Semi-diluted diamond composite polishing paste, preparation method and application thereof
The chemical mechanical polishing method using semi-dilute diamond composite polishing paste solved the problem of high surface roughness in zirconia artificial bone materials, achieving a high-efficiency, low-roughness polishing effect, avoiding scratches and damage layers, and improving surface quality and stability.
Patent Information
- Application Number
- CN202611264072.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-08-20
AI Technical Summary
Existing technologies for polishing zirconia artificial bone materials suffer from problems such as high surface roughness, deep scratches, and difficulty in removing the damaged layer, and it is difficult to balance removal efficiency and surface quality.
The semi-dilute diamond composite polishing paste contains polycrystalline diamond micro powder, silica powder, hydrophobically modified CeO2, La(NO3)3, Nd(NO3)3, citric acid, alanine/glycine mixture, PEG-200/400, glycerol, styrene O-25, PVP and fumed silica. Through chemical mechanical polishing and the synergistic effect of multiple abrasives, it achieves high-efficiency and low-roughness polishing.
It achieves efficient removal of zirconium dioxide materials and ultra-low roughness polishing, avoiding scratches and damage layers, and improving surface quality and stability.
Abstract
Description
Technical Field
[0001] This invention relates to the field of precision machining technology, specifically to a semi-dilute diamond composite polishing paste, its preparation method, and its application. Background Technology
[0002] In recent years, zirconia (ZrO2)-based artificial bone and dental prostheses have become important implant materials for bone defect repair and oral restoration in the biomedical field due to their excellent biocompatibility, good mechanical properties, and aesthetics. The surface quality of zirconia implants directly affects their biomechanical properties and osseointegration in vivo. Excessive surface roughness not only increases friction and wear between the implant and surrounding tissues but may also become a breeding ground for bacteria, affecting the long-term stability and lifespan of the implant. Studies have shown that fine polishing can effectively improve the surface smoothness of zirconia specimens, with effects comparable to glazing. Therefore, ultra-precision polishing of zirconia-based artificial bone materials to obtain a low-roughness, non-damaging, ultra-smooth surface is a key step in improving their clinical performance.
[0003] The aforementioned existing technology still has the following shortcomings when applied to polishing zirconia artificial bone materials: First, the high surface roughness after polishing makes it difficult to meet the surface quality requirements of medical implants. When using existing diamond abrasive pastes to polish zirconia-based artificial bone materials, deep scratches and damage layers often remain on the surface. Studies have shown that the polishing paste group of specimens has deep scratches accompanied by small particles. This is mainly because the diamond abrasive particles in existing abrasive pastes have a wide particle size distribution and are prone to agglomeration. Large agglomerates will cause deep scratches on the zirconia surface during polishing. At the same time, the mechanical removal effect of a single diamond abrasive is too strong, lacking a chemical synergistic polishing mechanism, making it difficult to achieve an ultra-smooth surface finish on zirconia materials. Second, a single abrasive cannot balance removal efficiency and surface quality. Diamond has extremely high hardness and strong mechanical removal ability, but using diamond abrasive alone easily causes scratches and damage layers on the processed surface. Cerium oxide has good chemical activity and can achieve high surface quality in chemical mechanical polishing, but its low hardness limits its material removal efficiency when used alone. While existing technologies offer solutions for simply combining multiple abrasives, the particle size matching and synergistic mechanism between different abrasives have not been fully optimized, making it difficult to simultaneously achieve efficient removal of zirconium dioxide materials and ultra-low roughness polishing. Summary of the Invention
[0004] Technical problem to be solved: The purpose of this invention is to provide a semi-diluted diamond composite polishing paste that solves the problem of high mechanical polishing damage and achieves high-efficiency, low-roughness, and scratch-free precision polishing of zirconia artificial bone materials.
[0005] Technical solution: A semi-dilute diamond composite polishing paste, wherein the composite polishing paste comprises the following components by mass percentage: 3-5% polycrystalline diamond micron powder 3-4% silica powder Hydrophobic modification of CeO2 2~2.5% La(NO3)3 0.2~0.25% Nd(NO3)3 0.2~0.25% Citric acid 0.5~0.6% Fumed silica 1.5~2% Alanine / glycine mixture 1.5~2.5% Pingping plus O-25 0.4~0.5% PVP 0.35~0.45% PEG-200 52~57% PEG-400 4~6% Glycerin 8~10% Trimethylolpropane oleate 1~1.2% Add deionized water to bring the total to 100%.
[0006] Preferably, the polycrystalline diamond micropowder has a particle size of W0.3~W1.0; the silica powder has a particle size of 0.1~0.3μm; and the hydrophobically modified CeO2 has a particle size of 30~50nm. Preferably, the mass ratio of alanine to glycine is 1:1.
[0007] Preferably, the PVP is PVP K30.
[0008] Preferably, the method for preparing the hydrophobically modified CeO2 is as follows: The silane coupling agent was dissolved in a 95% ethanol aqueous solution, the pH was adjusted to 4-5 with glacial acetic acid, and the solution was hydrolyzed by stirring at room temperature for 30-60 minutes to obtain a hydrolysate with a concentration of 2-5 wt%. Dry CeO2 powder was added to the above hydrolysate at a solid-liquid ratio of 1:10~20 g / mL. The powder was ultrasonically dispersed for 10~20 min to ensure thorough dispersion. Then, the mixture was stirred at 60~80°C for 4~8 h. After the reaction, the powder was collected and washed repeatedly with anhydrous ethanol 3~5 times to remove unreacted silane coupling agent. Finally, it was vacuum dried at 80~100°C for 4~6 h to obtain hydrophobically modified CeO2. CeO2 itself is a hydrophilic oxide with a surface rich in Ce-OH hydroxyl groups. Unmodified CeO2 exhibits severe compatibility problems in this low-water organic phase. The high interfacial tension between the hydrophilic surface and the organic continuous phase makes it difficult for CeO2 particles to be wetted by the organic phase, leading to spontaneous aggregation into large aggregates. These aggregates act as large-particle abrasives during polishing, causing deep scratches and damage layers on the zirconia surface. Hydrophobic modification was performed using silane coupling agents, and long-chain alkyl groups were grafted onto the surface of CeO2, changing its surface from hydrophilic to hydrophobic. This significantly improved its compatibility with the organic carrier phase, thereby achieving uniform and stable dispersion.
[0009] Preferably, the silane coupling agent is any one of octadecyltrimethoxysilane or dodecyltrimethoxysilane.
[0010] The preparation method of the above-mentioned semi-dilute diamond composite polishing paste includes the following steps: Step 1: Dissolve PVP in 30-40% of the total water mass of deionized water, stir evenly, then add PEG-200, polycrystalline diamond powder, silica powder, hydrophobically modified CeO2, and fumed silica in sequence, and then ultrasonically disperse for 20-30 minutes to obtain abrasive dispersion A. Step 2: Dissolve La(NO3)3 and Nd(NO3)3 in deionized water with a total water mass of 60-70%, add citric acid, react at 60℃ for 45 min, add alanine / glycine mixture and stir until homogeneous to obtain complex solution B; Step 3: Mix Pingpingjia O-25, PEG-400, glycerol, and trimethylolpropane oleate, and stir at 50~60℃ until completely dispersed to obtain carrier phase C; Step 4: Add abrasive dispersion A to carrier phase C, stir for 15-20 minutes, add the final complex solution B, stir rapidly for 10 minutes, adjust the pH to 5.8-6.2, and finally obtain the grinding paste.
[0011] The application of the aforementioned semi-dilute diamond composite polishing paste in the grinding and polishing of zirconium dioxide materials.
[0012] Beneficial effects: The grinding paste of the present invention has the following advantages: In this invention, polycrystalline diamond micropowder is used as the main abrasive. Utilizing its extremely high hardness and the self-sharpening property inherent in its polycrystalline structure, it efficiently removes material from the zirconia surface through plastic removal and brittle fracture. Simultaneously, numerous micro-cutting edges continuously provide fresh cutting surfaces, avoiding the passivation problem of single-crystal diamond. Silica powder, with a lower hardness than zirconia, undergoes a tribochemical reaction with ZrO2 under high pressure and friction at the polishing interface, forming Zr-O-Si bonds. This generates a relatively soft reaction layer, which is then mechanically removed, achieving a "soft abrasion, hard" chemical mechanical polishing effect, effectively reducing surface damage caused by pure mechanical polishing. Hydrophobically modified CeO2 serves as an auxiliary abrasive. Under polishing pressure and frictional heat, it undergoes a mild oxidation reaction with the zirconia surface, forming a thin chemical reaction layer to assist in softening the surface. Its relatively soft characteristics and the controlled reactivity after hydrophobic modification make it less prone to deep scratches. These three abrasives ensure a high material removal rate while effectively suppressing surface scratches and damage layers, overcoming the technical bottlenecks of high mechanical damage from single diamond abrasives and low removal efficiency from single CeO2 abrasives. This invention introduces La(NO3)3 and Nd(NO3)3, which react with citric acid to form a stable citric acid complex. During the polishing process, La... 3+ / Nd 3+ As the complex migrates to the zirconia surface, it forms La-O-Zr / Nd-O-Zr surface bonds through chemisorption, constructing a rare-earth-rich surface layer. This surface layer can effectively improve the stability of tetragonal zirconia and suppress the phase transformation induced by polishing mechanical stress. In this invention, alanine and glycine serve as polishing promoters, exerting a dual function at the polishing interface. On one hand, the carboxyl groups of the amino acid molecules can react with Ce... 4+ Complexation occurs, enhancing the oxidation reactivity of CeO2 and promoting the improvement of chemical mechanical polishing efficiency. On the other hand, the amino groups of amino acids are adsorbed onto the surface of zirconium oxide materials through hydrogen bonds, forming a molecular protective film. This film can both inhibit unnecessary excessive chemical reactions during polishing and prevent the formation of surface corrosion pits, and also act as an interface lubricant, reducing the coefficient of friction between the abrasive and the workpiece surface and reducing mechanical scratches. This invention employs PEG-200 / 400, glycerol, and trimethylolpropane oleate to construct a low-water organic continuous phase. Combined with the surface properties of PVP, fumed silica, and hydrophobically modified CeO2, uniform and stable dispersion of abrasives and additives in the paste is achieved. PEG-200 and PEG-400 are used as the main carrier solvents. By precisely adjusting the polarity and viscosity of the system through a specific ratio of low-molecular-weight PEG-200 to medium-molecular-weight PEG-400, the grinding paste exhibits a semi-thin state, ensuring both ease of application and effective retention of the abrasive in the grinding zone. Glycerol, as a wetting agent and auxiliary lubricant, effectively retains moisture in the paste and enhances the system's lubricity. Trimethylolpropane oleate, as a highly efficient lubricating film-forming agent, forms a physical lubricating film at the abrasive-workpiece interface, significantly reducing the coefficient of friction and minimizing the risk of burns and microcracks on the workpiece surface caused by frictional heat. It also facilitates the efficient removal of abrasive debris. The process involves timely discharge to improve the final surface quality; hydrophobic modification transforms CeO2 from hydrophilic to hydrophobic, ensuring good compatibility with the organic carrier phase and avoiding the aggregation and sedimentation problems of hydrophilic CeO2 in the organic phase; fumed silica constructs a three-dimensional thixotropic network through silanol hydrogen bonds in a low-water environment, ensuring both storage stability and meeting the requirements for spreadability and flowability during polishing; PVP assists in dispersion through steric hindrance mechanism, synergistically preventing abrasive agglomeration with fumed silica and avoiding surface scratches caused by large particle agglomerates; and Pingpingjia O-25, as a nonionic surfactant, further reduces interfacial tension and promotes the compatibility of each component. Detailed Implementation
[0013] The present invention will be further described below with reference to embodiments. These embodiments are illustrative of the present invention, but the present invention is not limited to these embodiments: Example 1
[0014] The preparation method of hydrophobically modified CeO2 is as follows: Octadecyltrimethoxysilane was dissolved in a 95% aqueous ethanol solution, the pH was adjusted to 4 with glacial acetic acid, and the solution was hydrolyzed by stirring at room temperature for 30 min to obtain a 2 wt% hydrolysate. The dried CeO2 powder was added to the above hydrolysate at a solid-liquid ratio of 1:10 g / mL. The powder was ultrasonically dispersed for 10 min to ensure full dispersion. Then, the mixture was stirred at 60°C for 8 h. After the reaction was completed, the powder was collected and washed three times with anhydrous ethanol to remove unreacted silane coupling agent. Finally, the powder was vacuum dried at 100°C for 4 h to obtain hydrophobically modified CeO2.
[0015] Example 2
[0016] The preparation method of hydrophobically modified CeO2 is as follows: Dodecyltrimethoxysilane was dissolved in a 95% aqueous ethanol solution, the pH was adjusted to 5 with glacial acetic acid, and the solution was hydrolyzed by stirring at room temperature for 60 min to obtain a 5 wt% hydrolysate. The dried CeO2 powder was added to the above hydrolysate at a solid-liquid ratio of 1:20 g / mL. The powder was ultrasonically dispersed for 20 min to ensure full dispersion. Then, the mixture was stirred at 80°C for 4 h. After the reaction was completed, the powder was collected and washed repeatedly with anhydrous ethanol 5 times to remove unreacted silane coupling agent. Finally, the powder was vacuum dried at 80°C for 6 h to obtain hydrophobically modified CeO2.
[0017] Example 3
[0018] A semi-dilute diamond composite polishing paste, the composite polishing paste comprising the following components by weight percentage: Polycrystalline diamond micron powder (particle size W0.3~W1.0) 4% Silica powder (particle size 0.1~0.3μm) 4% Example 1 prepared hydrophobically modified CeO2 (particle size 30-50 nm) 2% La(NO3)3 0.2% Nd(NO3) 30.2% Citric acid 0.5% 1.5% fumed silica 2.5% of alanine / glycine mixture at a mass ratio of 1:1. Pingping plus O-25 0.4% PVP K30 0.45% PEG-200 52% PEG-400 6% 10% glycerin 1% Trimethylolpropane oleate Deionized water should be replenished to 100%. The preparation method of the above-mentioned semi-dilute diamond composite polishing paste includes the following steps: Step 1: Dissolve PVP in 30% of the total water mass of deionized water, stir evenly, then add PEG-200, polycrystalline diamond powder, silica powder, hydrophobically modified CeO2, and fumed silica in sequence, and then ultrasonically disperse for 20 minutes to obtain abrasive dispersion A. Step 2: Dissolve La(NO3)3 and Nd(NO3)3 in deionized water with a total water mass of 70%, add citric acid, react at 60℃ for 45 min, add alanine / glycine mixture and stir until homogeneous to obtain complex solution B; Step 3: Mix Pingpingjia O-25, PEG-400, glycerol, and trimethylolpropane oleate, and stir at 60°C until completely dispersed to obtain carrier phase C; Step 4: Add abrasive dispersion A to carrier phase C, stir for 15 min, add the final complex solution B, stir rapidly for 10 min, adjust pH to 6.2, and finally obtain the grinding paste.
[0019] Example 4
[0020] A semi-dilute diamond composite polishing paste, the composite polishing paste comprising the following components by weight percentage: Polycrystalline diamond micron powder (particle size W0.3~W1.0) 5% Silica powder (particle size 0.1~0.3μm) 3% Example 2 prepared hydrophobically modified CeO2 (particle size 30-50 nm) 2.5% La(NO3)3 0.25% Nd(NO3) 30.25% Citric acid 0.6% 2% fumed silica 1.5% of alanine / glycine mixture at a mass ratio of 1:1. Pingping plus O-25 0.5% PVP K30 0.35% PEG-200 57% PEG-400 4% 8% glycerin Trimethylolpropane oleate 1.2% Deionized water should be replenished to 100%. The preparation method of the above-mentioned semi-dilute diamond composite polishing paste includes the following steps: Step 1: Dissolve PVP in 40% of the total water mass of deionized water, stir evenly, then add PEG-200, polycrystalline diamond powder, silica powder, hydrophobically modified CeO2, and fumed silica in sequence, and then ultrasonically disperse for 30 minutes to obtain abrasive dispersion A. Step 2: Dissolve La(NO3)3 and Nd(NO3)3 in deionized water with a total water mass of 60%, add citric acid, react at 60℃ for 45 min, add alanine / glycine mixture and stir until homogeneous to obtain complex solution B; Step 3: Mix Pingpingjia O-25, PEG-400, glycerol, and trimethylolpropane oleate, and stir at 50°C until completely dispersed to obtain carrier phase C; Step 4: Add abrasive dispersion A to carrier phase C, stir for 20 minutes, add the final complex solution B, stir rapidly for 10 minutes, adjust the pH to 5.8, and finally obtain the grinding paste.
[0021] Example 5
[0022] A semi-dilute diamond composite polishing paste, the composite polishing paste comprising the following components by weight percentage: Polycrystalline diamond micron powder (particle size W0.3~W1.0) 5% Silica powder (particle size 0.1~0.3μm) 3.5% Example 1 prepared hydrophobically modified CeO2 (particle size 30-50 nm) 2.5% La(NO3)3 0.25% Nd(NO3) 30.25% Citric acid 0.6% 1.8% fumed silica 2% alanine / glycine mixture at a mass ratio of 1:1 Pingping plus O-25 0.45% PVP K30 0.4% PEG-200 55% PEG-400 5% 9% glycerin 1% Trimethylolpropane oleate Deionized water should be replenished to 100%. The preparation method of the above-mentioned semi-dilute diamond composite polishing paste includes the following steps: Step 1: Dissolve PVP in 35% of the total water mass of deionized water, stir evenly, then add PEG-200, polycrystalline diamond powder, silica powder, hydrophobically modified CeO2, and fumed silica in sequence, and then ultrasonically disperse for 25 minutes to obtain abrasive dispersion A. Step 2: Dissolve La(NO3)3 and Nd(NO3)3 in deionized water with a total water mass of 65%, add citric acid, react at 60℃ for 45 min, add alanine / glycine mixture and stir until homogeneous to obtain complex solution B; Step 3: Mix Pingpingjia O-25, PEG-400, glycerol, and trimethylolpropane oleate, and stir at 60°C until completely dispersed to obtain carrier phase C; Step 4: Add abrasive dispersion A to carrier phase C, stir for 18 minutes, add the final complex solution B, stir rapidly for 10 minutes, adjust the pH to 6, and finally obtain the grinding paste.
[0023] Comparative Example 1 The difference between Comparative Example 1 and Example 5 is that no silica powder is added.
[0024] Comparative Example 2 The difference between Comparative Example 2 and Example 5 is that polycrystalline diamond powder is not added.
[0025] Comparative Example 3 The difference between Comparative Example 3 and Example 5 is that CeO2 is not modified to be hydrophobic.
[0026] Comparative Example 4 The difference between Comparative Example 4 and Example 5 is that the polycrystalline diamond micropowder accounts for 3% of the total mass; the silica powder accounts for 6% of the total mass; and the hydrophobically modified CeO2 accounts for 2.5% of the total mass. Comparative Example 5 The difference between Comparative Example 5 and Example 5 is that the particle size of the silica powder and the hydrophobically modified CeO2 is 0.5~1.5μm.
[0027] Comparative Example 6 The difference between Comparative Example 6 and Example 5 is that La(NO3)3, Nd(NO3)3, and citric acid are not added.
[0028] Comparative Example 7 The difference between Comparative Example 7 and Example 5 is that the alanine / glycine mixture is not added.
[0029] Comparative Example 8 The difference between Comparative Example 8 and Example 5 is that the mass percentage of PEG-200 was adjusted to 30%; the mass percentage of PEG-400 was 30%.
[0030] Comparative Example 9 The difference between Comparative Example 9 and Example 5 is that the mass percentage of PEG-200 is reduced to 40%.
[0031] Performance testing: Stability test: Place the grinding paste in a sealed container and observe the separation time at room temperature; place another portion of the sample in an 80℃ oven for 3 days and observe whether separation occurs. Roughness test: On a single-sided grinding machine, the semi-diluted diamond composite grinding paste prepared in Examples 3-5 and Comparative Examples 1-9 were uniformly coated on the grinding disc and the zirconia was ground and polished. The grinding and polishing were divided into coarse grinding and fine grinding. The coarse grinding speed was 1300 rpm, the pressure was 80 N, and the time was 10 min. The fine grinding speed was 200 rpm, no pressure was applied, and the time was 10 min. After grinding and polishing, the polished surface was observed and the Ra value after grinding and polishing was measured using a surface roughness meter (requirement: ≤0.02 μm). The specific grinding test results are shown in Table 1 below.
[0032] Table 1 Stratification time (d) High temperature stability Ceramic surface condition after polishing Surface roughness Ra (μm) Example 3 25 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0094 Example 4 28 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0081 Example 5 30 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0076 Comparative Example 1 28 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0352 Comparative Example 2 32 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0418 Comparative Example 3 8 Clearly layered minor scratches 0.0563 Comparative Example 4 26 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0287 Comparative Example 5 22 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0435 Comparative Example 6 28 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0185 Comparative Example 7 30 No layering Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0268 Comparative Example 8 5 Clearly layered minor scratches 0.0621 Comparative Example 9 12 Slight stratification Free from defects such as particulate contamination, spot-like chemical discoloration, small nicks, debris, dents, and cracks. 0.0324 As can be seen from Table 1, without the addition of silica powder, pure mechanical polishing dominates. Diamond micropowder directly cuts on the hard and brittle ZrO2 surface. Without the buffering effect of silica powder, the cutting force of the diamond abrasive acts entirely on the workpiece surface, resulting in material removal during surface grinding mainly through brittle fracture, leading to an increase in the Ra value. Without the addition of diamond, polishing is carried out solely by silica powder (hardness of about 7, lower than the hardness of ZrO2 of about 8.5) and CeO2 (hardness of about 6). Both of these materials have a hardness lower than the workpiece material, making it impossible to achieve effective mechanical removal.
[0033] CeO2 is a hydrophilic oxide with a surface rich in Ce-OH hydroxyl groups and extremely high surface energy. Unmodified CeO2 exhibits extremely high interfacial tension with the organic phase, making it unable to be effectively wetted. This leads to particle aggregation, forming micron-sized aggregates. During polishing, these aggregates act as large, hard particles, causing scratches on the ZrO2 surface and severely damaging its integrity. Furthermore, aggregation destabilizes the paste dispersion system, leading to rapid stratification during storage, and accelerated sedimentation at high temperatures.
[0034] In this invention, polycrystalline diamond has the highest content, silica powder has a medium content, and modified CeO2 has the lowest content. Polycrystalline diamond, with its extremely high hardness, undertakes the main material removal task; silica powder, with a hardness lower than ZrO2, cannot be directly cut, but can undergo a solid-state reaction with ZrO2 using frictional heat (forming Zr-O-Si bonds), softening the workpiece surface. The content must be sufficient to form a continuous reaction layer, but cannot exceed that of diamond, otherwise it will excessively dilute the cutting force of diamond; modified CeO2 can limit the mechanical scratching effect, preventing it from introducing new scratches due to excessive amounts. Besides the combination of abrasive materials with different hardnesses, there are also certain requirements regarding the particle size of the abrasive materials. As can be seen from Comparative Example 5, when the particle size of both silica powder and CeO2 is increased to 0.5~1.5μm, the scale difference between the three particle size grades decreases, and the multi-scale synergistic effect is destroyed. In particular, the particle size of CeO2 increases sharply from 30~50nm to 0.5~1.5μm, and it loses its ability to repair nanoscale scratches.
[0035] La 3+ and Nd 3+ In this invention, a stable rare-earth citric acid complex is formed with citric acid. During polishing, this complex migrates with the polishing paste to the ZrO2 surface, La... 3+ and Nd 3+A protective layer is constructed on the ZrO2 surface through La-O-Zr / Nd-O-Zr surface bonding formed by chemisorption. Rare earth ions in this protective layer can enter the ZrO2 lattice, occupy lattice sites, and increase the oxygen vacancy concentration, thereby stabilizing the tetragonal phase structure. Alanine / glycine is adsorbed onto the ZrO2 surface via hydrogen bonding, forming a molecular protective film with a thickness of approximately 1-2 nm. This film reduces the coefficient of friction between the abrasive and the workpiece, minimizing mechanical scratches; it also inhibits the excessive oxidation of CeO2 during polishing, preventing localized corrosion pits on the surface.
[0036] In this invention, PEG-200 serves as the main diluent, imparting good flowability and spreadability to the polishing paste. PEG-400, acting as a thickener / regulator, synergistically adjusts the system viscosity to the optimal thixotropic range with PEG-200. When the proportion of the diluent PEG-200 decreases, the three-dimensional thixotropic network constructed by fumed silica cannot be effectively opened due to a lack of sufficient low-viscosity medium, resulting in loss of thixotropy. The paste rapidly hardens and separates during storage. Meanwhile, the Brownian motion of abrasive particles in the high-viscosity medium is restricted, accelerating gravitational settling. Simultaneously, the paste cannot form a fresh abrasive replenishment layer at the polishing interface, leading to the workpiece surface in the local abrasive depletion zone not being polished. Effective processing was achieved, with an Ra value as high as 0.0621 μm. When PEG-200 was reduced from 55% to 40% (replenished to 100% with deionized water), the polarity of water was much higher than that of PEG, resulting in poor compatibility with the abrasive. The paste exhibited thixotropic rigidity, being too hard at rest and difficult to thin under shear, making coating difficult. Due to uneven paste coating, some areas on the grinding disc had excessively thick abrasive buildup, while others lacked abrasive. The areas with excessively high abrasive concentration experienced over-grinding under polishing pressure, resulting in surface pits and increased roughness (Ra=0.0324 μm); the areas lacking abrasive retained the original rough grinding marks, leading to uneven overall surface quality.
[0037] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A semi-dilute diamond composite polishing paste, characterized in that, The composite abrasive paste contains the following components by weight percentage: 3-5% polycrystalline diamond micron powder 3-4% silica powder Hydrophobic modification of CeO2 2~2.5% La(NO3)3 0.2~0.25% Nd(NO3)3 0.2~0.25% Citric acid 0.5~0.6% Fumed silica 1.5~2% Alanine / glycine mixture 1.5~2.5% Pingping plus O-25 0.4~0.5% PVP 0.35~0.45% PEG-200 52~57% PEG-400 4~6% Glycerin 8~10% Trimethylolpropane oleate 1~1.2% Deionized water should be replenished to 100%. The polycrystalline diamond micropowder has a particle size of W0.3~W1.0; the silica powder has a particle size of 0.1~0.3μm; and the hydrophobically modified CeO2 has a particle size of 30~50nm. The preparation method of the hydrophobically modified CeO2 is as follows: The silane coupling agent was dissolved in a 95% ethanol aqueous solution, the pH was adjusted to 4-5 with glacial acetic acid, and the solution was hydrolyzed by stirring at room temperature for 30-60 minutes to obtain a hydrolysate with a concentration of 2-5 wt%. Add the dried CeO2 powder to the above hydrolysate at a solid-liquid ratio of 1:10~20 g / mL, and ultrasonically disperse for 10~20 min to ensure full dispersion of the powder. Then, stir and react at 60~80°C for 4~8 h. After the reaction is complete, collect the powder and wash it repeatedly with anhydrous ethanol 3~5 times to remove unreacted silane coupling agent. Finally, vacuum dry at 80~100°C for 4~6 h to obtain hydrophobically modified CeO2.
2. The semi-dilute diamond composite polishing paste according to claim 1, characterized in that: The mass ratio of alanine to glycine is 1:
1.
3. The semi-dilute diamond composite polishing paste according to claim 1, characterized in that: The PVP is PVP K30.
4. The semi-diluted diamond composite polishing paste according to claim 1, characterized in that: The silane coupling agent is either octadecyltrimethoxysilane or dodecyltrimethoxysilane.
5. The method for preparing the semi-diluted diamond composite polishing paste according to claim 1, characterized in that, Includes the following steps: Step 1: Dissolve PVP in 30-40% of the total water mass of deionized water, stir evenly, then add PEG-200, polycrystalline diamond powder, silica powder, hydrophobically modified CeO2, and fumed silica in sequence, and then ultrasonically disperse for 20-30 minutes to obtain abrasive dispersion A. Step 2: Dissolve La(NO3)3 and Nd(NO3)3 in deionized water with a total water mass of 60-70%, add citric acid, react at 60℃ for 45 min, add alanine / glycine mixture and stir until homogeneous to obtain complex solution B; Step 3: Mix Pingpingjia O-25, PEG-400, glycerol, and trimethylolpropane oleate, and stir at 50~60℃ until completely dispersed to obtain carrier phase C; Step 4: Add abrasive dispersion A to carrier phase C, stir for 15-20 minutes, add the final complex solution B, stir rapidly for 10 minutes, adjust the pH to 5.8-6.2, and finally obtain the grinding paste.
6. The application of the semi-diluted diamond composite polishing paste according to any one of claims 1 to 4 in the grinding and polishing of zirconium dioxide materials.
Citation Information
Patent Citations
Grinding fluid for processing LED (light-emitting diode) substrate and preparation method thereof
CN102337084A
Method for grinding zirconia ceramics
CN109262373A