A method for preparing a bioelectrode
By coating ABS or PC materials with silver/silver chloride and conductive polymer paste, the issues of lightweighting and stability of bioelectrodes are solved, resulting in high-performance bioelectrodes suitable for portable electrocardiogram (ECG) detection.
Patent Information
- Application Number
- CN202510584963.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing bioelectrode materials have shortcomings in terms of lightweighting, wear resistance, and stability. In particular, the stability of ABS or PC materials coated with silver chloride layers is poor, they are prone to powdering, and there is a problem of increased toxicity due to chemical reactions during long-term use.
Using ABS or PC material as a base, silver/silver chloride paste is first applied, followed by conductive polymer paste, forming a multi-layer structure. By adjusting the proportion of each component, adhesion, conductivity, and stability are improved.
A highly sensitive, low-impedance, and stable bioelectrode was fabricated, suitable for portable electrocardiogram (ECG) detection, enabling accurate ECG detection in mobile scenarios.
Smart Images

Figure CN123058740A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of materials science and biomedicine, and specifically relates to a method for preparing a bioelectrode. Background Technology
[0002] Bioelectrodes are specialized electrodes used to detect, record, or stimulate electrical signals within or on the surface of living organisms. They can convert electrical signals generated by biological tissues (such as electroencephalograms, electrocardiograms, and electromyograms) into electrical signals, or influence the function of biological tissues by applying electrical signals. Bioelectrodes are widely used in medical diagnostics, physiological research, and biomedical engineering.
[0003] To meet the specific requirements of biocompatibility, high sensitivity, low impedance, stability, and safety for bioelectrodes, metals (such as silver and gold), conductive polymers, and carbon-based materials are typically used to fabricate them. For example, commonly used bioelectrodes for electrocardiogram (ECG) or electroencephalogram (EEG) detection are made of copper and plated with silver chloride.
[0004] Electrodes made of metal are typically heavy, failing to meet the lightweight requirements of wearable electrodes. Electrodes made of ABS or PC materials offer the advantage of light weight; however, the silver chloride coating on their surface exhibits poor stability, is prone to powdering, and is not wear-resistant. To improve the conductivity, stability, and wear resistance of the coating on ABS or PC materials, some researchers have used a method of first plating a layer of copper on the ABS or PC material and then plating silver chloride. However, the problem is that the two metal films are prone to chemical reactions during long-term use, leading to increased toxicity. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a method for preparing a bioelectrode. The method is characterized by: using ABS or PC material to fabricate the electrode, first coating its surface with a layer of silver / silver chloride paste, and then coating it with a layer of conductive polymer paste. This allows the electrode to possess complementary electronic and ionic conductivity, resulting in higher sensitivity and lower impedance characteristics, while also meeting the requirements for stability, wear resistance, biocompatibility, and safety.
[0006] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a method for preparing a bioelectrode.
[0007] According to one aspect of the present invention, in order to achieve the above-mentioned objective, the technical solution of the present invention is: a method for preparing a bioelectrode, characterized in that, on an ABS or PC injection-molded electrode, a layer of silver / silver chloride paste is first coated, cured by heating, and then a layer of conductive polymer paste is coated and cured by heating, comprising the following steps: Step 1: Inject the bioelectrode into the designed shape using ABS or PC. Step 2: Perform surface cleaning and roughening treatment on the injection-molded electrode; Step 3: Apply a layer of silver / silver chloride paste to the electrode surface after surface cleaning and roughening, and heat it to cure it, so as to form a 10μm to 20μm thin film coating layer. Step 4: Apply a layer of conductive polymer paste to the electrode coated with silver / silver chloride paste, and then heat and cure it to form a 1μm to 3μm thin film coating layer.
[0008] Preferably, the silver / silver chloride paste described in step 3 comprises silver powder, silver chloride powder, binder, and solvent: the silver powder accounts for 4-20% of the mass of the silver / silver chloride paste; the silver chloride powder accounts for 18-50% of the mass of the silver / silver chloride paste; the binder accounts for 2-4% of the mass of the silver / silver chloride paste; and the solvent is selected from propylene glycol, ethylene glycol monomethyl ether, ethyl acetate, divalent ester, etc., and accounts for 35-45% of the mass of the silver / silver chloride paste.
[0009] Furthermore, the silver powder includes flake silver powder and spherical silver powder, wherein the average particle size of the flake silver powder is 3 to 6 μm, and the average particle size of the spherical silver powder is 0.05 to 0.1 μm.
[0010] Furthermore, the average particle size of the silver chloride powder is 5–15 μm.
[0011] Preferably, the silver / silver chloride paste further includes additives, the additives accounting for 0.1-3% of the mass of the silver / silver chloride paste, and the additives include any one or a combination of at least two of the following: defoamer, coupling agent, wetting agent, quick-drying agent or leveling agent.
[0012] Furthermore, the coating method described in step 3 includes, but is not limited to, spraying, dipping, and smearing.
[0013] Furthermore, by adjusting the mass ratio of various raw materials in the silver / silver chloride paste, the present invention enables the paste to have the advantages of strong adhesion, low impedance, good electrode potential stability and high signal-to-noise ratio when applied to the electrode.
[0014] Preferably, the conductive polymer slurry in step 4 comprises a conductive polymer, a solvent, and additives: the conductive polymer accounts for 10-30% of the total mass of the conductive polymer slurry; the solvent accounts for 70-80% of the total mass of the conductive polymer slurry; and the additives account for 1%-5% of the total mass of the conductive polymer slurry.
[0015] Furthermore, by adjusting the mass ratio of the conductive polymer in the conductive polymer slurry, the conductivity, flexibility, and adhesion of the conductive film on the prepared electrode can be adjusted.
[0016] Furthermore, the solvent is selected based on the solubility of the conductive polymer, such as alcohols, ethers, esters, etc.
[0017] Furthermore, the additives are dispersants, plasticizers, stabilizers, etc. For example, dispersants are used to increase the dispersibility of the slurry and prevent agglomeration; plasticizers are used to improve the flexibility and processing performance of the slurry; and stabilizers are used to increase the stability of the slurry.
[0018] According to another aspect of the present invention, step 1, which involves injection molding the bioelectrode into a designed shape using ABS or PC, means that the bioelectrode can be manufactured into various shapes to suit different applications. In an embodiment of the present invention, a dry electrode for directly contacting the skin surface to detect electrocardiogram (ECG) signals is prepared. The shape includes a flat surface that contacts the human skin and a protruding post for connecting an ECG electrode clip. The contact surface is circular and has a certain number of tiny protrusions to increase the fit between the surface and the human skin.
[0019] Furthermore, the tiny protrusions are frustums formed on the circular contact surface.
[0020] Furthermore, in order to maintain the continuity of the coating film throughout the entire electrode coating process, i.e. to maintain the continuity of conductivity, each transition surface of the electrode is rounded.
[0021] The beneficial effects of this invention are: The direct benefits of this invention are: An electrode preparation method is provided, which is low in cost and simple in manufacturing process.
[0022] The electrode preparation method is characterized by first coating a silver / silver chloride paste onto an ABS or PC material electrode of arbitrary shape, and then coating a conductive polymer paste onto it, thereby preparing a high-performance ECG detection dry electrode with advantages such as high sensitivity, low impedance and good stability.
[0023] Dry electrodes bring great convenience to portable electrocardiogram (ECG) detectors, enabling accurate detection of daily ECGs in mobile scenarios and home environments. Attached Figure Description
[0024] Figure 1 This is a flowchart of a preferred embodiment of the preparation method of a bioelectrode of the present invention; Figure 2 This is a flowchart of a preferred embodiment of the present invention for preparing a bioelectrode; Figure 3 This is a schematic diagram of the shape of a bioelectrode according to a preferred embodiment of the present invention; Figure 4This is a flowchart of the silver / silver chloride paste preparation method of preferred embodiment 1 of the present invention; Figure 5 This is a flowchart of the conductive polymer slurry preparation method of preferred embodiment 1 of the present invention. Detailed Implementation
[0025] The present invention will now be described in further detail with reference to the accompanying drawings and preferred embodiments. These drawings are simplified schematic diagrams, illustrating only the basic principles, basic structure and basic functions of the invention, and therefore only show the components relevant to the invention.
[0026] Those skilled in the art may recognize some variations and equivalent substitutions of the present invention, but these variations and equivalent substitutions should not be construed as exceeding the scope of protection of the present invention.
[0027] Figure 1 This is a flowchart illustrating a preferred embodiment of the preparation method of a bioelectrode according to the present invention. Figure 1 As shown, a method for preparing a bioelectrode is characterized by comprising the following steps: S1. Inject the bioelectrode into the designed shape using ABS or PC. S2. The injection-molded electrode is subjected to surface cleaning and roughening treatment; S3. Apply a layer of silver / silver chloride paste to the electrode surface after surface cleaning and roughening, and heat it to cure it to form a 10μm to 20μm thin film coating layer. S4. Coat the electrode with a layer of conductive polymer paste after coating it with silver / silver chloride paste, and then heat and cure it to form a 1μm to 3μm thin film coating layer.
[0028] Preferably, the silver / silver chloride paste described in S3 comprises silver powder, silver chloride powder, binder, and solvent: the silver powder accounts for 4-20% of the mass of the silver / silver chloride paste; the silver chloride powder accounts for 18-50% of the mass of the silver / silver chloride paste; the binder accounts for 2-4% of the mass of the silver / silver chloride paste; and the solvent is selected from propylene glycol, ethylene glycol monomethyl ether, ethyl acetate, divalent ester, etc., and accounts for 35-45% of the mass of the silver / silver chloride paste.
[0029] Furthermore, the silver powder includes flake silver powder and spherical silver powder, wherein the average particle size of the flake silver powder is 3 to 6 μm, and the average particle size of the spherical silver powder is 0.05 to 0.1 μm.
[0030] Furthermore, the average particle size of the silver chloride powder is 5–15 μm.
[0031] Preferably, the silver / silver chloride paste further includes additives, the additives accounting for 0.1-3% of the mass of the silver / silver chloride paste, and the additives include any one or a combination of at least two of the following: defoamer, coupling agent, wetting agent, quick-drying agent or leveling agent.
[0032] Furthermore, by adjusting the mass ratio of various raw materials in the silver / silver chloride paste, the present invention enables the paste to have the advantages of strong adhesion, low impedance, good electrode potential stability and high signal-to-noise ratio when applied to the electrode.
[0033] Preferably, the conductive polymer slurry in S4 comprises a conductive polymer, a solvent, and additives: the conductive polymer accounts for 10-30% of the total mass of the conductive polymer slurry; the solvent accounts for 70-80% of the total mass of the conductive polymer slurry; and the additives account for 1%-5% of the total mass of the conductive polymer slurry.
[0034] Furthermore, by adjusting the mass ratio of the conductive polymer in the conductive polymer slurry, the conductivity, flexibility, and adhesion of the conductive film on the prepared electrode can be adjusted.
[0035] Furthermore, the solvent is selected based on the solubility of the conductive polymer, such as alcohols, ethers, esters, etc.
[0036] Furthermore, the additives are dispersants, plasticizers, stabilizers, etc. For example, dispersants are used to increase the dispersibility of the slurry and prevent agglomeration; plasticizers are used to improve the flexibility and processing performance of the slurry; and stabilizers are used to increase the stability of the slurry.
[0037] Furthermore, the method for coating the electrode surface with silver / silver chloride paste described in S3 employs an immersion method.
[0038] Specifically, in this embodiment of the invention, the electrode is immersed in the silver / silver chloride paste for a certain period of time (a few minutes to more than ten minutes), and then slowly removed, allowing excess paste to drip off naturally. The immersion process can be repeated as needed until the coating thickness reaches 10 μm to 20 μm. The electrode with the required coating thickness is then placed in the hot air chamber and heated at 60–100°C for 0.5–1 hour to dry and cure the silver / silver chloride coating.
[0039] Furthermore, the method of coating the electrode surface with conductive polymer slurry described in S4 employs an impregnation method.
[0040] Specifically, in this embodiment of the invention, the electrode is immersed in the conductive polymer slurry for a certain period of time (a few minutes to more than ten minutes), and then slowly removed, allowing excess slurry to drip off naturally. The immersion process can be repeated as needed until the coating thickness reaches 1 μm to 3 μm. The electrode with the required coating thickness is then placed in a hot air chamber and heated at 60–100°C for 0.5–1 hour to allow the conductive polymer coating to dry and cure.
[0041] Example 1 Figure 2 This is a flowchart of a preferred embodiment of the present invention for preparing a bioelectrode. Figure 2 The method for preparing the dry electrode shown includes the following steps: S21. The bioelectrode is injection molded using ABS according to the designed shape; S22. The injection-molded electrode is subjected to surface cleaning and roughening treatment; S23. Apply a layer of silver / silver chloride paste to the electrode surface after surface cleaning and roughening treatment, and heat it to cure it to form a 10μm to 20μm thin film coating layer. S24. Coat the electrode with a layer of conductive polymer paste after coating it with silver / silver chloride paste, and then heat and cure it to form a 1μm to 3μm thin film coating layer.
[0042] In this embodiment of the invention, the bioelectrode described in S21 is a dry electrode for electrocardiogram (ECG) detection, which directly contacts the skin surface during use to detect ECG signals on the human skin surface. Figure 3 As shown, the electrode shape includes a flat surface 31 that contacts human skin, a protruding post 32 for connecting to the ECG electrode clip, and a number of tiny protrusions on the contact surface, which are frustum-shaped teeth 33 formed on the circular contact surface, a transition step 34 for mounting, and a connecting small cylinder 35. Furthermore, in order to maintain the continuity of the film and conductivity throughout the electrode coating process, each transition surface of the electrode adopts an arc transition 36.
[0043] The electrode surface cleaning and roughening treatment described in S22 adopts an ultrasonic cleaning method, that is, the injection-molded electrode is placed in an ultrasonic cleaner and ultrasonically cleaned with acetone or ethanol for 15-30 minutes to remove surface oil and dust, then rinsed with deionized water and placed in a ventilated place to dry.
[0044] The mass ratio of the silver / silver chloride paste used in S23 is: 10% silver powder, 45% silver chloride powder, 3% binder, and 42% solvent. The silver powder includes flake silver powder and spherical silver powder, with the average particle size of the flake silver powder being 3-6 μm and the average particle size of the spherical silver powder being 0.05-0.1 μm; the average particle size of the silver chloride powder is 5-15 μm; the binder is acrylic resin; and the solvent is a dibasic acid ester (DBE), which is a mixture of three dibasic acid esters: dimethyl succinate, dimethyl glutarate, and dimethyl adipate.
[0045] Furthermore, the surface coating method described in S23 employs an immersion method.
[0046] Furthermore, the surface coating method described in S24 employs an immersion method.
[0047] Figure 4 This is a flowchart of the silver / silver chloride paste preparation method according to preferred embodiment 1 of the present invention. Figure 4 As shown, the preparation method of the silver / silver chloride paste includes the following steps: S41. Disperse the acrylic resin in the divalent ester solvent, maintain the temperature at 100 ℃ and stir at low speed for at least 3 hours until the dispersion is uniform, to obtain an adhesive resin solution with a solid content of 7%. S42. Add 6% flake silver powder, 4% spherical silver powder, 45% silver chloride powder, and 45% (7% solid content) binder resin solution by weight into the same container for premixing. S43. Pre-disperse the obtained premixed silver / silver chloride slurry, keeping the temperature below 50°C, and stir at low speed for at least 1 hour until it is evenly dispersed. S44. The obtained pre-dispersed silver / silver chloride is ground using a three-roll mill, and the slurry is ground 5 to 6 times at a temperature of 70°C. S45. The fineness, viscosity and sheet resistance of the slurry obtained by grinding are tested. If the slurry meets the requirements, the silver / silver chloride slurry is obtained. S46. Dilute the prepared silver / silver chloride paste with a solvent to a concentration of 15%-35%, and use it to soak the electrode to ensure that it fully absorbs the paste while avoiding excessive accumulation of the paste on the substrate surface. A lower concentration allows the paste to better penetrate into the pores of the substrate, forming a strong bond and resulting in a uniform coating thickness.
[0048] Furthermore, in this embodiment of the invention, the surface coating method described in S23 employs an immersion method to coat the electrode surface with a silver / silver chloride paste. Specifically, the electrode is immersed in the silver / silver chloride paste for a certain period (a few minutes to over ten minutes), then slowly removed, allowing excess paste to drip off naturally. The immersion process can be repeated as needed until the coating thickness reaches 10 μm to 20 μm. The electrode with the required coating thickness is then placed in a hot air chamber and heated at 80°C for 1 hour to dry and cure the silver / silver chloride coating.
[0049] Figure 5 This is a flowchart of the conductive polymer slurry preparation method according to preferred embodiment 1 of the present invention. Figure 5 As shown, the preparation method of the conductive polymer slurry includes the following steps: S51. Add 75% by mass of butyl acetate solvent to a clean container, then slowly add 22% of conductive polymer polypyrrole (PPy), and stir at an appropriate speed to gradually dissolve the conductive polymer. The stirring speed and time depend on the solubility of the polymer and the viscosity of the system. In this embodiment of the invention, the stirring time is 10 hours. S52. Add 2% dispersant and 1% stabilizer to the slurry prepared in S51 in sequence, continue stirring, and treat with ultrasound for 30 minutes to enhance the dispersion effect. S53. Test the viscosity, conductivity, solid content and other performance indicators of the slurry, and adjust the viscosity by adding solvents or thickeners, and increase the conductivity by appropriately adding conductive polymers; S54. Filter the slurry using a filter screen with an appropriate pore size to remove impurities and large, undispersed particles. Then, place the filtered slurry into a vacuum degassing machine to remove air bubbles and prevent them from affecting the subsequent film formation quality.
[0050] Furthermore, in this embodiment of the invention, the surface coating method described in S24 employs an immersion method to coat the electrode surface with a conductive polymer slurry. Specifically, the slurry prepared in S54 is first diluted with the solvent to a conductive polymer slurry concentration of 15%-35%. A lower concentration allows the slurry to better penetrate the pores of the substrate, forming a strong bond. The electrode is then immersed in the conductive polymer slurry for a certain period (a few minutes to tens of minutes) and slowly removed, allowing excess slurry to drip off naturally. The immersion process can be repeated as needed until the coating thickness reaches 2 μm. The electrode with the required coating thickness is then placed in a hot air chamber and heated at 80°C for 2 hours to dry and cure the conductive polymer coating.
[0051] The electrode prepared according to the formulation and manufacturing process of Embodiment 1 of the present invention meets the technical requirements in terms of adhesion, conductivity, stability and signal-to-noise ratio. Example
[0052] In Example 1, the mass ratio of the silver / silver chloride paste described in S23 was changed to: 20% silver powder, 35% silver chloride powder, 3% binder, and 42% solvent. The silver powder includes flake silver powder and spherical silver powder, with the flake silver powder having an average particle size of 3–6 μm and the spherical silver powder having an average particle size of 0.05–0.1 μm; the silver chloride powder has an average particle size of 5–15 μm; the binder is acrylic resin; and the solvent is a dibasic acid ester (DBE), i.e., a mixture composed of dimethyl succinate, dimethyl glutarate, and dimethyl adipate. Increasing the proportion of silver powder increases conductivity.
[0053] Preferably, the mass ratio of the conductive polymer slurry in S24 is changed to: 28% conductive polymer, 70% solvent, and 1% each of dispersant and stabilizer. This increases the proportion of conductive polymer and thus increases conductivity.
[0054] The electrode prepared according to the formulation of Example 2 and the manufacturing process of Example 1 of the present invention meets the technical requirements in terms of adhesion, conductivity, stability and signal-to-noise ratio.
[0055] Based on the embodiments of the present invention described above, and through the above description, those skilled in the art can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. A method for preparing a bioelectrode, characterized in that, On ABS or PC injection-molded electrodes, first apply a layer of silver / silver chloride paste, heat to cure, then apply a layer of conductive polymer paste and heat to cure, including the following steps: Step 1: Inject the bioelectrode into the designed shape using ABS or PC. Step 2: Clean and roughen the surface of the injection-molded electrode; Step 3: Apply a layer of silver / silver chloride paste to the electrode surface after surface cleaning and roughening, and heat it to cure it, so as to form a 10μm to 20μm thin film coating layer. Step 4: Apply a layer of conductive polymer paste to the electrode coated with silver / silver chloride paste, and then heat and cure it to form a 1μm to 3μm thin film coating layer.
2. The method for preparing a bioelectrode as described in claim 1, characterized in that, The silver / silver chloride paste comprises silver powder, silver chloride powder, binder, and solvent: the silver powder accounts for 4-20% of the mass of the silver / silver chloride paste; the silver chloride powder accounts for 18-50% of the mass of the silver / silver chloride paste; the binder accounts for 2-4% of the mass of the silver / silver chloride paste; and the solvent is selected from propylene glycol, ethylene glycol monomethyl ether, ethyl acetate, divalent ester, etc., and accounts for 35-45% of the mass of the silver / silver chloride paste.
3. The method for preparing a bioelectrode as described in claim 1, characterized in that, The silver powder includes flake silver powder and spherical silver powder, wherein the average particle size of the flake silver powder is 3 to 6 μm, and the average particle size of the spherical silver powder is 0.05 to 0.1 μm.
4. The method for preparing a bioelectrode as described in claim 1, characterized in that, By adjusting the mass ratio of various raw materials in the silver / silver chloride paste, the paste, when applied to the electrode, has the advantages of strong adhesion, low impedance, good electrode potential stability, and high signal-to-noise ratio.
5. The method for preparing a bioelectrode as described in claim 1, characterized in that, The conductive polymer slurry comprises a conductive polymer, a solvent, and additives: the conductive polymer accounts for 10-30% of the total mass of the conductive polymer slurry; the solvent accounts for 70-80% of the total mass of the conductive polymer slurry; and the additives account for 1%-5% of the total mass of the conductive polymer slurry.
6. The method for preparing a bioelectrode as described in claim 1, characterized in that, Adjusting the mass ratio of the conductive polymer in the conductive polymer slurry can adjust the conductivity, flexibility, and adhesion of the conductive film on the prepared electrode.
7. The method for preparing a bioelectrode as described in claim 1, characterized in that, The preferred surface coating method is the immersion method. When using the immersion method, the thickness of the coating layer is controlled by adjusting the slurry ratio and immersion time.
8. The method for preparing a bioelectrode as described in claim 1, characterized in that, The heating and curing process is carried out using a hot air box. When the electrode is placed in the hot air box for heating and curing, the heating temperature is controlled at 60-100 ºC and the drying time is controlled at 30-180 minutes.