A co-based catalyst, its preparation method and use

By using biomass carbon-modified supports to support Co-based catalysts, the problems of high cost and environmental unfriendliness of hydroformylation heterogeneous catalysts have been solved, achieving efficient and stable olefin hydroformylation reactions and promoting industrial applications.

CN123059673APending Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510585838.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing hydroformylation heterogeneous catalysts require the use of precious metals and phosphine-containing ligands, which are costly and environmentally unfriendly, making it difficult to meet industrial needs.

Method used

Co-based catalysts, including Co, Co2C, and CoO, are supported on biomass carbon-modified carriers. Through modification with biomass materials such as alginate, active metal Co and auxiliary metals are loaded, avoiding the use of precious metals and phosphine-containing ligands.

Benefits of technology

It reduces catalyst costs, improves catalytic activity and stability, and is suitable for olefin hydroformylation reactions, showing promising prospects for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123059673A_ABST
    Figure CN123059673A_ABST
Patent Text Reader

Abstract

The application provides a Co-based catalyst and a preparation method and application thereof. The Co-based catalyst comprises a biomass carbon modified carrier, active metal Co and an auxiliary metal; the active metal Co and the auxiliary metal are loaded on the biomass carbon modified carrier; the active metal Co exists in the catalyst in the form of Co, Co2C and CoO, wherein the mass ratio of Co, Co2C and CoO is (52-75):(1-7):(18-47). The Co-based catalyst provided by the application does not need to use noble metal as an active component, nor does it need to use an expensive phosphorus-containing organic ligand, so that the cost of the catalyst can be reduced, and the catalyst is environmentally friendly; and the Co-based catalyst has good catalytic performance and stability for olefin hydroformylation, and has a wide industrial application prospect in the field of olefin hydroformylation, especially olefin hydroformylation heterogeneous catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst technology, specifically relating to a Co-based catalyst, its preparation method, and its application. Background Technology

[0002] Hydroformylation is a reaction that produces aldehydes from olefins and syngas. It is environmentally friendly and 100% atom-economical. Currently, the annual production of aldehydes via hydroformylation exceeds 10 million tons. The resulting aldehydes can serve as important intermediates for the synthesis of various fine chemicals, such as alcohols, amines, and carboxylic acids, through one-step or multi-step reactions.

[0003] In my country, industrial hydroformylation reactions still primarily utilize homogeneous catalysts based on rhodium-phosphine complexes. While these catalysts exhibit high activity and selectivity, subsequent separation and processing are challenging and costly, especially in long-chain olefin reactions. Compared to homogeneous hydroformylation catalysts, heterogeneous hydroformylation catalysts offer the advantage of easy separation and typically employ noble metals (such as Pt, Pd, and Rh) supported on a solid-phase support. Bell et al. (ACS Catalysis. 2013, 3, 348-357) prepared various organophosphine ligand-modified Rh single-metal heterogeneous catalysts using SiO2 as a support and successfully applied these catalysts to the hydroformylation of propylene. To further improve the efficiency of the hydroformylation reaction, Wang et al. (Catalysts, 2017, 7:103) prepared a bimetallic heterogeneous catalyst of Rh and Co using Fe3O4 as a support. The addition of the promoter metal Co to this catalyst improved the dispersion of the main active component Rh, thus exhibiting good conversion and selectivity from dicyclopentadiene to diformyltricyclodecane with the assistance of organophosphorus ligands. However, this catalyst not only requires the use of expensive noble metals as active components, but also necessitates the introduction of costly phosphorus-containing ligands during preparation, making the process cumbersome. Furthermore, the phosphorus-containing waste generated during preparation and use is environmentally unfriendly. These problems significantly restrict the industrial development of hydroformylation heterogeneous catalysts.

[0004] Therefore, it is very important to develop non-precious metal heterogeneous catalysts for hydroformylation and various heterogeneous catalytic reactions in petrochemicals without using phosphine-containing ligands. Summary of the Invention

[0005] Based on the above analysis, the present invention aims to provide a Co-based catalyst, its preparation method, and its application, in order to solve the technical problems of existing hydroformylation heterogeneous catalysts, which require the use of precious metals and phosphine-containing ligands for preparation, resulting in high costs and environmentally unfriendly phosphorus waste.

[0006] The objective of this invention is mainly achieved through the following technical solutions.

[0007] In a first aspect, the present invention provides a Co-based catalyst, comprising a biomass carbon-modified support, an active metal Co, and an auxiliary metal; wherein the active metal Co and the auxiliary metal are supported on the biomass carbon-modified support; wherein the active metal Co exists in the catalyst in the forms of Co, Co2C, and CoO, wherein the mass ratio of Co, Co2C, and CoO is (52-75):(1-7):(18-47), preferably (52-73):(1-5):(22-47).

[0008] The catalyst provided by this invention uses a biomass carbon-modified support, which can not only serve as a support for loading active metal Co and auxiliary metals, but also provide a carbon source, thereby improving catalytic efficiency.

[0009] The active metal Co in the catalyst provided by this invention exists in the forms of Co, Co2C, and CoO simultaneously. Furthermore, if the mass ratio of Co, Co2C, and CoO in the catalyst is (52-75):(1-7):(18-47), especially if the mass ratio is (52-73):(1-5):(22-47), the catalyst can have higher catalytic activity, which is beneficial to improving the conversion rate of reactants.

[0010] According to some embodiments of the present invention, the biomass includes at least one of agarose, pectin (e.g., natural polysaccharide uronic acid pectin), gelatin, chitosan, alginic acid, cellulose, lignin, chitin and its derivatives, preferably alginic acid.

[0011] Alginic acid (C6H8O6) n Co is a natural high-molecular-weight polysaccharide and a major component of seaweed cell walls and intercellular matrix. In addition to its high biocompatibility and good biodegradability, it can also react rapidly with divalent or polyvalent metal cations. Using it to modify solid-phase supports with carbon can effectively interact with active metal Co and auxiliary metals, which is beneficial for the efficient loading of active metal Co and auxiliary metals, thereby improving the catalytic activity and stability of the catalyst.

[0012] In this invention, compared with other types of biomass, carbon modification of the solid support using alginic acid can give the prepared catalyst better catalytic performance and stability.

[0013] According to some embodiments of the present invention, the biomass carbon-modified carrier is obtained by carbon modification of a solid carrier with biomass. Specifically, this refers to modifying the solid carrier with biomass so that the carbon components in the biomass are retained on the solid carrier. For example, biomass is first loaded onto the solid carrier, and then in a subsequent process, high-temperature calcination is used to convert the biomass into carbon components that are retained on the solid carrier.

[0014] According to some embodiments of the present invention, the solid support includes at least one of oxides and molecular sieves.

[0015] According to some embodiments of the present invention, the solid support comprises Al2O3.

[0016] According to some embodiments of the present invention, the solid support comprises γ-Al2O3.

[0017] According to some embodiments of the present invention, the particle size of the solid support is ≤100μm and the specific surface area is ≥200m². 2 / g.

[0018] According to some embodiments of the present invention, the particle size of the solid support is 30–100 μm, and the specific surface area is 200–250 m². 2 / g.

[0019] According to some embodiments of the present invention, the mass ratio of biomass to solid carrier is 1:(0.1 to 10) (for example, it can be 1:0.1, 1:0.2, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, and any value within the range formed by any two of these point values), preferably 1:(0.1 to 5), more preferably 1:(0.1 to 1).

[0020] According to some embodiments of the present invention, the ratio of the mass of active metal Co to the sum of the masses of biomass and solid carrier is (0.5-40):100, preferably (5-35):100, and more preferably (10-30):100.

[0021] According to some embodiments of the present invention, the auxiliary metal is selected from at least one of Zn, Cu, Mn, Bi, Ga, In, Sb, Sn, Fe, Al, Mg, Ce, Cs, Li, Na, and K, preferably Zn and / or Fe.

[0022] In this invention, the auxiliary metal is selected from at least one of Zn and Fe, which can make the catalyst have better catalytic performance compared with other types of auxiliary metals.

[0023] According to some embodiments of the present invention, the auxiliary metal exists in the catalyst in the form of a metal oxide, for example, Zn can exist in the catalyst in the form of ZnO, and Fe can exist in the catalyst in the form of FeO, Fe2O3, etc.

[0024] According to some embodiments of the present invention, the mass ratio of active metal Co to auxiliary metal is 1:(0.05-2), preferably 1:(0.1-1), and more preferably 1:(0.2-0.6).

[0025] Secondly, the present invention provides a method for preparing a Co-based catalyst, comprising: loading biomass onto a solid support to obtain a support intermediate; loading active metal Co and auxiliary metal onto the support intermediate using a one-step isothermal stirring impregnation method, and then subjecting it to calcination to obtain the Co-based catalyst.

[0026] The catalyst provided by this invention is prepared by directly loading the active metal Co and the auxiliary metal onto a support intermediate and then calcining it. Compared with the catalyst prepared by first calcining the support intermediate to obtain a carbon-modified support and then loading the active metal Co and the auxiliary metal, it has significantly higher catalytic activity.

[0027] According to some embodiments of the present invention, the biomass includes at least one of agarose, pectin (e.g., natural polysaccharide uronic acid pectin), gelatin, chitosan, alginic acid, cellulose, lignin, chitin and its derivatives, preferably alginic acid.

[0028] According to some embodiments of the present invention, the solid support includes at least one of oxides and molecular sieves.

[0029] According to some embodiments of the present invention, the solid support comprises Al2O3.

[0030] According to some embodiments of the present invention, the solid support comprises γ-Al2O3.

[0031] According to some embodiments of the present invention, the particle size of the solid support is ≤100μm and the specific surface area is ≥200m². 2 / g.

[0032] According to some embodiments of the present invention, the particle size of the solid support is 30–100 μm, and the specific surface area is 200–250 m². 2 / g.

[0033] According to some embodiments of the present invention, the auxiliary metal is selected from at least one of Zn, Cu, Mn, Bi, Ga, In, Sb, Sn, Fe, Al, Mg, Ce, Cs, Li, Na, and K, preferably Zn and / or Fe.

[0034] According to some embodiments of the present invention, the preparation method includes: dispersing a carrier raw material comprising biomass and a solid support in water, stirring and mixing, separating the solid and liquid, drying the solid, and pulverizing it to obtain a carrier intermediate; obtaining a first dispersion comprising the carrier intermediate and a solvent; adding a Co precursor and an auxiliary metal precursor to the first dispersion, stirring at a constant temperature to obtain a second dispersion; performing solid-liquid separation on the second dispersion, and then calcining the obtained solid to obtain the Co-based catalyst.

[0035] According to some embodiments of the present invention, the solvent includes at least one selected from water, ethanol, methanol, n-hexane, and N,N-dimethylformamide.

[0036] According to some embodiments of the present invention, the Co precursor includes at least one of the chloride and nitrate salts of Co, preferably at least one of Co(NO3)2, Co(NO3)2·6H2O, CoSO4, CoSO4·7H2O, CoCl2, and CoCl2·6H2O.

[0037] According to some embodiments of the present invention, the auxiliary metal precursor includes at least one of the auxiliary metal nitrate, sulfate, and chloride.

[0038] According to some embodiments of the present invention, the auxiliary metal precursor includes at least one of Zn, Fe nitrate, sulfate, and chloride.

[0039] According to some embodiments of the present invention, the auxiliary metal precursor includes at least one selected from Fe(NO3)3, Fe2(SO4)3, FeCl3, Fe(NO3)2, Fe(SO4)2, FeCl2, FeCl2·4H2O, Zn(NO3)2, Zn(NO3)2·6H2O, ZnSO4, ZnSO4·7H2O, ZnCl2, and ZnCl2·xH2O.

[0040] According to some embodiments of the present invention, the mass ratio of biomass to solid carrier is 1:(0.1 to 10) (for example, it can be 1:0.1, 1:0.2, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, and any value within the range formed by any two of these point values), preferably 1:(0.1 to 5), more preferably 1:(0.1 to 1).

[0041] According to some embodiments of the present invention, the concentration of the carrier intermediate in the first dispersion is 0.5wt% to 10wt%, for example, it can be 0.5wt%, 0.6wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, and any value within the range formed by any two of these point values.

[0042] According to some embodiments of the present invention, the mass ratio of the Co precursor and the carrier intermediate, calculated as Co, is (0.5-40):100, preferably (5-35):100, and more preferably (10-30):100.

[0043] According to some embodiments of the present invention, the mass ratio of the Co precursor (calculated as Co) to the auxiliary metal precursor (calculated as auxiliary metal) is 1:(0.05-2), preferably 1:(0.1-1), and more preferably 1:(0.2-0.6).

[0044] According to some embodiments of the present invention, the temperature of the stirring and mixing is 0 to 100°C, preferably 20 to 40°C; the stirring and mixing time is 0.5 to 20 h, preferably 0.5 to 15 h, and more preferably 0.5 to 5 h.

[0045] In this invention, the purpose of pulverizing the dried solid is to disperse the solid that clumps together during the evaporation of moisture, so that the particles of the carrier intermediate are more uniform. Various common methods that can disperse solids, such as grinding, can be used.

[0046] According to some embodiments of the present invention, after solid-liquid separation, the solid is first washed and then dried.

[0047] According to some embodiments of the present invention, the temperature of the constant temperature stirring is 25 to 100°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 50°C, 55°C, 60°C, 70°C, 80°C, 90°C, 100°C, and any value within the range formed by any two of these point values.

[0048] According to some embodiments of the present invention, the constant temperature stirring time is 5 to 20 hours, preferably 6 to 15 hours.

[0049] According to some embodiments of the present invention, the second dispersion is cooled to room temperature before solid-liquid separation is performed.

[0050] According to some embodiments of the present invention, drying is performed before calcination; preferably, the drying is vacuum drying.

[0051] According to some embodiments of the present invention, the calcination treatment is carried out in an inert atmosphere.

[0052] According to some embodiments of the present invention, the inert atmosphere includes at least one of nitrogen and inert gases.

[0053] According to some embodiments of the present invention, the calcination treatment includes stepwise continuous calcination in multiple temperature ranges within the range of room temperature to 900°C; preferably, the calcination treatment includes: first heating to 200-250°C at a heating rate of 15-30°C / min, holding at that temperature for 1-2 hours; then heating at a rate of 1-10°C / min (for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, etc.). Heating at a rate of ℃ / min, and any value within a range formed by any two of these point values, to 300–900℃ (e.g., 300℃, 400℃, 500℃, 600℃, 700℃, 800℃, 900℃, and any value within a range formed by any two of these point values), and holding at this temperature for 1–10 h (e.g., 1h, 2h, 3h, 4h, 5h, 6h, 8h, 9h, 10h, and any value within a range formed by any two of these point values).

[0054] According to some embodiments of the present invention, after the calcination treatment is completed, the temperature is cooled to room temperature at a rate of 1 to 10 °C / min or at a natural cooling rate.

[0055] Thirdly, the present invention provides a Co-based catalyst prepared by the preparation method described in the second aspect.

[0056] Fourthly, the present invention provides the application of the Co-based catalyst described in the first aspect or the Co-based catalyst described in the third aspect in heterogeneous catalytic reactions, especially in the hydroformylation of olefins.

[0057] Compared with the prior art, the present invention can achieve at least the following beneficial effects:

[0058] The Co-based catalyst provided by this invention does not require the use of precious metals as active components or expensive phosphorus-containing organic ligands, which can reduce catalyst costs and is environmentally friendly. Furthermore, the Co-based catalyst exhibits good catalytic performance and stability for olefin hydroformylation reactions, and has broad industrial application prospects in the field of olefin hydroformylation, especially in the heterogeneous catalysis of olefin hydroformylation. Attached Figure Description

[0059] Figure 1 The XRD patterns of the alginate-carbon-modified γ-Al2O3-supported Co-based catalyst prepared in Example 1 and the unmodified γ-Al2O3-supported Co-based catalyst in Comparative Example 3 are shown.

[0060] The XRD pattern was determined using an X-ray diffractometer (model Smartlab SE). Detailed Implementation

[0061] To make the technical problem to be solved, the technical solution, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely for illustrating this patent and do not limit the scope of protection of this invention in any way.

[0062] Unless otherwise defined, the technical terms used in the following embodiments have the same meaning as commonly understood by those skilled in the art. Unless otherwise specified, the reagents used in the following embodiments are conventional biochemical reagents; the raw materials, instruments, and equipment used in the following embodiments can all be obtained commercially or by existing methods; unless otherwise specified, the reagent dosages are those used in routine experimental operations; unless otherwise specified, the experimental methods are conventional methods.

[0063] The mass percentage of Co in the catalysts prepared in the following examples (including Co, Co2C and CoO) was obtained by XPS (EscaLab 250Xi) peak splitting.

[0064] Example 1

[0065] (1) Preparation of carrier intermediate

[0066] 3g of alginic acid (Shanghai Aladdin Biochemical Technology Co., Ltd.) and 1g of γ-Al2O3 (particle size 30-100μm, specific surface area 200-250m²) were mixed. 2 / g) was dispersed in 100mL of deionized water and stirred at room temperature for 1h. The solid and liquid phases were separated by filtration. The obtained solid was washed alternately with water and ethanol, dried in a vacuum drying oven at 60℃ for 8h, and then pulverized to obtain the carrier intermediate.

[0067] (2) Preparation of catalyst

[0068] 1 g of the above-mentioned carrier intermediate was dispersed in 0.1 L of water, and 1 mL of a mixed aqueous solution of Co(NO3)2 and FeCl2·4H2O was added while stirring, so that the concentration of the intermediate in the dispersion was m Co / m 载体中间体 =12:100 and m Fe / m 载体中间体 The mixture was stirred at a constant temperature of 4:100 at 70°C for 8 hours. After cooling the mixture to room temperature, it was filtered and separated. The resulting solid was transferred to a vacuum drying oven and dried under vacuum at 60°C for 8 hours to obtain the metal-supported product.

[0069] The metal-supported product was transferred to a tube furnace. After completely purging the air from the furnace by purging with nitrogen, the temperature was increased to 200°C at a rate of 20°C / min under a nitrogen atmosphere and held at that temperature for 2 hours. Subsequently, the temperature was increased to 800°C at a rate of 5°C / min and held at that temperature for 2 hours. After the isothermal process, the heating was turned off and the furnace was allowed to cool naturally to room temperature to obtain the Co-based catalyst.

[0070] The XRD pattern of the Co-based catalyst prepared in this embodiment is shown below. Figure 1 As shown. From Figure 1 As can be seen from the above, the active metal Co exists in the catalyst in the forms of Co, Co2C, and CoO, while the promoter metal exists in the catalyst in the form of metal oxides. XPS measurements showed that the mass percentages of Co, Co2C, and CoO were 73%, 5%, and 22%, respectively.

[0071] Example 2

[0072] (1) The preparation of the carrier intermediate is the same as in Example 1, except that the amount of alginic acid is changed from 3g to 0.1g.

[0073] (2) The catalyst was prepared according to Example 1.

[0074] Example 3

[0075] (1) The preparation of the carrier intermediate is the same as in Example 1, except that the amount of alginate is changed from 3g to 2g.

[0076] (2) The catalyst was prepared according to Example 1.

[0077] Example 4

[0078] (1) The preparation of the carrier intermediate is the same as in Example 1, except that the amount of alginate is changed from 3g to 10g.

[0079] (2) The catalyst was prepared according to Example 1.

[0080] Example 5

[0081] (1) Preparation of the carrier intermediate: Refer to Example 1, except that γ-Al2O3 is replaced with an equal mass of active Al2O3 (particle size 30-100 μm, specific surface area 167-).

[0082] 192m 2 / g).

[0083] (2) The catalyst was prepared according to Example 1.

[0084] Example 6

[0085] (1) The preparation of the carrier intermediate was the same as in Example 1, except that γ-Al2O3 was replaced with an equal mass of silica (particle size 30-100 μm, specific surface area 200-250 m²). 2 / g).

[0086] (2) The catalyst was prepared according to Example 1.

[0087] Example 7

[0088] (1) The preparation of the carrier intermediate was carried out in accordance with Example 1, except that γ-Al2O3 was replaced with an equal mass of SBA-15 (particle size 30-100 μm, specific surface area 200-250 m²). 2 / g).

[0089] (2) The catalyst was prepared according to Example 1.

[0090] Example 8

[0091] (1) Preparation of the carrier intermediate is described in Example 1.

[0092] (2) The catalyst was prepared according to Example 1, except that the concentration of m in the dispersion was [missing information]. Co / m 载体中间体 =0.9:100 and m Fe / m 载体中间体 =0.3:100.

[0093] Example 9

[0094] (1) Preparation of the carrier intermediate is described in Example 1.

[0095] (2) The catalyst was prepared according to Example 1, except that the concentration of m in the dispersion was [missing information]. Co / m 载体中间体 =3:100 and m Fe / m 载体中间体 =1:100.

[0096] XRD results showed that the active metal Co existed in the forms of Co, Co₂C, and CoO. XPS analysis revealed that the mass percentages of Co, Co₂C, and CoO were 75%, 7%, and 18%, respectively.

[0097] Example 10

[0098] (1) Preparation of the carrier intermediate is described in Example 1.

[0099] (2) The catalyst was prepared according to Example 1, except that the concentration of m in the dispersion was [missing information]. Co / m 载体中间体 =30:100 and m Fe / m 载体中间体=10:100.

[0100] XRD results showed that the active metal Co existed in the forms of Co, Co₂C, and CoO. XPS analysis revealed that the mass percentages of Co, Co₂C, and CoO were 52%, 1%, and 47%, respectively.

[0101] Example 11

[0102] (1) Preparation of the carrier intermediate is described in Example 1.

[0103] (2) The catalyst was prepared according to Example 1, except that the metal-supported product was heated to 200°C at a rate of 20°C / min under a nitrogen atmosphere, and then immediately heated to 800°C at a rate of 5°C / min for 2 hours without holding the temperature for 2 hours.

[0104] Example 12

[0105] (1) Preparation of the carrier intermediate is described in Example 1.

[0106] (2) The catalyst was prepared according to Example 1, except that the metal-supported product was directly heated to 800°C at a rate of 20°C / min under a nitrogen atmosphere and then kept at the temperature for 2 hours.

[0107] Example 13

[0108] (1) Preparation of the carrier intermediate is described in Example 1.

[0109] (2) The catalyst was prepared according to Example 1, except that FeCl2·4H2O in the mixed aqueous solution was replaced with an equal mass (based on the metal element) of FeCl3.

[0110] Example 14

[0111] (1) Preparation of the carrier intermediate is described in Example 1.

[0112] (2) The catalyst was prepared according to Example 1, except that FeCl2·4H2O in the mixed aqueous solution was replaced with an equal mass (based on the metal element) of ZnCl2.

[0113] Example 15

[0114] (1) Preparation of the carrier intermediate is described in Example 1.

[0115] (2) The catalyst was prepared according to Example 1, except that FeCl2·4H2O in the mixed aqueous solution was replaced with an equal mass (based on the metal element) of CuCl. 2· 2H2O.

[0116] Example 16

[0117] (1) The preparation of the carrier intermediate was the same as in Example 1, except that alginate was replaced with an equal mass of natural polysaccharide uronic acid pectin (Shanghai Aladdin Biochemical Technology Co., Ltd.).

[0118] (2) The catalyst was prepared according to Example 1.

[0119] Example 17

[0120] (1) The preparation of the carrier intermediate was the same as in Example 1, except that alginate was replaced with an equal mass of cellulose (Shanghai Aladdin Biochemical Technology Co., Ltd.).

[0121] (2) The catalyst was prepared according to Example 1.

[0122] Example 18

[0123] (1) The preparation of the carrier intermediate was the same as in Example 1, except that alginate was replaced with an equal mass of chitin (Shanghai Aladdin Biochemical Technology Co., Ltd.).

[0124] (2) The catalyst was prepared according to Example 1.

[0125] Comparative Example 1

[0126] (1) Preparation of the carrier intermediate is described in Example 1.

[0127] (2) The catalyst was prepared according to Example 1, except that the mixed aqueous solution contained only Co(NO3)2 and not FeCl2·4H2O.

[0128] Comparative Example 2

[0129] (1) Preparation of carrier intermediate: Refer to Example 1, except that: alginic acid is replaced with an equal mass (based on the carbon support in the catalyst) of activated carbon (Shanghai Aladdin Biochemical Technology Co., Ltd.).

[0130] (2) The catalyst was prepared according to Example 1.

[0131] Comparative Example 3

[0132] (1) The preparation of the carrier intermediate is the same as in Example 1, except that alginic acid is not added.

[0133] (2) The catalyst was prepared according to Example 1.

[0134] The XRD data of the catalyst prepared in Comparative Example 3 are as follows: Figure 1 As shown. In the catalyst of this comparative example, the active metal Co exists in the forms of Co and CoO. XPS analysis revealed that the mass percentages of Co and CoO were 1% and 99%, respectively.

[0135] from Figure 1 As can be seen, compared with the catalyst prepared in Comparative Example 3, the catalyst prepared in Example 1, by adding alginate, mainly plays the following roles:

[0136] (1) It increased the loading of active metal Co and auxiliary metal in the catalyst;

[0137] (2) It provides a carbon source for the catalyst, which can improve catalytic efficiency;

[0138] (3) Part of CoO was reduced.

[0139] Comparative Example 4

[0140] (1) Preparation of carrier

[0141] 3g of alginic acid (Shanghai Aladdin Biochemical Technology Co., Ltd.) and 1g of γ-Al2O3 (particle size 30-100μm, specific surface area 200-250m²) were mixed. 2 (g) was dispersed in 100 mL of deionized water and stirred at room temperature for 1 h. The solid and liquid phases were separated by filtration. The obtained solid was washed alternately with water and ethanol and then dried in a vacuum drying oven at 60 °C for 8 h. It was then transferred to a tube furnace, and nitrogen gas was introduced to completely replace the air in the tube furnace. The temperature was then increased to 200 °C at a rate of 20 °C / min and held for 2 h under a nitrogen atmosphere. Subsequently, the temperature was increased to 800 °C at a rate of 5 °C / min and held for 2 h. After the isothermal process, the heating was turned off and the mixture was allowed to cool naturally to room temperature. Then, it was pulverized to obtain the carrier.

[0142] (2) Preparation of catalyst

[0143] Disperse 1g of the above carrier in 0.1L of water, and add 1mL of a mixed aqueous solution of Co(NO3)2 and FeCl2·4H2O while stirring, so that the concentration of the carrier in the dispersion is m Co / m (海藻酸+γ-Al2O3) =12:100 and m Fe / m (海藻酸+γ-Al2O3) The mixture was stirred at a constant temperature of 4:100 at 70°C for 8 hours. After cooling the mixture to room temperature, it was filtered and separated. The resulting solid was transferred to a vacuum drying oven and dried under vacuum at 60°C for 8 hours to obtain the metal-supported product.

[0144] The metal-supported product was transferred to a tube furnace. After completely purging the air from the furnace by purging with nitrogen, the temperature was increased to 200°C at a rate of 20°C / min under a nitrogen atmosphere and held at that temperature for 2 hours. Subsequently, the temperature was increased to 800°C at a rate of 5°C / min and held at that temperature for 2 hours. After the isothermal process, the heating was turned off and the furnace was allowed to cool naturally to room temperature to obtain the Co-based catalyst.

[0145] Catalyst performance evaluation:

[0146] (1) Evaluation of catalytic performance

[0147] Take 200 mg of each catalyst prepared in Examples 1-18 or Comparative Examples 1-4, mix them with 3.5 g of 1-octene and 6.5 g of n-heptane, and transfer them to a high-pressure reactor. Introduce a CO / H2 mixture (CO and H2 volume ratio of 1:1) into the reactor to replace the air in the reactor, then pressurize to 7 MPa, start stirring, and react at a constant temperature of 120 °C for 6 h. The reaction results are shown in Table 1.

[0148] (i) Conversion rate 烯烃 =(n 烷烃 +n 醛 +n 醇 ) / (n 烷烃 +n 醛 +n 醇 +n 剩余的烯烃 )×100%.

[0149] (ii) Selectivity (醛+醇) =(n 醛 +n 醇 ) / (n 烷烃 +n 醛 +n 醇 )×100%.

[0150] n in the formula 烷烃 n 醛 n 醇 n 剩余的烯烃 These refer to the molar amounts of alkanes, aldehydes, alcohols, and unreacted alkenes in the product, respectively.

[0151] Table 1

[0152]

[0153]

[0154] Note: m in Table 1 Co m 助剂金属 The calculation is based on a mass of 100 for the carrier intermediate (biomass + solid carrier).

[0155] (2) Stability evaluation

[0156] After the catalyst of Example 1, which has undergone catalytic performance evaluation, was separated from the reaction mixture, washed and dried, the catalytic performance evaluation reaction in (1) was repeated. The results of the 6 cycles are shown in Table 2.

[0157] Table 2

[0158]

[0159]

[0160] As can be seen from Table 2, after six cycles of use, the catalyst provided by this invention showed a decrease in conversion rate and selectivity of only 3.8% and 2.2%, respectively, demonstrating good stability.

[0161] As can be seen from the above catalyst performance evaluation results, the Co-based catalyst prepared in this invention has excellent catalytic performance and stability in the catalytic hydroformylation reaction of olefins.

[0162] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. A Co-based catalyst, characterized in that, It includes a biomass carbon-modified support, an active metal Co, and an auxiliary metal; the active metal Co and the auxiliary metal are supported on the biomass carbon-modified support; the active metal Co exists in the catalyst in the forms of Co, Co2C, and CoO, wherein the mass ratio of Co, Co2C, and CoO is (52-75):(1-7):(18-47), preferably (52-73):(1-5):(22-47).

2. The Co-based catalyst according to claim 1, characterized in that, The biomass includes at least one of agarose, pectin, gelatin, chitosan, alginic acid, cellulose, lignin, chitin and their derivatives, with alginic acid being preferred; And / or, The biomass carbon-modified carrier is obtained by carbon modification of a solid carrier by biomass. Preferably, the solid support comprises at least one of oxides and molecular sieves; more preferably, the solid support comprises Al2O3; even more preferably, the solid support comprises γ-Al2O3. Preferably, the solid support has a particle size ≤100μm and a specific surface area ≥200m². 2 / g; preferably, the particle size of the solid support is 30-100 μm and the specific surface area is 200-250 m² / g. 2 / g; Preferably, the mass ratio of biomass to solid carrier is 1:(0.1-10), more preferably 1:(0.1-5), and even more preferably 1:(0.1-1). Preferably, the ratio of the mass of active metal Co to the sum of the masses of biomass and solid carrier is (0.5-40):100, more preferably (5-35):100, and even more preferably (10-30):

100.

3. The Co-based catalyst according to claim 1 or 2, characterized in that, The auxiliary metal is selected from at least one of Zn, Cu, Mn, Bi, Ga, In, Sb, Sn, Fe, Al, Mg, Ce, Cs, Li, Na, and K, preferably Zn and / or Fe; And / or, the auxiliary metal exists in the catalyst in the form of a metal oxide; And / or, the mass ratio of active metal Co to auxiliary metal is 1:(0.05-2), preferably 1:(0.1-1), more preferably 1:(0.2-0.6).

4. A method for preparing a Co-based catalyst, characterized in that, include: Biomass is loaded onto a solid support to obtain a support intermediate; The active metal Co and the auxiliary metal were loaded onto a support intermediate using a one-step constant temperature stirring impregnation method, followed by calcination to obtain the Co-based catalyst.

5. The preparation method according to claim 4, characterized in that, The biomass includes at least one of agarose, pectin, gelatin, chitosan, alginic acid, cellulose, lignin, chitin and their derivatives, with alginic acid being preferred; And / or, the solid support comprises at least one of oxides and molecular sieves; more preferably, the solid support comprises Al2O3; even more preferably, the solid support comprises γ-Al2O3; And / or, the particle size of the solid support is ≤100μm and the specific surface area is ≥200m². 2 / g; preferably, the particle size of the solid support is 30-100 μm and the specific surface area is 200-250 m² / g. 2 / g And / or, the auxiliary metal is selected from at least one of Zn, Cu, Mn, Bi, Ga, In, Sb, Sn, Fe, Al, Mg, Ce, Cs, Li, Na, and K, preferably Zn and / or Fe.

6. The preparation method according to claim 4 or 5, characterized in that, The preparation method includes: dispersing a carrier raw material comprising biomass and a solid support in water, stirring and mixing, separating the solid and liquid, drying and pulverizing the solid to obtain a carrier intermediate; obtaining a first dispersion comprising the carrier intermediate and a solvent; adding a Co precursor and an auxiliary metal precursor to the first dispersion, stirring at a constant temperature to obtain a second dispersion; performing solid-liquid separation on the second dispersion, and then calcining the obtained solid to obtain the Co-based catalyst; Preferably, the solvent includes at least one selected from water, ethanol, methanol, n-hexane, and N,N-dimethylformamide; Preferably, the Co precursor includes at least one of the chloride and nitrate salts of Co, and more preferably at least one of Co(NO3)2, Co(NO3)2·6H2O, CoSO4, CoSO4·7H2O, CoCl2, and CoCl2·6H2O. Preferably, the auxiliary metal precursor includes at least one of the nitrate, sulfate, and chloride salts of the auxiliary metal; preferably, the auxiliary metal precursor includes at least one of the nitrate, sulfate, and chloride salts of Zn and Fe; more preferably, the auxiliary metal precursor includes at least one of Fe(NO3)3, Fe2(SO4)3, FeCl3, Fe(NO3)2, Fe(SO4)2, FeCl2, FeCl2·4H2O, Zn(NO3)2, Zn(NO3)2·6H2O, ZnSO4, ZnSO4·7H2O, ZnCl2, and ZnCl2·xH2O.

7. The preparation method according to claim 6, characterized in that, The mass ratio of biomass to solid carrier is 1:(0.1-10), preferably 1:(0.1-5), and more preferably 1:(0.1-1). And / or, the concentration of the carrier intermediate in the first dispersion is 0.5 wt% to 10 wt%; And / or, the mass ratio of the Co precursor to the carrier intermediate, calculated as Co, is (0.5-40):100, preferably (5-35):100, more preferably (10-30):100; And / or, the mass ratio of the Co precursor (calculated as Co) to the auxiliary metal precursor (calculated as auxiliary metal) is 1:(0.05-2), preferably 1:(0.1-1), more preferably 1:(0.2-0.6).

8. The preparation method according to claim 6 or 7, characterized in that, The mixing temperature is 0–100°C, preferably 20–40°C; the mixing time is 0.5–20 h, preferably 0.5–15 h, and more preferably 0.5–5 h. And / or, the temperature of the constant-temperature stirring is 25–100°C; And / or, the constant temperature stirring time is 5 to 20 hours, preferably 6 to 15 hours; And / or, the second dispersion is cooled to room temperature before solid-liquid separation.

9. The preparation method according to any one of claims 4-8, characterized in that, The calcination process is carried out in an inert atmosphere; And / or, the calcination treatment includes stepwise continuous calcination in multiple temperature ranges within the range of room temperature to 900°C; preferably, the calcination treatment includes: first heating to 200-250°C at a heating rate of 15-30°C / min and holding at that temperature for 1-2 hours; then heating to 300-900°C at a heating rate of 1-10°C / min and holding at that temperature for 1-10 hours; And / or, after the calcination treatment is completed, the temperature is cooled to room temperature at a rate of 1 to 10 °C / min or at a rate of natural cooling.

10. A Co-based catalyst, prepared by the preparation method according to any one of claims 4-9.

11. The use of the Co-based catalyst according to any one of claims 1-3 or the Co-based catalyst according to claim 10 in heterogeneous catalytic reactions, especially in the hydroformylation of olefins.