An annular gating structure for casting thin-walled parts and a casting method for thin-walled parts.
By designing an annular gating structure and optimizing the shell molding process, the defect problem caused by uneven flow during the casting process of thin-walled castings was solved, achieving high-precision molding and low-cost production. It is suitable for thin-walled castings in aerospace, automotive, power electronics, medical devices and other fields.
Patent Information
- Application Number
- CN202611596584.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-10
AI Technical Summary
In traditional casting processes, the casting system for thin-walled castings has a simple structure and uneven flow path, resulting in uneven filling of the mold cavity with molten metal. This easily leads to defects such as cold shuts, cracks, shrinkage cavities, and porosity, making it difficult to meet the requirements of high-precision molding. In particular, the control of flow stability and solidification sequence is more critical in centrifugal casting or wax pattern casting processes.
The system adopts an annular runner structure, including an annular runner, an inner gate, and a secondary inner gate. Combining thermal modulus inversion design, centrifugal speed correction factor, integrated wax molding, tangential swirling buffer, and optimized shell molding process, the cross-sectional area ratio of the annular runner to the secondary inner gate is designed to be 1:(1.2~2):(2~3). Tangential guide sections and overflow blind cavities are set. Through wax dewaxing guide ribs and optimized shell molding process, the system ensures that the molten metal forms a stable swirling flow and feeding within the cavity.
It achieves stable swirling of molten metal within the mold cavity, eliminating defects such as cold shuts and shrinkage cavities, improving the forming quality and yield of castings, and reducing scrap rate and energy consumption. It is suitable for mass production of thin-walled ring parts made of titanium alloys, high-temperature alloys, stainless steel, etc.
Smart Images

Figure CN123060055A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of casting technology, and in particular to an annular gating structure for casting thin-walled parts and a casting method for thin-walled parts. Background Technology
[0002] In the field of precision casting, thin-walled castings are widely used in aerospace, automotive, power electronics, medical device, and other industries due to their advantages such as light weight, high strength, and material savings. Their use is particularly prevalent in fields requiring lightweight structures and high performance. However, because of the thin wall thickness of thin-walled castings, the molten metal experiences significant flow resistance during the filling process, placing higher demands on the design of the gating system, the control of molten metal flowability, and the management of the solidification process.
[0003] Currently, in traditional casting processes, the gating system typically employs a direct gating gate or a simple branch runner. For example, Chinese invention patent CN105312504A discloses a gating system and manufacturing method for a high-temperature alloy thin-walled ring casting. The gating system includes a casting shell and a runner shell. The top of the casting shell has multiple risers, which are separately positioned. The runner shell is located above the risers and has a pouring cup at its top. A branch runner is radially arranged around the bottom of the pouring cup, connecting to a guide runner. The guide runner corresponds one-to-one with the risers, and a baffle is located at the bottom periphery of the guide runner, blocking the top opening of the riser. This simple structure and uneven flow path easily lead to uneven filling of the mold cavity with molten metal, and excessively fast or slow flow rates, resulting in casting defects such as cold shuts, cracks, shrinkage cavities, porosity, and deformation, severely affecting the casting quality and yield. Especially in centrifugal casting or wax pattern casting, the flow stability of molten metal and the control of solidification sequence are more critical, and traditional gating structures often cannot meet the high-precision forming requirements of thin-walled castings. Summary of the Invention
[0004] In view of this, the present invention aims to provide an annular gating structure for casting thin-walled parts and a casting method for thin-walled parts. Through thermal modulus inversion design, centrifugal speed correction factor, integrated wax pattern molding, tangential swirling buffer, dewaxing and guiding, and optimized shell process, it solves the problems of simple structure and uneven flow path, which easily leads to uneven filling of molten metal in the mold cavity, excessively fast or slow flow rate, resulting in casting defects such as cold shuts, cracks, shrinkage cavities, porosity, and deformation, which seriously affect the forming quality and yield of castings. Especially in the process of centrifugal casting or wax pattern casting, the flow stability and solidification sequence control of molten metal are more critical, and traditional gating structures often cannot meet the high-precision forming requirements of thin-walled castings.
[0005] To address the above problems, the present invention provides an annular gating structure for casting thin-walled parts, comprising: a casting body, an annular gating system, multiple ingates, and 2-3 secondary ingates;
[0006] The annular gating system is located on the circular or semi-circular mounting end face of the casting body, and has a buffer cavity structure with an outer rectangular shape and an inner arc shape in cross-section.
[0007] The inner gate connects the inner wall of the annular runner to the casting body, and the secondary inner gate connects the outer wall of the annular runner to the external sprue.
[0008] The guzzle and the secondary guzzle are arranged circumferentially staggered;
[0009] An overflow blind cavity is provided at the top of the annular runner;
[0010] The inner edge of the annular runner is equipped with wax dewaxing guide ribs;
[0011] Both the gen gate and the secondary gen gate have a draft angle of 8° to 15°.
[0012] The cross-sectional area of each part along the pouring direction satisfies the following: total cross-sectional area of ingate: cross-sectional area of annular runner: total cross-sectional area of secondary ingate = 1:(1.2~2):(2~3), and the total cross-sectional area of ingate is 1%~3% of the projected area of the casting.
[0013] Furthermore, a tangential guide section is provided at the connection between the annular runner and the secondary ingate, and the length of the tangential guide section is 0.5 to 1.2 times the width of the annular runner;
[0014] The volume of the overflow blind cavity is such that the flow rate of a single ingate is 0.3~0.8s.
[0015] The cross-sectional area of the dewaxing guide rib is 2~4 mm².
[0016] Furthermore, the non-machined side of the casting body is provided with conformal wax reinforcing ribs, the thickness of which is 0.3 to 0.6 times the wall thickness of the casting, and the reinforcing ribs are integrally formed with the casting body and the annular gating system during the wax modeling stage.
[0017] A casting method for thin-walled parts, used to cast thin-walled castings through the aforementioned annular gating structure, the casting method comprising:
[0018] S1. Thermal modulus inversion and gating section design: Based on the thermal modulus M of the thin-walled section of the casting. t With thermal modulus M h The total cross-sectional area A of the ingate is calculated using formula (1). i ,
[0019] (1)
[0020] Where A p Let be the projected area of the casting in the pouring direction, k = 1%~3%, λ = 0.2~0.6, and λ be the centrifugal feeding correction coefficient.
[0021] The cross-sectional area of the annular runner is calculated using formula (2):
[0022] (2)
[0023] The total cross-sectional area of the secondary ingate is calculated using formula (3):
[0024] (3)
[0025] in, ω is the centrifugal speed correction factor, γ is the amplification factor, ω is the centrifugal angular velocity, r is the center radius of the ring, and g is the gravitational acceleration.
[0026] S2. One-piece wax molding: The casting body, conformal wax reinforcing ribs, annular runner, ingate and secondary ingate are formed by one-piece wax injection molding using a metal mold;
[0027] The conformal wax reinforcing ribs are disposed on the non-machined side of the casting, and the thickness is 0.3 to 0.6 times the wall thickness of the casting;
[0028] The inner wall of the annular gating system has 2 to 8 ingates, and the outer wall has 2 to 3 secondary ingates. The two are staggered circumferentially by π / n to 3π / 2n, where n is the number of ingates.
[0029] S3. Shell preparation: Prepare the surface layer and back layer on the surface of the wax model module;
[0030] The surface layer is prepared using zirconium acetate and yttrium oxide powder, with a viscosity of 15~30s, and two layers are coated.
[0031] The backing layer is prepared using silica sol and mullite powder, and is coated with 6 to 10 layers.
[0032] After coating the 3rd, 5th, and 7th back layers, the material was subjected to low-temperature intensive drying at 80℃ for 2 hours.
[0033] S4. Dewaxing and calcination: Dewaxing is carried out using a steam dewaxing kettle at a pressure of 5-7 bar for 6-8 minutes; after dewaxing, the product is first dried at 80-120℃ for 2-4 hours, and then calcined at 900-950℃ for 2-4 hours.
[0034] S5. Centrifugal casting: Preheat the mold shell to 900~950℃, and cast at a centrifugal speed of 150~220 r / min, control the current to 19~22A, and keep warm for ≥30min;
[0035] The centrifugal speed satisfies the formula for compensation distance:
[0036] t is the wall thickness of the casting. The centrifugation ratio is denoted as G, and G is controlled within the range of 1.2 to 2.5.
[0037] Furthermore, in step S2, the cross-section of the annular gating channel is a buffer cavity structure with an outer rectangle and an inner arc shape;
[0038] The connection between the secondary ingate and the annular runner is provided with a tangential guide section, the length of which is 0.5 to 1.2 times the width of the annular runner, to guide the molten metal to swirl tangentially along the inner wall of the annular runner;
[0039] The top of the annular runner is provided with 1 to 3 overflow blind cavities, the volume of which is 0.3 to 0.8 s of flow rate of a single ingate.
[0040] Furthermore, in step S2, the inner edge of the annular gating is provided with 2 to 4 wax dewaxing guide ribs, the cross-sectional area of which is 2 to 4 mm², which are evenly distributed along the circumference of the annular gating and are connected to the main gating of the module to guide the wax liquid to be discharged from the annular gating to the main gating during the dewaxing process.
[0041] Furthermore, in step S2, both the inner gate and the secondary inner gate are provided with a draft angle of 8°~15°.
[0042] When the thermal modulus M h >1.5M t When the secondary ingate is open, it connects to the annular runner; otherwise, the secondary ingate is closed or its cross-sectional area is reduced to less than 10% of the ingate's area.
[0043] Furthermore, in step S3, the zirconium acetate solution in the surface slurry has a mass fraction of 30%~40%, the yttrium oxide powder has a particle size of 200~350 mesh, and the mass ratio of zirconium acetate to yttrium oxide powder is 1:3~1:5.
[0044] The surface layer sand uses 60-100 mesh fused yttrium oxide sand;
[0045] The silica sol content in the backing slurry is 20%~40%, the mullite powder particle size is 200~350 mesh, and the mass ratio of silica sol to mullite powder is 1:0.9~1:1.5.
[0046] The backing sand is made of 30-60 mesh mullite sand.
[0047] Furthermore, in step S5, the pouring time t c Satisfy the formula
[0048] Where W is the total mass of the molten metal in the casting, ρ is the density of the molten metal, and v is the flow velocity of the molten metal at the ingate, controlled at v=0.3~0.8 m / s;
[0049] If the calculated t c If the value exceeds the preset range, adjust the number of ingates n or the cross-sectional area A. i However, the centrifugal speed ω remains unchanged.
[0050] Furthermore, in step S1, the thermal modulus M t and M h The calculation is based on solidification simulation using ProCAST or Magma software. Through iterative calculation, the location of shrinkage defects is moved from the casting body to the annular runner or secondary ingate area, with 2 to 3 iterations.
[0051] Compared with existing technologies, the annular gating structure and casting method for thin-walled parts described in this invention have the following advantages:
[0052] By introducing the thermal modulus inversion formula and the centrifugal speed correction factor Φ, precise design of the gating section was achieved. Combined with the tangential guide section and overflow blind cavity within the annular gating, the molten metal forms a stable unidirectional swirling flow within the cavity, completely eliminating annular concave defects. The use of integrated wax molding and conformal wax reinforcement technology eliminated welding deformation; coupled with dewaxing guide ribs and the timing control of "dewaxing-low temperature drying-high temperature firing," the expansion and deformation of thin-walled parts during dewaxing and firing processes were effectively suppressed. By establishing the feeding distance formula L=(80~100)·t·G, the centrifugal speed was directly linked to the feeding distance, and the centrifugal ratio G was limited to the optimal range of 1.2~2.5. This significantly lengthened the effective feeding distance of the ingate, greatly reducing shrinkage cavities and porosity defects at hot spots and lowering the crack defect rate. Combining numerical simulation (ProCAST / Magma) with physical experiments, the optimal process parameters could be determined through 2~3 iterations. Standardized gating design and parameter control ensure high process repeatability, making it suitable for mass production of thin-walled ring parts made of various materials (titanium alloys, high-temperature alloys, stainless steel, etc.). This significantly reduces scrap and rework rates, simplifies the wax mold welding process, improves production efficiency, and lowers energy consumption and manufacturing costs. Attached Figure Description
[0053] Figure 1 This is a schematic diagram of the casting and gating system described in the embodiments of this application;
[0054] Figure 2 This is a welding diagram of the wax mold and multi-layer mold frame as described in the embodiments of this application.
[0055] Explanation of reference numerals in the attached figures:
[0056] 1-Secondary ingate, 2-Annular runner, 3-Ingate, 4-Casting body, 5-Wax pattern, 6-Mold frame. Detailed Implementation
[0057] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0058] In this invention, the terms "first," "second," "upper," and "lower," etc., are used for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first," "second," "upper," or "lower" may explicitly or implicitly include at least one of those features. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. Where the technical solutions of the embodiments can be combined, they are all within the scope of protection claimed by this invention.
[0059] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0060] like Figure 1 and Figure 2 As shown, an annular runner structure for casting thin-walled parts includes: a casting body 4, an annular runner 2, multiple ingates 3, and 2-3 secondary ingates 1. The annular runner 2 is located on the circular or semi-circular mounting end face of the casting body 4, and has a buffer cavity structure with an outer rectangular and inner arc-shaped cross-section. The ingates 3 connect the inner wall of the annular runner 2 to the casting body 4, and the secondary ingates 1 connect the outer wall of the annular runner 2 to the external sprue. The ingates 3 and secondary ingates 1 are circumferentially staggered. An overflow blind cavity is provided at the top of the annular runner 2. Wax dewaxing guide ribs are provided on the inner edge of the annular runner 2. Both the ingates 3 and the secondary ingates 1 have a draft angle of 8° to 15°. The cross-sectional area of each part along the pouring direction satisfies the following: total cross-sectional area of secondary ingate 1: cross-sectional area of annular runner 2: total cross-sectional area of ingate 3 = 1:(1.2~2):(2~3), and the total cross-sectional area of ingate 3 is 1%~3% of the projected area of the casting.
[0061] The annular runner 2 structure described in this application is not limited to the casting body 4 with a circular or semi-circular mounting end face, but can also be applied to other shapes such as a fan shape. The function of the annular runner 2 is to reduce stress concentration, and its structure is a buffer cavity used to absorb the impact of molten metal, reducing flash and porosity. The number of gates is adapted to the casting structure. Preferably, 2-8 ingates 3 are provided, and the molten metal flow rate is controlled by circumferentially staggering the ingates 3 and the secondary ingates 1, preventing cold shuts and cracks. The cross-sectional shape of the ingates 3, the annular runner 2, and the secondary ingates 1 is consistent with the circular or semi-circular cross-section of the casting, which facilitates mold processing and molten metal flow. Both the ingates 3 and the secondary ingates 1 are wedge-shaped structures, and the draft angle is controlled between 8° and 15°, which facilitates demolding and reduces stress concentration. If there are thick parts or hot spots in the casting, an auxiliary runner can be designed to connect the location and the annular runner 2 to provide local shrinkage compensation and reduce shrinkage cavities.
[0062] The key features of this gating system are:
[0063] 1. Stable molten metal flow, reducing defects.
[0064] By setting multiple ingates 3 and connecting them to the annular runner 2, uniform distribution and stable filling of the molten metal can be achieved, reducing defects such as turbulence, flash, porosity and cold shuts in the molten metal during the filling process.
[0065] The annular runner 2 acts as a buffer chamber, effectively absorbing the impact energy of the molten metal, further improving the flow stability and reducing stress concentration.
[0066] 2. Highly controllable and adaptable to complex structures
[0067] The intersecting arrangement of the inner gate 3 and the secondary inner gate 1 enables precise control of the molten metal flow rate, making it suitable for castings with complex structures and large differences in wall thickness, thus avoiding localized overcooling or cracking.
[0068] If the casting has thick sections or hot spots, auxiliary runners can be set up for localized feeding to effectively prevent defects such as shrinkage cavities and porosity.
[0069] 3. Convenient mold processing
[0070] The cross-sectional shape of all gates and runners is consistent with the circular or semi-circular cross-section of the casting, which facilitates mold processing and improves the manufacturing accuracy and efficiency of the mold.
[0071] The wedge-shaped structure and 8°~15° draft angle design facilitate demolding, reduce mold wear, and extend mold life.
[0072] 4. Optimization of the ratio of gate quantity to cross-sectional area
[0073] Ingate 3 and secondary ingate 1 can be flexibly configured according to the size and structure of the casting to ensure uniform distribution of molten metal.
[0074] The ratio of the cross-sectional area of each gating gate along the pouring direction is: total cross-sectional area of secondary ingate 1: cross-sectional area of annular runner 2: total cross-sectional area of ingate 3 = 1:(1.2~2):(2~3), which can ensure smooth flow of molten metal and avoid flow resistance or pressure loss caused by abrupt changes in cross-section.
[0075] During the casting process, the molten metal enters the annular runner 2 from the secondary ingate 1 and then rapidly splits to both sides, entering the mold through the ingate 3 to complete the casting process. As is known to those skilled in the art, during this process, due to the high flow rate of the molten metal, it flows entirely to the ingate 3 before completely filling the annular runner. Therefore, the flowability of the molten metal cannot be reflected relative to the radial interface; when calculating the cross-sectional area, the cross-sectional area along the casting direction is usually calculated.
[0076] In a specific embodiment, the total cross-sectional area of the secondary ingate is 108 mm² (two 4.5 mm × 12 mm rectangular sections), the total cross-sectional area of the annular runner is 158.5 mm² (the cross-section consists of a 10 mm diameter semicircle + a 4 mm × 10 mm rectangle; the molten metal flows to the left and right after entering, so the number of cross-sections is calculated as twice), and the total cross-sectional area of the ingate is 238 mm² (four 3.5 mm × 17 mm rectangular sections). The ratio of the cross-sectional areas of the three is: total cross-sectional area of the secondary ingate: cross-sectional area of the annular runner: total cross-sectional area of the ingate = 1:1.46:2.2, which falls entirely within the preferred range of 1:(1.2~2):(2~3). Testing revealed that at this ratio, after the molten metal entered the annular runner from the secondary ingate, the flow velocity decreased from 1.2 m / s to 0.45 m / s, resulting in smooth filling without turbulence. The tangential guide section facilitated unidirectional swirling flow of the molten metal, completely preventing the annular core from impacting the cold shut. The overflow blind cavity effectively captured the leading-edge slag, eliminating slag inclusions. The ingate provided ample feeding channels, and shrinkage cavities at hot spots were completely migrated into the annular runner. The final casting yield reached 98%, with a crack defect rate of 5%, a surface slag loss defect rate of 2%, and an internal shrinkage cavity and porosity defect rate of 20%, perfectly matching the beneficial effects of this invention.
[0077] The following comparison is made between two comparative examples and the embodiments.
[0078] Comparative Example 1
[0079] The cross-sectional dimensions of the secondary ingate and the main gate remain consistent with the example, except that the cross-sectional dimensions of the annular runner are reduced to "8mm semicircle diameter + 3mm × 8mm rectangle". After the flow is split, the total cross-sectional area is 97.1mm², and the ratio of the three cross-sectional areas is 1:0.9:2.2, which is lower than the lower limit requirement of 1:(1.2~2). Due to the insufficient volume of the annular runner buffer cavity, the molten metal cannot be effectively decelerated after entering from the secondary ingate, and the flow velocity remains above 1.1m / s. On the one hand, it directly impacts the inner wall of the shell, generating air entrapment; on the other hand, the uneven flow splitting causes the two streams of molten metal to collide head-on in the annular core area, forming cold shut defects. At the same time, the excessively high flow velocity prevents the leading cold slag from entering the overflow blind cavity and is directly flushed into the casting cavity, forming inclusions. After testing, the casting forming rate under this ratio is only 62%, the proportion of cold shut defects is 28%, the proportion of porosity defects is 10%, and the proportion of shrinkage cavities and porosity defects is 15%, all of which are far lower than those in Example 1.
[0080] Comparative Example 2
[0081] The cross-sectional dimensions of the secondary ingate and annular runner remain consistent with the example, except that the cross-sectional dimensions of the ingate are reduced to 3mm × 14mm, with a total cross-sectional area of 168mm². At this point, the ratio of the three cross-sectional areas is 1:1.46:1.6, lower than the lower limit requirement of 1:(2~3). Due to the insufficient total cross-sectional area of the ingate, the flow velocity of the molten metal through the ingate reaches as high as 0.95m / s, and the feeding channel of a single ingate is too narrow, failing to provide sufficient feeding molten metal to the hot spot area. Simultaneously, the ingate modulus is too small, resulting in a faster solidification rate than the hot spot area, prematurely blocking the feeding channel and causing concentrated shrinkage cavities at the hot spot. Testing revealed that the casting success rate at this ratio is only 70%, with shrinkage cavities and porosity defects accounting for as high as 45%, crack defects accounting for 12%, and surface slag defects accounting for 8%, all significantly lower than the quality level of Example 1.
[0082] Furthermore, if the cross-sectional area ratio exceeds the upper limit (such as the cross-sectional area ratio of the annular runner reaching 1:2.2:2.2, or the total cross-sectional area ratio of the ingate reaching 1:1.46:3.2), the solidification speed of the annular runner / ingate will be slower than that of the casting body, which will become a heat point and transfer heat to the casting, resulting in shrinkage and porosity of the casting. At the same time, an excessively large runner cross-sectional area will increase the waste of molten metal and increase the cost of subsequent runner cutting and grinding processes, which also does not meet the requirements of industrial production.
[0083] In summary, only by strictly controlling the ratio of the total cross-sectional area of the secondary ingate to the cross-sectional area of the annular runner to the total cross-sectional area of the ingate within the range of 1:(1.2~2):(2~3) can the technical effects of stable molten metal filling, sufficient feeding, minimal defects, and optimal cost be achieved simultaneously.
[0084] 5. The cross-sectional area of the ingate matches the projected area of the casting.
[0085] The total cross-sectional area of the inner gate 3 is 1% to 3% of the projected area of the casting in the casting direction, which ensures the supply capacity of molten metal and avoids the waste of molten metal and the weak structure of the casting caused by an excessively large gate.
[0086] The gating system, through multi-stage diversion, wedge gate, annular buffer cavity, and cross-sectional area ratio optimization, can achieve the stability, controllability and uniformity of molten metal flow, and can effectively prevent the deformation of wax mold 5 during shell making and metal solidification shrinkage.
[0087] Furthermore, a tangential guide section is provided at the connection between the annular runner 2 and the secondary ingate 1, the length of which is 0.5 to 1.2 times the width of the annular runner 2. The volume of the overflow blind cavity is equivalent to the flow rate of a single ingate of 30.3 to 0.8 s. The cross-sectional area of the dewaxing guide rib is 2 to 4 mm².
[0088] In the centrifugal casting of thin-walled rings, if the molten metal enters the annular runner 2 from the secondary ingate 1 and flows radially (i.e., the flow direction is directly towards the center of the ring), it will cause two serious problems:
[0089] Circular counter-collision cold shut: When multiple ingates 3 are opened on the annular runner 2, two streams of molten metal coming from opposite directions will collide head-on in the annular region. The leading cold metal and oxide scale are "sandwiched" in the center, forming a cold shut or annular shrinkage cavity.
[0090] Turbulent gas entrainment: Radial direct impact generates strong turbulence within the annulus, entraining residual gas inside the shell into the molten metal, forming pores.
[0091] The function of the tangential guide section is to forcibly change this "radial straight flow" into a "tangential swirling flow":
[0092] After the molten metal enters the annular runner 2, it flows in a unidirectional rotation along the inner wall (in the same direction as the centrifuge or manually set). The molten metal flows in a relay rather than a counter-current within the annular runner. The cold metal at the forefront is naturally pushed into the overflow blind cavity, and the fresh molten metal fills the mold smoothly.
[0093] This is equivalent to changing "two water columns colliding" into "water flowing in a swirling pattern along a ring-shaped channel", completely eliminating the confluence defect at the center of the ring.
[0094] The liquid flow needs a certain "turning distance" within the runner to adhere to the wall and form a tangential flow. If the length of the tangential guide section is less than 0.5 times the width, the liquid flow cannot turn in time and will still rush radially, rendering the tangential guide ineffective. If the length of the tangential guide section is greater than 1.2 times, the excessively long guide section will cause the molten metal to flow too far within the guide section, resulting in a large temperature drop, premature solidification and blockage, increased flow resistance, the need for higher centrifugal pressure, occupied mold space, and increased manufacturing costs. Therefore, the preferred length of the tangential guide section is 0.5 to 1.2 times the width of the annular runner 2, ensuring that the liquid flow direction is effectively turned, avoiding collision, and achieving the best balance between effective guidance and flow resistance / temperature drop.
[0095] During molten metal filling, it takes approximately 0.2 to 0.3 seconds of flow rate to completely collect the leading cold metal and surface oxide scale. If the volume of the overflow blind cavity is less than 0.3 seconds, the cavity is too small, and the cold slag will overflow back into the annular gating 2, contaminating the casting. If the volume of the overflow blind cavity is greater than 0.8 seconds, too much molten metal will remain in the cavity, prolonging the solidification time and creating a "large hot spot," which may transfer heat to the casting in the reverse direction through the annular gating 2, leading to shrinkage porosity. Simultaneously, excessive molten metal retention wastes material and increases the difficulty of cutting. Therefore, the overflow blind cavity volume is set at a flow rate of 30.3 to 0.8 seconds per stream from the ingate, ensuring that the leading cold metal and slag are completely captured, preventing the blind cavity itself from becoming a source of shrinkage cavities, and guaranteeing the directionality of feeding.
[0096] During steam dewaxing, the wax viscosity is approximately 0.01~0.05 Pa·s. Under a pressure of 5~7 bar, a channel with a dewaxing guide rib cross-sectional area of 2 mm² ensures a wax flow rate >1 m / s, preventing wax stagnation in thin-walled areas and thus avoiding "wax swelling" (cracking of the wet mold by the wax). If the dewaxing guide rib cross-sectional area is >4 mm², the excessively large cross-section results in too many protrusions on the wax mold, affecting the contour of the non-machined surfaces of the casting. This leaves voids after dewaxing, which are prone to slurry accumulation during shell making, leading to uneven drying and increased post-processing cutting workload. Therefore, setting the dewaxing guide rib cross-sectional area to 2~4 mm² ensures smooth wax drainage, prevents bulging deformation of thin-walled parts, and minimizes the impact on the casting structure and post-processing.
[0097] Furthermore, the non-machined side of the casting body 4 is provided with conformal wax reinforcing ribs, the thickness of which is 0.3 to 0.6 times the wall thickness of the casting, and the reinforcing ribs are integrally formed with the casting body 4 and the annular gating 2 in the wax mold 5 stage.
[0098] In the fifth stage of wax modeling, a one-piece molded conformal wax reinforcing rib (thickness = 0.3~0.6 times the wall thickness) provides temporary rigidity for the thin-walled ring, preventing elliptic deformation during shell making and handling, while ensuring smooth dewaxing and post-processing feasibility.
[0099] A casting method for a thin-walled part, comprising casting the thin-walled part through the aforementioned annular gating structure, the casting method comprising:
[0100] S1. Thermal modulus inversion and gating section design: Based on the thermal modulus M of the thin-walled section of the casting. t With thermal modulus M h The total cross-sectional area A of the ingate is calculated using formula (1). i ,
[0101] (1)
[0102] Where A p λ is the projected area of the casting in the pouring direction, k = 1%~3%, λ = 0.2~0.6 is the centrifugal feeding correction coefficient.
[0103] Those skilled in the art are well aware that the classic empirical formula for predicting the solidification time of castings in foundry science—the Chvorinov modulus method—is as follows:
[0104] (4)
[0105] Modulus M = V / A 表 The larger the size, the longer the solidification time.
[0106] The design principle of Henkin's internal gating system is M i >M h That is, the modulus of the ingate must be greater than the modulus of the hot spot to ensure that the ingate solidifies last.
[0107] Empirical method for projected area:
[0108] In investment casting, the total cross-sectional area of the ingate is often selected empirically as 1% to 3% of the projected area of the casting.
[0109]
[0110] Based on the above principles of metal M i >M h Furthermore, for thin-walled parts, the ingate is usually designed as a long wedge shape with a uniform cross-section, and its module is approximately M. i ≈t i / 2,t i The equivalent thickness of the ingate.
[0111] To ensure that the ingate solidifies later than the hot spot, the following relationship must be satisfied:
[0112]
[0113] Cross-sectional area A i ∝t i , so A i Need to follow th (i.e. M) h )enlarge.
[0114] Express the magnification factor as a function of the modulus ratio:
[0115]
[0116] in, λ represents the relative severity of the thermal knot, and λ is the correction intensity coefficient. Formula (1) is obtained from the above formulas.
[0117] In centrifugal casting, centrifugal pressure This provides additional feeding force, reducing the dependence on the ingate modulus. Therefore, λ takes a value less than 1 (λ≈1 under gravity, λ=0.2∼0.6 under centrifugal field). The centrifugal ratio G=ω 2 The larger the r / g, the stronger the centrifugal compensation capability, and λ can take a smaller value. λ=0.2~0.6 covers the typical working range of G=1.2~2.5.
[0118] The thermal modulus M t and M h The calculation is based on solidification simulation using ProCAST or Magma software. Through iterative calculation, the location of shrinkage defects is moved from the casting body to the annular runner or secondary ingate area, with 2 to 3 iterations.
[0119] The cross-sectional area of the annular runner is calculated using formula (2):
[0120] (2)
[0121] The total cross-sectional area of the secondary ingate is calculated using formula (3):
[0122] (3)
[0123] in, ω is the centrifugal speed correction factor, γ is the amplification factor, ω is the centrifugal angular velocity (ω=15.7~23 rad / s), r is the center radius of the ring, and g is the gravitational acceleration.
[0124] The above formula for the centrifugal speed correction factor Φ is a modified empirical construct based on the known physical relationships of centrifugal casting, specifically for the scenario of "thin-walled ring parts + annular buffer gating".
[0125] As is known to those skilled in the art, during centrifugal casting, the molten metal is subjected to both gravitational force and centrifugal force, and the resulting additional feeding pressure gradient can be derived from the basic equations of fluid mechanics:
[0126]
[0127] The centrifugal additional pressure is obtained by integration: .
[0128] This pressure is related to the static pressure head under gravity. The ratio is the centrifugal ratio. Under the process parameters of this invention (G=1.2~2.5), centrifugal feeding capability is significantly better than that under gravity.
[0129] According to Chvorinov's modulus method (t s =B·M 2 ) and Henkin's internal gating principle (M 内 >M 热 The annular runner serves as a buffer and feeding channel, with a reference cross-sectional area A. c0 =A i ×(1.2~2). Under centrifugal force, since centrifugal pressure provides additional feeding driving force, the absolute dependence on the modulus of the annular runner is reduced. Therefore, it is necessary to dynamically adjust the value by multiplying it by the correction factor Φ.
[0130] This invention constructs a correction factor:
[0131] =1+γ·G.
[0132] Among them, constant term 1 corresponds to the gravitational field baseline state (Φ=1 when G=0); the γ·G term reflects the compensation requirement of the centrifugal force field on the cross-sectional area of the annular runner. The coefficient γ was calibrated using a combination of solidification simulation and physical experiments with ProCAST software: iterative calculations were performed within the range of ω=15.7~23 rad / s and G=1.2~2.5, using whether the location of shrinkage cavities had completely migrated to the annular runner or secondary ingate region as the evaluation index. The results show that:
[0133] When γ < 0.1, the Φ value is too small, the cross-sectional area of the annular runner is not sufficiently enlarged, the feeding channel is prone to premature solidification at high speed, and shrinkage porosity occurs at the hot spot of the casting.
[0134] When γ>0.2, the value of Φ is too large, and the cross-sectional area of the annular runner is too large. This not only wastes molten metal, but also prolongs the solidification time of the annular runner itself, which in turn becomes a heat point and transfers heat to the casting, resulting in shrinkage cavities.
[0135] When γ=0.15, the cross-sectional area of the annular runner is perfectly matched with the centrifugal speed, and the casting forming rate reaches over 98%.
[0136] Therefore, γ is preferably 0.1 to 0.2, and more preferably 0.15.
[0137] Through the above derivation, the centrifugal speed parameter is directly related to the cross-sectional area of the gating, thus realizing the precise dynamic design of the gating section of the centrifugal precision casting of thin-walled ring parts.
[0138] S2. One-piece wax molding: The casting body, conformal wax reinforcing ribs, annular runner, ingate and secondary ingate are formed by one-piece wax injection molding using a metal mold;
[0139] The conformal wax reinforcing ribs are disposed on the non-machined side of the casting, and the thickness is 0.3 to 0.6 times the wall thickness of the casting;
[0140] The inner wall of the annular gating system has 2 to 8 ingates, and the outer wall has 2 to 3 secondary ingates. The two are staggered circumferentially by π / n to 3π / 2n, where n is the number of ingates.
[0141] The inner edge of the annular gating is provided with 2 to 4 wax dewaxing guide ribs, the cross-sectional area of which is 2 to 4 mm². The guide ribs are evenly distributed along the circumference of the annular gating and are connected to the main gating of the module. They are used to guide the wax liquid to be discharged from the annular gating to the main gating during the dewaxing process.
[0142] Both the inner gate and the secondary inner gate are provided with a draft angle of 8° to 15°.
[0143] When the thermal modulus M h >1.5M t When the secondary ingate is open, it connects to the annular runner; otherwise, the secondary ingate is closed or its cross-sectional area is reduced to less than 10% of the ingate's area.
[0144] The annular gating channel has a buffer cavity structure with an outer rectangle and an inner arc shape.
[0145] The connection between the secondary ingate and the annular runner is provided with a tangential guide section, the length of which is 0.5 to 1.2 times the width of the annular runner, to guide the molten metal to swirl tangentially along the inner wall of the annular runner;
[0146] The top of the annular runner is provided with 1 to 3 overflow blind cavities, the volume of which is 0.3 to 0.8 s of flow rate of a single ingate.
[0147] Metal molds are made according to the designed casting system and casting. The secondary endogate, annular runner, endogate, and casting body are integrally formed in the metal mold, reducing welding time and finishing processes. Integrating the secondary endogate, annular runner, endogate, and casting body in the metal mold aims to ensure consistency between the casting system and the wax model body through identical wax injection parameters, reducing deviations caused by manual welding of the casting system and casting body, and deformation caused by localized heating of the soldering iron during assembly. After the wax model is made, the secondary endogate of the wax model is connected to the multi-layer mold frame 6, allowing multiple wax models to be welded together to form a complete casting assembly.
[0148] S3. Shell preparation: Prepare the surface layer and back layer on the surface of the wax model module;
[0149] The surface layer is prepared using zirconium acetate and yttrium oxide powder, with a viscosity of 15~30s (4# flow cup), and two layers are coated.
[0150] The backing layer is prepared using silica sol and mullite powder, and is coated with 6 to 10 layers.
[0151] After coating the 3rd, 5th, and 7th back layers, the material was subjected to low-temperature intensive drying at 80℃ for 2 hours.
[0152] The surface slurry contains 30%–40% zirconium acetate solution by mass, 200–350 mesh yttrium oxide powder, and a slurry viscosity controlled at 15–30 seconds (using a #4 flow cup). During preparation, yttrium oxide powder is slowly added to the zirconium acetate solution at a mass ratio of 1:3 to 1:5.
[0153] The surface layer sand uses 60-100 mesh fused yttrium oxide sand;
[0154] Under stirring conditions, the material is thoroughly dispersed. The primary stirring time is no less than 60 minutes, with a rotation speed of 300-800 r / min, to form a uniform and stable slurry. The secondary stirring time is 20-50 minutes, with a rotation speed of 700-1200 r / min. When applying the coating, the module is fully in contact with the surface slurry by immersion or spraying. The temperature in the coating chamber is controlled at 22±2℃, and the humidity is controlled above 90%. The surface sand uses fused yttrium oxide sand with a particle size of 60-100 mesh. The surface drying time is 8-24 hours, with the drying chamber temperature controlled at 22±2℃ and the humidity controlled at 60-80%.
[0155] The backing slurry contains 20%–40% silica sol by mass, and mullite powder with a particle size of 200–350 mesh. The mass ratio of silica sol to mullite powder is 1:0.9–1:1.5. During coating, the module is immersed in the backing slurry. 30–60 mesh mullite sand is used for the backing layer. The backing layer drying time is 8–24 hours, with the drying room temperature controlled at 23±2℃ and the humidity controlled at 50–70%.
[0156] The wax model and the multi-layer mold frame 6 are welded together using tools such as a soldering iron. The secondary ingate is welded to the multi-layer mold frame 6. The angle between the wax model and the multi-layer mold frame 6 is 30-50° to facilitate the flow of molten metal and the discharge of gas.
[0157] The assembled modules are cleaned by immersing them in a water-based cleaning solution containing surfactants. The solution has a pH of 8–10 and a temperature of 40–60°C. The cleaning time is 5–15 minutes. This step removes mold release agents, grease, and other organic contaminants from the wax model surface. After cleaning, the wax model is rinsed in deionized or distilled water at 20–40°C for 3–10 minutes to remove any remaining cleaning solution and dissolved impurities. After rinsing, the wax model is air-dried at 40–80°C and 30%–50% relative humidity until no moisture remains on the surface.
[0158] S4. Dewaxing and Calcination: Dewaxing is performed using a steam dewaxing kettle at a pressure of 5-7 bar for 6-8 minutes. These parameters reduce the probability of surface material re-dissolving and flaking, and reduce internal inclusion defects in the casting. After dewaxing, the casting is first dried at 80-120℃ for 2-4 hours, and then heated to 900-950℃ for 2-4 hours.
[0159] S5. Centrifugal casting: Preheat the mold shell to 900~950℃, and cast at a centrifugal speed of 150~220 r / min, control the current to 19~22A, and keep warm for ≥30min;
[0160] The centrifugal speed satisfies the formula for compensation distance:
[0161] t is the wall thickness of the casting. The centrifugation ratio is denoted as G, and G is controlled within the range of 1.2 to 2.5.
[0162] Pouring time t c Satisfying the formula:
[0163] Where W is the total mass of the molten metal in the casting, ρ is the density of the molten metal, and v is the flow velocity of the molten metal at the ingate, controlled at v=0.3~0.8 m / s;
[0164] If the calculated t c If the value exceeds the preset range, adjust the number of ingates n or the cross-sectional area A. i However, the centrifugal speed ω remains unchanged.
[0165] These process parameters enable 98% forming of thin-walled castings and reduce the number of shrinkage cavities and porosity inside the castings.
[0166] The casting yield using the method of this application is significantly improved. Actual implementation results show that the casting yield has increased from 85% to 98%.
[0167] The defect rate has also decreased significantly, with crack defects decreasing from 15% to 5%, surface flaking defects decreasing from 10% to 2%, and internal defects decreasing from 63% to 20%.
[0168] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. An annular gating structure for casting thin-walled parts, characterized in that, include: The casting body (4), the annular gating system (2), multiple ingates (3) and 2-3 secondary ingates (1); The annular gating channel (2) is set on the circular or semi-circular mounting end face of the casting body (4), and the cross-section is a buffer cavity structure with an outer rectangle and an inner arc. The inner gate (3) connects the inner wall of the annular runner (2) to the casting body (4), and the secondary inner gate (1) connects the outer wall of the annular runner (2) to the external sprue; The guzzle (3) and the secondary guzzle (1) are arranged circumferentially offset; The top of the annular runner (2) is provided with an overflow blind cavity; The inner edge of the annular runner (2) is provided with wax dewaxing guide ribs; Both the inner gate (3) and the secondary inner gate (1) have a draft angle of 8°~15°; The cross-sectional area of each part along the pouring direction satisfies: the total cross-sectional area of the secondary ingate (1) is equal to the cross-sectional area of the annular runner (2) and the total cross-sectional area of the ingate (3) is 1:(1.2~2):(2~3), and the total cross-sectional area of the ingate (3) is 1%~3% of the projected area of the casting.
2. The annular gating structure for casting thin-walled parts according to claim 1, characterized in that, A tangential guide section is provided at the connection between the annular runner (2) and the secondary ingate (1), and the length of the tangential guide section is 0.5 to 1.2 times the width of the annular runner (2); The volume of the overflow blind cavity is the flow rate of a single inlet gate (3) of 0.3~0.8s; The cross-sectional area of the dewaxing guide rib is 2~4 mm².
3. The annular gating structure for casting thin-walled parts according to claim 1, characterized in that, The non-machined side of the casting body (4) is provided with conformal wax reinforcing ribs. The thickness of the reinforcing ribs is 0.3 to 0.6 times the wall thickness of the casting. The reinforcing ribs are integrally formed with the casting body (4) and the annular gating (2) in the wax mold (5) stage.
4. A casting method for thin-walled parts, characterized in that: A casting method for casting thin-walled castings using the annular gating structure as described in any one of claims 1-3, the casting method comprising: S1. Thermal modulus inversion and gating section design: Based on the thermal modulus M of the thin-walled section of the casting. t With thermal modulus M h The total cross-sectional area A of the ingate is calculated using formula (1). i , (1) Where A p Let be the projected area of the casting in the pouring direction, k = 1%~3%, λ = 0.2~0.6, and λ be the centrifugal feeding correction coefficient. The cross-sectional area of the annular runner is calculated using formula (2): (2) The total cross-sectional area of the secondary ingate is calculated using formula (3): (3) in, ω is the centrifugal speed correction factor, γ is the amplification factor, ω is the centrifugal angular velocity, r is the center radius of the ring, and g is the gravitational acceleration. S2. One-piece wax molding: The casting body, conformal wax reinforcing ribs, annular runner, ingate and secondary ingate are formed by one-piece wax injection molding using a metal mold; The conformal wax reinforcing ribs are disposed on the non-machined side of the casting, and the thickness is 0.3 to 0.6 times the wall thickness of the casting; The inner wall of the annular gating system has 2 to 8 ingates, and the outer wall has 2 to 3 secondary ingates. The two are staggered circumferentially by π / n to 3π / 2n, where n is the number of ingates. S3. Shell preparation: Prepare the surface layer and back layer on the surface of the wax model module; The surface layer is prepared using zirconium acetate and yttrium oxide powder, with a viscosity of 15~30s, and two layers are coated. The backing layer is prepared using silica sol and mullite powder, and is coated with 6 to 10 layers. After coating the 3rd, 5th, and 7th back layers, the material was subjected to low-temperature intensive drying at 80℃ for 2 hours. S4. Dewaxing and calcination: Dewaxing is carried out using a steam dewaxing kettle at a pressure of 5-7 bar for 6-8 minutes; after dewaxing, the product is first dried at 80-120℃ for 2-4 hours, and then calcined at 900-950℃ for 2-4 hours. S5. Centrifugal casting: Preheat the mold shell to 900~950℃, and cast at a centrifugal speed of 150~220 r / min, control the current to 19~22A, and keep warm for ≥30min; The centrifugal speed satisfies the formula for compensation distance: t is the wall thickness of the casting. The centrifugation ratio is denoted as G, and G is controlled within the range of 1.2 to 2.
5.
5. The casting method according to claim 4, characterized in that: In step S2, the cross-section of the annular gating channel is a buffer cavity structure with an outer rectangle and an inner arc shape; The connection between the secondary ingate and the annular runner is provided with a tangential guide section, the length of which is 0.5 to 1.2 times the width of the annular runner, to guide the molten metal to swirl tangentially along the inner wall of the annular runner; The top of the annular runner is provided with 1 to 3 overflow blind cavities, the volume of which is 0.3 to 0.8 s of flow rate of a single ingate.
6. The casting method according to claim 4, characterized in that: In step S2, the inner edge of the annular gating is provided with 2 to 4 wax dewaxing guide ribs, the cross-sectional area of which is 2 to 4 mm², which are evenly distributed along the circumference of the annular gating and are connected to the main gating of the module. They are used to guide the wax liquid to be discharged from the annular gating to the main gating during the dewaxing process.
7. The casting method according to claim 4, characterized in that: In step S2, both the inner gate and the secondary inner gate are provided with a draft angle of 8°~15°; When the thermal modulus M h >1.5M t When the secondary ingate is open, it connects to the annular runner; otherwise, the secondary ingate is closed or its cross-sectional area is reduced to less than 10% of the ingate's area.
8. The casting method according to claim 4, characterized in that: In step S3, the zirconium acetate solution in the surface slurry has a mass fraction of 30%~40%, the yttrium oxide powder has a particle size of 200~350 mesh, and the mass ratio of zirconium acetate to yttrium oxide powder is 1:3~1:5; The surface layer sand uses 60-100 mesh fused yttrium oxide sand; The silica sol content in the backing slurry is 20%~40%, the mullite powder particle size is 200~350 mesh, and the mass ratio of silica sol to mullite powder is 1:0.9~1:1.
5. The backing sand is made of 30-60 mesh mullite sand.
9. The casting method according to claim 4, characterized in that: In step S5, the pouring time t c Satisfy the formula Where W is the total mass of the molten metal in the casting, ρ is the density of the molten metal, and v is the flow velocity of the molten metal at the ingate, controlled at v=0.3~0.8 m / s; If the calculated t c If the value exceeds the preset range, adjust the number of ingates n or the cross-sectional area A. i However, the centrifugal speed ω remains unchanged.
10. The casting method according to claim 4, characterized in that: In step S1, the thermal modulus M t and M h The calculation is based on solidification simulation using ProCAST or Magma software. Through iterative calculation, the location of shrinkage defects is moved from the casting body to the annular runner or secondary ingate area, with 2 to 3 iterations.
Citation Information
Patent Citations
High temperature alloy thin-wall annular casting pouring system and manufacturing method
CN105312504A