Thermoplastic composite fiber wood mold and its vacuum mixing and extrusion production process

By using thermoplastic composite fiber materials and vacuum rubber extrusion technology, the problems of single performance and low production efficiency of traditional wood substitute formwork have been solved, resulting in high-strength, lightweight, and corrosion-resistant composite fiber formwork suitable for high-end equipment, reducing production costs and energy consumption.

CN123060892APending Publication Date: 2026-11-10FUJIAN QUANZHOU LUOJIANG ZHENFENG MOPEI MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611223598.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional wood-based formwork has limited performance, with difficulty in achieving a balance between strength, toughness, temperature resistance, and corrosion resistance. Poor compatibility between fillers and resins leads to products that are prone to cracking, deformation, and uneven density, failing to meet the requirements of high-end equipment. Furthermore, it has high production costs and low processing efficiency.

Method used

Using thermoplastic composite fiber materials, combined with vacuum rubber mixing and vacuum extrusion molding processes, and through the compounding of multifunctional fillers and multiple resins, the material is uniformly mixed and molded by using vacuum and temperature control. It is equipped with integrated continuous production equipment to achieve high strength, lightweight, corrosion resistance and reduce production costs.

Benefits of technology

The resulting thermoplastic composite fiber wood substitute formwork possesses high strength, wear resistance, corrosion resistance, and lightweight characteristics. It has a smooth surface, stable mechanical properties, and high production efficiency, making it suitable for high-end equipment and reducing production energy consumption and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060892A_ABST
    Figure CN123060892A_ABST
Patent Text Reader

Abstract

The present application relates to wood material forming equipment and preparation technical field, and disclose a kind of thermoplastic composite wood template, including sequentially communicating according to production procedure and being arranged raw material metering and pretreatment device, vacuum rubber mixing device, closed vacuum conveying device, vacuum extrusion forming device, cooling setting device and post-processing finishing device, the working vacuum degree of the vacuum rubber mixing device is-0.08~‑0.1MPa, the working vacuum degree of the vacuum extrusion forming device is-0.07~‑0.09MPa, and both are configured independent vacuum control system and temperature closed-loop control moduleThe thermoplastic composite fiber wood template, the thermoplastic composite fiber wood template utilizes quaternary thermoplastic resin compounding and multifunctional filler synergistic formulation setting, so that product has high strength, high wear resistance, temperature resistance, corrosion resistance and lightweight characteristics simultaneously, adapt to automobile mould, marine equipment, military equipment and other high-end scene use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wood substitute material molding equipment and preparation technology, specifically to a thermoplastic composite fiber wood substitute template and its vacuum rubber compounding and extrusion production process. Background Technology

[0002] Wood substitute formwork, as an engineering material that can replace solid wood for mold making and structural forming, is widely used in automotive molds, gauges, ship models, building formwork, and large equipment manufacturing. Traditional wood substitute materials are mostly based on thermosetting resins or single thermoplastic resins, combined with conventional inorganic fillers, and formed through simple extrusion and molding processes. This meets the basic usage requirements of ordinary models and simple components, and is currently a common wood substitute forming material in industrial production.

[0003] Existing traditional wood substitute formwork has significant technical defects in its formulation design and production process: First, the resin component is singular, and its strength, toughness, temperature resistance, and corrosion resistance are difficult to coordinate, making it unsuitable for high-end scenarios such as military and marine equipment; second, the filler and resin have poor compatibility, making the products prone to delamination, cracking, deformation, and short service life; third, conventional processes lack vacuum assistance, resulting in uneven material mixing and residual air bubbles, leading to uneven density, poor mechanical properties, rough surfaces, and a large amount of subsequent processing; fourth, it is difficult to balance weight and strength, either being too heavy for easy handling or too weak for easy damage, failing to meet the requirements of large-scale lightweight buildings and high-end equipment; fifth, the cost is too high, with low raw material utilization and cumbersome processing procedures, further increasing the overall production and use costs.

[0004] Therefore, a thermoplastic composite fiber wood substitute template and its vacuum rubber compounding and extrusion production process are proposed to solve the above-mentioned problems. Summary of the Invention

[0005] (a) Technical problems to be solved

[0006] To address the shortcomings of existing technologies, this invention provides a thermoplastic composite fiber wood substitute template and its vacuum rubber compounding and extrusion production process, which solves the problems of traditional wood substitute templates having single performance, poor molding quality, easy cracking and deformation, low processing efficiency, and inability to simultaneously meet the requirements of high strength, lightweight, temperature and corrosion resistance, and high-end equipment use.

[0007] (II) Technical Solution

[0008] To achieve the above objectives, the present invention provides the following technical solution: a thermoplastic composite fiber wood substitute template, comprising a raw material metering and pretreatment device, a vacuum rubber mixing device, a closed vacuum conveying device, a vacuum extrusion molding device, a cooling and shaping device, and a post-processing finishing device arranged sequentially in the production process. The working vacuum degree of the vacuum rubber mixing device is -0.08 to -0.1 MPa, and the working vacuum degree of the vacuum extrusion molding device is -0.07 to -0.09 MPa. Both are equipped with independent vacuum control systems and temperature closed-loop control modules.

[0009] Preferably, the raw material metering and pretreatment device includes an automatic metering and feeding mechanism, a low-temperature pulverizing mechanism, and a hot air circulating drying mechanism; the low-temperature pulverizing mechanism pulverizes polyethylene, polypropylene, nylon, and PEEK main materials to 80-120 mesh, the hot air circulating drying mechanism dries the main materials to a moisture content ≤0.5%, and dries aluminum hydroxide, talc, calcite powder, and nano-calcium carbonate auxiliary materials to a moisture content ≤0.3%.

[0010] Preferably, the vacuum rubber mixing device is a closed vacuum rubber mixing machine, which is equipped with a dual-rotor mixing mechanism, a jacket temperature control mechanism and a speed adjustment mechanism; the mixing temperature control range is 160-220℃, the rotor speed control range is 30-50r / min, and the single mixing time setting range is 15-25min.

[0011] Preferably, the sealed vacuum conveying device is a sealed spiral conveying mechanism or a negative pressure pneumatic conveying mechanism, which maintains a micro-vacuum state inside, and is used to convey the molten material after vacuum rubber mixing to the vacuum extrusion molding device without contact or bubbles.

[0012] Preferably, the vacuum extrusion molding device is a single-screw / twin-screw vacuum extruder, which includes a screw extrusion mechanism, a die forming mechanism, an extrusion temperature control mechanism, and a speed control mechanism; the extrusion temperature control range is 150-210℃, the extrusion linear speed control range is 5-10m / min, and the die outlet is equipped with an online thickness adjustment mechanism.

[0013] Preferably, the cooling and shaping device includes a multi-stage cooling water tank and a high-pressure air dryer; the multi-stage cooling water tank is temperature-controlled in sections, and the overall water temperature is maintained at 20-30℃, and the cooling path length meets the requirement of 10-15 minutes for the billet cooling and shaping time; the high-pressure air dryer is used to remove residual moisture from the surface of the billet after shaping.

[0014] Preferably, the post-processing finishing device includes a fixed-length cutting mechanism, a flat grinding mechanism, a mirror polishing mechanism, and an optional coating spraying mechanism, which can perform fixed-length, edge trimming, polishing, and surface protection treatment on the wood substitute template blank.

[0015] Preferably, both the vacuum rubber mixing device and the vacuum extrusion molding device are equipped with a real-time vacuum degree acquisition, display and over-tolerance alarm module, as well as a temperature, rotation speed and speed linkage PID adjustment module to achieve fully automatic and stable control of process parameters.

[0016] Preferably, the equipment is also equipped with a central control system, which is electrically connected to the raw material metering, vacuum rubber mixing, vacuum extrusion, cooling and shaping, and post-processing devices. This system is used to store multiple sets of formula parameters and realize one-click automated production.

[0017] A vacuum rubber compounding and extrusion production process for thermoplastic composite fiber wood substitute templates further includes the following steps:

[0018] Step 1: Raw material pretreatment and metering: The main and auxiliary materials are automatically metered according to the formula ratio. The main material is crushed to 80-120 mesh and dried to a moisture content of ≤0.5%. The inorganic powder auxiliary materials are dried to a moisture content of ≤0.3%.

[0019] Step 2: Put the pretreated main material and auxiliary material into the vacuum rubber mixing device, close the chamber and evacuate to -0.08~-0.1MPa, control the temperature at 160-220℃ and the rotation speed at 30-50r / min, mix for 15-25min, and continuously transport the molten mixture to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device.

[0020] Step 3: The molten mixture is continuously conveyed to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device. Then, the vacuum extrusion molding device is started, the barrel vacuum degree is maintained at -0.07~-0.09MPa, the extrusion temperature is controlled at 150-210℃ and the extrusion speed is 5-10m / min, and the continuous wood template blank is obtained by extrusion through the die head.

[0021] Step 4: Pour the extruded blank into a multi-stage cooling water tank at 20-30℃ for 10-15 minutes to cool and quickly set the shape. Then, remove the surface moisture by high-pressure air drying. Next, cut the shaped blank to a fixed length, grind the surface, and polish it to a mirror finish. Selectively apply a protective coating according to the usage requirements to finally obtain the finished thermoplastic composite fiber wood substitute template.

[0022] (III) Beneficial Effects

[0023] Compared with the prior art, the present invention provides a thermoplastic composite fiber wood substitute template, which has the following beneficial effects:

[0024] 1. This thermoplastic composite fiber wood substitute template utilizes a synergistic formula of quaternary thermoplastic resin compound and multifunctional filler to give the product high strength, high wear resistance, temperature resistance, corrosion resistance and lightweight properties, making it suitable for high-end applications such as automotive molds, marine equipment, and military equipment.

[0025] 2. This thermoplastic composite fiber wood substitute template utilizes a dual vacuum process of vacuum rubber mixing and vacuum extrusion molding to completely eliminate air bubbles inside the material, resulting in products with uniform density, smooth surface, and stable mechanical properties, significantly reducing the amount of subsequent processing work.

[0026] 3. This thermoplastic composite fiber wood substitute formwork utilizes integrated continuous production equipment and fully automatic parameter control settings to achieve adjustable formula, stable process, and high batch consistency. It can produce large-scale lightweight wood substitute formwork in multiple specifications, improving production efficiency and reducing energy consumption. Attached Figure Description

[0027] Figure 1 This is a flowchart illustrating the overall structure of a thermoplastic composite fiber wood substitute formwork device proposed in this invention.

[0028] Figure 2 This is a flow chart of a vacuum rubber compounding and extrusion process for a thermoplastic composite fiber wood substitute template proposed in this invention. Detailed Implementation

[0029] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] Please see Figure 1 - Figure 2 As shown, a thermoplastic composite fiber wood substitute template includes a raw material metering and pretreatment device, a vacuum rubber mixing device, a closed vacuum conveying device, a vacuum extrusion molding device, a cooling and shaping device, and a post-processing finishing device, arranged sequentially in the production process. The working vacuum degree of the vacuum rubber mixing device is -0.08 to -0.1 MPa, and the working vacuum degree of the vacuum extrusion molding device is -0.07 to -0.09 MPa. Both are equipped with independent vacuum control systems and temperature closed-loop control modules.

[0031] First, the raw material metering and pretreatment device includes an automatic metering and feeding mechanism, a low-temperature pulverizing mechanism, and a hot air circulating drying mechanism. The low-temperature pulverizing mechanism pulverizes polyethylene, polypropylene, nylon, and PEEK main materials to 80-120 mesh, while the hot air circulating drying mechanism dries the main materials to a moisture content of ≤0.5% and dries aluminum hydroxide, talc, calcite powder, and nano-calcium carbonate auxiliary materials to a moisture content of ≤0.3%. Through precise pulverization to refine the particle size and deep drying to strictly control moisture, the compatibility of the resin and inorganic filler interface is improved, and the introduction of air bubbles by moisture is avoided from the source, providing a high-quality raw material foundation for subsequent homogeneous mixing and stable extrusion.

[0032] Secondly, the vacuum rubber mixing device is a closed vacuum rubber mixing mill, which is equipped with a dual-rotor mixing mechanism, a jacket temperature control mechanism, and a speed adjustment mechanism. The mixing temperature control range is 160-220℃, the rotor speed control range is 30-50r / min, and the single mixing time setting range is 15-25min. Through the closed vacuum chamber, precise temperature control, and speed matching, the multi-component resin is fully melted and the filler is evenly dispersed, realizing vacuum bonding and bubble-free homogeneous mixing, ensuring the consistency of material performance.

[0033] Furthermore, the closed vacuum conveying device is a sealed screw conveyor or a negative pressure pneumatic conveying mechanism. It maintains a micro-vacuum state inside and is used to convey the molten material after vacuum rubber mixing to the vacuum extrusion molding device without contact or air bubbles. Through the closed micro-vacuum conveying throughout the process, secondary air intake and external pollution are eliminated, the homogeneous and stable state of the molten material is maintained, the material is prevented from being degraded or mixed with impurities, and the quality of the extruded billet is guaranteed to be stable.

[0034] Furthermore, the vacuum extrusion molding device is a single-screw / twin-screw vacuum extruder, including a screw extrusion mechanism, a die forming mechanism, an extrusion temperature control mechanism, and a speed control mechanism; the extrusion temperature control range is 150-210℃, the extrusion linear speed control range is 5-10m / min, and the die outlet is equipped with an online thickness adjustment mechanism. Through vacuum extrusion, precise temperature control, and stable extrusion speed, continuous and dense forming of the billet is achieved, and the dimensions are precisely controllable, improving the product strength, density, and surface finish, and making it suitable for use with high-end molds and equipment.

[0035] Furthermore, the cooling and shaping device includes a multi-stage cooling water tank and a high-pressure air dryer; the multi-stage cooling water tank has segmented temperature control, and the overall water temperature is maintained at 20-30℃. The cooling path length meets the requirement of 10-15 minutes for the billet cooling and shaping time. The high-pressure air dryer is used to remove residual moisture on the surface of the billet after shaping. Through gradient temperature-controlled water cooling and rapid air drying, the billet is quickly and uniformly shaped, suppressing the release of internal stress, preventing warping and deformation, and ensuring dimensional stability and surface cleanliness.

[0036] Furthermore, the post-processing finishing equipment includes a fixed-length cutting mechanism, a flat grinding mechanism, a mirror polishing mechanism, and an optional coating spraying mechanism. It can perform fixed-length cutting, trimming, polishing, and surface protection treatment on the wood template blanks. Through standardized finishing processes, it improves the dimensional accuracy and surface smoothness of the templates, further enhancing their wear resistance, water resistance, and corrosion resistance to meet the requirements of high-end application scenarios such as automotive molds and marine military equipment.

[0037] Furthermore, both the vacuum rubber mixing unit and the vacuum extrusion molding unit are equipped with a real-time vacuum degree acquisition, display, and over-tolerance alarm module, as well as a temperature, speed, and speed linkage PID control module to achieve fully automatic and stable control of process parameters. Through real-time monitoring, over-tolerance alarms, and multi-parameter linkage closed-loop control, the risks of temperature, vacuum degree, and speed fluctuations are effectively avoided, ensuring stable production processes and highly consistent performance of batch products.

[0038] Finally, the equipment is also equipped with a central control system, which is electrically connected to the raw material metering, vacuum rubber mixing, vacuum extrusion, cooling and shaping, and post-processing devices. It is used to store multiple sets of formula parameters and realize one-click automated production. Through centralized intelligent management and control, one-click recall of formula parameters and full-process linkage, it simplifies manual operation, reduces human error, significantly improves production efficiency, and realizes flexible continuous production of multiple formulas and specifications.

[0039] A vacuum rubber compounding and extrusion production process for thermoplastic composite fiber wood substitute templates further includes the following steps:

[0040] Step 1: Raw material pretreatment and metering: The main and auxiliary materials are automatically metered according to the formula ratio. The main material is crushed to 80-120 mesh and dried to a moisture content of ≤0.5%. The inorganic powder auxiliary materials are dried to a moisture content of ≤0.3%.

[0041] Step 2: Put the pretreated main material and auxiliary material into the vacuum rubber mixing device, close the chamber and evacuate to -0.08~-0.1MPa, control the temperature at 160-220℃ and the rotation speed at 30-50r / min, mix for 15-25min, and continuously transport the molten mixture to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device.

[0042] Step 3: The molten mixture is continuously conveyed to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device. Next, the vacuum extrusion molding device is started, maintaining the barrel vacuum degree at -0.07~-0.09MPa, controlling the extrusion temperature at 150-210℃ and the extrusion speed at 5-10m / min, and obtaining continuous wood template blanks through the die head.

[0043] Step 4: The extruded blank is poured into a multi-stage cooling water bath at 20-30℃ for 10-15 minutes to quickly set its shape; then it is air-dried under high pressure to remove surface moisture. Next, the shaped blank is cut to length, sanded, and mirror-polished in sequence. Depending on the usage requirements, a protective coating is selectively applied to finally obtain the finished thermoplastic composite fiber wood substitute template.

[0044] This invention provides a thermoplastic composite fiber wood substitute template that achieves performance enhancement through multi-resin compounding, synergistic use of multi-functional fillers, and a dual vacuum process of vacuum rubber mixing and vacuum extrusion. For ease of understanding, the following five specific embodiments provide a detailed description of the formulation composition, mass percentages, and applicable scenarios. This invention is not limited to these embodiments.

[0045] Basic Formulation Benchmark Table

[0046] This table lists the general basic components for all embodiments. PE wax has been added, and calcite powder has been broken down into five major components: calcium carbonate, magnesium oxide, silicon dioxide, iron, and hydrochloric acid-insoluble matter, clearly defining the material categories.

[0047] Components Quality percentage (%) illustrate Main ingredients 35 PE 10%, PP 10%, Nylon 10%, PEEK 5% (PEEK improves temperature resistance and abrasion resistance) Aluminum hydroxide 12 Flame retardant and filler, suitable for mold fire protection requirements. talcum powder 18 Improved hardness and wear resistance to meet the needs of repeated mold use. Calcium carbonate / Calcite powder as the main component improves dimensional stability and prevents mold deformation. magnesium oxide / Calcite powder composition optimizes filler dispersibility silicon dioxide / Calcite powder component enhances the wear resistance of the product. iron / Calcium powder impurity components Hydrochloric acid insoluble matter / Calcium powder impurity components Nano calcium carbonate 8 Refining grain size improves surface smoothness and reduces subsequent processing requirements. Barium stearate 4 Thermal stability and lubrication ensure smooth processing. Inorganic glass hollow microspheres / Organic foamed microspheres 6 Choose one of the two fillers to add, with the addition amount controlled within the range of 3-5%; inorganic glass hollow microspheres are used as inorganic fillers, and organic foamed microspheres are used as organic fillers. PE wax 4 Processing lubricant to improve material flowability and mold release efficiency Functional additives 3 Compatibilizer 1.5%, antioxidant 1%, lubricant 0.5%.

[0048] Example 1

[0049] This embodiment provides a thermoplastic composite fiber wood substitute template suitable for automotive molds and fixtures, focusing on improving material strength, wear resistance, and dimensional stability. The specific formula composition and mass percentage are shown in the table below:

[0050] Components Quality percentage (%) illustrate Main ingredients 35 PE 10%, PP 10%, Nylon 10%, PEEK 5% (PEEK improves temperature resistance and abrasion resistance) Aluminum hydroxide 12 Flame retardant and filler, suitable for mold fire protection requirements. talcum powder 18 Improved hardness and wear resistance to meet the needs of repeated mold use. Calcite powder 10 Improve dimensional stability and prevent mold deformation Nano calcium carbonate 8 Refining grain size improves surface smoothness and reduces subsequent processing requirements. Barium stearate 4 Thermal stability and lubrication ensure smooth processing. Organic foamed microbeads 7 Lightweight design while improving thermal insulation and soundproofing performance. Functional additives 3 Compatibilizer 1.5%, antioxidant 1%, lubricant 0.5% PE wax 4 Improve the flowability of molten material and enhance the stability of extrusion processing.

[0051] Example 2

[0052] This embodiment provides a thermoplastic composite fiber wood substitute template suitable for large marine equipment and military equipment, focusing on improving the material's corrosion resistance, temperature resistance, and flame retardancy. The specific formula composition and mass percentage are shown in the table below:

[0053] Components Quality percentage (%) illustrate Main ingredients 35 PE 8%, PP 8%, Nylon 12%, PEEK 7% (PEEK and Nylon improve temperature resistance and corrosion resistance) Aluminum hydroxide 25 The original 15%+ original calcite powder content, with its high addition level, achieves strong flame retardancy, meeting the fire protection requirements of military and marine equipment. talcum powder 12 Enhance strength to withstand the impact of the marine environment Calcite powder 12 Improve weather resistance and resist seawater corrosion Nano calcium carbonate 5 Improve material density and reduce seawater penetration Barium stearate 5 Enhanced thermal stability to adapt to high and low temperature marine environments Organic foamed microbeads 7 Lightweight design while improving thermal insulation and soundproofing performance. Functional additives 1 Compatibilizer 0.6%, antioxidant 0.4% (reduce the amount of additives to avoid affecting corrosion resistance) PE wax 4 Optimize material lubricity under high-temperature processing conditions

[0054] Example 3

[0055] This embodiment provides a thermoplastic composite fiber wood substitute formwork suitable for large-scale lightweight buildings and product models, focusing on improving the material's lightweight nature and ease of processing. The specific formula composition and mass percentage are shown in the table below:

[0056] Components Quality percentage (%) illustrate Main ingredients 35 PE 15%, PP 15%, Nylon 3%, PEEK 2% (PE and PP improve processability and reduce costs) Aluminum hydroxide 8 Basic flame retardancy, meeting building fire protection standards talcum powder 10 Improve foundation strength to prevent deformation of building formwork Calcite powder (calcium carbonate + magnesium oxide + silicon dioxide + iron + hydrochloric acid insoluble matter) 18 Original 8%+ Original aluminum hydroxide 8%, high filler reduces costs, improves processing fluidity, and offers excellent cost performance. Nano calcium carbonate 10 Improved surface smoothness facilitates model sculpting and architectural template assembly. Barium stearate 2 Basic lubrication ensures smooth extrusion molding. Inorganic glass hollow microspheres (inorganic filler) 3 Adding 3% lightweight filler reduces the self-weight of the template. Functional additives 5 2% compatibilizer, 1.5% antioxidant, and 1.5% lubricant improve processability and service life. PE wax 4 Improve the performance of secondary processing such as carving and cutting.

[0057] Example 4

[0058] This embodiment focuses on ultra-lightweight and low-density molding, replacing organic foamed microspheres (organic fillers) with thermally expandable microspheres from AkzoNobel (Germany) and Expancel (Japan), with the amount of microspheres added controlled in the range of 3-5%.

[0059] Components Quality percentage (%) illustrate Main ingredients 35 Composed of 12% PE, 12% PP, 6% nylon, and 5% PEEK, balancing strength and processability. Aluminum hydroxide 12 Basic flame retardancy, meeting general fire protection standards talcum powder 16 Balancing hardness and toughness to prevent product cracking Calcite powder (calcium carbonate + magnesium oxide + silicon dioxide + iron + hydrochloric acid insoluble matter) 8 Standard filling, stabilizing product dimensions Nano calcium carbonate 7 Refine grains and optimize surface texture Barium stearate 3 Basic thermal stability and lubrication Expancel thermally expandable microspheres (organic foamed microspheres / organic fillers) 4 Using two major brands, German AkzoNobel and Japanese Matsumoto, with an addition amount of 4%, organic fillers offer superior lightweight performance compared to inorganic microspheres. PE wax 4 Protect the structure of organic microbeads and prevent damage during high-temperature processing. Functional additives 3 Compatibilizer 1.5%, antioxidant 1%, lubricant 0.5%

[0060] Example 5

[0061] Components Quality percentage (%) illustrate Main ingredients 35 The composition is 16% PE, 14% PP, 3% nylon, and 2% PEEK, primarily using general-purpose resins to reduce costs. Aluminum hydroxide 7 Basic flame retardancy, meeting the requirements of civilian applications. talcum powder 9 Basic reinforcement to maintain structural strength Calcite powder (calcium carbonate + magnesium oxide + silicon dioxide + iron + hydrochloric acid insoluble matter) 10 High-performance filler reduces overall cost. Nano calcium carbonate 9 Improve surface finish Barium stearate 2 Simple lubrication, suitable for low-speed extrusion Expancel thermally expandable microspheres (organic foamed microspheres / organic fillers) 3 Organic filler, added at 3%, primarily for lightweighting, suitable for lightweight civilian products. PE wax 4 Improve material flowability under simple processing conditions Functional additives 4 Compatibilizer 2%, Antioxidant 1%, Lubricant 1%

Claims

1. A thermoplastic composite fiber wood substitute formwork, characterized in that, The device includes a raw material metering and pretreatment device, a vacuum rubber mixing device, a closed vacuum conveying device, a vacuum extrusion molding device, a cooling and shaping device, and a post-processing finishing device, which are connected in sequence according to the production process. The working vacuum degree of the vacuum rubber mixing device is -0.08 to -0.1 MPa, and the working vacuum degree of the vacuum extrusion molding device is -0.07 to -0.09 MPa. Both of them are equipped with independent vacuum control systems and temperature closed-loop control modules.

2. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The raw material metering and pretreatment device includes an automatic metering and feeding mechanism, a low-temperature pulverizing mechanism, and a hot air circulating drying mechanism. The low-temperature pulverizing mechanism pulverizes polyethylene, polypropylene, nylon, and PEEK main materials to 80-120 mesh. The hot air circulating drying mechanism dries the main materials to a moisture content of ≤0.5% and dries aluminum hydroxide, talc, calcite powder, and nano-calcium carbonate auxiliary materials to a moisture content of ≤0.3%.

3. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The vacuum rubber mixing device is a closed vacuum rubber mixing machine, which is equipped with a dual-rotor mixing mechanism, a jacket temperature control mechanism and a speed adjustment mechanism; the mixing temperature control range is 180-230℃, the rotor speed control range is 30-50r / min, and the single mixing time setting range is 15-25min.

4. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The sealed vacuum conveying device is a sealed spiral conveying mechanism or a negative pressure pneumatic conveying mechanism, which maintains a micro-vacuum state inside and is used to convey the molten material after vacuum rubber mixing to the vacuum extrusion molding device without contact or bubbles.

5. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The vacuum extrusion molding device is a single-screw / twin-screw vacuum extruder, which includes a screw extrusion mechanism, a die forming mechanism, an extrusion temperature control mechanism, and a speed control mechanism; the extrusion temperature control range is 150-210℃, the extrusion linear speed control range is 1-3m / min, and the die outlet is equipped with an online thickness adjustment mechanism.

6. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The cooling and shaping device includes a multi-stage cooling water tank and a high-pressure air dryer; the multi-stage cooling water tank is temperature-controlled in sections, and the overall water temperature is maintained at 20-30℃, and the cooling path length meets the requirement of 10-15 minutes for the billet cooling and shaping time.

7. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The post-processing finishing device includes a fixed-length cutting mechanism, a flat grinding mechanism, a mirror polishing mechanism, and an optional coating spraying mechanism, which can perform fixed-length, edge trimming, polishing, and surface protection treatment on the wood substitute template blank.

8. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: Both the vacuum rubber mixing device and the vacuum extrusion molding device are equipped with a real-time vacuum degree acquisition, display and over-tolerance alarm module, as well as a temperature, rotation speed and speed linkage PID adjustment module to achieve fully automatic and stable control of process parameters.

9. The thermoplastic composite fiber wood substitute formwork according to claim 1, characterized in that: The equipment is also equipped with a central control system, which is electrically connected to the raw material metering, vacuum rubber mixing, vacuum extrusion, cooling and shaping, and post-processing devices. It is used to store multiple sets of formula parameters and realize one-click automated production.

10. A vacuum rubber compounding and extrusion production process for thermoplastic composite fiber wood substitute templates, characterized in that, The thermoplastic composite fiber wood substitute formwork according to any one of claims 1-9 further includes the following steps: Step 1: Raw material pretreatment and metering: The main and auxiliary materials are automatically metered according to the formula ratio. The main material is crushed to 80-120 mesh and dried to a moisture content of ≤0.5%. The inorganic powder auxiliary materials are dried to a moisture content of ≤0.3%. Step 2: Put the pretreated main material and auxiliary material into the vacuum rubber mixing device, close the chamber and evacuate to -0.08~-0.1MPa, control the temperature at 160-220℃ and the rotation speed at 30-50r / min, mix for 15-25min, and continuously transport the molten mixture to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device. Step 3: The molten mixture is continuously conveyed to the vacuum extrusion molding device under micro-vacuum conditions through a closed vacuum conveying device. Next, the vacuum extrusion molding device is started, maintaining the barrel vacuum degree at -0.07~-0.09MPa, controlling the extrusion temperature at 150-210℃ and the extrusion speed at 5-10m / min, and obtaining a continuous wood template blank through the die head. Step 4: The extruded blank is poured into a multi-stage cooling water bath at 20-30℃ for 10-15 minutes to cool and quickly set the shape. Then, it is air-dried under high pressure to remove surface moisture. Next, the shaped blank is cut to length, sanded, and mirror-polished in sequence. Depending on the usage requirements, a protective coating is selectively applied to finally obtain the finished thermoplastic composite fiber wood substitute template.