Multi-polymer ultra-high temperature retarder and its preparation method
By combining multi-component copolymer main agent and compound additives, and using free radical copolymerization and a two-stage heating process, an interface-bulk retarding mode is formed, which solves the problems of easy molecular chain degradation and high dosage sensitivity of existing ultra-high temperature retarder, and achieves stable retarding effect and construction stability at high temperature.
Patent Information
- Application Number
- CN202611349221.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-09-02
AI Technical Summary
Existing ultra-high temperature retarders are prone to thermal degradation and desorption of molecular chains at high temperatures. The hydrolysis of amide bonds and removal of carboxyl groups lead to the loss of adsorption groups, resulting in a sharp decline in retardation performance. Furthermore, they are highly sensitive to dosage and have a steep thickening curve, which affects the water loss control performance and construction stability of cement paste.
By using a multi-component copolymer as the main agent, a liquid-phase chelation and deposition effect of compounded additives is formed through free radical copolymerization and post-crosslinking reaction, an interface-bulk retarding mode is formed to control the structural integrity and adsorption stability of the molecular chain. A two-stage heating program is used to control the crosslinking uniformity, and the pH value is controlled within the neutral range.
It maintains structural integrity and adsorption stability at temperatures ranging from 220℃ to 250℃, exhibits a stable retarding effect, avoids sudden performance changes of single main agents or small molecule additives at high temperatures, and improves storage stability and construction reliability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of oil well cement admixture technology, specifically relating to a multi-component polymer ultra-high temperature retarder and its preparation method. Background Technology
[0002] Cement retarders are indispensable functional admixtures in cementing engineering. Their main function is to regulate the thickening time of cement slurry, ensuring its pumpability during pumping and accurate solidification in the target well section, thereby ensuring cementing safety and quality. In cementing operations in deep wells, ultra-deep wells, and high-temperature, high-pressure gas wells, the bottom hole circulation temperature often exceeds 200°C, and in some ultra-deep wells, it even reaches above 230°C. Under such ultra-high temperature environments, the cement hydration rate accelerates dramatically. Without effective retardation measures, the cement slurry may thicken or even solidify before reaching the intended sealing position, leading to serious accidents such as pump stalling and stuck drill bit failure. Therefore, the performance of ultra-high temperature retarders directly determines the success or failure of cementing.
[0003] Currently, commonly used ultra-high temperature retarders both domestically and internationally mainly fall into two categories: synthetic polymer retarders and small molecule compound retarders. Synthetic polymer retarders are prepared by free radical polymerization of monomers such as 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, and acrylic acid. They utilize the adsorption of sulfonic acid and carboxylic acid functional groups on the molecular chain onto the surface of cement particles to form a hydration film, thereby delaying cement hydration. Small molecule compound retarders achieve retardation by chelating calcium ions with components such as borax, tartaric acid, and hydroxyethylidene diphosphonic acid, or by depositing them on the surface of cement particles to form a protective layer. Existing technologies have improved the temperature resistance of retarders to a certain extent by introducing heat-resistant rigid monomers, increasing the charge density of the molecular chain, and compounding with inorganic salts or organic phosphonates. This has enabled some products to reach an upper temperature resistance limit of 200-240℃, basically meeting the needs of conventional deep well cementing.
[0004] However, while existing technologies address the problem of ultra-high temperature retarding, they still have the following shortcomings. First, existing polymer retarders are prone to thermal degradation and desorption under ultra-high temperature conditions. Amide bond hydrolysis and carboxyl group removal lead to the loss of adsorption groups, causing the retarding performance to decline sharply with increasing temperature, making it difficult to maintain stable setting ability above 240℃. Second, some retarders are highly sensitive to dosage, requiring larger dosages at high temperatures to maintain sufficient thickening time. However, large dosages can lead to excessive retarding at the top of the cement slurry, affecting the early strength development of the cement stone at the top of long-sealed sections. Third, existing retarders and water loss control agents have similar molecular structures, making them prone to interference when combined, thus compromising the water loss control performance of the cement slurry. Fourth, some acidic retarders react with rust during storage and transportation in iron tanks, significantly shortening the thickening time of the cement slurry after aging, introducing uncertainty into on-site construction. These problems restrict the application of ultra-high temperature retarders in complex conditions such as deep wells, ultra-deep wells, and 10,000-meter exploration wells. Therefore, it is necessary to design multi-component polymer ultra-high temperature retarders and their preparation methods. Summary of the Invention
[0005] To overcome the shortcomings of existing technologies, a multi-component polymer ultra-high temperature retarder and its preparation method are provided.
[0006] To achieve the above objectives, the present invention provides the following technical solution: The multi-component polymer ultra-high temperature retarder, by mass parts, includes 28-32 parts of multi-component copolymer main agent and 68-72 parts of compounded additives; The preparation method of the multi-component copolymer main agent includes the following steps: 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, N-vinylpyrrolidone, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are subjected to free radical copolymerization reaction in water; when the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide is added for post-crosslinking reaction; then acrylic acid monomer is added for supplementary copolymerization reaction to obtain the multi-component copolymer main agent, and the multi-component copolymer main agent is added in the form of an aqueous solution with a solid content of 40%-50%; The compound additives, by mass parts, include 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 78-90 parts of deionized water.
[0007] The mass ratio of sodium ethylenediaminetetramethylenephosphonate, D-sorbitol, sodium tetraborate, sodium citrate and sodium gluconate in the compound additives is 4-6:3-5:1.5-2.5:2.5-3.5:3-4.
[0008] The preparation method of the compound additive includes the following steps: weigh out the sodium ethylenediaminetetramethylenephosphonate and sodium citrate according to the mass fraction, dissolve them in deionized water, heat to 45-55℃ and stir for 15-25 min, then add D-sorbitol and sodium gluconate, continue stirring for 10-15 min, then add sodium tetraborate, and after complete dissolution, cool to 25-35℃ to obtain the compound additive.
[0009] The stirring speed in the compound additive is 200-400 rpm, and the pH value of the compound additive is 6.5-7.5.
[0010] The main component of the multi-component copolymer, by weight, comprises 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water.
[0011] The preparation method of the multi-component copolymer main agent includes the following steps: a. Free radical copolymerization reaction: Weigh out 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid and N-vinylpyrrolidone according to the mass ratio and dissolve them in deionized water. Adjust the pH to 6.0-7.0 with sodium hydroxide with a mass concentration of 10%-20%. Add mercaptopropionic acid as a chain transfer agent and stir for 20-40 min under nitrogen protection. Then add vinylboric acid and methacryloyloxyethyltrimethylammonium chloride and continue stirring for 10-15 min until completely dissolved to obtain a monomer mixed solution. b. Initiator preparation: Prepare aqueous solutions of initial ammonium persulfate and sodium bisulfite with mass concentrations of 3%-5% and 2%-4%, respectively. c. Polymerization reaction: The monomer mixture solution is heated to 55-65℃, and the initial ammonium persulfate solution and sodium bisulfite solution are added simultaneously. After completion, the temperature is raised to 75-85℃ and the reaction is maintained at a constant temperature for 2.0-3.0h. A nitrogen atmosphere is maintained during the reaction. When the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide and additional ammonium persulfate are added. The amount of additional ammonium persulfate is 10%-20% of the mass of the initial ammonium persulfate. The reaction is continued at 75-85℃ for 30-50min to obtain the post-crosslinked copolymer solution. d. Supplement the copolymerization reaction by adding acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80°C for 20-40 minutes. e. Post-processing step: Add sodium sulfite to the product from step d, the amount of which is 0.2%-0.5% of the total mass of the product, stir at 25-35℃ for 15-25 min, and then adjust the pH to 6.5-7.5 with sodium hydroxide with a mass concentration of 10%-20% to obtain the multi-component copolymer main agent.
[0012] In step c, the solid content of the reaction system is controlled at 35%-45%, the total reaction time is controlled at 2.5-4.5 h, and the total conversion rate of monomers is determined by iodometric titration and controlled at 90%-95%.
[0013] The weight-average molecular weight of the multi-component copolymer main agent is 80,000-150,000, and the molecular weight distribution index is 2.0-3.5.
[0014] A method for preparing a multi-polymer ultra-high temperature retarder includes the following steps: Step 1: Weigh out the following components by weight: 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water. The second step involves dissolving 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone in deionized water, adjusting the pH to 6.0-7.0 with a 10-20% sodium hydroxide solution, adding mercaptopropionic acid, and stirring for 20-40 minutes under nitrogen protection. Subsequently, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are added, and stirring is continued for 10-15 minutes until completely dissolved to obtain a monomer mixed solution. The third step is to prepare aqueous solutions of the initial ammonium persulfate and sodium bisulfite with a mass concentration of 3%-5% and 2%-4%, respectively. Fourth step: Heat the monomer mixture solution to 55-65℃, and add ammonium persulfate solution and sodium bisulfite solution simultaneously. After completion, heat to 75-85℃ and react at a constant temperature for 2.0-3.0h. Maintain a nitrogen atmosphere during the reaction. When the monomer conversion rate reaches 80%-90%, add N,N-methylenebisacrylamide and supplement with ammonium persulfate. The amount of ammonium persulfate added is 10%-20% of the initial mass of ammonium persulfate. Continue the reaction at 75-85℃ for 30-50min to obtain the post-crosslinked copolymer solution. Fifth step: Add acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80℃ for 20-40 min. Step 6: Add sodium sulfite to the product from step 5, with an amount of 0.2%-0.5% of the total product mass. Stir at 25-35℃ for 15-25 minutes. Adjust the pH to 6.5-7.5 with sodium hydroxide at a mass concentration of 10%-20% to obtain the multi-component copolymer main agent. Step 7: Take 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 28-32 parts of the multi-component copolymer main agent. Add deionized water until the sum of the mass parts of each component is 100 parts. Dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 45-55℃ and stir for 15-25 minutes. Then add D-sorbitol and sodium gluconate and continue stirring for 10-15 minutes. Then add sodium tetraborate. After it is completely dissolved, cool to 25-35℃. Finally, add the multi-component copolymer main agent and stir for 20-30 minutes to mix evenly to obtain the multi-component polymer ultra-high temperature retarder.
[0015] In the fourth step, the reaction heating process adopts a two-stage program. In the first stage, the temperature is increased from room temperature to 55-65℃ at a rate of 1.0-2.0℃ / min, and in the second stage, the temperature is increased from 55-65℃ to 75-85℃ at a rate of 0.5-1.0℃ / min. After mixing in step seven, the resulting product is allowed to stand and mature at 25-35℃ for 10-20 hours. During the maturation process, the product is stirred at 50-100 rpm for 10-15 minutes every 2-4 hours.
[0016] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: 1. This application uses five monomers—2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, N-vinylpyrrolidone, vinylboric acid, and methacryloyloxyethyltrimethylammonium chloride—for free radical copolymerization. N,N-methylenebisacrylamide is introduced in the later stages of polymerization for post-crosslinking, followed by supplementary copolymerization with acrylic monomers. This allows the multi-component copolymer main agent to maintain structural integrity and adsorption stability at temperatures ranging from 220°C to 250°C, solving the problem of rapid performance degradation of existing polymer retarders due to thermal degradation and desorption at ultra-high temperatures.
[0017] 2. In this application, the multi-component copolymer main agent is adsorbed onto the surface of cement particles through molecular chains, and the compounded additives reduce the hydration rate through liquid-phase chelation and deposition. The two form an interface-bulk retarding mode in terms of space and action sequence, making the retarding effect more stable. This avoids the performance mutation caused by a single main agent or a single small molecule additive at high temperature due to a single action pathway, thus solving the problems of high dosage sensitivity and steep thickening curve of existing retarder.
[0018] 3. This application employs a two-stage heating program in the polymerization reaction stage. Gradual heating helps control the free radical release rate and monomer consumption rate, avoiding branching of molecular chains and uneven crosslinking caused by localized overheating. When the monomer conversion reaches 80% to 90%, N,N-methylenebisacrylamide and ammonium persulfate are added. At this point, a certain concentration of monomer and active chain ends remains in the system. The added initiator can form new active sites on the main chain through chain transfer reaction, ensuring that the crosslinked structure is mainly distributed between the main chains rather than forming independent crosslinked networks, thus guaranteeing the uniformity and mildness of crosslinking.
[0019] 4. The pH value of the multi-polymer ultra-high temperature retarder in this application is controlled between 6.5 and 7.5, which is close to neutral. This avoids the performance degradation caused by the reaction of strongly acidic retarders with rust during storage and transportation in iron tanks, and improves storage stability. The multi-polymer main agent is stored and transported in the form of an aqueous solution with a solid content of 40% to 50%, avoiding the problem of moisture absorption and clumping of dry powder products, and facilitating on-site measurement and addition. Detailed Implementation
[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] In the specific embodiments of this application, the sources of various main raw materials are briefly described as follows: 2-Acrylamido-2-methylpropanesulfonic acid: Hubei Jusheng Technology Co., Ltd., CAS No. 15214-89-8, purity ≥99%, appearance is white crystalline powder.
[0022] Itaconic acid: Jinan Century Tongda Chemical Co., Ltd., CAS No. 97-65-4, purity ≥99.5%, appearance is white crystalline powder.
[0023] N-Vinylpyrrolidone: Shandong Zouping Mingyuan Chemical Technology Co., Ltd., CAS No. 88-12-0, purity ≥99%, contains stabilizer N,N-di-sec-butyl-p-phenylenediamine.
[0024] Vinylboric acid: Shanghai Maclean Biochemical Technology Co., Ltd., CAS No. 13331-44-7, purity ≥99.5%, appearance is white to off-white powder, should be stored in the dark at 2℃-8℃.
[0025] Methacryloxyethyltrimethylammonium chloride: Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No. 5039-78-1, specification is 75% aqueous solution, containing the stabilizer methoxyhydroquinone.
[0026] N,N-Methylenebisacrylamide: Shanghai Maclean Biochemical Technology Co., Ltd., CAS No. 110-26-9, purity ≥99%, appearance is white crystalline powder.
[0027] Acrylic acid: Jinan Mingwei Chemical Co., Ltd., CAS No. 79-10-7, purity ≥99.5%, contains stabilizer methoxyhydroquinone, appearance is colorless and transparent liquid.
[0028] Ammonium persulfate: Guangzhou Zhongye Chemical Co., Ltd., CAS No. 7727-54-0, purity ≥98.5%, appearance is white crystalline powder.
[0029] Sodium bisulfite: Weifang Haihua Yufeng Chemical Co., Ltd., CAS No. 7631-90-5, purity ≥99%, appearance is white crystalline powder.
[0030] Mercaptopropionic acid: Wuhan Huajiu Pharmaceutical Technology Co., Ltd., CAS No. 107-96-0, purity ≥99%, appearance is colorless and transparent liquid.
[0031] Sodium hydroxide: Guangzhou Zhongye Chemical Co., Ltd., CAS No. 1310-73-2, purity ≥99%, appearance is flaky solid.
[0032] Sodium ethylenediaminetetramethylenephosphonate: Shandong Taihe Water Treatment Technology Co., Ltd., CAS No. 22036-77-7, a pale yellow transparent aqueous solution with an active ingredient mass concentration of 28%-32%.
[0033] D-Sorbitol: Shandong Lvjian Biotechnology Co., Ltd., CAS No. 50-70-4, purity ≥99%, appearance is white crystalline powder.
[0034] Sodium tetraborate: Jinan Jinhao Chemical Co., Ltd., CAS No. 1303-96-4, sodium tetraborate decahydrate, purity ≥99%, appearance is white crystalline powder.
[0035] Sodium citrate: Weifang Yingxuan Industrial Co., Ltd., CAS No. 6132-04-3, trisodium citrate dihydrate, purity ≥99%, appearance is white crystalline powder.
[0036] Sodium gluconate: Shandong Fuyang Biotechnology Co., Ltd., CAS No. 527-07-1, purity ≥98%, appearance is white to light yellow crystalline powder.
[0037] Sodium sulfite: Guangzhou Zhongye Chemical Co., Ltd., CAS No. 7757-83-7, anhydrous sodium sulfite, purity ≥93%, appearance is white crystalline powder.
[0038] Nitrogen: Jinan Gas Plant Co., Ltd., specification is high-purity nitrogen, purity ≥99.999%, pressure is 15Mpa, packaged in steel cylinder.
[0039] The technical solution of this application is as follows: The multi-component polymer ultra-high temperature retarder, by mass parts, includes 28-32 parts of multi-component copolymer main agent and 68-72 parts of compounded additives; The preparation method of the multi-component copolymer main agent includes the following steps: 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, N-vinylpyrrolidone, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are subjected to free radical copolymerization reaction in water; when the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide is added for post-crosslinking reaction; then acrylic acid monomer is added for supplementary copolymerization reaction to obtain the multi-component copolymer main agent, and the multi-component copolymer main agent is added in the form of an aqueous solution with a solid content of 40%-50%; The compound additives, by mass parts, include 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 78-90 parts of deionized water.
[0040] The mass ratio of sodium ethylenediaminetetramethylenephosphonate, D-sorbitol, sodium tetraborate, sodium citrate and sodium gluconate in the compound additives is 4-6:3-5:1.5-2.5:2.5-3.5:3-4.
[0041] The preparation method of the compound additive includes the following steps: weigh out the sodium ethylenediaminetetramethylenephosphonate and sodium citrate according to the mass fraction, dissolve them in deionized water, heat to 45-55℃ and stir for 15-25 min, then add D-sorbitol and sodium gluconate, continue stirring for 10-15 min, then add sodium tetraborate, and after complete dissolution, cool to 25-35℃ to obtain the compound additive.
[0042] The stirring speed in the compound additive is 200-400 rpm, and the pH value of the compound additive is 6.5-7.5.
[0043] The main component of the multi-component copolymer, by weight, comprises 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water.
[0044] The preparation method of the multi-component copolymer main agent includes the following steps: a. Free radical copolymerization reaction: Weigh out 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid and N-vinylpyrrolidone according to the mass ratio and dissolve them in deionized water. Adjust the pH to 6.0-7.0 with sodium hydroxide with a mass concentration of 10%-20%. Add mercaptopropionic acid as a chain transfer agent and stir for 20-40 min under nitrogen protection. Then add vinylboric acid and methacryloyloxyethyltrimethylammonium chloride and continue stirring for 10-15 min until completely dissolved to obtain a monomer mixed solution. b. Initiator preparation: Prepare aqueous solutions of the initial ammonium persulfate and sodium bisulfite with mass concentrations of 3%-5% and 2%-4%, respectively. c. Polymerization reaction: The monomer mixture solution is heated to 55-65℃, and the initial ammonium persulfate solution and sodium bisulfite solution are added simultaneously. After completion, the temperature is raised to 75-85℃ and the reaction is maintained at a constant temperature for 2.0-3.0h. A nitrogen atmosphere is maintained during the reaction. When the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide and additional ammonium persulfate are added. The amount of additional ammonium persulfate is 10%-20% of the mass of the initial ammonium persulfate. The reaction is continued at 75-85℃ for 30-50min to obtain the post-crosslinked copolymer solution. d. Supplement the copolymerization reaction by adding acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80°C for 20-40 minutes. e. Post-processing step: Add sodium sulfite to the product from step d, the amount of which is 0.2%-0.5% of the total mass of the product, stir at 25-35℃ for 15-25 min, and then adjust the pH to 6.5-7.5 with sodium hydroxide with a mass concentration of 10%-20% to obtain the multi-component copolymer main agent.
[0045] In step c, the solid content of the reaction system is controlled at 35%-45%, the total reaction time is controlled at 2.5-4.5 h, and the total conversion rate of monomers is determined by iodometric titration and controlled at 90%-95%.
[0046] The weight-average molecular weight of the multi-component copolymer main agent is 80,000-150,000, and the molecular weight distribution index is 2.0-3.5.
[0047] A method for preparing a multi-polymer ultra-high temperature retarder includes the following steps: Step 1: Weigh out the following components by weight: 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water. The second step involves dissolving 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone in deionized water, adjusting the pH to 6.0-7.0 with a 10-20% sodium hydroxide solution, adding mercaptopropionic acid, and stirring for 20-40 minutes under nitrogen protection. Subsequently, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are added, and stirring is continued for 10-15 minutes until completely dissolved to obtain a monomer mixed solution. The third step is to prepare aqueous solutions of the initial ammonium persulfate and sodium bisulfite with a mass concentration of 3%-5% and 2%-4%, respectively. Fourth step: Heat the monomer mixture solution to 55-65℃, and add ammonium persulfate solution and sodium bisulfite solution simultaneously. After completion, heat to 75-85℃ and react at a constant temperature for 2.0-3.0h. Maintain a nitrogen atmosphere during the reaction. When the monomer conversion rate reaches 80%-90%, add N,N-methylenebisacrylamide and supplement with ammonium persulfate. The amount of ammonium persulfate added is 10%-20% of the initial mass of ammonium persulfate. Continue the reaction at 75-85℃ for 30-50min to obtain the post-crosslinked copolymer solution. Fifth step: Add acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80℃ for 20-40 min. Step 6: Add sodium sulfite to the product from step 5, with an amount of 0.2%-0.5% of the total product mass. Stir at 25-35℃ for 15-25 minutes. Adjust the pH to 6.5-7.5 with sodium hydroxide at a mass concentration of 10%-20% to obtain the multi-component copolymer main agent. Step 7: Take 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 28-32 parts of the multi-component copolymer main agent. Add deionized water until the sum of the mass parts of each component is 100 parts. Dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 45-55℃ and stir for 15-25 minutes. Then add D-sorbitol and sodium gluconate and continue stirring for 10-15 minutes. Then add sodium tetraborate. After it is completely dissolved, cool to 25-35℃. Finally, add the multi-component copolymer main agent and stir for 20-30 minutes to mix evenly to obtain the multi-component polymer ultra-high temperature retarder.
[0048] In the fourth step, the reaction heating process adopts a two-stage program. In the first stage, the temperature is increased from room temperature to 55-65℃ at a rate of 1.0-2.0℃ / min, and in the second stage, the temperature is increased from 55-65℃ to 75-85℃ at a rate of 0.5-1.0℃ / min. After mixing in step seven, the resulting product is allowed to stand and mature at 25-35℃ for 10-20 hours. During the maturation process, the product is stirred at 50-100 rpm for 10-15 minutes every 2-4 hours.
[0049] This application employs five monomers—2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, N-vinylpyrrolidone, vinylboric acid, and methacryloyloxyethyltrimethylammonium chloride—for free radical copolymerization. N,N-methylenebisacrylamide is introduced in the later stages of polymerization for post-crosslinking, followed by supplementary copolymerization with acrylic monomers. This allows the multi-component copolymer main agent to maintain structural integrity and adsorption stability at temperatures ranging from 220°C to 250°C, solving the problem of rapid performance degradation in existing polymer retarders due to thermal degradation and desorption at ultra-high temperatures.
[0050] In this application, the multi-component copolymer main agent is adsorbed onto the surface of cement particles through molecular chains, and the compounded additives reduce the hydration rate through liquid-phase chelation and deposition. The two form an interface-bulk retarding mode in terms of space and action sequence, making the retarding effect more stable. This avoids the performance mutation that occurs at high temperatures due to the single action pathway of a single main agent or a single small molecule additive, thus solving the problems of high dosage sensitivity and steep thickening curve of existing retarder.
[0051] This application employs a two-stage heating program in the polymerization reaction stage. Gradual heating helps control the free radical release rate and monomer consumption rate, avoiding branching of molecular chains and uneven cross-linking caused by localized overheating. When the monomer conversion reaches 80% to 90%, N,N-methylenebisacrylamide and ammonium persulfate are added. At this point, a certain concentration of monomer and active chain ends remains in the system. The added initiator can form new active sites on the main chain through chain transfer reactions, ensuring that the cross-linked structure is mainly distributed between the main chains rather than forming independent cross-linked networks, thus guaranteeing the uniformity and mildness of cross-linking.
[0052] The pH value of the multi-polymer ultra-high temperature retarder in this application is controlled between 6.5 and 7.5, which is close to neutral. This avoids the performance degradation caused by the reaction of strongly acidic retarders with rust during storage and transportation in iron cans, and improves storage stability. The multi-polymer main agent is stored and transported in the form of an aqueous solution with a solid content of 40% to 50%, avoiding the problem of moisture absorption and clumping of dry powder products, while also facilitating on-site measurement and addition.
[0053] The present invention will be described in detail below through examples and comparative examples, but the scope of protection of the present invention is not limited to these examples. Unless otherwise specified, the chemical reagents and raw materials used in the following examples and comparative examples are all conventional commercially available products.
[0054] Example 1
[0055] A multi-polymer ultra-high temperature retarder, comprising, by mass parts, 32 parts of multi-polymer main agent and 68 parts of compounded additives.
[0056] The compound additives, by mass parts, consist of 4 parts sodium ethylenediaminetetramethylenephosphonate, 5 parts D-sorbitol, 1.5 parts sodium tetraborate, 3.5 parts sodium citrate, 3 parts sodium gluconate, and 90 parts deionized water.
[0057] The preparation method of the multi-component copolymer main agent is as follows: weigh 20 parts of 2-acrylamido-2-methylpropanesulfonic acid, 8 parts of itaconic acid, 4.8 parts of N-vinylpyrrolidone, 3.0 parts of vinylboric acid, 3.5 parts of methacryloyloxyethyltrimethylammonium chloride, 0.6 parts of N,N-methylenebisacrylamide, 0.4 parts of acrylic acid, 0.7 parts of ammonium persulfate, 0.25 parts of sodium bisulfite, 0.5 parts of mercaptopropionic acid, and 55 parts of deionized water.
[0058] 2-Acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone were dissolved in deionized water, and the pH was adjusted to 6.0 with 20% sodium hydroxide. Mercaptopropionic acid was added, and the mixture was stirred for 40 min under nitrogen protection. Then, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride were added, and the mixture was stirred for another 15 min until completely dissolved to obtain a monomer mixed solution.
[0059] Ammonium persulfate was prepared into a 3% aqueous solution, and sodium bisulfite was prepared into a 4% aqueous solution.
[0060] The monomer mixture solution was heated to 55°C, and the two initiator solutions mentioned above were added dropwise simultaneously. After the addition was complete, the temperature was raised to 85°C and the reaction was maintained at this temperature for 2.0 h, with a nitrogen atmosphere maintained throughout the reaction. When the monomer conversion rate reached 90%, N,N-methylenebisacrylamide and ammonium persulfate were added, with the amount added being 10% of the initial mass of ammonium persulfate. The reaction was continued at 85°C for 30 min to obtain the post-crosslinking copolymer solution.
[0061] Acrylic acid and ammonium persulfate were added to the crosslinked copolymer solution at a ratio of 15% of the initial mass of ammonium persulfate, and the reaction was carried out at 70°C for 40 min.
[0062] Sodium sulfite was added to the obtained product at a concentration of 0.2% of the total product mass. The mixture was stirred at 35°C for 15 minutes, and then the pH was adjusted to 7.5 with 10% sodium hydroxide solution to obtain the multi-component copolymer main agent. The main agent has a weight-average molecular weight of 150,000 and a molecular weight distribution index of 2.0.
[0063] The preparation method of the compound additive is as follows: Weigh each component according to the above mass proportions, dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 45℃ and stir for 25 min at a stirring speed of 200 rpm, add D-sorbitol and sodium gluconate, continue stirring for 15 min, then add sodium tetraborate, and after complete dissolution, cool to 25℃ to obtain the compound additive with a pH value of 7.5.
[0064] The above-mentioned multi-component copolymer main agent and compounded auxiliary agent were mixed in 32 parts and 68 parts respectively, and stirred at 25°C for 30 min to obtain a multi-component polymer ultra-high temperature retarder. The mixture was allowed to stand for 20 h, and stirred at 100 rpm for 10 min every 2 h during the maturation process.
[0065] Example 2
[0066] In this embodiment, the similarities to those in Embodiment 1 will not be repeated, and the differences are as follows: A multi-component polymer ultra-high temperature retarder, comprising, by mass parts, 28 parts of a multi-component copolymer main agent and 72 parts of compounded additives.
[0067] The compound additives, by mass parts, consist of 6 parts sodium ethylenediaminetetramethylenephosphonate, 3 parts D-sorbitol, 2.5 parts sodium tetraborate, 2.5 parts sodium citrate, 4 parts sodium gluconate, and 78 parts deionized water.
[0068] The preparation method of the multi-component copolymer main agent is as follows: weigh 22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7 parts of itaconic acid, 5.5 parts of N-vinylpyrrolidone, 2.5 parts of vinylboric acid, 4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3 parts of N,N-methylenebisacrylamide, 0.8 parts of acrylic acid, 0.5 parts of ammonium persulfate, 0.4 parts of sodium bisulfite, 0.35 parts of mercaptopropionic acid, and 62 parts of deionized water.
[0069] 2-Acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone were dissolved in deionized water, and the pH was adjusted to 7.0 with 10% sodium hydroxide. Mercaptopropionic acid was added, and the mixture was stirred for 20 min under nitrogen protection. Then, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride were added, and the mixture was stirred for another 10 min until completely dissolved to obtain a monomer mixed solution.
[0070] Ammonium persulfate was prepared into a 5% aqueous solution, and sodium bisulfite was prepared into a 2% aqueous solution.
[0071] The monomer mixture solution was heated to 65°C, and the two initiator solutions mentioned above were added dropwise simultaneously. After the addition was complete, the temperature was raised to 75°C, and the reaction was maintained at this temperature for 3.0 h under a nitrogen atmosphere. When the monomer conversion rate reached 80%, N,N-methylenebisacrylamide and ammonium persulfate were added, with the amount added being 20% of the initial mass of ammonium persulfate. The reaction was continued at 75°C for 50 min to obtain the post-crosslinking copolymer solution.
[0072] Acrylic acid and ammonium persulfate were added to the crosslinked copolymer solution at an amount equal to 8% of the initial mass of ammonium persulfate, and the reaction was carried out at 80°C for 20 min.
[0073] Sodium sulfite was added to the obtained product at a concentration of 0.5% of the total product mass. The mixture was stirred at 25°C for 25 minutes, and then the pH was adjusted to 6.5 with 20% sodium hydroxide solution to obtain the multi-component copolymer main agent. The main agent has a weight-average molecular weight of 80,000 and a molecular weight distribution index of 3.5.
[0074] The preparation method of the compound additive is as follows: Weigh each component according to the above mass proportions, dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 55℃ and stir for 15 min at a stirring speed of 400 rpm, add D-sorbitol and sodium gluconate, continue stirring for 10 min, then add sodium tetraborate, and after complete dissolution, cool to 35℃ to obtain the compound additive with a pH value of 6.5.
[0075] The above-mentioned multi-component copolymer main agent and compounded auxiliary agent were mixed in 28 parts and 72 parts respectively, and stirred at 35°C for 20 min to obtain a multi-component polymer ultra-high temperature retarder. The mixture was allowed to stand for 10 h, and stirred at 50 rpm for 15 min every 4 h during the maturation process.
[0076] Example 3
[0077] In this embodiment, the similarities to those in Embodiment 1 will not be repeated, and the differences are as follows: A multi-polymer ultra-high temperature retarder, comprising, by weight, 30 parts of a multi-polymer main agent and 70 parts of compounded additives.
[0078] The compound additives, by mass parts, consist of 5 parts sodium ethylenediaminetetramethylenephosphonate, 4 parts D-sorbitol, 2.0 parts sodium tetraborate, 3.0 parts sodium citrate, 3.5 parts sodium gluconate, and 84 parts deionized water.
[0079] The preparation method of the multi-component copolymer main agent is as follows: Weigh 21 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7.5 parts of itaconic acid, 5.15 parts of N-vinylpyrrolidone, 2.75 parts of vinylboric acid, 3.75 parts of methacryloyloxyethyltrimethylammonium chloride, 0.45 parts of N,N-methylenebisacrylamide, 0.6 parts of acrylic acid, 0.6 parts of ammonium persulfate, 0.325 parts of sodium bisulfite, 0.425 parts of mercaptopropionic acid, and 58.5 parts of deionized water.
[0080] 2-Acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone were dissolved in deionized water, and the pH was adjusted to 6.5 with 15% sodium hydroxide. Mercaptopropionic acid was added, and the mixture was stirred for 30 min under nitrogen protection. Then, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride were added, and the mixture was stirred for another 12 min until completely dissolved to obtain a monomer mixed solution.
[0081] Ammonium persulfate was prepared into a 4% aqueous solution, and sodium bisulfite was prepared into a 3% aqueous solution.
[0082] The monomer mixture solution was heated to 60°C, and the two initiator solutions mentioned above were added dropwise simultaneously. After the addition was complete, the temperature was raised to 80°C and the reaction was maintained at this temperature for 2.5 hours under a nitrogen atmosphere. When the monomer conversion rate reached 85%, N,N-methylenebisacrylamide and ammonium persulfate were added, with the amount added being 15% of the initial mass of ammonium persulfate. The reaction was continued at 80°C for 40 minutes to obtain the post-crosslinked copolymer solution.
[0083] Acrylic acid and ammonium persulfate were added to the crosslinked copolymer solution at a ratio of 11.5% of the initial mass of ammonium persulfate, and the reaction was carried out at 75°C for 30 min.
[0084] Sodium sulfite was added to the obtained product at a concentration of 0.35% of the total product mass. The mixture was stirred at 30°C for 20 minutes, and then the pH was adjusted to 7.0 with 15% sodium hydroxide solution to obtain the multi-component copolymer main agent. The main agent had a weight-average molecular weight of 115,000 and a molecular weight distribution index of 2.75.
[0085] The preparation method of the compound additive is as follows: Weigh each component according to the above mass proportions, dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 50℃ and stir for 20 min at a stirring speed of 300 rpm, add D-sorbitol and sodium gluconate, continue stirring for 12 min, then add sodium tetraborate, and after complete dissolution, cool to 30℃ to obtain the compound additive with a pH value of 7.0.
[0086] The above-mentioned multi-component copolymer main agent and compounded auxiliary agent were mixed in 30 parts and 70 parts respectively, and stirred at 30°C for 25 minutes to obtain a multi-component polymer ultra-high temperature retarder. The mixture was allowed to stand for 15 hours to mature, and stirred at 75 rpm for 12 minutes every 3 hours during the maturation process.
[0087] Comparative Example 1 In this comparative example, the similarities with Example 1 will not be repeated. The differences are as follows: N,N-methylenebisacrylamide is not added for post-crosslinking reaction during the preparation of the multi-component copolymer main agent. That is, the steps of adding crosslinking agent and supplementing initiator in the later stage of polymerization are deleted. The other conditions are exactly the same as those in Example 1.
[0088] Comparative Example 2 In this comparative example, the similarities with Example 2 will not be repeated. The differences are as follows: no supplementary copolymerization reaction is performed, that is, the steps of adding acrylic acid and adding ammonium persulfate are omitted, and the other conditions are exactly the same as in Example 2.
[0089] Comparative Example 3 In this comparative example, the similarities with Example 3 will not be repeated. The differences are as follows: sodium ethylenediaminetetramethylenephosphonate and sodium tetraborate are not added to the compound additives, but are replaced with an equal amount of deionized water. The other conditions are exactly the same as in Example 3.
[0090] Comparative Example 4 In this comparative example, the similarities with Example 1 will not be repeated. The differences are as follows: D-sorbitol and sodium gluconate in the compounding adjuvants are omitted and replaced with an equal amount of deionized water. The other conditions are exactly the same as in Example 1.
[0091] Comparative Example 5 In this comparative example, the similarities with Example 1 will not be repeated. The differences are as follows: the polymerization reaction stage adopts conventional one-stage isothermal polymerization, that is, the monomer mixed solution is directly heated to 80°C and all the initiator is added at one time. The isothermal reaction is carried out for 4.5 hours without two-stage heating. After the conversion rate reaches 80%, the operation is the same as in Example 1. The remaining conditions are exactly the same as in Example 1.
[0092] Performance Test Results and Analysis The performance of the multi-component polymer ultra-high temperature retarder obtained according to the parameters of the examples and comparative examples was evaluated according to the test methods.
[0093] The test method is as follows: Thickening time: According to standard GB / T 19139-2012, the thickening time of Grade G oil well cement slurry was determined using a high-temperature and high-pressure thickener at 220℃ and 250℃. The water-cement ratio was 0.40, and the amount of retarder added was based on the cement mass; unless otherwise specified, the amount added was 3.0% of the cement mass. The time corresponding to when the consistency reached 100 Bc was recorded as the thickening time.
[0094] Cement stone compressive strength: According to standard GB / T 19139-2012, the cement slurry after the thickening test is poured into a mold and cured at 220℃ and 250℃ for 24 hours. After demolding, the compressive strength is measured.
[0095] Molecular weight and molecular weight distribution: The molecular weight was determined by gel permeation chromatography using sodium polystyrene sulfonate as a standard in a mobile phase of 0.1 mol / L sodium nitrate aqueous solution.
[0096] Solid content: Calculated by weighing a quantitative sample and drying it to constant weight in an oven at 105℃.
[0097] The retarders prepared in Examples 1-3 and Comparative Examples 1-5 were used to prepare cement slurry according to the test method. The thickening time and 24-hour compressive strength were tested at 220℃ and 250℃, respectively. The amount of retarder added was 3.0% of the cement mass. A blank group without retarder was also set up. The test results are shown in Table 1.
[0098] Table 1 Analysis of Test Results
[0099] Test results show that under ultra-high temperature conditions of 220℃ and 250℃, the thickening time of blank cement slurry without retarder is only 45 min and 28 min, respectively, which cannot meet the safe pumping requirements of cementing construction. The thickening time of Examples 1-3 is significantly extended, reaching 362-385 min at 220℃ and 298-312 min at 250℃, while the 24-hour compressive strength remains at 27.9-29.1 MPa, which can meet the requirements of high-temperature cementing for cement stone strength development. Vinyl boric acid and cationic monomers are introduced into the multi-component copolymer main agent, combined with post-crosslinking and supplementary copolymerization modification, so that the polymer still has a rigid main chain structure and dense adsorption groups at ultra-high temperature. The organophosphonates, polyols and borates in the compound additives form a multi-level retardation synergy. Through chelation of calcium ions, hydrogen bond adsorption and boron-oxygen coordination, the hydration activity of cement particle surface is effectively reduced, realizing interface-bulk retardation, which significantly extends the thickening time and makes the curve stable.
[0100] Comparative Example 1 omitted the post-crosslinking reaction, and the main agent was only a linear copolymer. The thickening time at 250°C was reduced to 186 min, which was about 40% less than that in Example 1. This indicates that polymers without crosslinking structures are more prone to thermal degradation and conformational changes at ultra-high temperatures, leading to the destruction of the adsorption layer and a rapid decline in retarding ability. The mild network structure introduced by post-crosslinking plays an important role in maintaining structural integrity at ultra-high temperatures.
[0101] Comparative Example 2 omitted the supplementary copolymerization reaction, lacking the subsequent grafted acrylic acid segments, resulting in a lower side chain carboxyl group density and a thickening time of 209 min at 250°C, which was approximately 30% lower than that of Example 2. The additional carboxyl groups introduced by the supplementary copolymerization can enhance the multi-point adsorption of the polymer on the surface of cement particles, increase the adsorption layer density, and thus maintain an effective retarding barrier at extreme high temperatures.
[0102] In Comparative Example 3, the compound additives removed sodium ethylenediaminetetramethylenephosphonate and sodium tetraborate, relying solely on the main agent and the remaining polyol and hydroxycarboxylate. The thickening time at 250℃ dropped sharply to 162 min, even lower than Comparative Examples 1 and 2. This indicates that a single polymer main agent cannot independently achieve long-term retarding at ultra-high temperatures. The chelating effect of organophosphonates on calcium ions and the coordination and crosslinking function of borates play a crucial role in constructing a high-temperature stable retarding system.
[0103] Comparative Example 4, which removed D-sorbitol and sodium gluconate, showed a significant decrease in thickening time, which was 231 min at 250 °C. This indicates that the hydroxyl adsorption sites provided by the polyol and the regulation of the liquid phase ionic environment by gluconate would weaken the integrity of the retarder layer on the surface of cement particles.
[0104] Comparative Example 5 employed a one-stage isothermal polymerization process, resulting in a product with a thickening time of 255 min at 250°C, shorter than that of Example 1. The two-stage heating program allowed for the phased decomposition of the initiator, resulting in a better match between the free radical generation rate and the monomer consumption rate. This avoided uneven local crosslinking and an excessively wide molecular weight distribution caused by initial rapid polymerization, thus ensuring the uniformity of the post-crosslinked structure and the batch stability of the polymer. Although the one-stage polymerization product also underwent post-crosslinking, its thickening time was still significantly shorter than that of the two-stage process, indicating that the polymerization process's control over the product's microstructure can affect its high-temperature retarding properties.
[0105] This invention achieves effective control of cement paste thickening time at ultra-high temperatures of 220-250℃ through specific monomer combinations, post-crosslinking and supplementary copolymerization modification, and multi-level synergistic effects of compounded additives, while maintaining the mechanical properties of cement stone. It solves the problems of performance degradation and dosage sensitivity of existing retarders at ultra-high temperatures.
[0106] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A multi-polymer ultra-high temperature retarder, characterized in that: By mass parts, it includes 28-32 parts of multi-component copolymer main agent and 68-72 parts of compounding additives; The preparation method of the multi-component copolymer main agent includes the following steps: 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, N-vinylpyrrolidone, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are subjected to free radical copolymerization reaction in water; when the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide is added for post-crosslinking reaction; then acrylic acid monomer is added for supplementary copolymerization reaction to obtain the multi-component copolymer main agent, and the multi-component copolymer main agent is added in the form of an aqueous solution with a solid content of 40%-50%; The preparation method of the compound adjuvant includes the following steps: weigh out the sodium ethylenediaminetetramethylenephosphonate and sodium citrate according to the mass fraction, dissolve them in deionized water, heat to 45-55℃ and stir for 15-25 min, then add D-sorbitol and sodium gluconate, continue stirring for 10-15 min, then add sodium tetraborate, and after complete dissolution, cool to 25-35℃ to obtain the compound adjuvant; The raw materials in the preparation method of the compound adjuvant, by mass parts, include 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 78-90 parts of deionized water.
2. The multi-polymer ultra-high temperature retarder according to claim 1, characterized in that: The stirring speed in the compound additive is 200-400 rpm, and the pH value of the compound additive is 6.5-7.
5.
3. The multi-polymer ultra-high temperature retarder according to claim 2, characterized in that, The preparation method of the multi-component copolymer main agent includes the following steps: a. Free radical copolymerization reaction: Weigh out 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid and N-vinylpyrrolidone according to the mass ratio and dissolve them in deionized water. Adjust the pH to 6.0-7.0 with sodium hydroxide with a mass concentration of 10%-20%. Add mercaptopropionic acid as a chain transfer agent and stir for 20-40 min under nitrogen protection. Then add vinylboric acid and methacryloyloxyethyltrimethylammonium chloride and continue stirring for 10-15 min until completely dissolved to obtain a monomer mixed solution. b. Initiator preparation: Prepare aqueous solutions of initial ammonium persulfate and sodium bisulfite with mass concentrations of 3%-5% and 2%-4%, respectively. c. Polymerization reaction: The monomer mixture solution is heated to 55-65℃, and the initial ammonium persulfate solution and sodium bisulfite solution are added simultaneously. After completion, the temperature is raised to 75-85℃ and the reaction is maintained at a constant temperature for 2.0-3.0h. A nitrogen atmosphere is maintained during the reaction. When the monomer conversion rate reaches 80%-90%, N,N-methylenebisacrylamide and additional ammonium persulfate are added. The amount of additional ammonium persulfate is 10%-20% of the mass of the initial ammonium persulfate. The reaction is continued at 75-85℃ for 30-50min to obtain the post-crosslinked copolymer solution. d. Supplement the copolymerization reaction by adding acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80°C for 20-40 minutes. e. Post-processing step: Add sodium sulfite to the product from step d, the amount of which is 0.2%-0.5% of the total mass of the product, stir at 25-35℃ for 15-25 min, and then adjust the pH to 6.5-7.5 with sodium hydroxide with a mass concentration of 10%-20% to obtain the multi-component copolymer main agent.
4. The multi-polymer ultra-high temperature retarder according to claim 3, characterized in that: The raw materials in the preparation method of the multi-component copolymer main agent, by mass parts, include 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water.
5. The multi-polymer ultra-high temperature retarder according to claim 4, characterized in that: In step c, the solid content of the reaction system is controlled at 35%-45%, the total reaction time is controlled at 2.5-4.5 h, and the total conversion rate of monomers is determined by iodometric titration and controlled at 90%-95%.
6. The multi-polymer ultra-high temperature retarder according to claim 5, characterized in that: The weight-average molecular weight of the multi-component copolymer main agent is 80,000-150,000, and the molecular weight distribution index is 2.0-3.
5.
7. The preparation method of the multi-polymer ultra-high temperature retarder according to claim 6, characterized in that, Includes the following steps: Step 1: Weigh out the following components by weight: 20-22 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7-8 parts of itaconic acid, 4.8-5.5 parts of N-vinylpyrrolidone, 2.5-3.0 parts of vinylboric acid, 3.5-4.0 parts of methacryloyloxyethyltrimethylammonium chloride, 0.3-0.6 parts of N,N-methylenebisacrylamide, 0.4-0.8 parts of acrylic acid, 0.5-0.7 parts of ammonium persulfate, 0.25-0.4 parts of sodium bisulfite, 0.35-0.5 parts of mercaptopropionic acid, and 55-62 parts of deionized water. The second step involves dissolving 2-acrylamido-2-methylpropanesulfonic acid, itaconic acid, and N-vinylpyrrolidone in deionized water, adjusting the pH to 6.0-7.0 with a 10-20% sodium hydroxide solution, adding mercaptopropionic acid, and stirring for 20-40 minutes under nitrogen protection. Subsequently, vinylboric acid and methacryloyloxyethyltrimethylammonium chloride are added, and stirring is continued for 10-15 minutes until completely dissolved to obtain a monomer mixed solution. The third step is to prepare aqueous solutions of the initial ammonium persulfate and sodium bisulfite with a mass concentration of 3%-5% and 2%-4%, respectively. Fourth step: Heat the monomer mixture solution to 55-65℃, and simultaneously add the initial ammonium persulfate solution and sodium bisulfite solution. After completion, heat to 75-85℃ and react at a constant temperature for 2.0-3.0 hours. Maintain a nitrogen atmosphere during the reaction. When the monomer conversion rate reaches 80%-90%, add N,N-methylenebisacrylamide and supplement with ammonium persulfate. The amount of supplemented ammonium persulfate is 10%-20% of the initial ammonium persulfate mass. Continue the reaction at 75-85℃ for 30-50 minutes to obtain the post-crosslinked copolymer solution. Fifth step: Add acrylic acid and ammonium persulfate to the post-crosslinked copolymer solution. The amount of ammonium persulfate added is 8%-15% of the initial mass of ammonium persulfate. React at 70-80°C for 20-40 minutes. Step 6: Add sodium sulfite to the product from step 5, with an amount of 0.2%-0.5% of the total product mass. Stir at 25-35℃ for 15-25 minutes. Adjust the pH to 6.5-7.5 with sodium hydroxide at a mass concentration of 10%-20% to obtain the multi-component copolymer main agent. Step 7: Take 4-6 parts of sodium ethylenediaminetetramethylenephosphonate, 3-5 parts of D-sorbitol, 1.5-2.5 parts of sodium tetraborate, 2.5-3.5 parts of sodium citrate, 3-4 parts of sodium gluconate, and 28-32 parts of the multi-component copolymer main agent. Add deionized water until the sum of the mass parts of each component is 100 parts. Dissolve sodium ethylenediaminetetramethylenephosphonate and sodium citrate in deionized water, heat to 45-55℃ and stir for 15-25 minutes. Then add D-sorbitol and sodium gluconate and continue stirring for 10-15 minutes. Then add sodium tetraborate. After it is completely dissolved, cool to 25-35℃. Finally, add the multi-component copolymer main agent and stir for 20-30 minutes to mix evenly to obtain the multi-component polymer ultra-high temperature retarder.
8. The preparation method of the multi-polymer ultra-high temperature retarder according to claim 7, characterized in that: In the fourth step, the reaction heating process adopts a two-stage program. In the first stage, the temperature is increased from room temperature to 55-65℃ at a rate of 1.0-2.0℃ / min, and in the second stage, the temperature is increased from 55-65℃ to 75-85℃ at a rate of 0.5-1.0℃ / min. After mixing in step seven, the resulting product is allowed to stand and mature at 25-35℃ for 10-20 hours. During the maturation process, the product is stirred at 50-100 rpm for 10-15 minutes every 2-4 hours.
Citation Information
Patent Citations
Oil well cement inhibiting agent
CN101368091A
Superhigh temperature retarder and preparation process thereof
CN107828393A