A composite material capable of flue gas dust removal and VOCs adsorption and purification, its preparation method and its application

By alternately weaving catalytic metal fibers and activated carbon fibers onto micron-sized metal fibers, closely adjacent adsorption microregions and catalytic microregions are formed, solving the problems of single function and long mass transfer path of existing VOCs purification materials, and realizing efficient VOCs purification and self-regulation capabilities.

CN123059611APending Publication Date: 2026-11-10TIANJIN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611277243.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-10

Smart Images

  • Figure CN123059611A_ABST
    Figure CN123059611A_ABST
Patent Text Reader

Abstract

This invention discloses a composite material, its preparation method, and its application for flue gas dust removal and VOCs adsorption purification. The composite material is an integrated three-dimensional network structure formed by alternating weaving of catalytic metal fibers and activated carbon fibers. The catalytic metal fibers are surface-loaded catalyst fibers. The catalyst is discontinuously distributed on the surface of the metal fibers and is formed by chemical vapor deposition by controlling the linear velocity of the metal fibers passing through the deposition zone and the pulse spray injection frequency of the catalyst solution to meet a set relationship. The alternating weaving involves periodically alternating arrangement of catalytic metal fibers and activated carbon fibers in a certain proportion, forming alternating adsorption micro-regions and catalytic micro-regions within the material. This invention weaves the catalytic metal fibers into a catalytic metal fiber felt, and sets several layers of this felt around the composite material as a filter material and supporting framework. Regular cleaning using compressed air pulse cleaning can synergistically and efficiently remove dust and VOCs from flue gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of atmospheric pollution control and environmental protection materials technology, and relates to a fiber-based composite material that integrates dust filtration, volatile organic compound (VOCs) adsorption and catalytic oxidation functions, its preparation method and its application in flue gas purification. Background Technology

[0002] Volatile organic compounds (VOCs) are organic compounds with boiling points ranging from 50°C to 260°C at room temperature that are easily volatile. They are widely present in industrial and domestic waste gas emissions and are key precursors to the formation of atmospheric ozone and PM2.5. The concentrations of dust and VOCs in fumes emitted from steel mills, restaurant kitchens, industrial painting, and printing processes fluctuate greatly and their composition is complex, posing a serious threat to the environment and human health. Existing purification technologies, such as electrostatic precipitators, UV photolysis, and activated carbon adsorption, generally suffer from problems such as limited functionality, unstable purification efficiency, frequent replacement of consumables, and the potential for secondary pollution or safety hazards. Traditional processes use activated carbon adsorption and desorption, followed by catalytic oxidation of the desorbed VOCs to decompose them into CO2 and H2O. However, these catalytic materials lack adsorption and enrichment capabilities.

[0003] Existing technologies have introduced solutions that combine adsorption, catalytic oxidation, or filtration functions. For example, CN113813697A discloses a filter material with a catalyst-loaded substrate flame-sprayed onto a metal fiber felt, possessing both dust removal and catalytic functions. However, this filter material lacks the ability to adsorb and enrich VOCs. When the VOCs concentration is low or fluctuates significantly, the concentration of reactants on the catalyst surface is insufficient, resulting in a significant decrease in purification efficiency. Activated carbon fiber (ACF) has excellent adsorption performance, but simple adsorption cannot degrade pollutants. After adsorption saturation, it needs frequent replacement, generating hazardous waste. CN111851083A uses wet papermaking and sintering processes to encapsulate activated carbon particles in a three-dimensional network of stainless steel fibers, forming an "encapsulated" structure. However, the activated carbon is deeply embedded, resulting in a long mass transfer path between its adsorption sites and the external airflow and potential catalytic sites. The adsorbed VOCs are difficult to quickly desorb and migrate to the catalytic sites, leading to low adsorption-catalysis synergistic efficiency.

[0004] On the other hand, Chinese invention patent CN202111329379.7 discloses a method and apparatus for preparing an integrated 3D-printed carrier and a VOCs catalyst. This method uses molten aluminum alloy to form an aluminum foil carrier through casting and cold finishing, and then loads the catalyst using a pulsed spray flame synthesis method. However, the carrier in this technical solution is a continuous aluminum foil film, lacking a fibrous three-dimensional mesh filtration structure, thus lacking dust removal capabilities for particulate matter, and not containing any adsorption materials (such as activated carbon), making it unable to achieve VOCs adsorption and enrichment. Therefore, this technology still suffers from the problem of limited functionality and inability to achieve adsorption-catalysis synergy. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing VOCs purification materials, such as single function, poor synergy, long mass transfer paths, and unstable efficiency under complex working conditions, as well as the technical difficulty of controllable catalyst loading on micron-scale metal fibers. This invention provides a fiber-based composite material with both adsorption and catalytic purification functions for VOCs, and its preparation method. This invention constructs a fiber-based composite material with closely adjacent adsorption and catalytic microregions at the microscale through "alternating weaving." Utilizing the periodic spatial arrangement of the two functional fibers, the airflow is forced to repeatedly alternate through the adsorption and catalytic zones. A specific process parameter relationship is established: f=v / d (f - the pulse atomization frequency of the pulsed spray evaporation flame, in Hz or s). -1 v - linear velocity of the metal fiber through the deposition zone, in m / s; d - target deposition cycle length, in m) to complete the controllable loading of catalyst on the micron-scale metal fiber, ultimately realizing the functional integration of VOCs adsorption and enrichment and short-range catalytic degradation.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] A composite material capable of flue gas dust removal and VOCs adsorption and purification, comprising an integrated three-dimensional network structure of catalytic metal fibers and activated carbon fibers woven together in an alternating manner; the catalytic metal fibers are metal fibers with a catalyst layer loaded on their surface, and the diameter of the metal fibers is 1~10μm; the catalyst layer is discontinuously distributed on the surface of the metal fibers, and the catalyst layer is formed by controlling the linear velocity of the metal fibers passing through the deposition zone. Pulse atomization frequency of pulse spray evaporation flame Satisfying the relation Formed by sedimentary fixation, among which The target deposition cycle length is defined as 50~200μm.

[0008] The alternating weaving involves the catalytic metal fibers and the activated carbon fibers being periodically interwoven in a fiber ratio of 1:1 to 3:1 in the thickness direction; the average spacing between adjacent catalytic metal fibers and activated carbon fibers is 50 to 500 μm, so as to form alternating adsorption microregions and catalytic microregions inside the material.

[0009] Furthermore, the metal fiber is made of 316L stainless steel, 310S stainless steel, or FeCrAl alloy.

[0010] Furthermore, the activated carbon fiber is polyacrylonitrile-based activated carbon fiber, viscose-based activated carbon fiber, or pitch-based activated carbon fiber; the specific surface area of ​​the activated carbon fiber is 800~1500m² / g.

[0011] Furthermore, the catalyst active component in the catalyst layer includes at least one of iridium oxide, palladium oxide, ruthenium oxide, rhodium oxide, iron oxide, cerium oxide, aluminum oxide, chromium oxide, barium oxide, zinc oxide, lanthanum cobalt oxide, lanthanum manganese oxide, and perovskite.

[0012] Furthermore, the alternating weaving method can be plain weave, twill weave, interlayer weave, or three-dimensional weave.

[0013] This invention also provides a method for preparing a composite material, comprising:

[0014] S1. A pulsed spray evaporation flame synthesis device is used to propel metal fibers at a linear velocity of 0.002~0.1 m / s. The material passes through a flame deposition zone at a temperature of 1200~2000℃; simultaneously, a solution containing a catalyst active component precursor is sprayed into the flame deposition zone via pulsed atomization, causing the catalyst nanoparticles generated from the pyrolysis of the precursor to be directly deposited and immobilized on the surface of the metal fibers to form the catalytic metal fibers; wherein, the frequency of pulsed atomization is controlled. The frequency range is 0.5~100Hz, the pulse width is 2~50ms, and it is consistent with the linear velocity. Satisfying the above relation ;

[0015] S2. The activated carbon fiber is pretreated by impregnation in a 0.5%~2% aqueous solution of polyacrylate and then dried.

[0016] S3. The catalytic metal fiber obtained in step S1 and the activated carbon fiber pretreated in step S2 are alternately woven as warp and weft yarns to form the composite material.

[0017] Furthermore, in step S1, when the metal fiber passes through the flame deposition zone, multiple sets of flame distributors are symmetrically arranged on both sides of the metal fiber, and the flame temperature is 1400~1600℃.

[0018] Furthermore, in step S3, catalytic metal fibers and activated carbon fibers are used as warp and weft yarns in a ratio of 1:1 to 3:1, and are alternately woven through a textile weaving process to form a composite material; the composite material is then processed into cubic, cylindrical, or corrugated plate modules.

[0019] This invention also provides the application of composite materials in flue gas purification systems. Catalytic metal fibers are woven into catalytic metal fiber felts, and several layers of catalytic metal fiber felts are used as filter materials and support frames around the composite material. The material is cleaned periodically using compressed air pulse cleaning. It can be used to remove dust and volatile organic compounds (VOCs) from flue gas under short-process conditions. The flue gas purification system can be used as an industrial waste gas purification device, a catering fume purification device, or a low-temperature plasma VOCs purification device.

[0020] Compared with the prior art, the beneficial effects of the technical solution of the present invention are:

[0021] 1. By establishing and controlling the key process parameter relationship f=v / d, the heating time of the fiber in the flame and the catalyst deposition mode are precisely controlled. When d is 50~200μm, on the one hand, the discontinuous distribution of catalyst particles is ensured, avoiding the formation of a continuous brittle shell and preserving the flexibility of the metal fiber matrix; on the other hand, the metal fiber passes through the millisecond-level pulsed flame at a speed of 0.002~0.1m / s, with only the surface micro-regions reaching the melting anchoring temperature, while the fiber core remains at a low temperature. This achieves reliable local melting and anchoring of the catalyst while ensuring the overall mechanical strength of the fiber.

[0022] 2. Through an alternating weave structure, activated carbon fibers and catalytic metal fibers are arranged alternately within an ultra-close distance of 50~500μm. When VOC-containing flue gas passes through the composite material, VOC molecules are first adsorbed and enriched by adjacent activated carbon fibers. Driven by the concentration gradient, the adsorbed VOC molecules only need to migrate a very short distance (micrometer level) to reach the active sites on the surface of adjacent catalytic metal fibers, where they are catalytically oxidized and decomposed. According to Fick's first law, the diffusion time t is proportional to the square of the diffusion distance L (t∝L). 2 / D). The migration distance (L1=50~500μm) of this application is compared to the millimeter to centimeter distance (L2≥5mm) in traditional "encapsulation" or layered structures, and the diffusion time is shortened to (50 / 5000). 2 =0.0001 times, which means that the mass transfer rate is increased by about four orders of magnitude.

[0023] 3. The activated carbon fiber layer, acting as an adsorption and enrichment material, can temporarily store excess VOCs when VOC concentration surges. Once the concentration returns to normal, the stored VOCs gradually desorb and migrate to the catalytic sites for decomposition. This adsorption-catalysis coupling mechanism enables the composite material to self-regulate in response to concentration fluctuations, resulting in a stable outlet concentration.

[0024] 4. Catalytic metal fiber felt, woven from catalytic metal fibers, is placed around the composite material. This not only serves as a skeleton to support the composite material and enable it to filter dust, but also, due to the composite material's three-dimensional network structure, it exhibits lower airflow resistance compared to particle-filled beds, thus reducing system energy consumption. The catalytic metal fiber skeleton also provides excellent structural strength and thermal shock resistance. The catalyst is synthesized in situ on the fiber surface via flame, forming a locally molten anchor that is not easily detached. Furthermore, the entire material can be regenerated through methods such as hot air backflushing, extending its service life. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of the composite material preparation process.

[0026] Figure 2 This is a side view of the pulsed spray evaporation flame synthesis device.

[0027] Figure 3 This is a schematic diagram of the alternating braided structure of the composite material of the present invention.

[0028] Figure 4a and Figure 4b A schematic diagram of the appearance of a cubic module formed by processing the composite material and its skeleton according to the present invention.

[0029] Figure 5 A schematic diagram (partial cross-section) of the short-range synergistic effect of "adsorption-catalysis" when flue gas passes through the composite material. Detailed Implementation

[0030] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention.

[0031] Example 1

[0032] This embodiment provides a composite material capable of adsorbing and purifying VOCs. The composite material is an integrated three-dimensional network structure formed by alternating weaving of catalytic metal fibers and activated carbon fibers. The catalytic metal fibers are metal fibers with a catalyst layer loaded on their surface, and the diameter of the metal fibers is 1~10μm. The catalyst layer is discontinuously distributed on the surface of the metal fibers, and the catalyst layer is formed by controlling the linear velocity of the metal fibers passing through the deposition zone. Pulse atomization frequency of pulse spray evaporation flame Satisfying the relation Formed by sedimentary fixation, among which The target deposition cycle length is 50~200μm.

[0033] Specifically, such as Figure 3 As shown, fiber A represents catalytic metal fiber, and fiber B represents activated carbon fiber. When catalytic metal fiber (fiber A) and activated carbon fiber (fiber B) are interwoven, various methods can be employed, including intra-layer hybrid weaving, inter-layer hybrid weaving, intra-layer-inter-layer hybrid weaving, core hybrid weaving, chopped fiber hybrid weaving, and mixed woven fabrics. Catalytic metal fiber bundles and activated carbon fiber bundles are used as warp and weft yarns, respectively, and are plain-woven in ratios of 1:1, 1:2, etc., to produce a composite fabric of a certain thickness. In this structure, the two types of fibers are alternately and closely arranged in a plane. The average spacing between adjacent catalytic metal fibers and activated carbon fibers is 50~500μm, forming alternating adsorption and catalytic microregions within the material.

[0034] Example 2

[0035] This embodiment provides a method for preparing the composite material in Embodiment 1 above, such as... Figure 1 As shown, specifically:

[0036] The materials involved in this preparation method include metal fibers, catalytic metal fibers, solutions containing precursors of catalyst active components, and activated carbon fibers; the equipment involved includes a pulsed spray evaporation flame synthesis device.

[0037] First, the metal fiber preparation process is as follows: steel wires are bundled and drawn together using a composite assembly process, followed by multiple multi-strand drawing to produce micron-sized metal fiber filaments. The material of the metal fiber filaments can be 316L stainless steel, 310S stainless steel, or FeCrAl alloy. Different types and sizes of metal fiber filaments can be selected depending on the density of the loaded catalyst. Stainless steel metal fiber filaments can be used for extended periods below 450℃, while FeCrAl fiber filaments can be used for extended periods below 600℃. As a filter media, metal fiber filaments are easy to clean and can be recycled after use, without causing secondary pollution to the environment.

[0038] Secondly, such as Figure 2As shown, the pulse spray evaporation flame synthesis device includes two synthesis units arranged opposite each other. Each synthesis unit consists of one burner 6. The top of the burner 6 is provided with a first air inlet 4, and the front end of the first air inlet 4 is provided with a first flow controller connected to the oxidant pipe. Pulse nozzles 3 and second air inlets 5 are respectively provided on both sides of the top of the burner 6. The front end of the second air inlet 5 is provided with a second flow controller connected to the fuel pipe and a third flow controller connected to the bath gas pipe. Multiple flame distributors 8 are evenly spaced at opposite ends of the burner 6. The number and distribution of the burner 6 and the flame distributors 8 in a single burner 6 can be adjusted according to production requirements. The pulse nozzles 3 are connected to the precursor solution container 2.

[0039] The subsequent process of supporting the catalyst with metal fibers is as follows:

[0040] Simultaneously with the preparation of metal fiber 1, a precursor solution can be prepared. The precursor solution includes a precursor containing the catalyst active component and a combustible solvent. In this embodiment, the precursor can be iridium acetylacetone, palladium acetate, or ruthenium acetate. The concentration of the precursor solution is adjusted according to the characteristics of the catalyst and temperature requirements; the concentration of the precursor solution is on the order of millimoles per liter. The combustible agent can be ethanol or other alcohol solvents. The precursor solution is placed in a precursor solution container 2.

[0041] The selection of catalysts is related to the preparation requirements of metal fiber filaments. The design of catalyst selection, precursor solution preparation, and atomization injection frequency should be considered in conjunction with the preparation requirements of metal fiber filaments.

[0042] The precursor solution is delivered to multiple burners using atomized sample delivery, and the atomized precursor solution is mixed with the oxidant in burner 6. Atomized sample delivery methods include pulse atomization and gas impact. In pulse atomization, the precursor solution is atomized using pulse nozzles 3 and then delivered to burner 6; multiple pulse nozzles 3 can be used.

[0043] The amount of atomized precursor solution entering the burner can be controlled by adjusting the on / off duration of the pulse nozzle. Atomized injection ensures stable catalyst concentration, resulting in a final product with uniform morphology and stable performance.

[0044] The oxidant enters the burner 6 through the first air inlet 4 and mixes with the atomized precursor solution in the burner. The oxidant includes one of the following: air, oxygen, or a mixture of air and oxygen.

[0045] Fuel and bath gas are introduced into the burner 6 through the second air inlet 5, allowing the atomized precursor solution, oxidant, fuel, and bath gas to combust together. The fuel can be a gaseous or liquid fuel. The bath gas can be nitrogen or an inert gas.

[0046] The amount of oxidant entering the burner is controlled by a first flow controller; the amount of fuel entering the burner is controlled by a second flow controller; and the amount of bath gas entering the burner is controlled by a third flow controller. The catalyst structure can be adjusted by controlling the amounts of the atomized precursor solution, oxidant, fuel, and bath gas.

[0047] After atomization, the precursor solution 7 undergoes pyrolysis to form catalyst nuclei. These catalyst nuclei aggregate, grow, and deposit onto the metal fiber substrate. The agglomeration and growth of the catalyst nuclei form a catalyst particle layer 9. The metal fiber 1 moves at a certain speed between two synthesis units of the pulsed spray evaporation flame synthesis device, ensuring that the catalyst particle layer 9 is uniformly deposited onto the metal fiber 1, thus forming a catalyst-loaded metal fiber 1.

[0048] By controlling the integrated density of the flame distributor, the catalyst loading density can be adjusted, thereby preparing different metal fiber filter media. In this embodiment, the synthesis unit is located on both sides of the metal fiber substrate. By adjusting the switching of the burners on both sides of the metal fiber substrate, catalyst can be simultaneously loaded on both sides of the metal fiber substrate.

[0049] The prepared metal fibers are subjected to performance testing and processing to facilitate subsequent weaving processes.

[0050] Next, the activated carbon fiber is pretreated. The activated carbon fiber prepared using existing technology is surface cleaned and pretreated by coating with polymer slurry, such as polyacrylate or phenolic resin, to improve the fiber spinnability, reduce fuzzing, and increase the adhesion to metal fibers.

[0051] Finally, the composite material is prepared by fiber weaving. After preparing activated carbon fibers and catalyst-loaded metal fibers, the fibers are interwoven to form a composite material. The woven composite material can be cut and shaped into three-dimensional shapes such as cubes or cuboids with a length, width, and height of 50-500 mm, and cylinders with a diameter and height of 50-500 mm. Catalytic metal fiber felt is placed around the composite material as a skeleton support and filter material. See the example image of the cube module. Figure 4a and Figure 4b It can be filled into exhaust gas purifiers for catering fumes, steel industry waste gas, etc.

[0052] Specifically, the working mechanism of the prepared composite material is explained as follows:

[0053] like Figure 5 As shown, when flue gas containing dust and VOCs passes through the composite material of the present invention at a certain flow rate:

[0054] (1) First, the dust in the flue gas is trapped on the surface of the catalytic metal fiber felt to form a surface dust layer, thereby filtering the dust. The surface dust is also cleaned regularly with pulse compressed air.

[0055] (2) Then, VOCs molecules in the flue gas are adsorbed and enriched when they flow through the activated carbon fiber (adsorption micro-region), making the local concentration much higher than the main concentration of the flue gas.

[0056] (3) Under the heat carried by the flue gas, external auxiliary heating, or plasma synergy, the VOCs molecules adsorbed on the surface of activated carbon fibers gain enough energy to overcome the adsorption barrier and desorb, and rapidly diffuse to the surface of adjacent catalytic metal fibers driven by the concentration gradient. Since the spacing is only 50~500μm, according to Fick's diffusion law, the mass transfer rate of this step is more than 10,000 times that of the traditional millimeter-level distance, and hardly constitutes a kinetic barrier.

[0057] (4) At the set temperature, VOCs molecules are catalytically oxidized and decomposed into CO2 and H2O under the action of catalyst on the surface of catalytic metal fiber, and at the same time, the heat of reaction is released. This heat can be used to maintain the temperature of the catalyst bed, which helps to reduce the energy consumption of operation.

[0058] (5) As the adsorption micro-regions and catalytic micro-regions are arranged alternately at the microscale, the entire purification process presents a dynamic equilibrium state of "adsorption, desorption and catalysis at the same time". The activated carbon fiber always maintains a certain proportion of unsaturated adsorption sites, thus ensuring the stability and anti-penetration ability of long-term operation.

[0059] Example 3

[0060] This embodiment provides a fiber-based composite material with flue gas dust removal and VOCs adsorption and purification capabilities, and its preparation method is as follows:

[0061] S1. Preparation of catalytic metal fibers:

[0062] FeCrAl alloy fibers (8 μm in diameter, commercially available, temperature resistant up to 600℃ or higher) were used as the substrate. Ferric acetylacetone was dissolved in ethanol to prepare a precursor solution with a concentration of 50 mmol / L. [The text then abruptly shifts to a different topic:] ... Figure 2 The pulsed spray evaporation flame synthesis device shown is set with a pulse frequency of f=20s. -1 The pulse width is 10ms, and the combustion flame temperature is 1500℃ (adjusted by the methane / air ratio). According to the formula f=v / d (f - pulse atomization frequency of the pulsed spray evaporation flame, unit Hz or s),... -1 v - linear velocity of the metal fiber through the deposition zone, in m / s; d - target deposition period length, in m). Given a target deposition period length d = 100 μm, the linear velocity of the metal fiber is determined as v = f × d = 20 s.-1 ×100×10 −6 m = 0.002 m / s. This linear velocity falls within the range of 0.002~0.1 m / s defined in this invention. The metal fibers are passed through the flame deposition zone at this linear velocity; each burner contains five flame distributors. Under pulsed atomization, the precursor solution droplets instantly evaporate and pyrolyze in the flame, generating iron oxide (Fe2O3) nanoparticles, which are then deposited on the fiber surface. The deposition time is controlled so that the catalyst loading is approximately 8% of the fiber weight, and the resulting catalyst particles on the surface of the catalytic metal fiber are discontinuously distributed.

[0063] S2. Pretreatment of activated carbon fiber:

[0064] Commercial viscose-based activated carbon fibers (specific surface area 1100 m² / g, fiber diameter 10 μm) were selected and immersed in a 1% (mass fraction) polyacrylate aqueous solution for 5 minutes. After removal, they were dried at 80°C for 2 hours. This pretreatment improves the flexibility and breakage resistance of the activated carbon fibers, facilitating subsequent weaving.

[0065] S3. Alternating weave:

[0066] The catalytic metal fibers obtained in step S1 (as warp yarns) and the activated carbon fibers treated in step S2 (as weft yarns) are plain-weave woven on an automatic weaving machine at a yarn count ratio of 2:1. The specific weaving parameters are: 40 warp yarns per centimeter and 30 weft yarns per centimeter. The two fibers are tightly interwoven at the weaving nodes to form a composite fiber felt material with a thickness of approximately 3 mm. Measurements show that the average spacing between adjacent catalytic metal fibers and activated carbon fibers is approximately 250 μm.

[0067] S4. Molding:

[0068] The above-mentioned composite material is cut, sorted, and shaped into a 100mm×100mm×100mm cube module for later use.

[0069] Example 4

[0070] The method for preparing the composite material in this embodiment is basically the same as that in Example 2 above, except that: the catalyst active component is cerium oxide (the precursor is cerium nitrate), the metal fiber is 316L stainless steel with a diameter of 5μm; the pulse frequency is f=50Hz, according to the formula f=v / d (f-pulse atomization frequency of pulsed spray evaporation flame, unit Hz or s). -1 v - linear velocity of the metal fiber through the deposition zone, in m / s; d - target deposition period length, in m). Taking the target deposition period length d = 50 μm, the linear velocity is calculated as v = f × d = 50 s. -1 ×50×10 −6m = 0.0025 m / s; the braiding ratio is 1:1 (catalytic metal fiber: activated carbon fiber). The resulting composite material has a thickness of approximately 5 mm and an average spacing of approximately 150 μm between adjacent fibers.

[0071] Example 5

[0072] The method for preparing the composite material in this embodiment is basically the same as that in Example 2 above, except that: the catalyst component is perovskite (LaCoO3), the precursor is lanthanum nitrate and cobalt nitrate (molar ratio 1:1), the flame temperature is 1800℃, and the pulse frequency is f=80Hz. According to the formula f=v / d (f-pulse atomization frequency of the pulsed spray evaporation flame, unit Hz or s),... -1 v - linear velocity of the metal fiber through the deposition zone, in m / s; d - target deposition period length, in m). Taking the target deposition period length d = 150 μm, the calculated linear velocity v = f × d = 80 s. -1 ×150×10 −6 m=0.012m / s, catalyst loading 6%. The weaving method is three-dimensional weaving, forming a composite material with a thickness of 8mm.

[0073] The above embodiments fully demonstrate the effectiveness and superiority of the composite material and its preparation method of the present invention. Through material design and process innovation, the present invention successfully solves the bottleneck problem of single-functional materials in complex flue gas purification, and has high practical value and promising prospects for application.

[0074] This invention is not limited to the embodiments described above. The above description of specific embodiments is intended to illustrate and explain the technical solutions of this invention. The specific embodiments described above are merely illustrative and not restrictive. Without departing from the spirit and scope of the claims, those skilled in the art can make many specific modifications based on the teachings of this invention, and these modifications all fall within the scope of protection of this invention.

Claims

1. A composite material capable of flue gas dust removal and VOCs adsorption and purification, characterized in that, The composite material is an integrated three-dimensional network structure formed by alternating weaving of catalytic metal fibers and activated carbon fibers. The catalytic metal fibers are metal fibers with a catalyst layer loaded on their surface, and the diameter of the metal fibers is 1~10μm. The catalyst layer is discontinuously distributed on the surface of the metal fibers, and the catalyst layer is formed by controlling the linear velocity of the metal fibers as they pass through the deposition zone. The pulse atomization frequency of the pulse spray evaporation flame Satisfying the relation Formed by sedimentary fixation, among which The target deposition cycle length is defined as 50~200μm. The alternating weaving refers to the periodic alternating arrangement and interweaving of the catalytic metal fibers and the activated carbon fibers in the thickness direction at a fiber number ratio of 1:1 to 3:

1. The average spacing between adjacent catalytic metal fibers and activated carbon fibers is 50~500μm, so as to form alternating adsorption microregions and catalytic microregions inside the material.

2. The composite material according to claim 1, characterized in that, The metal fibers are made of 316L stainless steel, 310S stainless steel, or FeCrAl alloy.

3. The composite material according to claim 1, characterized in that, The activated carbon fiber is a polyacrylonitrile-based activated carbon fiber, a viscose-based activated carbon fiber, or a pitch-based activated carbon fiber; the specific surface area of ​​the activated carbon fiber is 800~1500m² / g.

4. The composite material according to claim 1, characterized in that, The catalyst active component in the catalyst layer includes at least one of iridium oxide, palladium oxide, ruthenium oxide, rhodium oxide, iron oxide, cerium oxide, aluminum oxide, chromium oxide, barium oxide, zinc oxide, lanthanum cobalt oxide, lanthanum manganese oxide, and perovskite.

5. The composite material according to claim 1, characterized in that, The alternating weaving method includes plain weave, twill weave, interlayer weave, or three-dimensional weave.

6. A method for preparing a composite material as described in any one of claims 1 to 5, characterized in that, include: S1. A pulsed spray evaporation flame synthesis device is used to propel metal fibers at a linear velocity of 0.002~0.1 m / s. The material passes through a flame deposition zone at a temperature of 1200~2000℃; simultaneously, a solution containing a catalyst active component precursor is sprayed into the flame deposition zone via pulsed atomization, causing the catalyst nanoparticles generated from the pyrolysis of the precursor to be directly deposited and immobilized on the surface of the metal fibers to form the catalytic metal fibers; wherein, the frequency of pulsed atomization is controlled. The frequency range is 0.5~100Hz, the pulse width is 2~50ms, and it is consistent with the linear velocity. Satisfying the above relation ; S2. The activated carbon fiber is pretreated by impregnation in a 0.5%~2% aqueous solution of polyacrylate and then dried. S3. The catalytic metal fiber obtained in step S1 and the activated carbon fiber pretreated in step S2 are alternately woven as warp and weft yarns to form the composite material.

7. The preparation method according to claim 6, characterized in that, In step S1, when the metal fiber passes through the flame deposition zone, multiple sets of flame distributors are symmetrically arranged on both sides of the metal fiber, and the flame temperature is 1400~1600℃.

8. The preparation method according to claim 6, characterized in that, In step S3, catalytic metal fibers and activated carbon fibers are used as warp and weft yarns in a ratio of 1:1 to 3:1, and are alternately woven through a textile weaving process to form a composite material; the composite material is then processed into cubic, cylindrical, or corrugated plate modules.

9. The application of the composite material according to any one of claims 1 to 5 in a flue gas purification system, characterized in that, Used to remove dust and volatile organic compounds (VOCs) from flue gas; the flue gas purification system can be used as an industrial waste gas purification device, a catering fume purification device, or a low-temperature plasma VOCs purification device.

Citation Information

Patent Citations

  • Method for producing activated carbon cloth

    CN111851083A

  • Metal fiber filter material with dust removal and VOCs catalytic purification functions and preparation method thereof

    CN113813697A

  • Preparation method and device of integrated 3D printing carrier and loaded VOCs catalyst

    CN113909500A