A laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composites
By using laser-arc composite additive manufacturing technology, uniform dispersion and interfacial bonding of TC4 particles in AZ91 magnesium matrix were achieved, solving the problems of uneven distribution of reinforcing phase and porosity defects in traditional methods, and improving material utilization and preparation efficiency.
Patent Information
- Application Number
- CN202611305299.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional methods struggle to achieve uniform dispersion and good interfacial bonding of TC4 particles in magnesium alloy matrices, resulting in uneven distribution of reinforcing phases, difficulty in controlling interfacial reactions, and porosity defects. Furthermore, the preparation process is costly and time-consuming.
Using laser-arc composite additive manufacturing technology, a multi-laser coaxial composite additive manufacturing equipment integrating wire feeder, powder feeder, and laser and arc composite heat source is used. TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire are used as raw materials. The additive manufacturing parameters are optimized to achieve uniform dispersion and interfacial bonding of TC4 particles in AZ91 magnesium matrix.
This method achieves uniform dispersion and good interfacial bonding of TC4 particles in AZ91 magnesium matrix, avoiding uneven distribution of reinforcing phase and porosity defects in traditional methods. It also results in high material utilization and suitability for industrial applications.
Smart Images

Figure CN123060116A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing technology of metal matrix composites, specifically relating to a laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composites. Background Technology
[0002] Magnesium alloys, as the lightest metallic structural materials, possess high specific strength, high specific stiffness, excellent damping properties, and electromagnetic shielding performance, making them promising for applications in aerospace, automotive lightweighting, and electronic communications. However, traditional magnesium alloys (such as AZ91) suffer from low absolute strength, insufficient elastic modulus, poor high-temperature performance, and poor wear resistance, limiting their application in critical load-bearing components. By introducing high-strength, high-modulus ceramic or metallic particles (such as SiC, TiC, and Ti particles) into the magnesium alloy matrix to prepare particle-reinforced magnesium matrix composites, their mechanical properties and service performance can be significantly improved.
[0003] TC4 titanium alloy particles possess high melting point, high specific strength, and certain interfacial compatibility with magnesium alloys, making them ideal candidates for reinforcing phases. However, the melting point of TC4 particles (approximately 1600℃) is much higher than that of AZ91 magnesium alloy (approximately 596℃). When preparing TC4 / AZ91 magnesium-based composites using traditional casting or stir casting methods, defects such as uneven distribution of the reinforcing phase, severe agglomeration, coarse matrix grains, and porosity are prone to occur. Furthermore, these methods require molds, resulting in high costs and long production cycles.
[0004] Additive manufacturing technology offers new approaches to the preparation of metal matrix composites. Among these, WAAM (Wire-Arc Additive Manufacturing) is highly efficient and low-cost, but its limited heat source energy density makes it difficult to fully melt high-melting-point TC4 particles. While laser-powder bed melting (LPBF) can achieve precise micro-area melting, it is inefficient, expensive, and the flammable and explosive nature of magnesium alloy powder poses significant safety hazards. Laser-arc composite additive manufacturing technology combines the advantages of high laser energy density and high heat input efficiency of electric arc. By coordinating the temperature and flow fields of the molten pool through dual heat sources, it makes it possible to achieve a good composite of high-melting-point reinforcing phases and low-melting-point metal matrices. Furthermore, the strategy of simultaneous wire and powder feeding allows for precise control of the composite material's composition and microstructure.
[0005] Currently, there are no reports on the preparation of TC4 / AZ91 magnesium-based composite materials based on laser-arc composite additive manufacturing with simultaneous wire and powder delivery. Summary of the Invention
[0006] The technical problem to be solved by this invention is to address the shortcomings of the prior art by providing a laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composites. This method employs a multi-laser coaxial composite additive manufacturing device integrating a wire feeder, a powder feeder, and a laser and arc combined heat source. Using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, it performs laser-arc composite additive manufacturing of TC4 particle-reinforced AZ91 magnesium matrix composites, solving key technical problems such as uniform dispersion of high-melting-point TC4 particles in a low-melting-point AZ91 magnesium matrix, controllable interfacial reaction, and dense and efficient forming.
[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite materials, characterized in that the method uses a multi-laser coaxial composite additive manufacturing equipment integrating a wire feeder, a powder feeder, and a laser and arc composite heat source, and uses TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, and proceeds according to the following steps: Step 1: Conduct a single-pass laser-arc composite additive manufacturing experiment on an AZ80 magnesium alloy substrate to optimize and determine the additive manufacturing parameters; Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component, slice the 3D model to obtain layer data, and simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the multi-laser coaxial composite additive manufacturing equipment. Step 3: Fix the AZ80 magnesium alloy substrate on the worktable of the multi-laser coaxial composite additive manufacturing equipment in Step 2 with the additive manufacturing path and parameters imported in Step 2. Use the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface, adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate, and preheat the AZ80 magnesium alloy substrate to obtain a preheated substrate and a ready additive manufacturing equipment. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment obtained in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate and the distance from the composite heat source. At the same time, adjust the angle and position of the powder feeder nozzle so that the powder beam and the wire are fed synchronously into the path where they converge in the action area of the composite heat source. Argon gas is introduced coaxially or side-axis into the action area of the composite heat source as a protective gas to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the equipment to be additively manufactured obtained in Step 4. The wire and powder are fed simultaneously by coaxial wire feeding and off-axis powder feeding. At the same time, turn on the laser and arc welding gun to perform laser-arc composite additive manufacturing on the preheated substrate to obtain the deposited part. Step 6: The deposited part obtained in step 5 is cooled in situ under an argon atmosphere to obtain a TC4 particle-reinforced AZ91 magnesium-based composite material workpiece.
[0008] This invention utilizes the synergistic effect of a combined laser and electric arc heat source: the laser primarily acts on TC4 particles, rapidly heating their surface and partially melting them, thus improving their wettability with the magnesium melt; simultaneously, the laser reheats the molten pool formed by the electric arc, eliminating incomplete fusion and porosity defects, and improving the matrix structure; the electric arc is mainly responsible for melting the AZ91 wire, forming the molten pool, preventing the complete melting of TC4 particles from causing excessive interfacial reactions that generate brittle phases, while ensuring good spreading of the magnesium alloy matrix, eliminating incomplete fusion and porosity defects, and forming a particle-reinforced composite material.
[0009] The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material described above, wherein the optimized and determined additive manufacturing parameters in step one are: laser power 800W~2500W, arc current 80A~180A, arc voltage 8V~15V, wire feeding speed 8m / min~12m / min, powder feeding rate 1g / min~8g / min, and powder feeding gas flow rate 1L / min~3L / min. The optimization of this invention refers to the pre-processing of single-pass TC4 particle-reinforced AZ91 magnesium matrix composite laser-arc composite additive manufacturing on a substrate. The feasibility of the deposition parameters is confirmed based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness, thereby obtaining the optimal deposition parameters. The molten pool temperature can be effectively controlled by adjusting the energy ratio of the two heat sources. The energy ratio of the two heat sources refers to the energy of the laser and the arc. The reasonable range for laser power is 800W~2500W, while the arc energy is reflected by the arc current and arc voltage, with reasonable ranges of arc current 80A~180A and arc voltage 8V~15V, respectively. By using the optimal deposition parameters, the mass fraction of TC4 particles in the AZ91 matrix is controlled, ensuring uniform particle distribution and no significant agglomeration. This prevents insufficient particle melting due to excessively low laser power and insufficient interfacial reaction due to excessively high laser power. The powder feeding rate must be matched with the wire feeding speed to obtain the target reinforcement ratio.
[0010] In the aforementioned laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material, the thickness of the AZ80 magnesium alloy substrate in step three is not less than 20 mm, and the substrate shape is square or circular, with its length, width, or diameter greater than that of the target component. This invention, by controlling the substrate thickness, achieves a moderate heat capacity, providing sufficient rigidity while facilitating preheating and temperature control. Furthermore, the length, width, or diameter of the substrate is determined by the size of the target component and is greater than that of the target component.
[0011] In the aforementioned laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material, the vertical distance between the composite heat source of the laser and arc welding torch and the AZ80 magnesium alloy substrate in step three is 10mm~25mm. In additive manufacturing, controlling the vertical distance between the end of the arc welding torch and the substrate or the surface of the deposited layer essentially determines the arc length and wire extension, which is one of the core parameters affecting process stability and final forming quality. Specifically, this is reflected in the following aspects: First, precise control of heat input: as the distance increases, the arc length increases, the voltage increases, and the heat input increases. Magnesium alloy conducts heat extremely quickly, and the heat provided within this distance range is just enough to maintain the molten pool temperature, avoiding incomplete fusion defects; Second, stable droplet transfer: the distance directly affects the wire extension, and this range facilitates stable droplet transfer, reduces spatter, and ensures a smooth additive manufacturing process; Third, flexible adjustment of forming dimensions: the distance affects the weld width. The distance between the weld pool and the electrode height is crucial. A larger distance typically allows for a wider molten pool, suitable for rapid filling; a smaller distance allows for a more concentrated arc, facilitating fine forming. Fourthly, it protects the molten pool and adapts to the working conditions: a suitable distance ensures effective coverage of the shielding gas, preventing magnesium alloy oxidation. At the same time, this range also provides operating space for the welding torch in complex paths and allows for adjustments to processes such as substrate preheating or interlayer cooling. In summary, the 10mm~25mm range is an optimized range derived by comprehensively considering heat input, droplet transfer, forming control, gas protection, and process adaptability. In actual operation, the optimal value needs to be fine-tuned within this range according to the specific alloy, equipment, and the morphology and size of the deposited part.
[0012] In the aforementioned laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material, the preheating temperature in step three is 100℃~250℃. This invention reduces the cooling rate of the deposited layer, decreases thermal stress, and prevents cracking by controlling the preheating temperature.
[0013] In the aforementioned laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite materials, the diameter of the AZ91 magnesium alloy wire in step four is 0.8 mm to 1.6 mm, and the particle size of the TC4 spherical powder is 40 μm to 200 μm. This invention utilizes spherical powder to improve powder flowability and ensure powder feeding stability. By controlling the particle size of the TC4 spherical powder, a suitable residence time can be obtained in the molten pool, avoiding splashing of excessively fine particles or unmelted particles of excessively coarse particles. Simultaneously, it ensures precise control of the powder feeder's feed rate. Furthermore, by controlling the diameter of the AZ91 magnesium alloy wire, it achieves compatibility with commonly used arc wire melting equipment and provides optimal laser-arc composite additive manufacturing results.
[0014] In the aforementioned laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material, the argon gas flow rate in step four is 15 L / min to 30 L / min. This invention introduces argon gas coaxially or laterally as a protective gas in the composite heat source region. Magnesium alloys have low melting and boiling points and are easily oxidized. Furthermore, alloying elements in magnesium alloys are prone to volatilization during deposition, and the molten pool is prone to splashing. Introducing argon gas primarily protects the deposited molten pool from oxidation, while also suppressing the volatilization of alloying elements and molten pool splashing to a certain extent. Controlling the flow rate prevents insufficient protection of the molten pool due to low flow rates, which can lead to severe oxidation.
[0015] The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite materials described above, in step five, involves each deposition pass on the same deposition plane depositing along the same direction, i.e., using a linear deposition pattern. Simultaneously, a zigzag deposition pattern is used on individual deposition passes. In this invention, each deposition pass on the same deposition plane depositing along the same direction, i.e., using a linear deposition pattern, simplifies the deposition path and improves deposition efficiency. Simultaneously, the zigzag deposition pattern on individual deposition passes allows the molten droplets to spread out, increasing the width of the deposition passes, reducing the excess height of the deposition passes, and creating overlap between deposition passes, increasing the contact area between passes, enhancing the lateral strength of the deposited billet, and reducing the height difference between deposition passes, thus preventing the formation of porosity defects at their interfaces.
[0016] In the laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material described above, after each deposition layer is completed in step five of the laser-arc composite additive manufacturing process, the deposition layer is left to stand for 5 to 15 minutes under argon protection to allow the temperature of the deposition layer to drop to the preheating temperature of the substrate. The thickness of the deposition layer at various locations is measured to ensure the dimensional accuracy of the deposited part. The surface of the deposition layer is then polished with a steel brush before the next layer is deposited. In this invention, due to the low melting and boiling points of magnesium alloys, continuous deposition can lead to the collapse of the molten pool or the deposited billet, affecting the final dimensional accuracy of the deposited workpiece. Furthermore, magnesium alloys are prone to oxidation, and continuous deposition can cause severe oxidation of the melt, affecting the quality of the deposited part. In addition, continuous deposition can easily lead to overheating of the deposited billet, affecting the alloy microstructure and causing grain growth and coarsening. Simultaneously, columnar crystal structures are easily formed along the deposition direction, all of which are detrimental to the mechanical properties of the deposited workpiece. However, by allowing the deposited melt to stand under argon protection for 5-15 minutes after deposition, the deposited melt can be appropriately cooled, preventing the collapse and oxidation of the molten pool or the deposited billet, while also preventing grain growth and coarsening and the formation of columnar crystals, ensuring that the deposited billet forms equiaxed crystals and isotropic. Furthermore, by using a steel brush to polish the surface of the deposited layer to remove the surface oxide layer, oxidation inclusion defects are eliminated, improving product quality.
[0017] In the laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material described above, the mass fraction of TC4 in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece in step six is 1%~15%.
[0018] Compared with the prior art, the present invention has the following advantages: 1. This invention combines laser-arc composite additive manufacturing technology with wire and powder co-feeding to prepare TC4 particle-reinforced AZ91 magnesium-based composite materials. It achieves uniform dispersion and good interfacial bonding of the high-melting-point reinforcing phase in the low-melting-point matrix, and solves the problems of uneven distribution of reinforcing phase, difficult control of interfacial reaction and many pore defects in the preparation of magnesium-based composite materials by traditional methods.
[0019] 2. This invention effectively enhances the bonding strength between the reinforcing phase and the matrix interface by controlling the energy ratio of the dual heat sources, while avoiding particle agglomeration, porosity and shrinkage defects in traditional casting methods.
[0020] 3. This invention requires no mold, has high material utilization, can form complex structural parts, has a short manufacturing cycle, and uses wire and powder to avoid the safety risks associated with using magnesium alloy powder, making it suitable for industrial promotion and application.
[0021] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0022] Figure 1 This is a schematic diagram illustrating the principle of the laser-arc composite heat source and the simultaneous feeding of wire and powder in the laser-arc composite additive manufacturing process of this invention.
[0023] Figure 2 This is a schematic diagram of the deposition path in the laser-arc composite additive manufacturing process of the present invention.
[0024] Figure 3 This is a morphology diagram of the TC4 titanium alloy spherical powder used in Example 1 of the present invention.
[0025] Figure 4 This is a macroscopic microstructure diagram of the TC4 particle-reinforced AZ91 magnesium-based composite material workpiece obtained in Example 1 of the present invention.
[0026] Figure 5 This is a microstructure diagram of the TC4 particle-reinforced AZ91 magnesium-based composite material workpiece obtained in Example 1 of the present invention.
[0027] Figure 6 This is a microstructure diagram of the TC4 and AZ91 interface in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in Example 1 of the present invention.
[0028] Figure 7 This is a microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in Example 1 of the present invention.
[0029] Figure 8 This is a tensile strength diagram of the TC4 particle-reinforced AZ91 magnesium-based composite workpiece obtained in Example 1 of the present invention.
[0030] Figure 9 This is a first microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in Comparative Example 1 of the present invention.
[0031] Figure 10 This is a second microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in Comparative Example 1 of the present invention.
[0032] Figure 11 This is a tensile strength diagram of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in Comparative Example 1 of the present invention.
[0033] Figure 12 This is a tensile strength diagram of the AZ91 magnesium alloy workpiece obtained in Comparative Example 2 of the present invention. Detailed Implementation
[0034] Figure 1 This is a schematic diagram illustrating the principle of the laser-arc composite heat source and the simultaneous feeding of wire and powder in laser-arc composite additive manufacturing according to the present invention. Figure 1As can be seen, this invention uses a multi-laser coaxial composite additive manufacturing equipment that integrates a wire feeder, a powder feeder, and a laser and electric arc composite heat source to perform laser-arc composite additive manufacturing on an AZ80 magnesium alloy substrate, using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, to obtain TC4 particle-reinforced AZ91 magnesium-based composite material.
[0035] Example 1 In this embodiment, TC4 titanium alloy spherical powder with a particle size of 75μm~150μm and AZ91 magnesium alloy wire with a diameter of 1.2mm are used as raw materials to prepare TC4 particle-reinforced AZ91 magnesium matrix composite material with a TC4 mass fraction of 5%. The TC4 titanium alloy spherical powder is composed of the following components by mass percentage: Al 5.91%, V 4.24%, and the balance is Ti. The AZ91 magnesium alloy wire is composed of the following components by mass percentage: Al 8.79%, Zn 0.53%, and the balance is Mg.
[0036] This embodiment includes the following steps: Step 1: Using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, retrieve the optimal deposition parameter package for AZ91 magnesium alloy from the database. Conduct a single-pass laser-arc composite additive manufacturing experiment on an AZ80 magnesium alloy substrate with a thickness of 20mm. Confirm the feasibility of the deposition parameters based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness. Optimize and determine the additive manufacturing parameters as follows: laser power 1200W, arc current 135A, arc voltage 12.2V, wire feed speed 9.8m / min, powder feed rate 2g / min, and powder gas flow rate 1.5L / min. Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component. Slice the 3D model to obtain layer data. Simultaneously, simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the CML Hybrid multi-laser coaxial composite additive manufacturing equipment. The target TC4 particle-reinforced AZ91 magnesium matrix composite component is a cuboid with dimensions of 100mm × 60mm × 100mm. Step 3: Fix the AZ80 magnesium alloy substrate onto the worktable of the multi-laser coaxial composite additive manufacturing equipment, in which the additive manufacturing path and parameters were imported in Step 2. Use the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface. Adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate to 10mm, and preheat the AZ80 magnesium alloy substrate to 200℃ to obtain a preheated substrate and a ready additive manufacturing equipment. The AZ80 magnesium alloy substrate is square in shape, and its length and width are greater than the length and width of the target component. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment prepared in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate to 90° and the distance from the composite heat source. At the same time, adjust the angle and position of the powder feeder nozzle so that the powder beam and the wire feeding path intersect in the action area of the composite heat source. In the action area of the composite heat source, argon gas with a flow rate of 25L / min is coaxially introduced as a protective gas to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the additive manufacturing equipment obtained in Step 4. Achieve simultaneous wire and powder feeding via coaxial wire feeding and off-axis powder feeding. Simultaneously turn on the laser and arc welding torch to perform laser-arc composite additive manufacturing on the preheated substrate. Each deposition pass on the same deposition plane deposits along the same direction, i.e., a straight-line deposition from left to right. The deposition pass direction of the next deposition plane is opposite to that of the previous layer, i.e., a straight-line deposition from right to left. Simultaneously, a zigzag deposition pattern is used on a single deposition pass, with a width of 20 mm and a period of 3 mm. See [link to details]. Figure 2 After each deposition layer is completed, it is left to stand for 8 minutes under argon protection to allow the temperature of the deposition layer to drop to the preheating temperature of the substrate. The thickness of the deposition layer at various locations is measured to ensure the dimensional accuracy of the deposited part. Before starting to deposit the next layer, the surface of the deposition layer is polished with a steel brush until it is smooth and bright to obtain the deposited part. Step 6: Allow the deposited part obtained in step 5 to cool in situ under an argon atmosphere. Then, use an electrical discharge wire cutter to cut the deposited part off the AZ80 magnesium alloy substrate and use a steel brush to polish the surface of the deposited part to obtain a TC4 particle-reinforced AZ91 magnesium matrix composite workpiece with dimensions of 105mm×65mm×105mm.
[0037] Figure 3 This is a morphology image of the TC4 titanium alloy spherical powder used in this embodiment, from... Figure 3 As can be seen from the image, the TC4 titanium alloy spherical powder used in this embodiment is all spherical.
[0038] Figure 4 This is a macroscopic microstructure diagram of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment. Figure 4 As can be seen from the figure, the size of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment is 105mm×65mm×105mm.
[0039] Figure 5 This is a microstructure diagram of the TC4 particle-reinforced AZ91 magnesium-based composite workpiece obtained in this embodiment. Figure 5As can be seen from the figure, in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment, the TC4 particles are uniformly distributed in the AZ91 matrix, and the matrix structure is very dense.
[0040] Figure 6 This is a microstructure diagram of the TC4 and AZ91 interface in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment. Figure 6 As can be seen from the above, the TC4 particles in the AZ91 magnesium matrix composite workpiece reinforced with TC4 particles are very densely and tightly bonded to the AZ91 matrix, and there are no micropores or microcracks at the interface, exhibiting metallurgical bonding characteristics.
[0041] Figure 7 This is a microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment. Figure 7 As can be seen from the figure, the matrix structure of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment is very dense, with no micropores or lack of fusion, and a large number of precipitated phases are formed in the matrix.
[0042] Figure 8 The tensile strength diagram of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment is shown. Samples of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece were taken in the length, width, and height directions using an electrical discharge wire cutting machine and processed into tensile samples of the dimensions shown in the diagram. The room temperature tensile properties in the three directions are similar, with an average room temperature tensile property of [value missing]. Figure 8 ,from Figure 8 As can be seen from the figure, the yield strength of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment is 162.43 MPa, the tensile strength is 281.91 MPa, and the elongation is 9.65%.
[0043] Comparative Example 1 This comparative example uses TC4 titanium alloy spherical powder with a particle size of 75μm~150μm and AZ91 magnesium alloy wire with a diameter of 1.2mm as raw materials to prepare TC4 particle-reinforced AZ91 magnesium matrix composite material with a TC4 mass fraction of 5%. The TC4 titanium alloy spherical powder is composed of the following mass percentages: Al 5.91%, V 4.24%, with the balance being Ti; the AZ91 magnesium alloy wire is composed of the following mass percentages: Al 8.79%, Zn 0.53%, with the balance being Mg.
[0044] This comparative example includes the following steps: Step 1: Using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, retrieve the optimal deposition parameter package for AZ91 magnesium alloy from the database. Conduct a single-pass arc additive manufacturing test on an AZ80 magnesium alloy substrate with a thickness of 20mm. Confirm the feasibility of the deposition parameters based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness. Optimize and determine the additive manufacturing parameters as follows: arc current 160A, arc voltage 14.2V, wire feed speed 9.8m / min, powder feed rate 2g / min, and powder feed gas flow rate 1.5L / min. Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component. Slice the 3D model to obtain layer data. Simultaneously, simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the arc additive manufacturing equipment. The target TC4 particle-reinforced AZ91 magnesium matrix composite component is a cuboid with dimensions of 100mm × 60mm × 100mm. Step 3: Fix the AZ80 magnesium alloy substrate onto the worktable of the arc additive manufacturing equipment, in which the additive manufacturing path and parameters were imported in Step 2. Using the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface, adjust the vertical distance between the arc welding gun and the AZ80 magnesium alloy substrate to 10mm, and preheat the AZ80 magnesium alloy substrate to 200℃ to obtain a preheated substrate and a ready additive manufacturing equipment. The AZ80 magnesium alloy substrate is square in shape, with its length and width greater than the length and width of the target component. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment prepared in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire outlet of the wire feeder and the upper surface of the AZ80 magnesium alloy substrate to 90° and the distance from the arc welding gun. At the same time, adjust the angle and position of the powder feeding nozzle of the powder feeder so that the powder beam and the wire feeding path intersect in the action area of the arc welding gun. Then, coaxially introduce argon gas with a flow rate of 25L / min as a protective gas in the action area of the arc welding gun to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the additive manufacturing equipment obtained in Step 4. Wire and powder are fed simultaneously via coaxial wire feeding and off-axis powder feeding. Simultaneously, turn on the arc welding torch to perform arc additive manufacturing on the preheated substrate. Each deposition pass on the same deposition plane deposits along the same direction, i.e., a straight-line deposition from left to right. The deposition pass direction of the next deposition plane is opposite to that of the previous layer, i.e., a straight-line deposition from right to left. At the same time, a zigzag deposition pattern is used on a single deposition pass, with a width of 20 mm and a period of 3 mm. See [link to details]. Figure 2After each deposition layer is completed, it is left to stand for 8 minutes under argon protection to allow the temperature of the deposition layer to drop to the preheating temperature of the substrate. The thickness of the deposition layer at various locations is measured to ensure the dimensional accuracy of the deposited part. Before starting to deposit the next layer, the surface of the deposition layer is polished with a steel brush until it is smooth and bright to obtain the deposited part. Step 6: Allow the deposited part obtained in step 5 to cool in situ under an argon atmosphere. Then, use an electrical discharge wire cutter to cut the deposited part off the AZ80 magnesium alloy substrate and use a steel brush to polish the surface of the deposited part to obtain a TC4 particle-reinforced AZ91 magnesium matrix composite workpiece with dimensions of 105mm×65mm×105mm.
[0045] Figure 9 The first microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparative example. Figure 10 The second microstructure diagram of the AZ91 matrix in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparative example is shown below. Figure 9 and Figure 10 As can be seen from the comparison, most areas of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparison are relatively dense, but there are still pores and incomplete fusion defects in the microstructure.
[0046] Figure 11 The tensile strength diagram of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparative example is shown. Samples of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparative example were taken in the length, width, and height directions using an electrical discharge wire cutting machine and then processed into… Figure 8 Tensile strength tests were conducted on medium-sized tensile specimens. The room temperature tensile properties in the three directions were similar, with an average room temperature tensile property of [value missing]. Figure 11 ,from Figure 11 As can be seen from the data, the yield strength of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this comparative example is 151.78 MPa, the tensile strength is 217.18 MPa, and the elongation is 1.83%.
[0047] A comparison between Example 1 and Comparative Example 1 shows that the TC4 particle-reinforced AZ91 magnesium-based composite material workpiece prepared by arc additive manufacturing in Comparative Example 1 still has pores and incomplete fusion defects in its microstructure, resulting in poor mechanical properties.
[0048] Comparative Example 2 This comparative example uses AZ91 magnesium alloy wire with a diameter of 1.2 mm as raw material to prepare AZ91 magnesium alloy material; the AZ91 magnesium alloy wire is composed of the following components by mass percentage: Al 8.79%, Zn 0.53%, and the balance is Mg.
[0049] This comparative example includes the following steps: Step 1: Using AZ91 magnesium alloy wire as raw material, retrieve the optimal deposition parameter package for AZ91 magnesium alloy from the database. Conduct a single-pass laser-arc composite additive manufacturing test on an AZ80 magnesium alloy substrate with a thickness of 20mm. Confirm the feasibility of the deposition parameters based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness. Optimize and determine the additive manufacturing parameters as follows: laser power 800W, arc current 140A, arc voltage 12V, wire feed speed 10m / min. Step 2: Use computer software to create a 3D model of the target AZ91 magnesium alloy material component. Slice the 3D model to obtain layer data. Simultaneously, simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the CML Hybrid multi-laser coaxial composite additive manufacturing equipment. The AZ91 magnesium alloy material component is a cuboid with dimensions of 100mm × 60mm × 100mm. Step 3: Fix the AZ80 magnesium alloy substrate onto the worktable of the multi-laser coaxial composite additive manufacturing equipment, in which the additive manufacturing path and parameters were imported in Step 2. Using the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface, adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate to 15mm, and preheat the AZ80 magnesium alloy substrate to 100°C to obtain a preheated substrate and a ready additive manufacturing equipment. The AZ80 magnesium alloy substrate is square in shape, with its length and width greater than the length and width of the target component. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment obtained in Step 3. Then adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate to 90° and the distance from the composite heat source. Introduce argon gas at a flow rate of 25L / min as a protective gas in the action area of the composite heat source to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder of the additive manufacturing equipment obtained in Step 4, and simultaneously turn on the laser and arc welding gun. Perform laser-arc composite additive manufacturing on the preheated substrate. Each deposition pass on the same deposition plane is deposited in the same direction, i.e., a straight-line deposition from left to right. The deposition pass direction of the next deposition plane is opposite to that of the previous layer, i.e., a straight-line deposition from right to left. Simultaneously, a zigzag deposition pattern is used on a single deposition pass, with a width of 20 mm and a period of 3 mm. See [link to relevant documentation]. Figure 2 After each deposition layer is completed, it is left to stand for 8 minutes under argon protection to allow the temperature of the deposition layer to drop to the preheating temperature of the substrate. The thickness of the deposition layer at various locations is measured to ensure the dimensional accuracy of the deposited part. Before starting to deposit the next layer, the surface of the deposition layer is polished with a steel brush until it is smooth and bright to obtain the deposited part. Step 6: Allow the deposited part obtained in Step 5 to cool in situ under an argon atmosphere. Then, use an electrical discharge wire cutter to cut the deposited part off the AZ80 magnesium alloy substrate and use a steel brush to polish the surface of the deposited part to obtain an AZ91 magnesium alloy workpiece with dimensions of 105mm×65mm×105mm.
[0050] Figure 12 The tensile strength diagram of the AZ91 magnesium alloy workpiece obtained in this comparative example is shown. Samples of the AZ91 magnesium alloy workpiece were taken in the length, width, and height directions using an electrical discharge wire cutting machine and then processed into… Figure 8 Tensile strength tests were conducted on medium-sized tensile specimens. The room temperature tensile properties in the three directions were similar, with an average room temperature tensile property of [value missing]. Figure 12 ,from Figure 12 As can be seen from the data, the yield strength of the AZ91 magnesium alloy workpiece obtained in this comparative example is 153.62 MPa, the tensile strength is 241.97 MPa, and the elongation is 12%.
[0051] A comparison between Example 1 and Comparative Example 2 shows that the mechanical properties of the AZ91 magnesium alloy workpiece obtained without TC4 particles in Comparative Example 2 are lower than those of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained with TC4 particles in Example 1.
[0052] Example 2 In this embodiment, TC4 titanium alloy spherical powder with a particle size of 45μm~100μm and AZ91 magnesium alloy wire with a diameter of 0.8mm are used as raw materials to prepare TC4 particle-reinforced AZ91 magnesium matrix composite material with a TC4 mass fraction of 1%. The TC4 titanium alloy spherical powder is composed of the following components by mass percentage: Al 5.91%, V 4.24%, and the balance is Ti. The AZ91 magnesium alloy wire is composed of the following components by mass percentage: Al 8.79%, Zn 0.53%, and the balance is Mg.
[0053] This embodiment includes the following steps: Step 1: Using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, retrieve the optimal deposition parameter package for AZ91 magnesium alloy from the database. Conduct a single-pass laser-arc composite additive manufacturing test on an AZ80 magnesium alloy substrate with a thickness of 20mm. Confirm the feasibility of the deposition parameters based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness. Optimize and determine the additive manufacturing parameters as follows: laser power 800W, arc current 80A, arc voltage 8V, wire feed speed 12m / min, powder feed rate 1g / min, and powder feed gas flow rate 1L / min. Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component. Slice the 3D model to obtain layer data. Simultaneously, simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the CML Hybrid multi-laser coaxial composite additive manufacturing equipment. The target TC4 particle-reinforced AZ91 magnesium matrix composite component is a cube with dimensions of 100mm × 100mm × 100mm. Step 3: Fix the AZ80 magnesium alloy substrate onto the worktable of the multi-laser coaxial composite additive manufacturing equipment, in which the additive manufacturing path and parameters were imported in Step 2. Using the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface, adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate to 15mm, and preheat the AZ80 magnesium alloy substrate to 100°C to obtain a preheated substrate and a ready additive manufacturing equipment. The AZ80 magnesium alloy substrate is circular in shape, and its diameter is larger than that of the target component. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment prepared in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate to 90° and the distance from the composite heat source. At the same time, adjust the angle and position of the powder feeder nozzle so that the powder beam and the wire feeding path intersect in the action area of the composite heat source. In the action area of the composite heat source, argon gas with a flow rate of 15L / min is coaxially introduced as a protective gas to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the additive manufacturing equipment obtained in Step 4. Achieve simultaneous wire and powder feeding via coaxial wire feeding and off-axis powder feeding. Simultaneously turn on the laser and arc welding torch to perform laser-arc composite additive manufacturing on the preheated substrate. Each deposition pass on the same deposition plane deposits along the same direction, i.e., a straight-line deposition from left to right. The deposition pass direction of the next deposition plane is opposite to that of the previous layer, i.e., a straight-line deposition from right to left. Simultaneously, a zigzag deposition pattern is used on a single deposition pass, with a width of 20 mm and a period of 3 mm. See [link to details]. Figure 2 After each deposition layer is completed, it is left to stand for 5 minutes under argon protection to allow the temperature of the deposition layer to drop to the substrate preheating temperature. The layer thickness at each location of the deposition layer is measured to ensure the dimensional accuracy of the deposited part. When the next layer is deposited, the surface of the deposition layer is polished with a steel brush until it is smooth and bright to obtain the deposited part. Step 6: Allow the deposited part obtained in Step 5 to cool in situ under an argon atmosphere. Then, use an electrical discharge wire cutter to cut the deposited part off the AZ80 magnesium alloy substrate and use a steel brush to polish the surface of the deposited part to obtain a TC4 particle-reinforced AZ91 magnesium matrix composite workpiece with dimensions of 100mm×100mm×100mm.
[0054] Testing revealed that the TC4 particles in the AZ91 magnesium matrix composite workpiece prepared in this embodiment were uniformly distributed within the TC4 matrix, and the matrix structure was very dense. The TC4 particles and the AZ91 matrix were tightly bonded together, with no micropores or microcracks at the interface, exhibiting metallurgical bonding characteristics. The matrix structure was very dense, without micropores or incomplete fusion, and a large number of precipitated phases were observed in the matrix. Samples of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment were taken in the length, width, and height directions using an electrical discharge wire cutting machine and processed into tensile samples of the dimensions shown in the figure. Tensile strength tests were then conducted, and the room temperature tensile properties in the three directions were similar, with a yield strength of 146.18 MPa, a tensile strength of 257.93 MPa, and an elongation of 10.27%.
[0055] Example 3 In this embodiment, TC4 titanium alloy spherical powder with a particle size of 100μm~200μm and AZ91 magnesium alloy wire with a diameter of 1.6mm are used as raw materials to prepare TC4 particle-reinforced AZ91 magnesium matrix composite material with a TC4 mass fraction of 15%. The TC4 titanium alloy spherical powder is composed of the following components by mass percentage: Al 5.91%, V 4.24%, and the balance is Ti. The AZ91 magnesium alloy wire is composed of the following components by mass percentage: Al 8.79%, Zn 0.53%, and the balance is Mg.
[0056] This embodiment includes the following steps: Step 1: Using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, retrieve the optimal deposition parameter package for AZ91 magnesium alloy from the database. Conduct a single-pass laser-arc composite additive manufacturing experiment on an AZ80 magnesium alloy substrate with a thickness of 20mm. Confirm the feasibility of the deposition parameters based on the smoothness of the single-pass deposition layer and the uniformity of the weld bead thickness. Optimize and determine the additive manufacturing parameters as follows: laser power 2500W, arc current 180A, arc voltage 15V, wire feed speed 8m / min, powder feed rate 8g / min, and powder feed gas flow rate 3L / min. Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component. Slice the 3D model to obtain layer data. Simultaneously, simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the CML Hybrid multi-laser coaxial composite additive manufacturing equipment. The target TC4 particle-reinforced AZ91 magnesium matrix composite component is a cube with dimensions of 100mm × 100mm × 100mm. Step 3: Fix the AZ80 magnesium alloy substrate onto the worktable of the multi-laser coaxial composite additive manufacturing equipment, in which the additive manufacturing path and parameters were imported in Step 2. Use the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface. Adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate to 25mm, and preheat the AZ80 magnesium alloy substrate to 250℃ to obtain a preheated substrate and a ready additive manufacturing equipment. The AZ80 magnesium alloy substrate is circular in shape, and its diameter is larger than that of the target component. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment obtained in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate to 90° and the distance from the composite heat source. At the same time, adjust the angle and position of the powder feeder nozzle so that the powder beam and the wire feeding path intersect in the action area of the composite heat source. In the action area of the composite heat source, argon gas with a flow rate of 30L / min is coaxially introduced as a protective gas to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the additive manufacturing equipment obtained in Step 4. Achieve simultaneous wire and powder feeding via coaxial wire feeding and off-axis powder feeding. Simultaneously turn on the laser and arc welding torch to perform laser-arc composite additive manufacturing on the preheated substrate. Each deposition pass on the same deposition plane deposits along the same direction, i.e., a straight-line deposition from left to right. The deposition pass direction of the next deposition plane is opposite to that of the previous layer, i.e., a straight-line deposition from right to left. Simultaneously, a zigzag deposition pattern is used on a single deposition pass, with a width of 20 mm and a period of 3 mm. See [link to details]. Figure 2 After each deposition layer is completed, it is left to stand for 15 minutes under argon protection to allow the temperature of the deposition layer to drop to the substrate preheating temperature. The layer thickness at each location of the deposition layer is measured to ensure the dimensional accuracy of the deposited part. When the next layer is deposited, the surface of the deposition layer is polished with a steel brush until it is smooth and bright to obtain the deposited part. Step 6: Allow the deposited part obtained in Step 5 to cool in situ under an argon atmosphere. Then, use an electrical discharge wire cutter to cut the deposited part off the AZ80 magnesium alloy substrate and use a steel brush to polish the surface of the deposited part to obtain a TC4 particle-reinforced AZ91 magnesium matrix composite workpiece with dimensions of 100mm×100mm×100mm.
[0057] Testing revealed that the TC4 particles in the AZ91 magnesium matrix composite workpiece prepared in this embodiment were uniformly distributed within the TC4 matrix, and the matrix structure was very dense. The TC4 particles and the AZ91 matrix were tightly bonded together, with no micropores or microcracks at the interface, exhibiting metallurgical bonding characteristics. The matrix structure was very dense, without micropores or incomplete fusion, and a large number of precipitated phases were observed in the matrix. Samples of the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece obtained in this embodiment were taken in the length, width, and height directions using an electrical discharge wire cutting machine and processed into tensile samples of the dimensions shown in the figure. Tensile strength tests were then conducted, and the room temperature tensile properties in the three directions were similar, with a yield strength of 162.43 MPa, a tensile strength of 268.76 MPa, and an elongation of 7.32%.
[0058] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.
Claims
1. A laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite materials, characterized in that, This method employs a multi-laser coaxial composite additive manufacturing equipment integrating a wire feeder, a powder feeder, and a laser and electric arc combined heat source, using TC4 titanium alloy spherical powder and AZ91 magnesium alloy wire as raw materials, and proceeds according to the following steps: Step 1: Conduct a single-pass laser-arc composite additive manufacturing experiment on an AZ80 magnesium alloy substrate to optimize and determine the additive manufacturing parameters; Step 2: Use computer software to create a 3D model of the target TC4 particle-reinforced AZ91 magnesium matrix composite component, slice the 3D model to obtain layer data, and simulate the additive manufacturing path. Import the additive manufacturing path and the additive manufacturing parameters optimized and determined in Step 1 into the control system of the multi-laser coaxial composite additive manufacturing equipment. Step 3: Fix the AZ80 magnesium alloy substrate on the worktable of the multi-laser coaxial composite additive manufacturing equipment in Step 2 with the additive manufacturing path and parameters imported in Step 2. Use the upper surface of the AZ80 magnesium alloy substrate as the additive manufacturing reference surface, adjust the vertical distance between the composite heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate, and preheat the AZ80 magnesium alloy substrate to obtain a preheated substrate and a ready additive manufacturing equipment. Step 4: Fix the AZ91 magnesium alloy wire spool into the wire feeder of the additive manufacturing equipment obtained in Step 3, and load TC4 spherical powder into the powder feeder. Then, adjust the angle between the wire feeder outlet and the upper surface of the AZ80 magnesium alloy substrate and the distance from the composite heat source. At the same time, adjust the angle and position of the powder feeder nozzle so that the powder beam and the wire feeding path intersect in the action area of the composite heat source. Argon gas is introduced coaxially or side-axis into the action area of the composite heat source as a protective gas to obtain the equipment to be additively manufactured. Step 5: Start the wire feeder and powder feeder of the equipment to be additively manufactured obtained in Step 4. The wire and powder are fed simultaneously by coaxial wire feeding and off-axis powder feeding. At the same time, turn on the laser and arc welding gun to perform laser-arc composite additive manufacturing on the preheated substrate to obtain the deposited part. Step 6: The deposited part obtained in step 5 is cooled in situ under an argon atmosphere to obtain a TC4 particle-reinforced AZ91 magnesium-based composite material workpiece.
2. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, The optimized and determined additive manufacturing parameters in step one are: laser power 800W~2500W, arc current 80A~180A, arc voltage 8V~15V, wire feed speed 8m / min~12m / min, powder feed rate 1g / min~8g / min, and powder feed gas flow rate 1L / min~3L / min.
3. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, The thickness of the AZ80 magnesium alloy substrate mentioned in step three is not less than 20mm, and the substrate shape is square or round, with its length, width or diameter being greater than the length, width or diameter of the target component.
4. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, In step three, the vertical distance between the combined heat source of the laser and the arc welding gun and the AZ80 magnesium alloy substrate is 10mm~25mm.
5. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, The preheating temperature mentioned in step three is 100℃~250℃.
6. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, In step four, the diameter of the AZ91 magnesium alloy wire is 0.8 mm to 1.6 mm, and the particle size of the TC4 spherical powder is 40 μm to 200 μm.
7. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, The flow rate of argon gas in step four is 15 L / min to 30 L / min.
8. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, In step five, in the laser-arc composite additive manufacturing process, each deposition pass on the same deposition plane is deposited in the same direction, i.e., a straight-line deposition is used. At the same time, a zigzag deposition is used on a single deposition pass.
9. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium-based composite material according to claim 1, characterized in that, After each deposition layer in the laser-arc composite additive manufacturing process described in step five is completed, the deposition layer is left to stand for 5 to 15 minutes under argon protection to allow the temperature of the deposition layer to drop to the preheating temperature of the substrate. The thickness of the deposition layer at each location is measured to ensure the dimensional accuracy of the deposited part. The surface of the deposition layer is then polished with a steel brush before the next layer is deposited.
10. The laser-arc composite additive manufacturing method for TC4 particle-reinforced AZ91 magnesium matrix composite material according to claim 1, characterized in that, The mass fraction of TC4 in the TC4 particle-reinforced AZ91 magnesium matrix composite workpiece described in step six is 1% to 15%.