Composite gas chromatography packing materials and their preparation methods, gas chromatography columns, and applications.

By forming a silane coupling agent and a polydopamine interface layer on the surface of the microsphere carrier, combined with the metal-organic framework layer UiO-66-NH2, the problem of insufficient interfacial bonding stability of metal-organic framework chromatographic packing materials is solved, thereby improving separation performance and detection reproducibility.

CN123059631APending Publication Date: 2026-11-10SOUTHERN POWER GRID DIGITAL GRID RESEARCH INSTITUTE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611536621.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Metal-organic framework chromatographic packing materials have insufficient interfacial bonding stability during use, leading to decreased separation performance and poor detection reproducibility.

Method used

A composite gas chromatography packing material is used, including a microsphere carrier, a composite interface layer, and a metal-organic framework layer. By forming a silane coupling agent and a polydopamine interface layer on the surface of the microsphere carrier, combined with the metal-organic framework layer UiO-66-NH2, the interfacial bonding stability is enhanced.

Benefits of technology

It improves the separation performance stability and detection reproducibility of chromatographic packing materials, reduces the risk of metal-organic framework layer detachment during carrier gas scouring and column aging, and improves separation efficiency and selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123059631A_ABST
    Figure CN123059631A_ABST
Patent Text Reader

Abstract

This application provides a composite gas chromatography packing material, its preparation method, a gas chromatography column, and its application. The composite gas chromatography packing material includes a microsphere carrier, a composite interface layer, and a metal-organic framework layer. The microsphere carrier includes silica. The composite interface layer includes a first interface layer on the surface of the microsphere carrier and a second interface layer on the surface of the first interface layer. The first interface layer includes a silane coupling agent, and the second interface layer includes polydopamine. The metal-organic framework layer is located on the surface of the second interface layer and includes UiO-66-NH2. In the composite gas chromatography packing material provided by this application, the interfacial bonding stability between the metal-organic framework layer and the microsphere carrier is good, which can reduce the risk of the metal-organic framework layer falling off during carrier gas scouring and column aging, thereby improving the separation performance stability of the chromatographic packing material during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of chromatographic separation materials technology, specifically to a composite gas chromatography packing material and its preparation method, a gas chromatography column, and its application. Background Technology

[0002] Power transformers are core equipment in power grid systems. Dissolved gas analysis in oil is an important means of assessing latent faults in transformers and ensuring the safe operation of the power grid. It relies on gas chromatography to separate and quantitatively detect multi-component gases. The performance of the chromatographic packing material affects the accuracy and reproducibility of the test results.

[0003] Common packing materials for dissolved gas chromatography in oil include molecular sieves, carbon molecular sieves, and porous polymers. However, these packing materials have limitations in terms of gas separation selectivity and stability. Metal-organic frameworks (MOFs), with their tunable pores and abundant functional sites, have attracted attention in the field of gas separation. However, when MOFs are used as chromatographic packing materials, the insufficient bonding stability between the functional materials and the support leads to a tendency for separation performance to degrade during use, making it difficult to guarantee the reproducibility of detection results. Therefore, it is necessary to improve traditional MOF chromatographic packing materials to address the problem of insufficient interfacial bonding stability. Summary of the Invention

[0004] In view of this, this application provides a composite gas chromatography packing material, its preparation method, a gas chromatography column, and its application to solve the above-mentioned technical problems.

[0005] To achieve the above objectives, in a first aspect, this application provides a composite gas chromatography packing material, which includes a microsphere carrier, a composite interface layer, and a metal-organic framework layer; the microsphere carrier includes silica; the composite interface layer includes a first interface layer located on the surface of the microsphere carrier and a second interface layer located on the surface of the first interface layer, the first interface layer including a silane coupling agent and the second interface layer including polydopamine; the metal-organic framework layer is located on the surface of the second interface layer, and the metal-organic framework layer includes UiO-66-NH2.

[0006] Based on the first aspect, in some embodiments, the UiO-66-NH2 in the metal-organic framework layer has ligand-deficient defect sites and exposed unsaturated Zr metal sites.

[0007] Based on the first aspect, in some embodiments, the silane coupling agent includes an amino-containing silane coupling agent.

[0008] Based on the first aspect, in some embodiments, the amino-containing silane coupling agent includes one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and N-β-aminoethyl-γ-aminopropyltrimethoxysilane.

[0009] Based on the first aspect, in some embodiments, the particle size of the microsphere carrier is from 1 μm to 10 μm.

[0010] Based on the first aspect, in some embodiments, the microsphere carrier has a porous structure with a pore size of 5 nm to 30 nm.

[0011] Based on the first aspect, in some embodiments, the thickness of the composite interface layer is 5 nm to 50 nm;

[0012] Based on the first aspect, in some embodiments, the thickness ratio of the first interface layer to the second interface layer in the composite interface layer is 1:20 to 1:2.

[0013] Based on the first aspect, in some embodiments, the thickness of the metal-organic framework layer is 30 nm to 300 nm.

[0014] Secondly, this application provides a method for preparing the above-mentioned composite gas chromatography packing material, comprising the following steps: activating a microsphere carrier to hydroxylate the microsphere carrier; reacting the hydroxylated microsphere carrier with a silane coupling agent to form a first interface layer on the surface of the microsphere carrier, thus preparing an intermediate; mixing the intermediate with dopamine to allow the dopamine to self-polymerize under weakly alkaline conditions, forming a second interface layer on the surface of the first interface layer, thereby preparing a composite interface layer on the surface of the microsphere carrier; adding the microsphere carrier with the composite interface layer to a reaction system containing a zirconium source and 2-aminoterephthalic acid, and performing a solvothermal reaction to form a metal-organic framework layer on the surface of the composite interface layer, thus preparing the composite gas chromatography packing material.

[0015] Based on the second aspect, in some embodiments, the reaction system also contains a monocarboxylic acid regulator.

[0016] Based on the second aspect, in some embodiments, the monocarboxylic acid modifier includes one or more of formic acid, acetic acid, trifluoroacetic acid, benzoic acid, a mixture of trifluoroacetic acid and acetic acid, and a mixture of formic acid and acetic acid.

[0017] Based on the second aspect, in some embodiments, the molar ratio of the monocarboxylic acid modifier to 2-aminoterephthalic acid is from 5:1 to 2000:1.

[0018] Based on the second aspect, in some embodiments, the molar ratio of zirconium source to 2-aminoterephthalic acid is 1:1 to 8:1.

[0019] Based on the second aspect, in some embodiments, the activation treatment includes acid activation or oxidative activation.

[0020] Based on the second aspect, in some embodiments, the pH of the weakly alkaline conditions is 8.0 to 9.0.

[0021] Based on the second aspect, in some embodiments, the concentration of dopamine is from 0.5 mg / mL to 5 mg / mL, and the self-polymerization time is from 3 h to 24 h.

[0022] Based on the second aspect, in some embodiments, the reaction solvent in the solvothermal reaction includes one or more of N,N-dimethylformamide, ethanol, water, and methanol.

[0023] Based on the second aspect, in some embodiments, the temperature of the solvothermal reaction is 90°C to 150°C, and the time is 4 h to 36 h.

[0024] Based on the second aspect, in some embodiments, after the solvothermal reaction, the preparation method further includes a step of solvent replacement using an organic solvent.

[0025] Based on the second aspect, in some embodiments, the organic solvent includes one or more of ethanol, methanol, acetone, and acetonitrile.

[0026] Based on the second aspect, in some implementations, the replacement time is 12 h to 72 h.

[0027] Based on the second aspect, in some embodiments, after the solvothermal reaction, the preparation method further includes a drying step.

[0028] Based on the second aspect, in some embodiments, the drying temperature is 60°C to 150°C, and the drying time is 6 h to 24 h.

[0029] Thirdly, this application provides a gas chromatography column, including a column tube and a gas chromatography packing material packed inside the column tube, wherein the gas chromatography packing material includes the above-mentioned composite gas chromatography packing material or the composite gas chromatography packing material prepared by the above-mentioned preparation method.

[0030] Fourthly, this application provides the application of the above-mentioned gas chromatography column in the separation and detection of dissolved gases in transformer oil.

[0031] Based on the fourth aspect, in some embodiments, the dissolved gas includes one or more of H2, CO, CO2, CH4, C2H4, C2H2, and C2H6.

[0032] In this application, the composite gas chromatography packing has a specific composite structure, with a microsphere carrier including silica as a mechanical support, and a composite interface layer is provided on the surface of the microsphere carrier. The first interface layer in the composite interface layer includes a silane coupling agent, the second interface layer includes polydopamine, and the second interface layer is located on the surface of the first interface layer. The metal-organic framework layer is located on the surface of the composite interface layer and includes UiO-66-NH2. In the aforementioned composite structure, the microsphere carrier and the metal-organic framework layer are indirectly bonded through a composite interface layer. The silica-based microsphere carrier provides mechanical support, which is beneficial for adapting to the packing and operating conditions of the chromatographic column. The silane coupling agent in the composite interface layer helps to form a stable first interface layer on the surface of the silica microsphere carrier. Polydopamine has good adhesion properties and abundant functional groups, which helps to firmly adhere to the surface of the first interface layer and provide anchoring points for UiO-66-NH2. This helps to enhance the interfacial bonding stability between the metal-organic framework layer and the microsphere carrier, reduce the risk of the metal-organic framework layer falling off during carrier gas scouring and column aging, and thus improve the separation performance stability of the chromatographic packing material during use. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the preparation process of the composite gas chromatography packing material provided in Examples 1-42 of this application.

[0034] Figure 2 This is a powder X-ray diffraction pattern of the metal-organic framework in the composite gas chromatography packing material provided in Example 3 of this application.

[0035] Figure 3 The infrared spectrum of the metal-organic framework in the composite gas chromatography packing provided in Example 3 of this application.

[0036] Figure 4 This is a scanning electron microscope image of the metal-organic framework in the composite gas chromatography packing material provided in Example 3 of this application.

[0037] Figure 5 The standard gas mixture chromatogram of dissolved characteristic gases (H2, CO, CO2, CH4, C2H4, C2H2 and C2H6) in transformer oil is provided by gas chromatography column separation in Example 3 of this application.

[0038] Figure 6 This is a standard mixed gas chromatogram of dissolved characteristic gases in transformer oil obtained by gas chromatography column separation according to Example 43 of this application.

[0039] Figure 7 The separation reproducibility of the gas chromatography column provided in Comparative Example 1 of this application was investigated.

[0040] Figure 8This is a comparison of the separation performance of the gas chromatography column before and after aging, provided as Comparative Example 2 of this application. Detailed Implementation

[0041] To facilitate understanding of the technical solutions of this application, a more comprehensive description of the technical solutions of this application will be provided below with reference to the accompanying drawings, which illustrate preferred embodiments of the technical solutions of this application. However, the technical solutions of this application can be implemented in many different forms and are not limited to the embodiments described herein. Rather, these embodiments are provided to enable a more thorough and comprehensive understanding of the disclosure of the technical solutions of this application.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0043] To address the issue of insufficient interfacial stability in traditional metal-organic framework (MOF) chromatographic packing materials, this study found that when MOF materials are simply blended or physically composited with microsphere carriers, there is a lack of effective chemical bonding or strong interactions between the two, resulting in weak interfacial adhesion. During continuous carrier gas scouring and column aging, the MOF layer easily detaches from the carrier surface, leading to decreased separation performance and reduced detection reproducibility. Taking the MOF UiO-66-NH2 as an example, UiO-66-NH2 is constructed from zirconium metal clusters and 2-aminoterephthalic acid, exhibiting good thermal and chemical stability. Its framework carries amino active sites, enabling the recognition of small molecule gases through sieving, hydrogen bonding, and Lewis acid-base interactions, thus adapting to differences in molecular size and polarity of characteristic gases dissolved in oil. However, when UiO-66-NH2 powder is directly used as a packing material for dissolved gas chromatography in oil, its fine particle size leads to uneven packing into the column bed, resulting in large column pressure fluctuations. Furthermore, its weak mechanical strength causes pulverization and particle migration under continuous carrier gas scouring, leading to poor separation reproducibility. While physically mixing the carrier to compensate for the performance defects of UiO-66-NH2 powder, the weak interfacial bonding between the carrier and the powder causes the MOF layer formed by UiO-66-NH2 to easily detach. In addition, UiO-66-NH2 powder also suffers from high pore mass transfer resistance and slow adsorption-desorption kinetics for small molecule gases, making it difficult to meet the requirements of rapid detection scenarios in dissolved gas analysis in oil.

[0044] Based on this, this application introduces an interface layer between the microsphere carrier and the metal-organic framework layer, and utilizes this interface layer to form a strong bond with the microsphere carrier and the metal-organic framework layer respectively, thereby stably anchoring the metal-organic framework layer on the surface of the microsphere carrier.

[0045] Based on this, one embodiment of this application provides a composite gas chromatography packing material, which includes a microsphere carrier, a composite interface layer, and a metal-organic framework layer. The microsphere carrier includes silica; the composite interface layer includes a first interface layer located on the surface of the microsphere carrier and a second interface layer located on the surface of the first interface layer, the first interface layer including a silane coupling agent and the second interface layer including polydopamine; the metal-organic framework layer is located on the surface of the second interface layer, and the metal-organic framework layer includes UiO-66-NH2.

[0046] In this application, the composite gas chromatography packing has a specific composite structure, with a microsphere carrier including silica as a mechanical support, and a composite interface layer is provided on the surface of the microsphere carrier. The first interface layer in the composite interface layer includes a silane coupling agent, the second interface layer includes polydopamine, and the second interface layer is located on the surface of the first interface layer. The metal-organic framework layer is located on the surface of the composite interface layer and includes UiO-66-NH2. In the aforementioned composite structure, the microsphere carrier and the metal-organic framework layer are indirectly bonded through a composite interface layer. The silica-based microsphere carrier provides mechanical support, which is beneficial for adapting to the packing and operating conditions of the chromatographic column. The silane coupling agent in the composite interface layer helps to form a stable first interface layer on the surface of the silica microsphere carrier. Polydopamine has good adhesion properties and abundant functional groups, which helps to firmly adhere to the surface of the first interface layer and provide anchoring points for UiO-66-NH2. This helps to enhance the interfacial bonding stability between the metal-organic framework layer and the microsphere carrier, reduce the risk of the metal-organic framework layer falling off during carrier gas scouring and column aging, and thus improve the separation performance stability of the chromatographic packing material during use.

[0047] In some embodiments, the UiO-66-NH2 in the metal-organic framework layer has ligand-deficient defect sites and exposed unsaturated Zr metal sites. Furthermore, introducing ligand-deficient defect sites into UiO-66-NH2 helps reduce the mass transfer resistance of gas molecules within the UiO-66-NH2 channels, while introducing exposed unsaturated Zr metal sites provides additional active adsorption sites. The combined effect of these two factors helps accelerate the adsorption-desorption kinetics of gas molecules and improve chromatographic peak shape. Therefore, based on improved interfacial binding stability, this further enhances the separation efficiency and selectivity of the composite gas chromatography packing material.

[0048] In some embodiments, the silane coupling agent includes an amino-containing silane coupling agent. Furthermore, the amino-containing silane coupling agent facilitates the formation of stable chemical bonds with the surface of the microsphere carrier. Simultaneously, its amino groups provide active sites for subsequent polydopamine deposition and facilitate coordination with the Zr metal sites in UiO-66-NH2, thereby improving interfacial bonding stability and further enhancing the adhesion between the composite interface layer and the metal-organic framework layer.

[0049] In some embodiments, the amino-containing silane coupling agent includes one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and N-β-aminoethyl-γ-aminopropyltrimethoxysilane. The above-mentioned amino-containing silane coupling agents exhibit high reactivity and good lamination properties, which is beneficial for forming a uniform and stable first interfacial layer on the surface of the microsphere carrier.

[0050] In some embodiments, the particle size of the microsphere carrier is from 1 μm to 10 μm. For example, the particle size of the microsphere carrier can be 1 μm, 1.9 μm, 2.8 μm, 3.7 μm, 4.6 μm, 5.5 μm, 6.4 μm, 7.3 μm, 8.2 μm, 9.1 μm, 10 μm, or any value within the range of any two of the above values. Furthermore, controlling the particle size of the microsphere carrier within the above range helps to balance packing density and column pressure stability.

[0051] In some embodiments, the microsphere carrier has a porous structure with a pore size of 5 nm to 30 nm. For example, the pore size of the microsphere carrier can be 5 nm, 7.5 nm, 10 nm, 12.5 nm, 15 nm, 17.5 nm, 20 nm, 22.5 nm, 25 nm, 27.5 nm, 30 nm, or any value within the range of any two of the above values. Furthermore, controlling the pore size of the microsphere carrier within the above range helps to provide sufficient specific surface area and pore accessibility, thereby facilitating further improvement in the packing performance and usability of the composite gas chromatography packing material.

[0052] In some embodiments, the thickness of the composite interface layer is from 5 nm to 50 nm. For example, the thickness of the composite interface layer can be 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, or any value within the range of any two of the above values. Furthermore, controlling the thickness of the composite interface layer within the above range is beneficial in providing sufficient anchoring points and bonding strength while reducing the risk of increased gas mass transfer resistance when the interface layer is thicker, thereby further facilitating a balance between interfacial bonding stability and separation mass transfer efficiency.

[0053] In some embodiments, the thickness ratio of the first interface layer to the second interface layer in the composite interface layer is 1:20 to 1:2. For example, the thickness ratio of the first interface layer to the second interface layer in the composite interface layer can be 1:20, 1:18, 1:16, 1:14, 1:12, 1:10, 1:8, 1:6, 1:4, 1:3, 1:2, or any value within the range of any two of the above values. Furthermore, controlling the thickness ratio of the first interface layer to the second interface layer within the above range is beneficial for the silane coupling agent layer to provide suitable amino anchors, while the polydopamine layer provides sufficient adhesion properties and functional groups. These two elements synergistically enhance the bonding force between the metal-organic framework layer and the microsphere carrier, thereby further improving the loading uniformity and bonding stability of the metal-organic framework layer.

[0054] In some embodiments, the thickness of the metal-organic framework layer is from 30 nm to 300 nm. For example, the thickness of the metal-organic framework layer can be 30 nm, 60 nm, 90 nm, 120 nm, 150 nm, 180 nm, 210 nm, 240 nm, 270 nm, 300 nm, or any value within the range of any two of the above values. Furthermore, controlling the thickness of the metal-organic framework layer within the above range helps to ensure sufficient gas adsorption and separation sites while reducing the risk of excessively long mass transfer paths when the functional layer is thicker, thereby further improving the separation efficiency and mass transfer performance of the composite gas chromatography packing material.

[0055] An embodiment of this application also provides a method for preparing the above-mentioned composite gas chromatography packing material, comprising the following steps:

[0056] Step 1: Activate the microsphere carrier to hydroxylate it.

[0057] In the above steps, the microsphere carrier is activated to hydroxylate, which helps to form abundant hydroxyl groups on the surface of the microsphere carrier, providing reaction sites for the subsequent reaction of the silane coupling agent.

[0058] In some embodiments, the activation treatment includes acid activation or oxidative activation. Furthermore, both acid activation and oxidative activation contribute to the formation of abundant hydroxyl groups on the surface of the microsphere carrier, providing ample reaction sites for the subsequent reaction of the silane coupling agent.

[0059] Step 2: The hydroxylated microsphere carrier is reacted with a silane coupling agent to form a first interfacial layer on the surface of the microsphere carrier, and an intermediate is prepared. The intermediate is mixed with dopamine, and the dopamine is allowed to self-polymerize under weakly alkaline conditions to form a second interfacial layer on the surface of the first interfacial layer, thereby preparing a composite interfacial layer on the surface of the microsphere carrier.

[0060] In the above steps, the hydroxylated microsphere carrier is reacted with a silane coupling agent to form a first interface layer on the surface of the microsphere carrier. The silane coupling agent binds to the hydroxyl groups on the surface of the microsphere carrier through chemical bonds, which is beneficial to the formation of a stable first interface layer. The intermediate is mixed with dopamine, which allows the dopamine to self-polymerize under weakly alkaline conditions to form a second interface layer on the surface of the first interface layer. The polydopamine formed by the self-polymerization of dopamine has good adhesion and can firmly adhere to the surface of the first interface layer, which is beneficial to the preparation of a structurally stable composite interface layer on the surface of the microsphere carrier.

[0061] In some embodiments, the pH of the weakly alkaline conditions is between 8.0 and 9.0. For example, the pH of the weakly alkaline conditions can be 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, or any value within the range of any two of the above values. Furthermore, controlling the pH of the weakly alkaline conditions within the above range is beneficial for the smooth progress of the dopamine self-polymerization reaction, resulting in the formation of a uniform and stable polydopamine layer.

[0062] In some embodiments, the concentration of dopamine is from 0.5 mg / mL to 5 mg / mL, and the self-polymerization time is from 3 h to 24 h. For example, the concentration of dopamine can be 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, 3 mg / mL, 3.5 mg / mL, 4 mg / mL, 4.5 mg / mL, 5 mg / mL, or any value within the range of any two of the above values, and the self-polymerization time can be 3 h, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, or any value within the range of any two of the above values. Furthermore, controlling the concentration of dopamine and the self-polymerization time within the above ranges helps to form a second interface layer of suitable thickness on the surface of the microsphere carrier, which is beneficial for further improving the loading uniformity and binding stability of UiO-66-NH2 on the silica surface.

[0063] Step 3: Add the microsphere carrier with the composite interface layer to the reaction system containing zirconium source and 2-aminoterephthalic acid, and carry out a solvothermal reaction to form a metal-organic framework layer on the surface of the composite interface layer, thus preparing the composite gas chromatography packing.

[0064] In the above steps, the microsphere carrier with the composite interface layer is added to the reaction system containing zirconium source and 2-aminoterephthalic acid for a solvothermal reaction, forming a metal-organic framework layer on the surface of the composite interface layer. The polydopamine and silane coupling agent in the composite interface layer can provide anchoring sites for the nucleation and growth of UiO-66-NH2, which is beneficial for the uniform growth of UiO-66-NH2 on the surface of the composite interface layer. The preparation method of this application, through the above steps, helps to obtain a composite gas chromatography packing material with good interfacial bonding stability, thereby helping to solve the problem of insufficient interfacial bonding stability of metal-organic framework chromatographic packing materials.

[0065] In some embodiments, the reaction system further contains a monocarboxylic acid regulator. Furthermore, the addition of a monocarboxylic acid regulator to the reaction system can induce the formation of ligand-deficient defect sites and expose unsaturated Zr metal sites during the growth of UiO-66-NH2 crystals. This is beneficial for improving the mass transfer kinetics of gas molecules within the UiO-66-NH2 channels, and by improving interfacial bonding stability, it further enhances the separation efficiency and selectivity of the composite gas chromatography packing material.

[0066] In some embodiments, the monocarboxylic acid modifier includes one or more of formic acid, acetic acid, trifluoroacetic acid, benzoic acid, a mixture of trifluoroacetic acid and acetic acid, and a mixture of formic acid and acetic acid. The above-mentioned monocarboxylic acid modifiers have strong coordination ability and can compete with the zirconium source for coordination, which is beneficial for the formation of controllable defect sites in UiO-66-NH2.

[0067] In some embodiments, the molar ratio of the monocarboxylic acid modifier to 2-aminoterephthalic acid is from 5:1 to 2000:1. For example, the molar ratio of the monocarboxylic acid modifier to 2-aminoterephthalic acid can be 5:1, 50:1, 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, 1000:1, 1100:1, 1200:1, 1300:1, 1400:1, 1500:1, 1600:1, 1700:1, 1800:1, 1900:1, 2000:1, or any value within the range of any two of the above values. Furthermore, controlling the molar ratio of monocarboxylic acid regulator to 2-aminoterephthalic acid within the above range helps to form an appropriate number of defect sites in UiO-66-NH2, thereby balancing skeletal integrity and mass transfer efficiency.

[0068] In some embodiments, the molar ratio of zirconium source to 2-aminoterephthalic acid is from 1:1 to 8:1. For example, the molar ratio of zirconium source to 2-aminoterephthalic acid can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 6:1, 7:1, 8:1, or any value within the range of any two of the above values. Furthermore, controlling the molar ratio of zirconium source to 2-aminoterephthalic acid within the above range helps to introduce an appropriate number of defect sites and exposed unsaturated Zr metal sites while ensuring the formation of the UiO-66-NH2 framework. This is beneficial for balancing framework stability and gas mass transfer efficiency, and further optimizing the separation performance of the composite gas chromatography packing material.

[0069] In some embodiments, the reaction solvent in the solvothermal reaction includes one or more of N,N-dimethylformamide, ethanol, water, and methanol. These solvents facilitate the dissolution and reaction of the zirconium source and 2-aminoterephthalic acid, thereby promoting the uniform nucleation and growth of UiO-66-NH2.

[0070] In some embodiments, the temperature of the solvothermal reaction is 90°C to 150°C, and the time is 4 h to 36 h. For example, the temperature of the solvothermal reaction can be 90°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or any value within the range of any two of the above values, and the time can be 4 h, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, or any value within the range of any two of the above values. Furthermore, controlling the temperature and time of the solvothermal reaction within the above ranges is beneficial for the uniform growth of UiO-66-NH2 on the surface of the composite interface layer, forming a continuous and stable metal-organic framework layer, thereby further improving the structural stability and separation performance of the composite gas chromatography packing material.

[0071] In some embodiments, after the solvothermal reaction, the preparation method further includes a solvent replacement step using an organic solvent. In some embodiments, the organic solvent includes one or more of ethanol, methanol, acetone, and acetonitrile. Further, solvent replacement using the aforementioned organic solvent after the solvothermal reaction helps to remove residual N,N-dimethylformamide and unreacted monocarboxylic acid modifiers from the UiO-66-NH2 channels, further improving the channel openness and accessibility of active sites.

[0072] In some embodiments, the replacement time is from 12 h to 72 h. For example, the replacement time can be 12 h, 18 h, 24 h, 30 h, 36 h, 42 h, 48 h, 54 h, 60 h, 66 h, 72 h, or any value within the range of any two of the above values. Furthermore, controlling the replacement time within the above range is beneficial for reducing the adverse effects on the composite interface layer structure when the replacement time is longer, while ensuring sufficient removal of residues, thereby further improving the chromatographic separation performance and reusability stability of the composite gas chromatography packing material.

[0073] In some embodiments, the preparation method further includes a drying step after the solvothermal reaction. Further, drying after the solvothermal reaction helps remove residual solvent within the pores, exposes the defect sites and amino interaction sites of UiO-66-NH2, and simultaneously helps maintain the structural integrity of the composite interface layer.

[0074] In some embodiments, the drying temperature is 60°C to 150°C, and the drying time is 6 h to 24 h. For example, the drying temperature can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or any value within the range of any two of the above values, and the drying time can be 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, or any value within the range of any two of the above values. Furthermore, controlling the drying temperature and drying time within the above ranges is beneficial for further improving the separation performance and thermal stability of the composite gas chromatography packing material while ensuring sufficient activation.

[0075] An embodiment of this application also provides a gas chromatography column, including a column tube and a gas chromatography packing material packed inside the column tube. The gas chromatography packing material includes the above-described composite gas chromatography packing material or the composite gas chromatography packing material prepared by the above-described preparation method.

[0076] In this application, the composite gas chromatography packing material has improved interfacial bonding stability. The gas chromatography column packed with this composite gas chromatography packing material can maintain column bed stability during packing and use, and reduce the risk of column pressure fluctuations and separation performance degradation caused by packing material shedding or migration, thereby improving the service life of the chromatographic column and the reproducibility of detection results.

[0077] One embodiment of this application also provides the application of the above-described gas chromatography column in the separation and detection of dissolved gases in transformer oil.

[0078] In this application, the composite gas chromatography packing material packed in the gas chromatography column has a multi-level structure with microsphere carrier, composite interface layer and metal-organic framework layer arranged in sequence. The metal-organic framework layer is indirectly bound to the microsphere carrier through the composite interface layer, which helps to enhance the stability of the interface binding and reduce the risk of the metal-organic framework layer falling off during carrier gas scouring and column aging. Therefore, when this gas chromatography column is used for the separation and detection of dissolved gases in transformer oil, it is beneficial to maintain the stability of the column bed during packing and use, reduce the risk of separation performance degradation caused by packing material falling off or migrating, and thus improve the reproducibility and reliability of the separation and detection of dissolved gases in transformer oil.

[0079] In some embodiments, the dissolved gas includes one or more of H2, CO, CO2, CH4, C2H4, C2H2, and C2H6. Furthermore, when the UiO-66-NH2 in the composite gas chromatograph packing has ligand-deficient defect sites and exposed unsaturated Zr metal sites, and its framework contains functional groups such as amino groups, it is beneficial to achieve differentiated adsorption and retention of gases such as H2, CO, CO2, CH4, C2H4, C2H2, and C2H6. Therefore, it is advantageous to further achieve the separation and detection of one or more of the above-mentioned characteristic gases, meeting the requirements for multi-component separation in the analysis of dissolved gases in transformer oil.

[0080] The present application will be described below through specific embodiments and comparative examples. Those skilled in the art should understand that the preparation methods described in this application are merely examples, and any other suitable preparation methods are within the scope of this application.

[0081] Example 1:

[0082] A composite gas chromatography packing material, the preparation method of which is as follows:

[0083] Step 1: Add 5.0 g of porous silica microspheres to a 10% hydrochloric acid solution and reflux at 80°C for 4 h. Wash with deionized water until neutral, then wash with ethanol and vacuum dry at 60°C for 12 h to obtain hydroxylated silica microspheres.

[0084] Step 2: Add the above hydroxylated silica microspheres to 100 mL of anhydrous toluene, sonicate for 30 min, add 5 mL of 3-aminopropyltriethoxysilane, react at 90 °C for 12 h under nitrogen protection, wash with toluene, ethanol and deionized water in sequence, and dry under vacuum at 60 °C to obtain silanized silica microspheres with a first interface layer on the surface.

[0085] Step 3: Prepare a Tris-HCl buffer solution with a pH of 8.5, dissolve dopamine hydrochloride in it to make the dopamine concentration 2 mg / mL; take 2.0 g of the above silanized silica microspheres and add them to the dopamine solution, stir at room temperature for 6 h to allow dopamine to self-polymerize and deposit on the surface of the silanized silica microspheres, collect the solid by centrifugation, wash with deionized water and ethanol to obtain silica microspheres with a composite interface layer.

[0086] Step 4: Add 1.0 mmol ZrCl4, 0.5 mmol 2-aminoterephthalic acid, and 10 mL acetic acid to 80 mL N,N-dimethylformamide, stir to dissolve, then add 1.0 g of the above-mentioned silica microspheres with composite interface layer, sonicate for 20 min, transfer to a reaction vessel, and react at 120℃ for 12 h; after the reaction is completed, cool to room temperature, centrifuge to collect the solid, wash with N,N-dimethylformamide and ethanol in sequence, and replace with ethanol for 24 h, and finally dry under vacuum at 80℃ to obtain the composite gas chromatography packing material.

[0087] Example 2:

[0088] The difference from Example 1 is that the amount of acetic acid used is 5 mL, while the rest of the steps are basically the same as in Example 1.

[0089] Example 3:

[0090] The difference from Example 1 is that the amount of acetic acid used is 20 mL, while the rest of the steps are basically the same as in Example 1.

[0091] Example 4:

[0092] The difference from Example 1 is that the amount of acetic acid used is 40 mL, while the rest of the steps are basically the same as in Example 1.

[0093] Example 5:

[0094] The difference from Example 1 is that acetic acid is replaced with trifluoroacetic acid, and the amount of trifluoroacetic acid used is 10 mL. The remaining steps are basically the same as in Example 1.

[0095] Example 6:

[0096] The difference from Example 1 is that acetic acid is replaced with trifluoroacetic acid, and the amount of trifluoroacetic acid used is 30 mL. The remaining steps are basically the same as in Example 1.

[0097] Example 7:

[0098] The difference from Example 1 is that acetic acid is replaced with trifluoroacetic acid, and the amount of trifluoroacetic acid used is 60 mL. The remaining steps are basically the same as in Example 1.

[0099] Example 8:

[0100] The difference from Example 1 is that the regulator is a mixture of acetic acid and trifluoroacetic acid, with 5 mL of acetic acid and 1 mL of trifluoroacetic acid. The remaining steps are basically the same as in Example 1.

[0101] Example 9:

[0102] The difference from Example 1 is that the regulator is a mixture of acetic acid and trifluoroacetic acid, with 15 mL of acetic acid and 10 mL of trifluoroacetic acid. The remaining steps are basically the same as in Example 1.

[0103] Example 10:

[0104] The difference from Example 1 is that the regulator is a mixture of acetic acid and trifluoroacetic acid, with 30 mL of acetic acid and 20 mL of trifluoroacetic acid used. The remaining steps are basically the same as in Example 1.

[0105] Example 11:

[0106] The difference from Example 1 is that the amount of 3-aminopropyltriethoxysilane used in the second step is 1 mL, while the rest of the steps are basically the same as in Example 1.

[0107] Example 12:

[0108] The difference from Example 1 is that the amount of 3-aminopropyltriethoxysilane used in the second step is 3 mL, while the rest of the steps are basically the same as in Example 1.

[0109] Example 13:

[0110] The difference from Example 1 is that the amount of 3-aminopropyltriethoxysilane used in the second step is 8 mL, while the rest of the steps are basically the same as in Example 1.

[0111] Example 14:

[0112] The difference from Example 1 is that the amount of 3-aminopropyltriethoxysilane used in the second step is 10 mL, while the rest of the steps are basically the same as in Example 1.

[0113] Example 15:

[0114] The difference from Example 1 is that the dopamine concentration in the third step is 0.5 mg / mL, the polymerization time is 12 h, and the remaining steps are basically the same as in Example 1.

[0115] Example 16:

[0116] The difference from Example 1 is that the dopamine concentration in the third step is 1 mg / mL and the polymerization time is 12 h, while the remaining steps are basically the same as in Example 1.

[0117] Example 17:

[0118] The difference from Example 1 is that the dopamine concentration in the third step is 3 mg / mL and the polymerization time is 12 h, while the remaining steps are basically the same as in Example 1.

[0119] Example 18:

[0120] The difference from Example 1 is that the dopamine concentration in the third step is 5 mg / mL and the polymerization time is 12 h, while the remaining steps are basically the same as in Example 1.

[0121] Example 19:

[0122] The difference from Example 1 is that in the fourth step, the amount of ZrCl4 used is 2.0 mmol, the amount of 2-aminoterephthalic acid used is kept at 0.5 mmol, and the remaining steps are basically the same as in Example 1.

[0123] Example 20:

[0124] The difference from Example 1 is that in the fourth step, the amount of ZrCl4 used is 1.5 mmol, the amount of 2-aminoterephthalic acid used is kept at 0.5 mmol, and the remaining steps are basically the same as in Example 1.

[0125] Example 21:

[0126] The difference from Example 1 is that in the fourth step, the amount of ZrCl4 used is 3.0 mmol, the amount of 2-aminoterephthalic acid used is kept at 0.5 mmol, and the remaining steps are basically the same as in Example 1.

[0127] Example 22:

[0128] The difference from Example 1 is that in the fourth step, the amount of ZrCl4 used is 4.0 mmol, the amount of 2-aminoterephthalic acid used is kept at 0.5 mmol, and the remaining steps are basically the same as in Example 1.

[0129] Example 23:

[0130] The difference from Example 1 is that in the fourth step, the amount of 2-aminoterephthalic acid used is 0.25 mmol, the amount of ZrCl4 used is kept at 2.0 mmol, and the remaining steps are basically the same as in Example 1.

[0131] Example 24:

[0132] The difference from Example 1 is that in the fourth step, the amount of 2-aminoterephthalic acid used is 0.75 mmol, the amount of ZrCl4 used is kept at 2.0 mmol, and the remaining steps are basically the same as in Example 1.

[0133] Example 25:

[0134] The difference from Example 1 is that in the fourth step, the amount of 2-aminoterephthalic acid used is 1.0 mmol, the amount of ZrCl4 used is kept at 2.0 mmol, and the remaining steps are basically the same as in Example 1.

[0135] Example 26:

[0136] The difference from Example 1 is that in the fourth step, the amount of 2-aminoterephthalic acid used is 2 mmol, the amount of ZrCl4 used is kept at 2.0 mmol, and the remaining steps are basically the same as in Example 1.

[0137] Example 27:

[0138] The difference from Example 1 is that the solvothermal reaction temperature in the fourth step is 90°C, while the remaining steps are basically the same as in Example 1.

[0139] Example 28:

[0140] The difference from Example 1 is that the solvothermal reaction temperature in the fourth step is 100°C, while the remaining steps are basically the same as in Example 1.

[0141] Example 29:

[0142] The difference from Example 1 is that the solvothermal reaction temperature in the fourth step is 140°C, while the remaining steps are basically the same as in Example 1.

[0143] Example 30:

[0144] The difference from Example 1 is that the solvothermal reaction temperature in the fourth step is 150°C, while the remaining steps are basically the same as in Example 1.

[0145] Example 31:

[0146] The difference from Example 1 is that the solvothermal reaction time in the fourth step is 4 hours, while the remaining steps are basically the same as in Example 1.

[0147] Example 32:

[0148] The difference from Example 1 is that the solvothermal reaction time in the fourth step is 8 hours, while the remaining steps are basically the same as in Example 1.

[0149] Example 33:

[0150] The difference from Example 1 is that the solvothermal reaction time in the fourth step is 18 h, while the remaining steps are basically the same as in Example 1.

[0151] Example 34:

[0152] The difference from Example 1 is that the solvothermal reaction time in the fourth step is 24 h, while the remaining steps are basically the same as in Example 1.

[0153] Example 35:

[0154] The difference from Example 1 is that the solvothermal reaction time in the fourth step is 36 h, while the remaining steps are basically the same as in Example 1.

[0155] Example 36:

[0156] The difference from Example 1 is that methanol was used for solvent replacement after the fourth step reaction was completed, and the replacement time was 24 hours. The remaining steps were basically the same as in Example 1.

[0157] Example 37:

[0158] The difference from Example 1 is that acetone was used for solvent replacement after the fourth step reaction was completed, and the replacement time was 24 hours. The remaining steps were basically the same as in Example 1.

[0159] Example 38:

[0160] The difference from Example 1 is that acetonitrile was used for solvent replacement after the fourth step reaction was completed, and the replacement time was 24 hours. The remaining steps were basically the same as in Example 1.

[0161] Example 39:

[0162] The difference from Example 1 is that the final vacuum drying temperature in the fourth step is 60°C and the drying time is 12 hours. The remaining steps are basically the same as in Example 1.

[0163] Example 40:

[0164] The difference from Example 1 is that the final vacuum drying temperature in the fourth step is 100°C and the drying time is 12 hours. The remaining steps are basically the same as in Example 1.

[0165] Example 41:

[0166] The difference from Example 1 is that the final vacuum drying temperature in the fourth step is 120°C and the drying time is 12 hours. The remaining steps are basically the same as in Example 1.

[0167] Example 42:

[0168] The difference from Example 1 is that the final vacuum drying temperature in the fourth step is 150°C and the drying time is 12 hours. The remaining steps are basically the same as in Example 1.

[0169] Example 43:

[0170] The difference from Example 1 is that no monocarboxylic acid regulator is added in the fourth step, while the remaining steps are basically the same as in Example 1.

[0171] Comparative Example 1:

[0172] A UiO-66-NH2 powder filler, the preparation method of which is as follows:

[0173] Step 1: Add 1.0 mmol ZrCl4, 0.5 mmol 2-aminoterephthalic acid, and 10 mL acetic acid to 80 mL N,N-dimethylformamide and stir to dissolve.

[0174] Step 2: Transfer the mixture to a reaction vessel and react at 120°C for 12 hours.

[0175] Step 3: After the reaction is complete, cool to room temperature, centrifuge to collect the solid, wash with N,N-dimethylformamide and ethanol in sequence, replace with ethanol for 24 h, and finally dry under vacuum at 80℃ to obtain UiO-66-NH2 powder.

[0176] Comparative Example 2:

[0177] A composite gas chromatography packing material, the preparation method of which is as follows:

[0178] Step 1: Take 1.0 mmol ZrCl4, 0.5 mmol 2-aminoterephthalic acid and 10 mL acetic acid and add them to 80 mL N,N-dimethylformamide. Stir to dissolve and react at 120℃ for 12 h. Centrifuge, wash and dry to obtain UiO-66-NH2 powder.

[0179] Step 2: Take 5.0 g of porous silica microspheres and physically mix them with the above UiO-66-NH2 powder at a mass ratio of 1:1 to obtain a composite gas chromatography packing.

[0180] Please refer to the preparation process of the composite gas chromatography packing materials provided in Examples 1-42 of this application. Figure 1 . Figure 1In this example, porous silica microspheres are acid-activated to hydroxylate their surface, resulting in hydroxylated silica microspheres, which serve as microsphere carriers for composite gas chromatography packing. The hydroxylated silica microspheres are then reacted with 3-aminopropyltriethoxysilane, where the silane coupling agent chemically bonds with the hydroxyl groups on the microsphere carrier surface, forming a first interfacial layer and yielding silanized silica microspheres. The silanized silica microspheres are then added to a weakly alkaline buffer solution containing dopamine. Under these weakly alkaline conditions, dopamine undergoes self-polymerization and deposits on the surface of the first interfacial layer, forming a second interfacial layer. This results in a composite interfacial layer on the microsphere carrier surface, composed of the first and second interfacial layers. Finally, the microspheres with the composite interfacial layer are added to a reaction system containing a zirconium source, 2-aminoterephthalic acid, and a monocarboxylic acid regulator for a solvothermal reaction. UiO-66-NH2 nucleates and grows in situ on the surface of the composite interfacial layer, forming a metal-organic framework layer. Therefore, the composite gas chromatography packing material obtained in Example 1 has a multi-level composite structure from the inside out: a microsphere carrier including silica as the core, with a first interface layer, a second interface layer, and a metal-organic framework layer sequentially disposed on the surface of the microsphere carrier; wherein, the first interface layer includes a silane coupling agent and is located on the surface of the microsphere carrier, the second interface layer includes polydopamine and is located on the surface of the first interface layer, and the metal-organic framework layer includes UiO-66-NH2 and is located on the surface of the second interface layer. The microsphere carrier and the metal-organic framework layer are indirectly bonded through the composite interface layer. The silane coupling agent in the composite interface layer helps to form a stable first interface layer on the surface of the microsphere carrier, and the polydopamine helps to firmly adhere to the surface of the first interface layer and provide anchoring points for UiO-66-NH2, thereby helping to enhance the interfacial bonding stability between the metal-organic framework layer and the microsphere carrier.

[0181] In this application, the composite gas chromatography packing materials obtained in Examples 1-43 above, as well as the packing materials provided in Comparative Examples 1 and 2, were respectively packed into gas chromatography columns, and their separation performance was tested under the same chromatographic conditions (high-purity argon was used as the carrier gas, and the column temperature was programmed).

[0182] Please see Figure 2 Taking Example 3 as an example, the powder X-ray diffraction pattern of UiO-66-NH2 in the composite gas chromatograph packing obtained in Example 3 shows characteristic diffraction peaks corresponding to the topological structure of UiO-66 around 2θ of 7° to 8°, indicating that a UiO-66-NH2 crystal structure was formed on the composite interface layer on the surface of silica microspheres.

[0183] Please see Figure 3 Taking Example 3 as an example, the infrared spectrum of UiO-66-NH2 in the composite gas chromatograph packing material obtained in Example 3 is at approximately 3400 cm⁻¹. -1 Up to 3500 cm -1Absorption occurs at approximately 1650 cm⁻¹ due to the NH stretching vibration of the amino group. -1 Absorption occurs at approximately 1250 cm⁻¹ due to the C=O stretching vibration of the ligand's carboxylic acid group. -1 Up to 1350 cm -1 The presence of CN stretching vibration absorption at this location indicates that the 2-aminoterephthalic acid ligand has been successfully introduced into the UiO-66-NH2 framework; simultaneously, at approximately 600 cm⁻¹... -1 Up to 700 cm -1 The characteristic absorption of Zr-O bonds at the location indicates that the zirconium metal cluster has formed a coordination structure with the ligand.

[0184] Please see Figure 4 Taking Example 3 as an example, the scanning electron microscope image of the composite gas chromatography packing obtained in Example 3 shows that UiO-66-NH2 crystals are uniformly distributed in the form of particles on the surface of the microsphere carrier. The crystal particles are interconnected to form a continuous metal-organic framework layer, indicating that the composite interface layer is conducive to the uniform nucleation and growth of UiO-66-NH2 on the surface of the microsphere carrier and helps to improve the interfacial bonding stability between the metal-organic framework layer and the microsphere carrier.

[0185] Please see Figure 5 and Figure 6 Taking Examples 3 and 43 as examples, the defective composite packing material obtained in Example 3 and the composite packing material obtained in Example 43 were packed into a gas chromatography column. Under the conditions of high-purity argon as the carrier gas and programmed column temperature, a standard mixed gas containing H2, CO, CO2, CH4, C2H4, C2H2 and C2H6 was introduced for separation and testing. The chromatogram showed that the seven characteristic gases eluted in sequence, and the components were separated. Moreover, the column pressure of the chromatographic column packed with the packing material obtained in Example 3 was stable, and the RSD of the retention time after multiple injections was small, indicating that the composite gas chromatography packing material of this application is beneficial to meeting the separation and detection requirements of dissolved gases in transformer oil.

[0186] This application also analyzes the separation effect of the above-mentioned gas chromatography columns on dissolved characteristic gases in transformer oil, and the analysis results are as follows:

[0187] According to Examples 1-4, as the amount of acetic acid increased, the crystal size of UiO-66-NH2 decreased, while the number of defect sites increased. Medium-defect packing materials exhibited both good mass transfer efficiency and separation selectivity; while high-defect packing materials had more adsorption sites, excessive defects could lead to a decrease in local structural order. In Examples 5-7, the monocarboxylic acid regulator was replaced with trifluoroacetic acid, resulting in a looser UiO-66-NH2 layer on the surface of the packing material, exposing more defect sites. In Examples 8-10, the monocarboxylic acid regulator was replaced with a mixture of acetic acid and trifluoroacetic acid. Acetic acid and trifluoroacetic acid synergistically regulated the nucleation, growth, and defect formation processes of UiO-66-NH2 crystals, resulting in a composite packing material with both a high number of defect sites and good framework stability. In Example 43, no monocarboxylic acid regulator was added, and its UiO-66-NH2 did not have ligand-deficient defect sites induced by the monocarboxylic acid regulator. Compared to Example 3, the packing material obtained in Example 43 showed more pronounced peak tailing for CO2 and acetylene, indicating that defect regulation helps improve peak shape and mass transfer performance.

[0188] According to Examples 1 and 11-14, as the amount of 3-aminopropyltriethoxysilane increases, the amino density on the surface of the silica microspheres increases, which is beneficial for subsequent polydopamine deposition and UiO-66-NH2 crystal anchoring. A suitable degree of amination can improve the uniformity and solvent resistance of the MOF layer.

[0189] According to Examples 1 and 15-18, the thickness of the polydopamine interface layer on the silica microsphere surface increases with increasing dopamine concentration and polymerization time. An appropriately thick polydopamine layer is beneficial for improving the loading uniformity and bonding stability of UiO-66-NH2 on the silica surface.

[0190] According to Examples 1 and 19-22, as the amount of ZrCl4 increases, the concentration of metal nodes in the system increases, and the number of UiO-66-NH2 nucleation sites on the surface of silica microspheres increases. Appropriately increasing the amount of ZrCl4 can increase the MOF loading and the number of surface active sites.

[0191] According to Examples 23-26, with the increase of 2-aminoterephthalic acid content, the UiO-66-NH2 framework becomes more complete, and the crystal order is enhanced. Lower ligand content is beneficial for the formation of defect sites, while higher ligand content is beneficial for improving framework integrity. By adjusting the ligand content, the degree of defect, pore structure, and separation selectivity of the composite packing can be synergistically regulated.

[0192] According to Examples 1, 27-30, the nucleation and growth rate of UiO-66-NH2 crystals accelerated with increasing reaction temperature. A suitable temperature is beneficial for forming a uniform and continuous MOF coating layer.

[0193] According to Examples 1 and 31-35, the loading of UiO-66-NH2 on the surface of silica microspheres gradually increases with increasing reaction time. A suitable reaction time can yield a uniform and stable MOF layer; too short a reaction time results in insufficient MOF growth, while too long a reaction time may lead to crystal agglomeration or pore blockage.

[0194] According to Examples 1 and 36-38, different solvent replacement methods can affect the removal efficiency of residual DMF and regulators in MOF channels. Appropriately extending the replacement time is beneficial to improving the channel openness and chromatographic separation performance. The packing material after sufficient replacement exhibits good thermal stability, low leaching, and reusability stability.

[0195] According to Examples 1, 39-42, appropriately increasing the activation drying temperature helps to remove residual solvent in the pores and expose UiO-66-NH2 defect sites and amino interaction sites.

[0196] For comparison with embodiments 1-43 of this application, please refer to Figure 7 Comparative Example 1 used pure UiO-66-NH2 powder to directly pack the chromatographic column without setting up silica microsphere carrier, silane coupling agent layer and polydopamine layer, which resulted in large column pressure fluctuations, large retention time RSD after multiple injections and poor separation reproducibility.

[0197] Compared to embodiments 1 to 43 of this application, please refer to Figure 8 In Comparative Example 2, UiO-66-NH2 powder was simply physically mixed with silica microspheres without the addition of a silane coupling agent layer and a polydopamine layer. This resulted in weak interfacial bonding between the MOF layer and the support, making the MOF layer prone to detachment during carrier gas scouring and column aging, leading to a rapid decline in separation performance.

[0198] The comparative examples above show that this application anchors UiO-66-NH2 on the surface of silica microspheres through a composite interface layer, and with the addition of defect control, it is beneficial to improve the packing stability, interfacial bonding stability and separation reproducibility of the filler.

[0199] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0200] The embodiments described above are merely illustrative of several implementations of the technical solution of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the technical solution of this application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the inventive concept of this application, and these modifications and improvements all fall within the protection scope of this application. Therefore, the protection scope of this application should be determined by the appended claims.

Claims

1. A composite gas chromatography packing material, characterized in that, The composite gas chromatography packing material includes a microsphere carrier, a composite interface layer, and a metal-organic framework layer; The microsphere carrier comprises silica; The composite interface layer includes a first interface layer located on the surface of the microsphere carrier and a second interface layer located on the surface of the first interface layer. The first interface layer includes a silane coupling agent, and the second interface layer includes polydopamine. The metal-organic framework layer is located on the surface of the second interface layer, and the metal-organic framework layer comprises UiO-66-NH2.

2. The composite gas chromatography packing material as described in claim 1, characterized in that, The UiO-66-NH2 in the metal-organic framework layer has ligand-deficient defect sites and exposed unsaturated Zr metal sites.

3. The composite gas chromatography packing material as described in claim 1, characterized in that, The silane coupling agent includes an amino-containing silane coupling agent; Optionally, the amino-containing silane coupling agent includes one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and N-β-aminoethyl-γ-aminopropyltrimethoxysilane.

4. The composite gas chromatography packing material according to any one of claims 1 to 3, characterized in that, The composite gas chromatography packing material satisfies at least one of the following conditions: (1) The particle size of the microsphere carrier is 1 μm to 10 μm; (2) The microsphere carrier has a porous structure with a pore size of 5 nm to 30 nm; (3) The thickness of the composite interface layer is 5 nm to 50 nm; (4) In the composite interface layer, the thickness ratio of the first interface layer to the second interface layer is 1:20 to 1:2; (5) The thickness of the metal-organic framework layer is 30 nm to 300 nm.

5. A method for preparing a composite gas chromatography packing material according to any one of claims 1 to 4, characterized in that, Includes the following steps: The microsphere carrier is activated to hydroxylate it. The hydroxylated microsphere carrier is reacted with the silane coupling agent to form the first interface layer on the surface of the microsphere carrier, thereby preparing an intermediate. The intermediate is mixed with dopamine, and the dopamine is allowed to self-polymerize under weakly alkaline conditions to form the second interface layer on the surface of the first interface layer, thereby preparing the composite interface layer on the surface of the microsphere carrier. The microsphere carrier having the composite interface layer is added to a reaction system containing zirconium source and 2-aminoterephthalic acid, and a solvothermal reaction is carried out to form the metal-organic framework layer on the surface of the composite interface layer, thus preparing the composite gas chromatography packing.

6. The preparation method according to claim 5, characterized in that, The reaction system also contains a monocarboxylic acid regulator; Optionally, the monocarboxylic acid modifier includes one or more of formic acid, acetic acid, trifluoroacetic acid, benzoic acid, a mixture of trifluoroacetic acid and acetic acid, and a mixture of formic acid and acetic acid; Optionally, the molar ratio of the monocarboxylic acid modifier to 2-aminoterephthalic acid is from 5:1 to 2000:1; Optionally, the molar ratio of the zirconium source to 2-aminoterephthalic acid is from 1:1 to 8:

1.

7. The preparation method according to claim 5 or 6, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The activation treatment includes acid activation or oxidative activation; (2) The pH of the weakly alkaline conditions is 8.0 to 9.0; (3) The concentration of the dopamine is 0.5 mg / mL to 5 mg / mL, and the self-polymerization time is 3 h to 24 h; (4) The reaction solvent in the solvothermal reaction includes one or more of N,N-dimethylformamide, ethanol, water and methanol; (5) The temperature of the solvothermal reaction is 90°C to 150°C, and the time is 4 h to 36 h; (6) After the solvothermal reaction, the preparation method further includes: a step of solvent replacement using an organic solvent; optionally, the organic solvent includes one or more of ethanol, methanol, acetone and acetonitrile; optionally, the replacement time is 12 h to 72 h. (7) After the solvothermal reaction, the preparation method further includes a drying step; optionally, the drying temperature is 60°C to 150°C and the drying time is 6 h to 24 h.

8. A gas chromatography column, characterized in that, The invention includes a column and a gas chromatography packing material packed within the column, wherein the gas chromatography packing material includes a composite gas chromatography packing material as described in any one of claims 1 to 4 or a composite gas chromatography packing material prepared according to the preparation method as described in any one of claims 5 to 7.

9. The application of the gas chromatography column as described in claim 8 in the separation and detection of dissolved gases in transformer oil.

10. The application as described in claim 9, characterized in that, The dissolved gas includes one or more of H2, CO, CO2, CH4, C2H4, C2H2, and C2H6.