A new fin processing method for finned diamond copper liquid cooling plate

By combining laser in-situ modification pretreatment with combined sawing and online monitoring and control, the problems of tool wear and quality inconsistency in the processing of diamond copper composite fins were solved, achieving efficient and controllable fin processing and improving processing quality and efficiency.

CN123060237APending Publication Date: 2026-11-10HENAN SHUHUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611503391.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently process diamond-copper composite fins, resulting in problems such as severe tool wear, easy chipping and breakage, high processing costs, and inconsistent fin quality.

Method used

The process employs in-situ laser modification pretreatment combined with combined saw blade processing, along with online monitoring and adaptive control. Nanosecond pulsed lasers are used to modify the fin processing surface, and combined saw blades are used for alternating layered cutting and slotting. Real-time monitoring and control are achieved through a triaxial piezoelectric force gauge and a broadband piezoelectric acoustic emission sensor.

Benefits of technology

It reduces sawing difficulty, minimizes random chipping and pull-out of diamond particles, improves fin processing quality and efficiency, ensures fin perpendicularity, thickness consistency and thermal conductivity, and avoids tooth chipping and tool breakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060237A_ABST
    Figure CN123060237A_ABST
Patent Text Reader

Abstract

This invention discloses a novel fin processing method for finned diamond-copper liquid cooling plates, belonging to the field of diamond-copper composite material processing technology. The novel fin processing method for finned diamond-copper liquid cooling plates includes the following steps: S1, material preparation and clamping positioning; S2, laser in-situ modification pretreatment: using a nanosecond pulsed laser to perform laser in-situ modification treatment on the area to be sawed on the fin processing surface; this invention combines laser in-situ modification pretreatment with saw blade-type fin processing, utilizing the significant difference in laser absorption rates between diamond and copper, so that laser energy is preferentially absorbed by diamond particles, causing local graphitization transformation of the diamond surface layer, forming a mechanically removable modified layer. This transforms "hard-on-hard sawing of diamond against diamond" into "controllable removal of the modified layer by PCD cutting teeth," reducing sawing difficulty and minimizing random breakage and pull-out of diamond particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of diamond-copper composite material processing technology, and in particular to a novel fin processing method for finned diamond-copper liquid cooling plates. Background Technology

[0002] Diamond-copper composites combine the ultra-high thermal conductivity of diamond with the machinability of copper, and are considered a core material for next-generation liquid cooling plates. Liquid cooling plates typically enhance convective heat transfer by machining microchannels and fin arrays inside or on their surface. For pure copper or aluminum alloy liquid cooling plates, the industry commonly uses end milling with micro-diameter end mills to machine the fins / channels, with typical fin thicknesses of 0.2–0.4 mm and aspect ratios exceeding 10. However, this process faces fundamental challenges when the matrix is ​​replaced with diamond-copper composites.

[0003] The cutting tool experiences high wear and is prone to chipping and breakage. The diamond particles have a Mohs hardness of 10, while the copper matrix is ​​extremely soft, resulting in a significant hardness difference between the two phases. The micro-diameter end mill has a large overhang length-to-diameter ratio. During milling, the erosion of the cutting edge by the diamond particles reduces the tool life to only 1 / 6 to 1 / 8 of that for machining pure copper, leading to uncontrolled processing costs. Furthermore, the copper matrix is ​​rapidly removed while the diamond particles are hardly removed, resulting in an uneven morphology of "copper pits + diamond protrusions" on the channel sidewalls. This results in high roughness, easily forming flow dead zones, and simultaneously damaging the integrity of the composite material.

[0004] To address these challenges, current research has primarily shifted towards non-contact methods such as laser processing and plasma etching. However, laser equipment is expensive, the heat-affected zone is difficult to completely eliminate, and processing efficiency and cost remain bottlenecks for large-scale deployment; plasma etching has a low rate, making large-area fabrication difficult.

[0005] On the other hand, in the field of machining ordinary metal (copper, aluminum) fins, there is already a technology that uses multi-layer stacked saw blade milling cutters (combination saw cutters) to cut and form multiple parallel grooves in one pass. The principle is to fit multiple equally spaced saw blades onto the cutter shaft, with the interval between adjacent saw blades equal to the fin thickness and the saw blade thickness equal to the groove width, so that the entire set of fins can be machined in one pass. However, when applied to ultra-hard composite materials such as diamond copper, conventional cemented carbide saw blades will wear out and fail instantly in materials containing the diamond phase, and thin saw blades (thickness <1mm) are very prone to breakage when intermittently cutting high-hardness particles, and the consistency of the groove width cannot be guaranteed.

[0006] Furthermore, during diamond copper sawing, the random distribution of diamond particles causes drastic fluctuations in cutting force. The stress and grinding force fluctuations when grinding diamond reinforcing particles are significantly greater than the corresponding values ​​when grinding the copper matrix. When the abrasive grains cut into the diamond reinforcing particles, the grinding force increases sharply and fluctuates considerably during the grinding process. This force fluctuation is the direct cause of tooth breakage, fin deformation, and inconsistent machining quality in thin saw blades.

[0007] Therefore, this application proposes a fin processing method that can overcome the high hardness of diamond copper and the high wear of saw blades. Summary of the Invention

[0008] The purpose of this invention is to solve the problems in the prior art by proposing a novel fin processing method for finned diamond copper liquid cooling plates.

[0009] To achieve the above objectives, the present invention adopts the following technical solution: A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: S2. Laser in-situ modification pretreatment: (1) A nanosecond pulsed laser was used to perform in-situ laser modification on the area to be sawed on the fin processing surface; S3, saw blade type fin processing: (1) Use a combination saw blade set: the saw blades are mounted on the cutter shaft at equal intervals through spacers, and the interval between adjacent saw blades is two fin thicknesses + saw blade thickness; S4. Online monitoring and adaptive control: (1) During the sawing process, the sawing status signal is collected in real time by a triaxial piezoelectric force gauge and a broadband piezoelectric acoustic emission sensor; (2) Map the real-time signal to normal sawing, diamond particle cutting, tool wear, signs of tooth breakage, or poor chip removal. S5. Post-processing: After sawing, the fin array is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0010] In some embodiments, in step S3, an alternating slotting method is used: first, all odd-numbered slots are sawn; after completing the odd-numbered slots, all even-numbered slots are sawn.

[0011] In some embodiments, in step S3, before sawing all even-numbered slots, waxy support medium is filled into the already sawn odd-numbered slots to provide lateral rigid support for the thin-walled fins that are being formed.

[0012] In some embodiments, in step S4, the mean and fluctuation amplitude of the normal force Fn and the tangential force Ft, as well as the frequency domain features, are extracted from the force signal; the root mean square value, event count rate, and spectral centroid are extracted from the acoustic emission signal.

[0013] In some embodiments, in step S4, when "diamond particle cutting" is identified, the feed rate v2 is reduced to 70% of the current value, while the saw blade linear speed v1 is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the position is recorded; when "poor chip removal" is identified, the coolant pressure is increased or the system is switched to pulse-type high-pressure internal cooling.

[0014] In some embodiments, in step S1, a diamond-copper composite substrate prepared by gas pressure melting infiltration is selected, and the fin processing surface is planar ground before processing to remove the surface copper layer so that the diamond reinforcement phase is uniformly exposed.

[0015] In some embodiments, in step S3, a layered cutting method is used to saw the material layer by layer until the target depth is reached.

[0016] In some embodiments, in step S2, the laser scanning path coincides with the subsequent sawing trajectory; the modification depth is the same as the subsequent single-layer sawing depth.

[0017] In some embodiments, in step S2, the laser scanning path width is 1.3 times the saw blade thickness t, ensuring that the PCD cutting teeth mainly contact the diamond-modified layer rather than the original diamond surface during sawing.

[0018] In some embodiments, in step S3, the saw teeth adopt a staggered tooth structure, so that each tooth removes material in layers during the sawing process and alternately polishes the processed sidewalls.

[0019] Compared with the prior art, the present invention provides a novel fin processing method for finned diamond copper liquid cooling plates, which has the following beneficial effects: 1. This invention combines in-situ laser modification pretreatment with saw blade-type fin processing. By utilizing the significant difference in laser absorption rates between diamond and copper, laser energy is preferentially absorbed by diamond particles, causing local graphitization transformation of the diamond surface layer and forming a mechanically removable modified layer. This transforms "hard-on-hard sawing of diamond" into "controllable removal of the modified layer by PCD cutter teeth," reducing sawing difficulty and minimizing random breakage and pull-out of diamond particles.

[0020] 2. This invention achieves process synergy through modification pretreatment and online monitoring. Laser modification pretreatment reduces the "uncontrollability" of diamond particles, while online monitoring provides assurance when modification is incomplete or distribution is abnormal. Together, they constitute full-process control of the diamond copper sawing process.

[0021] 3. This invention suppresses fin deformation by layered cutting, alternating grooves, and support filling: the target fin height is sawed in layers and then supported by a wax medium in the groove sawing sequence, so that there is always material support on both sides of the processed fin, effectively suppressing the tilting and bending of thin-walled fins.

[0022] Other advantages, objectives and features of the invention will be set forth in part in the description which follows; and in part will be apparent to those skilled in the art upon examination of the following description; or may be learned from practice of the invention. Attached Figure Description

[0023] Figure 1 This is a flowchart of the present invention.

[0024] Figure 2 This is a schematic diagram of the combined saw blade assembly in this invention.

[0025] Figure 3 This is a schematic diagram of the fin array structure in this invention.

[0026] Figure 4 This is a schematic diagram illustrating the principle and structure of saw blade-type fin processing in this invention.

[0027] Figure 5 This is a schematic diagram of alternating sawing with grooves in this invention.

[0028] In the picture: 1. Substrate; 2. Processed surface; 3. Fin; 4. Mounting surface; 5. Saw blade; 6. Spacer sleeve. Detailed Implementation

[0029] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0030] Example 1 Reference Figure 1-5 A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: (1) A diamond-copper composite substrate 1 prepared by gas pressure melting infiltration method is selected. The diamond volume fraction is about 50% and the average particle size is 150μm. One side of the substrate 1 is the mounting surface 4, which is used for subsequent bonding of chips or thermal interface materials; the other side is the fin 3 processing surface 2. Before processing, the fin 3 processing surface 2 is planar ground with diamond grinding wheel #200 and grinding depth 0.02mm / time. It is then polished to Ra<1μm to remove the surface copper layer so that the diamond reinforcement phase is uniformly exposed to ensure that the subsequent sawing removal rate is consistent. (2) Place the substrate 1 on the vacuum chuck with the fin 3 processing surface 2 facing upward. Use the vacuum chuck to ensure that the bottom surface of the substrate 1 is in close contact with the reference and the flatness is ≤0.08mm.

[0031] S2. Laser in-situ modification pretreatment: (1) A nanosecond pulsed laser with a wavelength of 1064 nm, a pulse width of 50 ns, and a pulse energy density of 15 J / cm² was used. 2 The scanning speed is 500 mm / s and the spot overlap rate is 60%. Laser in-situ modification treatment is performed on the sawing area of ​​the processing surface 2 of fin 3. (2) The laser scanning path coincides with the subsequent sawing trajectory. The width of the laser scanning path is 1.3 times the thickness t of the saw blade 5, ensuring that the PCD cutting teeth mainly contact the diamond modified layer rather than the original diamond surface during sawing. (3) The modification depth is 0.2 mm, which is the same as the subsequent single-layer sawing depth; the surface of the diamond particles undergoes local graphitization transformation, forming a graphitized modification layer with a thickness of about 10 to 20 μm; the copper substrate is less affected by laser heat due to its high reflectivity to 1064 nm laser.

[0032] S3, saw blade type 5 fin 3 processing: (1) Five sets of combined saw blades are used: the saw blade 5 is a PCD tooth tip thin blade saw blade 5 with a thickness t=0.3mm and an outer diameter D=50mm. The saw blade 5 is mounted on the cutter shaft at equal intervals through spacer sleeves 6. The interval between adjacent saw blades 5 is s=0.7mm (i.e., the thickness of two fins 3 + the thickness of saw blade 5, the thickness of fins 3 is w=0.2mm), and the thickness of saw blade 5 is t=0.3mm (i.e., the gap between fins 3 is I=0.3mm). The tooth shape of the saw blade 5 adopts a staggered tooth structure, so that each tooth removes material in layers during the sawing process and alternately polishes the processed sidewalls. (2) A layered cutting method is adopted. The target fin height h=4mm, the cutting depth of each layer is 0.2mm, and a total of 20 layers are added layer by layer to saw to the target depth. The sawing process parameters are: saw blade 5 linear speed v1=20m / s, feed speed v2=30mm / min, forced cooling and chip removal are adopted with lubricating mist cutting fluid, and the sawing direction is reverse sawing so that the cutting force is directed to the root of fin 3. (3) Using the alternating slot method, first saw all odd-numbered slots, at which point each fin 3 is supported by unprocessed solid material on both sides; after completing the odd-numbered slots, saw all even-numbered slots; through this sequence, at any given moment, the fin 3 being formed will have at least one side rigidly supported, effectively suppressing the lateral tilting and vibration of the high aspect ratio thin-walled fin 3. (4) Before sawing all even-numbered slots, fill the already sawed odd-numbered slots with wax support medium to provide lateral rigid support for the thin-walled fins 3 that are being formed; after sawing, remove the support medium by heating and melting or ultrasonic cleaning.

[0033] S4. Online monitoring and adaptive control: (1) During the sawing process, the sawing status signal is collected in real time by a triaxial piezoelectric force gauge (installed between the fixture and the machine tool table, with a sampling frequency of 10kHz) and a broadband piezoelectric acoustic emission sensor (frequency range of 100kHz to 1MHz, sampling frequency of 2MHz, installed on the substrate 1 near the sawing area). (2) Extract the mean and fluctuation amplitude of the normal force Fn and the tangential force Ft and the frequency domain characteristics from the force signal; extract the root mean square value, event count rate and spectral centroid from the acoustic emission signal, and map the real-time signal to normal sawing, diamond particle cutting, tool wear, tooth breakage precursor or poor chip removal status; (3) When "diamond particle cutting" is identified, the feed rate v2 is reduced to 70% of the current value, while the saw blade linear speed v1 is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the position is recorded; when "poor chip removal" is identified, the coolant pressure is increased or the pulse-type high-pressure internal cooling is switched. For layer sawing process, the status statistics of each layer are recorded after each layer is sawed. When the abnormal index of a certain layer exceeds the set threshold, the cutting depth of the subsequent layers is automatically reduced by 10% to 20% until the status returns to normal.

[0034] S5. Post-processing: After sawing, the fin array 3 is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0035] Testing revealed that the sidewall perpendicularity of fin 3 obtained in this embodiment is ≤0.04mm / 5mm, surface roughness Ra≈2.5μm, and fin thickness consistency is ±0.015mm. The thermal conductivity retention rate of the processed plate is approximately 93%, with no tooth chipping or tool breakage. The processing cycle for a single group (5 slots) is approximately 2 minutes, representing an efficiency improvement of approximately 4 times compared to end milling with a micro-diameter milling cutter of the same specifications. After laser in-situ modification pretreatment, the sawing force fluctuation amplitude under the same sawing parameters is reduced, and the saw blade 5 lifespan is extended.

[0036] Example 2 A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: (1) A diamond-copper composite substrate 1 prepared by gas pressure melting infiltration method was selected. The diamond volume fraction was about 50% and the average particle size was 150μm. The surface 2 of the fin 3 was ground by surface grinding with diamond grinding wheel #200 and grinding depth of 0.02mm / time. The surface was then polished to Ra<1μm. (2) Place the substrate 1 on the vacuum chuck with the fin 3 processing surface 2 facing upward. Use the vacuum chuck to ensure that the bottom surface of the substrate 1 is in close contact with the reference and the flatness is ≤0.08mm.

[0037] S2, Saw blade type 5 fin 3 processing: (1) Five sets of combined saw blades are used: the saw blade 5 is a PCD tooth tip thin blade saw blade 5 with a thickness t=0.3mm and an outer diameter D=50mm. The saw blades 5 are equally spaced on the cutter shaft through spacer sleeves 6. The interval between adjacent saw blades 5 is s=0.7mm (i.e., the thickness of two fins 3 + the thickness of saw blade 5, the thickness of fins 3 is w=0.2mm), and the thickness of saw blade 5 is t=0.3mm (i.e., the gap between fins 3 is I=0.3mm). The tooth shape of saw blade 5 adopts a staggered tooth structure. (2) A layered cutting method is adopted. The target fin height h=4mm, the cutting depth of each layer is 0.2mm, and a total of 20 layers are added layer by layer to saw to the target depth. The sawing process parameters are: saw blade 5 linear speed v1=20m / s, feed speed v2=30mm / min, and forced cooling and chip removal are carried out using lubricating mist cutting fluid. (3) Using an alternating slot method, first saw all odd-numbered slots, then saw all even-numbered slots; (4) Before sawing all even-numbered slots, fill the already sawn odd-numbered slots with wax support medium. After sawing, remove the support medium by heating to melt or ultrasonic cleaning.

[0038] S3. Online monitoring and adaptive control: (1) During the sawing process, the sawing status signal is collected in real time by a triaxial piezoelectric force gauge and a broadband piezoelectric acoustic emission sensor; (2) Extract the mean and fluctuation amplitude of the normal force Fn and the tangential force Ft and the frequency domain characteristics from the force signal; extract the root mean square value, event count rate and spectral centroid from the acoustic emission signal, and map the real-time signal to normal sawing, diamond particle cutting, tool wear, tooth breakage precursor or poor chip removal status; (3) When "diamond particle cutting" is identified, the feed rate v2 is reduced to 70% of the current value, while the saw blade linear speed v1 is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the position is recorded; when "poor chip removal" is identified, the coolant pressure is increased or the pulse-type high-pressure internal cooling is switched. For layer sawing process, the status statistics of each layer are recorded after each layer is sawed. When the abnormal index of a certain layer exceeds the set threshold, the cutting depth of the subsequent layers is automatically reduced by 10% to 20% until the status returns to normal.

[0039] S4. Post-processing: After sawing, the fin array 3 is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0040] Upon testing, the verticality of the sidewall of fin 3 obtained in this embodiment is ≤0.09mm / 5mm, the surface roughness Ra≈3.8μm, the thickness consistency of fin 3 is ±0.04mm, the thermal conductivity retention rate of the plate after processing is about 88%, slight tooth chipping occurs, and the processing cycle of a single group (5 slots) is about 3.2min.

[0041] Example 3 A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: (1) A diamond-copper composite substrate 1 prepared by gas pressure melting infiltration method was selected. The diamond volume fraction was about 50% and the average particle size was 150μm. The surface 2 of the fin 3 was ground by surface grinding with diamond grinding wheel #200 and grinding depth of 0.02mm / time. The surface was then polished to Ra<1μm. (2) Place the substrate 1 on the vacuum chuck with the fin 3 processing surface 2 facing upward. Use the vacuum chuck to ensure that the bottom surface of the substrate 1 is in close contact with the reference and the flatness is ≤0.08mm.

[0042] S2, Laser in-situ modification pretreatment (1) A nanosecond pulsed laser with a wavelength of 1064 nm, a pulse width of 50 ns, and a pulse energy density of 15 J / cm² was used. 2 The scanning speed is 500 mm / s and the spot overlap rate is 60%. Laser in-situ modification treatment is performed on the sawing area of ​​the processing surface 2 of fin 3. (2) The laser scanning path coincides with the subsequent sawing trajectory, and the width of the laser scanning path is 1.3 times the thickness t of the saw blade 5; (3) The modification depth is 0.2 mm, which is the same as the subsequent single-layer sawing depth; a graphitized modification layer with a thickness of about 10 to 20 μm is formed on the surface of the diamond particles.

[0043] S3, saw blade type 5 fin 3 processing: (1) Five sets of combined saw blades are used: the saw blade 5 is a PCD tooth tip thin blade saw blade 5 with a thickness t=0.3mm and an outer diameter D=50mm. The saw blades 5 are mounted on the cutter shaft at equal intervals through spacer sleeves 6. The interval between adjacent saw blades 5 is s=0.7mm (i.e., the thickness of the two fins 3 + the thickness of the saw blade 5, the thickness of the fins 3 is w=0.2mm), and the thickness of the saw blade 5 is t=0.3mm (i.e., the gap between the fins 3 is I=0.3mm). The tooth shape of the saw blade 5 adopts a staggered tooth structure. (2) A layered cutting method is adopted. The target fin height h=4mm, the cutting depth of each layer is 0.2mm, and a total of 20 layers are added layer by layer to saw to the target depth. The sawing process parameters are: saw blade 5 linear speed v1=20m / s, feed speed v2=30mm / min, and forced cooling and chip removal are carried out using lubricating mist cutting fluid.

[0044] S3. Online monitoring and adaptive control: (1) During the sawing process, the sawing status signal is collected in real time by a triaxial piezoelectric force gauge and a broadband piezoelectric acoustic emission sensor; (2) Extract the mean and fluctuation amplitude of the normal force Fn and the tangential force Ft and the frequency domain characteristics from the force signal; extract the root mean square value, event count rate and spectral centroid from the acoustic emission signal, and map the real-time signal to normal sawing, diamond particle cutting, tool wear, tooth breakage precursor or poor chip removal status; (3) When "diamond particle cutting" is identified, the feed rate v2 is reduced to 70% of the current value, while the saw blade linear speed v1 is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the position is recorded; when "poor chip removal" is identified, the coolant pressure is increased or the pulse-type high-pressure internal cooling is switched. For layer sawing process, the status statistics of each layer are recorded after each layer is sawed. When the abnormal index of a certain layer exceeds the set threshold, the cutting depth of the subsequent layers is automatically reduced by 10% to 20% until the status returns to normal.

[0045] S4. Post-processing: After sawing, the fin array 3 is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0046] Upon testing, the verticality of the sidewall of fin 3 obtained in this embodiment is ≤0.10mm / 5mm, Ra≈3.5μm, the thickness uniformity of fin 3 is ±0.045mm, the thermal conductivity retention rate is about 89%, fin 3 shows lateral tilting, and the processing cycle of a single group (5 slots) is about 2.8m.

[0047] Example 4 A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: (1) A diamond-copper composite substrate 1 prepared by gas pressure melting infiltration method was selected. The diamond volume fraction was about 50% and the average particle size was 150μm. The surface 2 of the fin 3 was ground by surface grinding with diamond grinding wheel #200 and grinding depth of 0.02mm / time. The surface was then polished to Ra<1μm. (2) Place the substrate 1 on the vacuum chuck with the fin 3 processing surface 2 facing upward. Use the vacuum chuck to ensure that the bottom surface of the substrate 1 is in close contact with the reference and the flatness is ≤0.08mm.

[0048] S2, Laser in-situ modification pretreatment (1) A nanosecond pulsed laser with a wavelength of 1064 nm, a pulse width of 50 ns, and a pulse energy density of 15 J / cm² was used. 2 The scanning speed is 500 mm / s and the spot overlap rate is 60%. Laser in-situ modification treatment is performed on the sawing area of ​​the processing surface 2 of fin 3. (2) The laser scanning path coincides with the subsequent sawing trajectory, and the width of the laser scanning path is 1.3 times the thickness t of the saw blade 5; (3) The modification depth is 0.2 mm, which is the same as the subsequent single-layer sawing depth; a graphitized modification layer with a thickness of about 10 to 20 μm is formed on the surface of the diamond particles.

[0049] S3, saw blade type 5 fin 3 processing: (1) Five sets of combined saw blades are used: the saw blade 5 is a PCD tooth tip thin blade saw blade 5 with a thickness t=0.3mm and an outer diameter D=50mm. The saw blades 5 are mounted on the cutter shaft at equal intervals through spacer sleeves 6. The interval between adjacent saw blades 5 is s=0.7mm (i.e., the thickness of the two fins 3 + the thickness of the saw blade 5, the thickness of the fins 3 is w=0.2mm), and the thickness of the saw blade 5 is t=0.3mm (i.e., the gap between the fins 3 is I=0.3mm). The tooth shape of the saw blade 5 adopts a staggered tooth structure. (2) A layered cutting method is adopted. The target fin height h=4mm, the cutting depth of each layer is 0.2mm, and a total of 20 layers are added layer by layer to saw to the target depth. The sawing process parameters are: saw blade 5 linear speed v1=20m / s, feed speed v2=30mm / min, and forced cooling and chip removal are carried out using lubricating mist cutting fluid. (3) Using an alternating slot method, first saw all odd-numbered slots, then saw all even-numbered slots; (4) Before sawing all even-numbered slots, fill the already sawed odd-numbered slots with wax support medium; after sawing, remove the support medium by heating to melt or ultrasonic cleaning.

[0050] S4. Post-processing: After sawing, the fin array 3 is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0051] Upon testing, the verticality of the sidewall of fin 3 obtained in this embodiment is ≤0.07mm / 5mm, Ra≈3.2μm, the thickness consistency of fin 3 is ±0.03mm, the thermal conductivity retention rate is about 90%, slight tooth breakage occurs, and the processing cycle of a single group (5 slots) is about 2.6min.

[0052] Example 5 A novel finning method for a finned diamond copper liquid cooling plate includes the following steps: S1. Material preparation and clamping positioning: (1) A diamond-copper composite substrate 1 prepared by gas pressure melting infiltration method was selected. The diamond volume fraction was about 50% and the average particle size was 150μm. The surface 2 of the fin 3 was ground by surface grinding with diamond grinding wheel #200 and grinding depth of 0.02mm / time. The surface was then polished to Ra<1μm. (2) Place the substrate 1 on the vacuum chuck with the fin 3 processing surface 2 facing upward. Use the vacuum chuck to ensure that the bottom surface of the substrate 1 is in close contact with the reference and the flatness is ≤0.08mm.

[0053] S2, Laser in-situ modification pretreatment (1) A nanosecond pulsed laser with a wavelength of 1064 nm, a pulse width of 50 ns, and a pulse energy density of 15 J / cm² was used. 2 The scanning speed is 500 mm / s and the spot overlap rate is 60%. Laser in-situ modification treatment is performed on the sawing area of ​​the processing surface 2 of fin 3. (2) The laser scanning path coincides with the subsequent sawing trajectory, and the width of the laser scanning path is 1.3 times the thickness t of the saw blade 5; (3) The modification depth is 0.2 mm, which is the same as the subsequent single-layer sawing depth; a graphitized modification layer with a thickness of about 10 to 20 μm is formed on the surface of the diamond particles.

[0054] S3, saw blade type 5 fin 3 processing: (1) Five sets of combined saw blades are used: the saw blade 5 is a PCD tooth tip thin blade saw blade 5 with a thickness t=0.3mm and an outer diameter D=50mm. The saw blades 5 are mounted on the cutter shaft at equal intervals through spacer sleeves 6. The interval between adjacent saw blades 5 is s=0.7mm (i.e., the thickness of the two fins 3 + the thickness of the saw blade 5, the thickness of the fins 3 is w=0.2mm), and the thickness of the saw blade 5 is t=0.3mm (i.e., the gap between the fins 3 is I=0.3mm). The tooth shape of the saw blade 5 adopts a staggered tooth structure. (2) A layered cutting method is adopted. The target fin height h=4mm, the cutting depth of each layer is 0.2mm, and a total of 20 layers are added layer by layer to saw to the target depth. The sawing process parameters are: saw blade 5 linear speed v1=20m / s, feed speed v2=30mm / min, and forced cooling and chip removal are carried out using lubricating mist cutting fluid. (3) Using an alternating slot method, first saw all odd-numbered slots, then saw all even-numbered slots.

[0055] S4. Online monitoring and adaptive control (1) The sawing status signal was collected in real time by a triaxial piezoelectric force gauge (sampling frequency 10kHz) and a broadband piezoelectric acoustic emission sensor (100kHz–1MHz, sampling frequency 2MHz); (2) Extract the mean value, fluctuation amplitude, and frequency domain characteristics of the force signal, as well as the root mean square value of acoustic emission, event count rate, and spectral centroid to identify the sawing state; (3) When "diamond particle cutting" is identified, the feed rate is reduced to 70% of the current value and the linear speed is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the location is recorded; when "poor chip removal" is identified, the coolant pressure is increased or pulse-type high-pressure internal cooling is switched. After each layer of sawing, the status statistics are recorded. When the abnormal index exceeds the threshold, the cutting depth of the subsequent layer is automatically reduced by 10%–20%.

[0056] S5. Post-processing: After sawing, the fin array 3 is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed, and dried.

[0057] Upon testing, the verticality of the sidewall of fin 3 obtained in this embodiment is ≤0.08mm / 5mm, Ra≈3.0μm, the thickness uniformity of fin 3 is ±0.035mm, the thermal conductivity retention rate is about 90%, slight vibration and lateral displacement of fin 3 are observed, and the processing cycle of a single group (5 slots) is about 2.4min.

[0058] In summary, after removing laser modification in Example 2, the sawing force fluctuation increased, and the perpendicularity, roughness, and thickness consistency all deteriorated significantly, with slight tooth breakage occurring. This indicates that the laser modification layer can effectively reduce the impact of diamond particles on the PCD cutting teeth. In Example 3, after removing the alternating slots, both sides of fin 3 lost support simultaneously, resulting in severe lateral tilting and the worst perpendicularity and thickness consistency. In Example 4, after removing online monitoring, it was unable to respond promptly to the signs of diamond particle cutting and tooth breakage, resulting in slight tooth breakage and medium quality. In Example 5, after removing wax filling, the empty slots in odd-numbered slots caused slight vibration and displacement of fin 3 during sawing in even-numbered slots, resulting in lower-than-average quality.

[0059] Example 1 has the best overall quality: perpendicularity ≤0.04mm / 5mm, Ra≈2.5μm, thickness consistency ±0.015mm, thermal conductivity retention rate 93%, no tooth breakage or tool breakage, cycle time 2min, balancing quality and efficiency.

[0060] In this invention, by combining in-situ laser modification pretreatment with saw blade 5 for fin 3 processing, the significant difference in laser absorption rates between diamond and copper is utilized to ensure that laser energy is preferentially absorbed by diamond particles. This causes localized graphitization transformation of the diamond surface, forming a mechanically removable modified layer. This transforms the "hard-on-hard sawing of diamond" into "controllable removal of the modified layer by PCD cutter teeth," reducing sawing difficulty and minimizing random chipping and pull-out of diamond particles. Through composite monitoring and adaptive control, the sawing process possesses real-time status perception capabilities. Addressing the randomness of diamond particle distribution, the adaptive control strategy is designed for "passing through densely populated areas" and "identifying early signs of wear," achieving a closed-loop control of "perception-decision-execution." The efficiency is doubled by combining saw blade 5 to form multiple grooves in one step. Deformation of fin 3 is suppressed through layered cutting, alternating grooves, and support filling.

[0061] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

[0062] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0063] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A novel fin processing method for a finned diamond copper liquid cooling plate, characterized in that, Includes the following steps: S1. Material preparation and clamping positioning: S2. Laser in-situ modification pretreatment: (1) A nanosecond pulsed laser is used to perform in-situ laser modification on the processing surface (2) of the fin (3) to be sawed. S3, saw blade (5) type fin (3) processing: (1) Using a combination saw blade (5) group: the saw blade (5) is mounted on the cutter shaft at equal intervals through the spacer sleeve (6), and the interval between adjacent saw blades (5) is the thickness of two fins (3) + the thickness of the saw blade (5); S4. Online monitoring and adaptive control: (1) During the sawing process, the sawing status signal is collected in real time by a triaxial piezoelectric force gauge and a broadband piezoelectric acoustic emission sensor; (2) Map the real-time signal to normal sawing, diamond particle cutting, tool wear, signs of tooth breakage, or poor chip removal. S5. Post-processing: After sawing, the fin array (3) is deburred, ultrasonically cleaned with anhydrous ethanol for 15 minutes to remove chips and residual abrasive particles, trimmed and dried.

2. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S3, an alternating slotting method is used: first, all odd-numbered slots are sawn; after completing the odd-numbered slots, all even-numbered slots are sawn.

3. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S3, before sawing all even-numbered slots, waxy support medium is filled into the already sawn odd-numbered slots to provide lateral rigid support for the thin-walled fins (3) that are being formed.

4. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S4, the mean and fluctuation amplitude of the normal force Fn and the tangential force Ft, as well as the frequency domain characteristics, are extracted from the force signal. Extract the root mean square value, event count rate, and spectral centroid from the acoustic emission signal.

5. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S4, when "diamond particle cutting" is identified, the feed rate v2 is reduced to 70% of the current value, while the saw blade (5) linear speed v1 is increased to 110% of the current value; when "tool wear / tooth breakage precursor" is identified, an alarm is triggered and the position is recorded; when "poor chip removal" is identified, the coolant pressure is increased or the pulse high-pressure internal cooling is switched.

6. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S1, a diamond-copper composite substrate (1) prepared by gas pressure melting infiltration is selected. Before processing, the processing surface (2) of the fins (3) is ground to remove the surface copper layer so that the diamond reinforcement phase is uniformly exposed.

7. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S3, a layered cutting method is adopted, and sawing is carried out layer by layer until the target depth is reached.

8. The novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S2, the laser scanning path coincides with the subsequent sawing trajectory; the modification depth is the same as the subsequent single-layer sawing depth.

9. A novel fin processing method for a finned diamond copper liquid cooling plate according to claim 8, characterized in that, In step S2, the width of the laser scanning path is 1.3 times the thickness t of the saw blade (5) to ensure that the PCD blade teeth mainly contact the diamond modified layer rather than the original diamond surface during sawing.

10. A novel fin processing method for a finned diamond copper liquid cooling plate according to claim 1, characterized in that, In step S3, the saw blade (5) adopts a staggered tooth structure, so that each tooth removes material in layers during the sawing process and alternately polishes the processed sidewalls.