in the anode crucible. The mixture undergoes a reduction reaction at around 3000℃ and forms a molten pool. The generated metallic magnesium escapes rapidly in the form of vapor and is introduced into the condensation unit for recovery. The condensed magnesium is collected at a temperature of 60℃.

[0079] In this embodiment, the reduction rate of the reduction reaction after 20 minutes was 90.15%, and the slag production per ton of magnesium was 2.58 tons.

[0080] Example 3 A method for smelting magnesium, comprising the following steps: S1, magnesium oxide (99% purity), 75# ferrosilicon, calcium fluoride, and calcium oxide are ball-milled together in a ball mill jar to obtain a mixed powder; wherein, magnesium oxide, 75# ferrosilicon, and calcium oxide are magnesium-containing base materials.

[0081] The molar ratio of silicon in magnesium oxide and 75# ferrosilicon is 2:1.1, the mass percentage of calcium oxide in the magnesium-containing base material is 15%, and the amount of calcium fluoride added is 1% of the mass of the magnesium-containing base material; the ball milling speed is 200 rpm, the ball milling time is 60 min, and the ball-to-material ratio is 8:1.

[0082] The mixed powder was vacuum dried for 6 hours at a pressure of 100 Pa. After vacuum drying, the mixed powder was pressed using a tablet press at a pressure of 25 MPa for 5 minutes to obtain a cylindrical mixture.

[0083] S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings.

[0084] The transfer arc plasma reactor has an anode crucible and a cathode tungsten needle. The anode crucible is located below the cathode tungsten needle, and a transfer arc plasma is formed between the two during the reduction process.

[0085] The reduction process is as follows: the mixture is placed in the anode crucible, the transfer arc plasma reactor is evacuated to a vacuum using a vacuum pump and then argon is added. The inlet and outlet gas balance system is used to maintain the reaction pressure of the mixture at 90000 Pa. The plasma power supply arc ignition device is activated with a reaction current of 250A. The anode crucible, mixture, argon gas, and cathode tungsten needle form a conductive path, creating an ultra-high temperature reaction zone in the anode crucible. The mixture undergoes a reduction reaction at around 3000℃ and forms a molten pool. The generated metallic magnesium escapes rapidly in the form of vapor and is introduced into the condensation unit for recovery. The condensed magnesium is collected at a temperature of 60℃.

[0086] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 87.33%, and the slag production per ton of magnesium was 2.43 tons.

[0087] Example 4 Compared to Example 1, this embodiment adjusts the reaction current to 200A and the reduction reaction temperature to around 2500℃, while keeping other conditions unchanged.

[0088] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 90.36%, and the slag production per ton of magnesium was 2.45 tons.

[0089] Example 5 Compared to Example 1, the mass ratio of calcium oxide in the magnesium-containing base material in this embodiment is adjusted to 30%, while other conditions remain unchanged.

[0090] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 94.38%, and the slag production per ton of magnesium was 3.01 tons.

[0091] Example 6 Compared to Example 1, the mass ratio of calcium oxide in the magnesium-containing base material in this embodiment is adjusted to 25%, while other conditions remain unchanged.

[0092] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 93.85%, and the slag production per ton of magnesium was 2.76 tons.

[0093] Example 7 Compared to Example 1, the mass ratio of calcium oxide in the magnesium-containing base material in this embodiment is adjusted to 20%, while other conditions remain unchanged.

[0094] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 93.16%, and the slag production per ton of magnesium was 2.56 tons.

[0095] Example 8 Compared to Example 1, the mass ratio of calcium oxide in the magnesium-containing base material in this embodiment is adjusted to 10%, while other conditions remain unchanged.

[0096] In this embodiment, the reduction rate after 20 minutes of reduction reaction was 77.33%, and the slag production per ton of magnesium was 2.80 tons.

[0097] Comparative Example 1 Compared to Example 1, the mass percentage of calcium oxide in the magnesium-containing base material in this comparative example was adjusted to 5%, while other conditions remained unchanged.

[0098] In this comparative example, the reduction rate after 20 minutes of reduction reaction was 69.18%, and the slag production per ton of magnesium was 3.03 tons.

[0099] Comparative Example 2 Compared to Example 1, this comparative example omits the addition of calcium oxide, while keeping other conditions unchanged.

[0100] In this comparative example, the reduction rate after 20 minutes of reduction reaction was 66.7%. (See [reference needed]). Figure 3 As shown, impurities such as Mg2Si appear in the magnesium metal products; the slag yield per ton of magnesium is 2.97 tons.

[0101] Comparative Example 3 Compared to Example 1, the mass ratio of calcium oxide in the magnesium-containing base material was adjusted to 40% in this comparative example, while other conditions remained unchanged.

[0102] In this comparative example, the reduction rate after 20 minutes of reduction reaction was 94.38%, and the slag production per ton of magnesium was 3.68 tons.

[0103] Comparative Example 4 Compared to Example 1, this comparative example adjusts the reaction current to 75A, the reduction reaction temperature to around 1850°C, and keeps other conditions unchanged.

[0104] In this comparative example, the reduction rate after 20 minutes of reduction reaction was 58.65%, and the slag production per ton of magnesium was 4.31 tons.

[0105] Comparative Example 5 Compared to Example 1, this comparative example did not use a transferred arc plasma reactor for reduction treatment, but instead used an induction heating reactor for reduction treatment.

[0106] In this comparative example, the steps of the magnesium smelting method are as follows: S1, magnesium oxide (99% purity), 75# ferrosilicon, calcium fluoride, and calcium oxide are ball-milled together in a ball mill jar to obtain a mixed powder; wherein, magnesium oxide, 75# ferrosilicon, and calcium oxide are magnesium-containing base materials.

[0107] The molar ratio of silicon in magnesium oxide and 75# ferrosilicon is 2:1.1, the mass percentage of calcium oxide in the magnesium-containing base material is 15%, and the amount of calcium fluoride added is 5% of the mass of the magnesium-containing base material; the ball milling speed is 200 rpm, the ball milling time is 60 min, and the ball-to-material ratio is 8:1.

[0108] The mixed powder was vacuum dried for 6 hours at a pressure of 100 Pa. After vacuum drying, the mixed powder was pressed using a tablet press at a pressure of 25 MPa for 5 minutes to obtain a cylindrical mixture.

[0109] S2, the mixture is placed in an induction heating reactor for reduction treatment to obtain metallic magnesium and tailings; the reduction treatment conditions are: reaction pressure 50000Pa, heating rate 20℃ / min, and the reduction reaction temperature after the heating is completed is 1200℃.

[0110] In this comparative example, the reduction rate after 20 minutes was only 8.28%, indicating that the reaction was essentially non-existent.

[0111] Comparative Example 6 Compared to Example 1, this comparative example did not use a transferred arc plasma reactor for the reduction reaction, but instead used a non-transferred arc plasma reactor for the reduction treatment.

[0112] In this comparative example, the steps of the magnesium smelting method are as follows: S1, magnesium oxide (99% purity), 75# ferrosilicon, calcium fluoride, and calcium oxide are ball-milled together in a ball mill jar to obtain a mixed powder; wherein, magnesium oxide, 75# ferrosilicon, and calcium oxide are magnesium-containing base materials.

[0113] The molar ratio of silicon in magnesium oxide and 75# ferrosilicon is 2:1.1, the mass percentage of calcium oxide in the magnesium-containing base material is 15%, and the amount of calcium fluoride added is 5% of the mass of the magnesium-containing base material; the ball milling speed is 200 rpm, the ball milling time is 60 min, and the ball-to-material ratio is 8:1.

[0114] The mixed powder was vacuum dried for 6 hours at a pressure of 100 Pa. After vacuum drying, the mixed powder was pressed using a tablet press at a pressure of 25 MPa for 5 minutes to obtain a cylindrical mixture.

[0115] S2, the mixture is placed in a non-transfer arc plasma reactor for reduction treatment, and the reduction reaction occurs under the conditions of 250A current and 50000Pa pressure to obtain metallic magnesium and tailings.

[0116] In this comparative example, the reduction rate after 20 minutes of reduction reaction was 51.81%, and the slag production per ton of magnesium was 5.28 tons.

[0117] The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A low-slag plasma-based process for the production of magnesium by silicon thermal reduction, characterized in that, Including the following steps: S1 provides a mixture of magnesium-based material and flux; the magnesium-based material includes magnesium oxide, reducing agent, and calcium oxide; the mass percentage of calcium oxide in the magnesium-based material is 15-25%; the calcium oxide in the magnesium-based material is exogenous calcium oxide. S2, the mixture is placed in a transfer arc plasma reactor for reduction treatment to obtain metallic magnesium and tailings; the reaction temperature of the reduction treatment is 2000-4000℃.

2. The plasma-based low-slag silicon thermal smelting magnesium method according to claim 1, characterized in that, During the reduction process, the transfer arc plasma reactor contains an inert gas; The transferred arc plasma reactor has an anode and a cathode, and the anode, the mixture, the inert gas, and the cathode form a conductive path during the reduction process; The inert gas is plasmaized under the action of the conductive path; The mixture reaches the reaction temperature under the action of the conductive path.

3. The plasma-based low-slag silicon thermal smelting magnesium method according to claim 2, characterized in that, The reaction pressure of the mixture is 500-200000 Pa; The inert gas is in a state of inlet and outlet balance in the transfer arc plasma reactor; The inert gas includes at least one of argon and helium.

4. The plasma-based low-slag silicon thermal smelting method for magnesium according to claim 1, characterized in that, In the magnesium oxide material, the mass percentage of magnesium oxide is not less than 90%.

5. The plasma-based low-slag silicothermal magnesium smelting method according to claim 1, characterized in that, The mixture does not contain calcium carbonate.

6. The plasma-based low-slag silicothermal magnesium smelting method according to claim 1, characterized in that, The reducing agent includes ferrosilicon, and the molar ratio of magnesium oxide in the magnesium oxide material to silicon in the ferrosilicon is 2:1.1-1.5; in the ferrosilicon, the mass percentage of silicon is 50-90%.

7. The plasma-based low-slag silicothermal magnesium smelting method according to claim 1, characterized in that, The mass ratio of the flux to the magnesium-containing base material is no more than 5% by percentage; the flux includes metal fluorides; the metal fluorides include at least one of calcium fluoride, sodium fluoride, aluminum fluoride, potassium fluoride, and magnesium fluoride.

8. The plasma-based low-slag silicothermal magnesium smelting method according to claim 1, characterized in that, The method for obtaining the mixture includes: first preparing the mixture into powder, and then pressing it.

9. The plasma-based low-slag silicothermal magnesium smelting method according to claim 8, characterized in that, The method for obtaining the powder includes: ball milling the magnesium-containing base material and the flux together; the ball milling speed is 100-600 rpm, and the ball milling time is 10-80 min; The pressing pressure is 10-125 MPa, and the pressing holding time is not less than 3 minutes.

10. The plasma-based low-slag silicothermal magnesium smelting method according to any one of claims 1-9, characterized in that, The reaction time for the reduction treatment is no more than 120 min; The mixture is conductive; the mixture forms a molten pool during the reduction process; The reaction current of the transferred arc plasma reactor during the reduction process is 20A-200kA.

Citation Information

Patent Citations

  • Method for preparing metal magnesium by using dolomite as raw material

    CN101812599B

  • Method for smelting magnesium metal through plasma electric arc furnace

    CN120818705A