Aluminum alloy member and forging method thereof
By subjecting aluminum alloy forging billets to specific temperature annealing and water cooling treatment, the content of large-angle grain boundaries is reduced and the content of small-angle grain boundaries is increased, thus solving the corrosion problem of aluminum alloy materials in highly corrosive environments, improving their corrosion resistance and service life, and promoting the development of aerospace, rail transportation and chip manufacturing fields.
Patent Information
- Application Number
- CN202611351304.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-10
AI Technical Summary
Existing aluminum alloy materials are prone to surface corrosion, intergranular corrosion, and particle shedding in highly corrosive environments, resulting in a shortened structural service life and failing to meet the long-term service and clean environment requirements of aerospace, rail transportation, and chip manufacturing.
By performing a heat treatment process of annealing the hot-deformed aluminum alloy forging billet at a specific temperature and using water cooling as the cooling method, the content of large-angle grain boundaries is reduced, the content of small-angle grain boundaries is increased, and the non-equilibrium segregation of solute atoms and the continuous precipitation of harmful phases along grain boundaries are suppressed.
It effectively improves the corrosion resistance of aluminum alloy materials, prevents corrosion from spreading along grain boundaries, enhances the material's resistance to intergranular corrosion and exfoliation corrosion in highly corrosive environments, and extends its service life.
Smart Images

Figure CN123060032A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy technology, and more specifically to aluminum alloy parts and their forging methods. Background Technology
[0002] Aluminum alloys, due to their low density, high specific strength, good thermal and electrical conductivity, and ease of processing and forming, are widely used in aerospace, shipbuilding and marine engineering, rail transportation, chemical equipment, and chip manufacturing. However, the working environments in these fields are often accompanied by strong corrosive factors such as high humidity, salt spray, acidic and alkaline media, and industrial atmospheres. Especially in chip manufacturing, conventional aluminum alloy parts are prone to surface corrosion, intergranular corrosion, and particle shedding in highly corrosive environments at 400℃, leading to a significant reduction in structural lifespan and contamination problems caused by particle shedding, making it difficult to meet the requirements for long-term service and clean environments. Therefore, the industry has been trying to develop aluminum alloys that balance mechanical properties and corrosion resistance.
[0003] In existing technologies, conventional aluminum alloy manufacturing processes include semi-continuous casting, homogenization treatment, hot deformation, and solution aging treatment. Aluminum alloy materials usually need to undergo multiple recrystallization processes. Although over-aging treatment or the addition of trace amounts of elements to inhibit recrystallization can be adopted, a grain structure dominated by high proportions of large-angle grain boundaries will still be formed. As a result, the prepared aluminum alloy materials cannot have superior corrosion resistance to meet the industrial needs of various highly corrosive environments.
[0004] In order to overcome the above-mentioned defects in the existing technology, there is an urgent need in the field for aluminum alloy parts and their forging methods, which can effectively reduce the content of large-angle grain boundaries in aluminum alloy materials, thereby inhibiting the micro-galvanic corrosion behavior of aluminum alloy materials, improving their corrosion resistance, and promoting the further development of aerospace, rail transportation and chip manufacturing and other fields. Summary of the Invention
[0005] The following provides a brief overview of one or more aspects to offer a basic understanding of them. This overview is not an exhaustive summary of all conceived aspects, nor is it intended to identify key or decisive elements of all aspects, nor to define the scope of any or all aspects. Its sole purpose is to present some concepts of one or more aspects in a simplified form as a prelude to the more detailed descriptions that follow.
[0006] To overcome the aforementioned deficiencies in existing technologies, this invention provides aluminum alloy parts and their forging methods. By performing a heat treatment process of annealing the hot-deformed aluminum alloy forging billet at a specific temperature and selecting water cooling as the cooling method for the heat treatment process, the content of large-angle grain boundaries in the aluminum alloy material is reduced, while the content of small-angle grain boundaries is increased. This effectively suppresses the non-equilibrium segregation of solute atoms and the continuous precipitation of harmful phases along grain boundaries. This not only weakens the micro-galvanic corrosion behavior of the aluminum alloy material, but also prevents localized corrosion from spreading to the depth of the material due to the weak connectivity of small-angle grain boundaries. Therefore, it effectively improves the corrosion resistance of aluminum alloy materials, which can promote the further development of aerospace, rail transportation, and chip manufacturing.
[0007] Specifically, the aluminum alloy forging method provided by the first aspect of the present invention includes the following steps: preparing an aluminum alloy forging billet that has undergone a multi-directional forging process; preheating the aluminum alloy forging billet to a first temperature for a hot deformation process; heating the aluminum alloy forging billet that has undergone the hot deformation process to a second temperature and performing a heat treatment process for a first duration at the second temperature, wherein the second temperature is higher than the first temperature and higher than the service temperature of the forged aluminum alloy part; and cooling the aluminum alloy forging billet that has undergone the heat treatment process to obtain the aluminum alloy part.
[0008] Furthermore, in some embodiments of the present invention, the hot deformation process includes multiple process passes, wherein the cumulative deformation of the aluminum alloy forging billet by the multiple process passes is between 40% and 80%.
[0009] Furthermore, in some embodiments of the present invention, the plurality of process passes are selected from at least one of direct extrusion, hot rolling, and equal-channel corner extrusion.
[0010] Furthermore, in some embodiments of the present invention, the step of preparing the aluminum alloy forging billet after the multi-directional forging process includes: preparing an aluminum alloy rough billet; heating the aluminum alloy rough billet to 150°C~300°C to perform the multi-directional forging process on the aluminum alloy rough billet; and cooling the aluminum alloy rough billet after the multi-directional forging process to obtain the aluminum alloy forging billet.
[0011] Furthermore, in some embodiments of the present invention, the forging ratio of the multi-directional forging process is between 1.5 and 4.
[0012] Furthermore, in some embodiments of the present invention, the step of cooling the aluminum alloy billet after the multi-directional forging process to obtain the aluminum alloy forging billet includes: heating the cooled aluminum alloy billet to 200°C~450°C and holding it at that temperature for 1h~4h to perform an annealing process; and cooling the aluminum alloy billet after the annealing process to obtain the aluminum alloy forging billet.
[0013] Furthermore, in some embodiments of the present invention, the step of preheating the aluminum alloy forging billet to a first temperature for hot deformation includes: preheating the aluminum alloy forging billet to a first temperature and holding it at that temperature for 1 hour to 3 hours; and after holding it at that temperature for 1 hour to 3 hours, performing the hot deformation process on the aluminum alloy forging billet.
[0014] Furthermore, in some embodiments of the present invention, the first temperature is between 200°C and 400°C, the second temperature is between 435°C and 550°C, the service temperature is between 350°C and 435°C, and the first duration is between 0.5h and 3h.
[0015] Furthermore, the aluminum alloy part provided by the second aspect of the present invention is prepared by the preparation method provided by the first aspect of the present invention.
[0016] Furthermore, according to the aluminum alloy provided in the third aspect of the present invention, the content of large-angle grain boundaries in the aluminum alloy part is not greater than 30%, the strongest texture type of the grains in the aluminum alloy part is
[111] texture, and the texture intensity of the
[111] texture is greater than 6. Attached Figure Description
[0017] The above-described features and advantages of the present invention will be better understood after reading the following detailed description of embodiments of the present disclosure in conjunction with the accompanying drawings. In the drawings, components are not necessarily drawn to scale, and components having similar related properties or features may have the same or similar reference numerals.
[0018] Figure 1 A schematic diagram of the texture intensity distribution of an aluminum alloy part according to some embodiments of the present invention is shown.
[0019] Figure 2 A schematic flowchart of an aluminum alloy forging method according to some embodiments of the present invention is shown.
[0020] Figure 3A A cross-sectional structural schematic diagram of a 5N5 pure aluminum corrosion layer provided according to some reference embodiments of the present invention is shown.
[0021] Figures 3B-3DThe diagrams show the thickness of a 5N5 pure aluminum corrosion layer at a first position, a second position, and a third position, according to some reference embodiments of the present invention.
[0022] Figure 4A A cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some embodiments of the present invention is shown.
[0023] Figures 4B-4D The diagrams show the thickness of another 5N5 pure aluminum corrosion layer at a first position, a second position, and a third position, respectively, according to some embodiments of the present invention.
[0024] Figure 5A A cross-sectional structural schematic diagram of a 1050 aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown.
[0025] Figures 5B-5D The diagrams show the thickness of a 1050 aluminum alloy corrosion layer at a first position, a second position, and a third position, according to some reference embodiments of the present invention.
[0026] Figure 6A A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown.
[0027] Figures 6B-6D The diagrams show the thickness of the corrosion layer of another 1050 aluminum alloy at a first position, a second position, and a third position, respectively, according to some embodiments of the present invention.
[0028] Figure 7A A cross-sectional structural schematic diagram of a 1060s aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown.
[0029] Figures 7B-7D The diagrams show the thickness of a 1060s aluminum alloy corrosion layer at a first position, a second position, and a third position, respectively, according to some reference embodiments of the present invention.
[0030] Figure 8A A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown.
[0031] Figure 8B A schematic diagram of fluorine distribution in another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown.
[0032] Figure 9AA cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some reference embodiments of the present invention is shown.
[0033] Figure 9B A cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some embodiments of the present invention is shown.
[0034] Figure 9C A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown.
[0035] Figure 9D A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown.
[0036] Figure 9E A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown.
[0037] Figure 9F A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown. Detailed Implementation
[0038] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. Although the description of the present invention is presented in conjunction with preferred embodiments, this does not mean that the features of the invention are limited to these embodiments. On the contrary, the purpose of describing the invention in conjunction with embodiments is to cover other options or modifications that may be derived based on the claims of the present invention. To provide a thorough understanding of the invention, many specific details will be included in the following description. The invention may also be implemented without using these details. Furthermore, to avoid confusion or obscuring the focus of the invention, some specific details will be omitted in the description.
[0039] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0040] Furthermore, the terms "upper," "lower," "left," "right," "top," "bottom," "horizontal," and "vertical" used in the following description should be understood as the orientations shown in the relevant paragraphs and accompanying drawings. These relative terms are for illustrative purposes only and do not imply that the described apparatus must be manufactured or operated in a specific orientation, and therefore should not be construed as limiting the invention.
[0041] It is understood that although terms such as "first," "second," and "third" may be used herein to describe various components, regions, layers, and / or parts, these components, regions, layers, and / or parts should not be limited by these terms, and these terms are only used to distinguish different components, regions, layers, and / or parts. Therefore, the first components, regions, layers, and / or parts discussed below may be referred to as second components, regions, layers, and / or parts without departing from some embodiments of the present invention.
[0042] In existing technologies, conventional aluminum alloy manufacturing processes include semi-continuous casting, homogenization treatment, hot deformation, and solution aging treatment. Aluminum alloy materials typically undergo multiple recrystallization processes. Although over-aging treatment or the addition of trace amounts of elements to inhibit recrystallization can be adopted, a grain structure dominated by high-proportion large-angle grain boundaries will still be formed. Because large-angle grain boundaries have high interfacial energy and relatively open atomic structures, they are very likely to become non-equilibrium agglomeration or non-uniform nucleation sites for solute atoms, impurity elements, and precipitated phases. Therefore, aluminum alloy materials with a high content of large-angle grain boundaries will provide a large number of anodic channels for microgalvanic corrosion, initiating intergranular corrosion. Consequently, conventional aluminum alloy materials do not have superior corrosion resistance to meet the industrial needs of various high-corrosion environments.
[0043] To overcome the aforementioned deficiencies in existing technologies, this invention provides aluminum alloy parts and their forging methods. By performing a heat treatment process of annealing the hot-deformed aluminum alloy forging billet at a specific temperature and selecting water cooling as the cooling method for the heat treatment process, the content of large-angle grain boundaries in the aluminum alloy material is reduced, while the content of small-angle grain boundaries is increased. This effectively suppresses the non-equilibrium segregation of solute atoms and the continuous precipitation of harmful phases along grain boundaries. This not only weakens the micro-galvanic corrosion behavior of the aluminum alloy material, but also prevents localized corrosion from spreading to the depth of the material due to the weak connectivity of small-angle grain boundaries. Therefore, it effectively improves the corrosion resistance of aluminum alloy materials, which can promote the further development of aerospace, rail transportation, and chip manufacturing.
[0044] Please refer to Figure 1 . Figure 1 A schematic diagram of the texture intensity distribution of an aluminum alloy part according to some embodiments of the present invention is shown.
[0045] In some non-limiting embodiments, the aluminum alloy part provided by the second aspect of the invention can be obtained by the aluminum alloy forging method provided by the first aspect of the invention, wherein the content of large-angle grain boundaries in the aluminum alloy part is not greater than 30%, and as... Figure 1 As shown, the strongest grain texture type in this aluminum alloy part is
[111] texture, and the texture intensity of
[111] texture is greater than 6. Here, a large-angle grain boundary is a grain boundary where the phase difference between adjacent grains is greater than 10°.
[0046] Please refer to Figure 2 . Figure 2 A schematic flowchart of an aluminum alloy forging method according to some embodiments of the present invention is shown.
[0047] like Figure 2 As shown, in some embodiments, the aluminum alloy forging method provided by the first aspect of the present invention includes the following steps: Step S1: Prepare aluminum alloy forging billets that have undergone multi-directional forging process.
[0048] Specifically, step S1 can be specified by including the following steps: Step S11: Prepare aluminum alloy billet. Specifically, in some embodiments, the aluminum alloy billet is an aluminum alloy product formed by melting, refining and casting Al and alloy powder, preferably a 1-series aluminum alloy billet.
[0049] Those skilled in the art will understand that the above-described embodiments using 1-series aluminum alloy blanks are merely some non-limiting implementations provided by the present invention, intended to clearly demonstrate the main concept of the present invention and provide some specific solutions that are easy for the public to implement, rather than intended to limit the scope of protection of the present invention.
[0050] Alternatively, in other embodiments, the aluminum alloy blank can also be a 3-series, 5-series, or 6-series aluminum alloy blank.
[0051] Step S12: Heat the aluminum alloy billet to 150℃~300℃ to perform a multi-directional forging process. Specifically, during the aluminum alloy casting process, due to solidification shrinkage and changes in gas solubility, the aluminum alloy billet inevitably contains primary defects such as pores, dendrite segregation, coarse second phases, and coarse grains. Therefore, this invention employs a multi-directional forging process to apply strong compressive stress along different axes of the aluminum alloy billet, forming a multi-directional alternating triaxial compressive stress state, thereby generating extremely high hydrostatic pressure. Under this pressure, porosity defects such as looseness and micropores undergo plastic collapse and close. Simultaneously, under the hot deformation conditions of 150℃~300℃, the newly formed clean metal surface comes into close contact under shear force, and atoms diffuse across the interface, thereby achieving metallurgical welding. Furthermore, coarse eutectic phases or iron impurity phases often exist in the cast aluminum alloy billets. These coarse phases have a large potential difference with the aluminum matrix, which can easily cause severe localized electrochemical corrosion. Through multi-directional forging process, the present invention can continuously change the load axis, so that the material is subjected to alternating strong shear stress, thereby destroying the brittle skeleton of the coarse second phase, shearing and breaking it into micron-sized or even nano-sized fine particles, and making these particles uniformly dispersed in the aluminum matrix, thereby eliminating the potential difference concentration caused by the local coarse second phase and significantly reducing the tendency of microcell corrosion.
[0052] Specifically, in some embodiments, step S12 above can be further specified to include the following steps: Step S121: Billet preparation and pretreatment. A high-temperature lubricant (e.g., graphite lubricant or molybdenum disulfide lubricant) is applied to the surface of the above-mentioned aluminum alloy billet to reduce the friction between the billet and the die / anvil during forging.
[0053] Step S122: Preheating and Holding. The aluminum alloy billet, lubricated in step S121, is placed in a heating furnace and preheated to 150℃~300℃. The holding time is determined based on the billet's cross-sectional dimensions to ensure the core and surface temperatures of the billet are consistent, avoiding uneven deformation due to internal and external temperature differences.
[0054] Step S123: Multi-directional cyclic forging. Place the preheated aluminum alloy billet on the forging anvil. Apply pressure along the Z-axis (vertical direction) for compression. After compression along the Z-axis, rotate the billet horizontally so that the original Y-axis becomes the direction of perpendicular pressure. Start the press to perform compression in the second direction along this axis. Rotate the billet again so that the original X-axis becomes the direction of perpendicular pressure, and perform compression deformation in the third direction. After the sequential compression in the above three directions, a complete multi-directional forging cycle is completed. Repeat the above steps according to the preset forging ratio. If the surface temperature of the aluminum alloy billet drops below 200°C due to heat dissipation, the aluminum alloy billet needs to be sent back to the heating furnace for rapid reheating.
[0055] Specifically, in some embodiments, the forging ratio is defined as the cumulative equivalent true plastic strain, with a value between 1.5 and 4. Thus, by limiting the multi-directional forging ratio to this specific range of 1.5 to 4, the present invention achieves a balance between eliminating casting defects, controlling microstructure, and avoiding thermal deformation cracking of the material. When the forging ratio is below 1.5, the accumulated plastic deformation energy within the aluminum alloy material is insufficient. Large shrinkage cavities and porosity inside the aluminum alloy billet only undergo flattening deformation under low strain, and the cavities cannot be completely closed. Simultaneously, the low deformation amount makes it difficult to generate sufficient alternating shear stress to effectively break up the coarse eutectic phase. Furthermore, aluminum alloys have high stacking fault energy and a significant tendency for dynamic recovery; excessively low deformation amounts cannot initiate continuous dynamic recrystallization, making it difficult to trigger the grain refinement process. Conversely, if the forging ratio exceeds 4, as the strain continues to increase, the dislocation density tends to saturate, the aluminum alloy material undergoes severe work hardening, the plasticity decreases sharply, and microcracks or even macroscopic splitting are easily formed inside, leading to a decrease in the yield of finished products. At the same time, excessively high cumulative deformation will also significantly increase the operating load, aggravate mold wear, and prolong the processing time, increasing the overall preparation cost of aluminum alloys.
[0056] Step S13: Cool the aluminum alloy billet after multi-directional forging to obtain an aluminum alloy forging blank. Thus, by using water cooling to cool the aluminum alloy billet after multi-directional forging, this invention can effectively lock the deformation structure, dislocation structure, and alloy element distribution formed by multi-directional forging. Simultaneously, it promotes aluminum alloy billets of different batches, sizes, and locations to enter the subsequent annealing process with relatively consistent temperature and microstructure, thereby establishing unified and controllable initial annealing conditions and improving the process consistency of the final aluminum alloy forging.
[0057] In traditional aluminum alloy forging processes, there is usually a temperature difference between forging temperature and annealing temperature. Therefore, it is not possible to directly switch the aluminum alloy billet from the forging temperature to the annealing temperature. Only controlled slow cooling can be used to cool it down, which leads to excessively long cooling time. The dislocation configuration and deformation structure formed by multi-directional forging recover during the long cooling process, and the control effect of multi-directional forging on the aluminum alloy billet is greatly weakened.
[0058] Furthermore, by using water cooling to cool the aluminum alloy billet after multi-directional forging, this invention avoids the drawbacks of slow air cooling, preventing solute atoms from having sufficient time to diffuse to the high-energy interface, thereby avoiding the precipitation of coarse and continuously distributed equilibrium or transition phases at the grain boundaries. Especially in the field of chip manufacturing, semiconductor processing requires operation in a high-temperature fluorine radical corrosive environment. Significant chemical potential differences exist between the coarse grain boundary phase and the matrix, as well as between PFZ and the matrix, easily leading to severe intergranular electrochemical corrosion and chemical exfoliation, causing the material to rapidly penetrate along the grain boundaries in a tunnel-like manner. This invention, through rapid water cooling, prevents solute atoms from diffusing over long distances, inhibiting the precipitation of the second phase at the grain boundaries, avoiding grain boundary segregation and the formation of non-precipitated zones, thus retaining alloying elements in the matrix lattice to form a uniform supersaturated solid solution. This eliminates electrochemical inhomogeneity at the grain boundaries, improving the aluminum alloy's resistance to intergranular corrosion and exfoliation corrosion in a fluorine radical environment.
[0059] Specifically, in some embodiments, step S13 may be specified as including the following steps: Step S131: Heat the cooled aluminum alloy billet to 200℃~450℃ and hold for 1h~4h to perform the annealing process. The annealing process can be further specified as follows: Step S1311: Annealing preparation. The aluminum alloy billet is placed in a box-type resistance furnace with a protective gas (e.g., high-purity nitrogen or argon). Thus, by surrounding the aluminum alloy billet with a protective gas, the present invention can prevent selective oxidation of the aluminum alloy billet surface during high-temperature annealing, thereby ensuring the chemical purity of the base metal.
[0060] Step S1312: Isothermal annealing. By performing the annealing process at a constant temperature, the present invention can rapidly release the distortion energy locked in the multi-directional forging water-cooling stage, allowing recrystallized grains to nucleate in a short time, thereby completely transforming the original deformed structure into strain-free equiaxed recrystallized grains.
[0061] Thus, by performing a heat preservation annealing process on the aluminum alloy billet, the present invention can promote the formation of uniform equiaxed fine grains inside the aluminum alloy, cut off the rapid and deep erosion channels of fluorine free radicals along the grain boundaries, thereby improving the aluminum alloy's resistance to intergranular corrosion and exfoliation corrosion in a fluorine free radical environment.
[0062] Step S132: Cool the annealed aluminum alloy billet to obtain an aluminum alloy forging billet. Thus, by employing water cooling in the annealing process, this invention avoids the drawbacks of slow air cooling, preventing solute atoms from having sufficient time to diffuse to the high-energy interface. This avoids the precipitation of coarse and continuously distributed equilibrium or transition phases at the grain boundaries, thereby eliminating electrochemical inhomogeneities at the grain boundaries and improving the aluminum alloy's resistance to intergranular corrosion and exfoliation corrosion in a fluorine radical environment.
[0063] Step S2: Preheat the aluminum alloy forging billet to a first temperature for hot deformation. Specifically, step S2 can be specified by including the following steps: Step S21: Preheat the aluminum alloy forging billet to a first temperature and hold it at that temperature for 1 to 3 hours. Here, the first temperature is between 200°C and 400°C. In this way, by controlling the heat deformation temperature within a relatively mild range, the present invention can limit the content of large-angle grain boundaries in the aluminum alloy and improve the grain texture strength.
[0064] Step S22: After a heat preservation process of 1h to 3h, the aluminum alloy forging billet is subjected to a hot deformation process.
[0065] Furthermore, in some embodiments, the above-mentioned hot deformation process includes multiple process passes. Thus, by employing multiple process passes to achieve progressive deformation of the aluminum alloy forging billet, rather than a single large deformation or a conventional deformation method without pass control, the present invention can form a single and extremely strong
[111] textured grain and block the nucleation and growth of dynamic recrystallization, thereby maintaining a microstructure dominated by small-angle grain boundaries, avoiding the formation of large-angle grain boundaries, and thus improving the corrosion resistance of the aluminum alloy.
[0066] Specifically, grain rotation is a gradual physical process. During deformation in multiple process passes, grains accumulate strain and rotate smoothly and continuously along a specific slip system. By the time the final rolling or extrusion stage is reached, the close-packed
[111] planes of most grains are highly parallel to the deformed surface, thus forming a single and extremely strong
[111] texture. In addition, the deformation in multiple process passes adopts a small-step, fast-running preparation strategy. Therefore, during the interval between passes, the aluminum alloy material can undergo moderate static or dynamic recovery, thereby consuming some of the excess dislocations. At the same time, the subgrain structure is preserved. This mild energy release mechanism can effectively block the nucleation and growth of dynamic recrystallization, thereby maintaining a microstructure dominated by small-angle grain boundaries, avoiding the formation of large-angle grain boundaries, and improving the corrosion resistance of the aluminum alloy.
[0067] Furthermore, in some embodiments, the cumulative deformation of the aluminum alloy forging billet by multiple process passes is between 40% and 80%. Thus, by setting the cumulative deformation of hot deformation within this specific range of 40% to 80%, the present invention can promote the formation of strong
[111] texture and limit the proportion of large-angle grain boundaries in the aluminum alloy material.
[0068] Specifically, if the cumulative deformation amount of hot deformation is less than 40%, the deformation amount is insufficient to drive the lattice to rotate fully and it is difficult to form a strong
[111] texture. Conversely, if the cumulative deformation amount is greater than 80%, the deformation distortion energy accumulated inside the aluminum alloy material is extremely high. With the assistance of thermal activation, it is very easy to cross the nucleation thermodynamic barrier of dynamic recrystallization. Once large-scale dynamic recrystallization occurs, the orientation of the newly formed equiaxed grains will be highly randomized. This will not only severely erode and weaken the already formed
[111] texture, resulting in a significant decrease in texture strength, but also increase the proportion of large-angle grain boundaries in the aluminum alloy. In addition, the plasticity of aluminum alloy in the warm deformation zone is limited. The cumulative deformation amount exceeding 80% will lead to work hardening and stress concentration, which will easily generate microcracks on the edge of the plate or the surface of the rod, thereby reducing the yield of finished products.
[0069] Furthermore, in some embodiments, the aforementioned multiple process passes are selected from at least one of direct extrusion, hot rolling, and equal-channel corner extrusion.
[0070] Specifically, in some embodiments, the direct extrusion process includes the following steps: The deformation per pass is controlled at 10%~20%. After the first extrusion pass, if the surface temperature of the aluminum alloy forging billet drops below 200℃ due to contact heat transfer, the billet needs to be quickly returned to the heating furnace for supplemental heating for 5~15 minutes to restore its temperature to 200~400℃. Then, a series of extrusion dies with progressively smaller apertures are used, and the above extrusion and temperature control steps are repeated for 2~10 passes, preferably 2~8 passes. As the number of passes increases, the metal lattice undergoes continuous slippage and rotation. Extrusion is stopped when the cumulative deformation reaches a set value of 40%~80%. Here, the cumulative deformation can be calculated using the cross-sectional area shrinkage rate before and after extrusion.
[0071] Thus, by adopting a direct extrusion process with multiple process passes, the present invention can achieve directional strengthening of the anisotropic texture of aluminum alloy materials, so that the service exposed surface presents a highly corrosion-resistant texture
[111] , while limiting the proportion of large-angle grain boundaries, so that the corrosion rate at the grain boundaries tends to be consistent with that within the grains, thereby improving the corrosion resistance of aluminum alloys and optimizing the uniformity of the corrosion layer thickness.
[0072] Specifically, in some embodiments, the hot rolling process includes the following steps: The deformation per pass is controlled at 10%~15%. After the first extrusion pass, if the surface temperature of the aluminum alloy forging billet drops below 200℃ due to contact heat transfer, the billet needs to be quickly returned to the heating furnace for supplemental heating for 5~15 minutes to restore its temperature to 200~400℃. Then, the hot rolling and temperature control steps are repeated with a decreasing roll spacing, for 2~10 passes, preferably 4~10 passes. As the number of passes increases, the metal lattice undergoes continuous slippage and rotation. Hot rolling is stopped when the cumulative deformation reaches the set value of 40%~80%.
[0073] Thus, by adopting a hot rolling process with multiple passes, the present invention can achieve directional strengthening of the anisotropic texture of aluminum alloy materials, so that the service exposed surface presents a highly corrosion-resistant texture
[111] , while limiting the proportion of large-angle grain boundaries, so that the corrosion rate at the grain boundary tends to be consistent with that within the grain, thereby improving the corrosion resistance of aluminum alloy and optimizing the uniformity of the corrosion layer thickness.
[0074] Specifically, in some embodiments, the equal channel corner extrusion process includes the following steps: The deformation per pass is controlled at 10%~15%. After the first extrusion pass, if the surface temperature of the aluminum alloy forging billet drops below 200℃ due to contact heat transfer, the billet needs to be quickly returned to the heating furnace for supplemental heating for 5~15 minutes to restore its temperature to 200~400℃. Then, replace the die with an equal-channel angular extrusion die with progressively smaller orifice sizes, and repeat the above extrusion and temperature control steps for 2~10 passes, preferably 2~6 passes. As the number of passes increases, the metal lattice undergoes continuous slippage and rotation. When the cumulative deformation reaches a set value of 40%~80%, the equal-channel angular extrusion is stopped. Here, the cumulative deformation can be calculated using the cross-sectional area shrinkage rate before and after the equal-channel angular extrusion.
[0075] Thus, by adopting a multi-pass equal-channel corner extrusion process, the present invention can achieve directional strengthening of the anisotropic texture of aluminum alloy materials, so that the service exposed surface presents a highly corrosion-resistant texture
[111] , while limiting the proportion of large-angle grain boundaries, so that the corrosion rate at the grain boundary tends to be consistent with that within the grain, thereby improving the corrosion resistance of aluminum alloy and optimizing the uniformity of the corrosion layer thickness.
[0076] Step S3: The aluminum alloy forging billet, which has undergone hot deformation, is heated to a second temperature for a first-duration heat treatment process. Here, the second temperature is higher than the first temperature and also higher than the service temperature of the forged aluminum alloy part.
[0077] Specifically, in some embodiments, the second temperature is between 435°C and 550°C, the service temperature is between 350°C and 435°C, and the first duration is between 0.5h and 3h. Thus, by heating the aluminum alloy forging billet after hot deformation to between 435°C and 550°C and holding it at that temperature for 0.5h to 3h, this invention not only ensures that the final forged aluminum alloy part meets the service temperature requirements for subsequent operations, but also inhibits abnormal grain growth within the aluminum alloy at 400°C, thereby avoiding the formation of large-angle grain boundaries and controlling the content of large-angle grain boundaries to ensure the corrosion resistance of the aluminum alloy.
[0078] Step S4: Cool the heat-treated aluminum alloy forging billet to obtain an aluminum alloy part. Specifically, the heat-treated aluminum alloy forging billet is cooled to 20°C~40°C, preferably 25°C, to obtain an aluminum alloy part. Thus, by performing water cooling after the aluminum alloy hot deformation process, the present invention can lock the control results of hot deformation, prevent microstructure degradation, thereby limiting the proportion of large-angle grain boundaries in the aluminum alloy, promoting the generation of strong
[111] texture, and thus improving the corrosion resistance of the aluminum alloy.
[0079] Specifically, traditional aluminum alloy forging processes employ air cooling, which makes the aluminum alloy material prone to static recrystallization during this stage. This leads to abnormal grain growth, resulting in a significant decrease in
[111] texture strength, dislocation annihilation, and an increase in the proportion of large-angle grain boundaries. Furthermore, the aforementioned air cooling method also increases the surface chemical activity of the aluminum alloy, making it easier for fluorine radicals to rapidly erode deeper along channels such as large-angle grain boundaries and non-precipitated zones, causing grain spalling and localized pitting corrosion. Therefore, this invention replaces traditional air cooling with water cooling, which can limit static recrystallization, prevent abnormal grain growth, improve
[111] texture strength, limit the proportion of large-angle grain boundaries, and simultaneously make the aluminum alloy surface chemically inert, effectively reducing the frontal reaction rate of fluorine radicals, thereby improving the aluminum alloy's resistance to intergranular corrosion and exfoliation corrosion in a fluorine radical environment.
[0080] In summary, this invention, through a heat treatment process involving specific-temperature annealing of hot-deformed aluminum alloy forgings and the selection of water cooling as the cooling method, achieves a reduction in the content of large-angle grain boundaries and an increase in the content of small-angle grain boundaries in the aluminum alloy material. This effectively suppresses the non-equilibrium segregation of solute atoms and the continuous precipitation of harmful phases along grain boundaries. It not only weakens the micro-galvanic corrosion behavior of the aluminum alloy material, but also prevents localized corrosion from propagating deep into the material due to the weak connectivity of small-angle grain boundaries, thus effectively improving the corrosion resistance of the aluminum alloy material. Furthermore, the hot deformation and heat treatment process at specific temperatures induces plastic deformation in the aluminum alloy material, reducing the energy difference between grain boundaries and within grains, resulting in a more uniform corrosion layer thickness. This effectively prevents corrosion layer detachment, ensures the cleanliness of the industrial environment, and ultimately promotes further development in fields such as aerospace, rail transportation, and chip manufacturing.
[0081] The following examples, combining forging of different types of material blanks using the forging method provided in the first aspect of this invention with reference examples of the aforementioned different types of material blanks without forging, describe the working principle of the aluminum alloy forging method that can produce materials with better corrosion resistance. Those skilled in the art will understand that these examples of the offline fitting stage of the processing method are merely non-limiting embodiments provided by this invention, intended to clearly demonstrate the main concept of the invention and provide some specific solutions convenient for public implementation, rather than limiting all functions or all working methods of the aluminum alloy forging method. Similarly, the forging of different types of material blanks described above is also only a non-limiting embodiment provided by this invention and does not limit the execution order or the subject of execution in the preparation method.
[0082] Please refer to Figures 3 through 9. Figure 3A A cross-sectional structural schematic diagram of a 5N5 pure aluminum corrosion layer provided according to some reference embodiments of the present invention is shown. Figures 3B-3D The diagrams show the thickness of a 5N5 pure aluminum corrosion layer at a first position, a second position, and a third position, according to some reference embodiments of the present invention. Figure 4A A cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some embodiments of the present invention is shown. Figures 4B-4D The diagrams show the thickness of another 5N5 pure aluminum corrosion layer at a first position, a second position, and a third position, respectively, according to some embodiments of the present invention. Figure 5A A cross-sectional structural schematic diagram of a 1050 aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown. Figures 5B-5DThe diagrams show the thickness of a 1050 aluminum alloy corrosion layer at a first position, a second position, and a third position, according to some reference embodiments of the present invention. Figure 6A A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown. Figures 6B-6D The diagrams show the thickness of the corrosion layer of another 1050 aluminum alloy at a first position, a second position, and a third position, respectively, according to some embodiments of the present invention. Figure 7A A cross-sectional structural schematic diagram of a 1060s aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown. Figures 7B-7D The diagrams show the thickness of a 1060s aluminum alloy corrosion layer at a first position, a second position, and a third position, respectively, according to some reference embodiments of the present invention. Figure 8A A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown. Figure 8B A schematic diagram of fluorine distribution in another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown. Figure 9A A cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some reference embodiments of the present invention is shown. Figure 9B A cross-sectional structural schematic diagram of another 5N5 pure aluminum corrosion layer provided according to some embodiments of the present invention is shown. Figure 9C A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown. Figure 9D A cross-sectional structural schematic diagram of another 1050 aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown. Figure 9E A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some reference embodiments of the present invention is shown. Figure 9F A cross-sectional structural schematic diagram of another 1060s aluminum alloy corrosion layer provided according to some embodiments of the present invention is shown.
[0083] like Figure 3A , Figure 5A as well as Figure 7A As shown, 5N5 pure aluminum, 1050 aluminum alloy, and 1060s aluminum alloy, without undergoing deformation heat treatment (TMP), formed fluorinated corrosion layers of varying thicknesses in the same corrosive environment. These were observed using a 500x scanning microscope. Figure 3A , Figure 5A as well as Figure 7A It can be obtained as follows Figures 3B-3D , Figures 5B-5D as well as Figures 7B-7DThe diagram shows the corrosion layer thickness. At the first location, the average corrosion layer thickness is 25 μm for 5N5 pure aluminum, 16 μm for 1050 aluminum alloy, and 6 μm for 1060s aluminum alloy. At the second location, the average corrosion layer thickness is 22 μm for 5N5 pure aluminum, 7 μm for 1050 aluminum alloy, and 5 μm for 1060s aluminum alloy. At the third location, the average corrosion layer thickness is 20 μm for 5N5 pure aluminum, 12 μm for 1050 aluminum alloy, and 4 μm for 1060s aluminum alloy.
[0084] like Figure 4A , Figure 6A as well as Figure 8A As shown, after deformation heat treatment using the aluminum alloy forging method provided in the first aspect of the present invention, three materials—5N5 pure aluminum, 1050 aluminum alloy, and 1060s aluminum alloy—formed fluorinated corrosion layers of varying thicknesses in the same corrosive environment. These were observed using a 500x (500X) scanning microscope. Figure 4A , Figure 6A as well as Figure 8A It can be obtained as follows Figures 4B-4D and Figures 6B-6D The diagram showing the corrosion layer thickness, and as shown below Figure 8B The diagram shows the fluorine distribution. The average corrosion layer thickness at the first location for 5N5 pure aluminum is 13 μm, for 1050 aluminum alloy it is 5 μm, and for 1060s aluminum alloy it is too low to measure an effective corrosion layer thickness. The average corrosion layer thickness at the second location for 5N5 pure aluminum is 10 μm, for 1050 aluminum alloy it is 6 μm, and for 1060s aluminum alloy it is too low to measure an effective corrosion layer thickness. The average corrosion layer thickness at the third location for 5N5 pure aluminum is 10 μm, for 1050 aluminum alloy it is 7 μm, and for 1060s aluminum alloy it is too low to measure an effective corrosion layer thickness.
[0085] Based on the above data, calculations show that the average depth of the fluorinated layer in 5N5 pure aluminum obtained directly from casting is 22.33 μm, while the average depth after TMP treatment is 11 μm, a reduction of 50.74%. The average depth of the fluorinated layer in 1050 aluminum alloy obtained directly from casting is 11.67 μm, while the average depth after TMP treatment is 6 μm, a reduction of 48.59%. The average depth of the fluorinated layer in 1060s aluminum alloy obtained directly from casting is 5.33 μm, and the surface of most areas of the 1060s aluminum alloy after TMP treatment lacks a fluorinated layer. Therefore, the aluminum alloy forging method provided by the first aspect of this invention can effectively improve the corrosion resistance of the material and enhance the aluminum alloy's resistance to intergranular corrosion and exfoliation corrosion in a fluorine radical environment.
[0086] like Figures 9A-9F As shown, under the same corrosive environment, observation using a 1000x (1000X) scanning microscope revealed that the uniformity of the corrosion layer of 5N5 pure aluminum, 1050 aluminum alloy, and 1060s aluminum alloy forged using the aluminum alloy forging method provided in the first aspect of the present invention was significantly higher than that of 5N5 pure aluminum, 1050 aluminum alloy, and 1060s aluminum alloy that had not been forged. This demonstrates that the aluminum alloy forging method provided in the first aspect of the present invention can effectively improve the uniformity of the corrosion layer thickness, thereby preventing corrosion layer detachment.
[0087] Although the methods described above are illustrated and depicted as a series of actions for the sake of simplicity, it should be understood and appreciated that these methods are not limited by the order of the actions, as some actions may occur in a different order and / or concurrently with other actions from the illustrations and descriptions herein or not illustrated and described herein but which may be understood by those skilled in the art, according to one or more embodiments.
[0088] The prior description of this disclosure is provided to enable any person skilled in the art to make or use this disclosure. Various modifications to this disclosure will be apparent to those skilled in the art, and the general principles defined herein may be applied to other variations without departing from the spirit or scope of this disclosure. Therefore, this disclosure is not intended to be limited to the examples and designs described herein, but should be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for forging aluminum alloys, characterized in that, Includes the following steps: Prepare aluminum alloy forging billets that have undergone multi-directional forging process; The aluminum alloy forging billet is preheated to a first temperature for hot deformation process; The aluminum alloy forging billet that has undergone the hot deformation process is heated to a second temperature and subjected to a heat treatment process for a first duration at the second temperature, wherein the second temperature is higher than the first temperature and higher than the service temperature of the aluminum alloy part obtained by forging. as well as The aluminum alloy forging billet that has undergone the heat treatment process is cooled to obtain the aluminum alloy part.
2. The aluminum alloy forging method according to claim 1, characterized in that, The hot deformation process includes multiple process passes, wherein the cumulative deformation of the aluminum alloy forging billet by the multiple process passes is between 40% and 80%.
3. The aluminum alloy forging method according to claim 2, characterized in that, The plurality of process passes are selected from at least one of direct extrusion, hot rolling, and equal channel corner extrusion.
4. The aluminum alloy forging method according to claim 1, characterized in that, The steps for preparing the aluminum alloy forging billet through the multi-directional forging process include: Prepare aluminum alloy billets; The aluminum alloy billet is heated to 150°C~300°C to perform the multi-directional forging process on the aluminum alloy billet; and The aluminum alloy billet that has undergone the multi-directional forging process is cooled to obtain the aluminum alloy forging billet.
5. The aluminum alloy forging method according to claim 4, characterized in that, The forging ratio of the multi-directional forging process is between 1.5 and 4.
6. The aluminum alloy forging method according to claim 4, characterized in that, The step of cooling the aluminum alloy billet after the multi-directional forging process to obtain the aluminum alloy forging billet includes: The cooled aluminum alloy billet is heated to 200℃~450℃ and held at that temperature for 1h~4h for annealing; and The aluminum alloy billet that has undergone the annealing process is cooled to obtain the aluminum alloy forging billet.
7. The aluminum alloy forging method according to claim 1, characterized in that, The step of preheating the aluminum alloy forging billet to a first temperature for hot deformation includes: The aluminum alloy forging billet is preheated to a first temperature and held at that temperature for 1 to 3 hours; and After the 1-3 hour heat preservation process, the aluminum alloy forging billet is subjected to the hot deformation process.
8. The aluminum alloy forging method according to claim 1, characterized in that, The first temperature is between 200℃ and 400℃, the second temperature is between 435℃ and 550℃, the service temperature is between 350℃ and 435℃, and the first duration is between 0.5h and 3h.
9. An aluminum alloy part, characterized in that, The aluminum alloy part is prepared by the aluminum alloy forging method according to any one of claims 1 to 8.
10. An aluminum alloy part, characterized in that, The content of large-angle grain boundaries in the aluminum alloy part is not greater than 30%, the strongest texture type of the grains in the aluminum alloy part is [111] texture, and the texture intensity of the [111] texture is greater than 6.