Textile fabric with moisture absorption function and preparation method thereof

By using a three-layer textile fabric design, combining an inner hydrophobic and fast-wicking layer, a middle hydrophilic core layer, and an outer hydrophilic layer, the problem of insufficient moisture absorption and poor breathability of existing fabrics is solved, achieving the effects of rapid moisture absorption, moisture wicking, dryness, and water resistance, thus improving wearing comfort.

CN123060982APending Publication Date: 2026-11-10NANTONG FUEN NEW MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611585962.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing moisture-wicking textile fabrics have insufficient moisture-wicking capacity in their outer layer, making it difficult to meet the multiple requirements of efficient moisture absorption, rapid moisture wicking, long-lasting dryness, and water resistance. In addition, traditional fabrics have poor breathability, a stiff feel, and tend to retain and recirculate sweat.

Method used

The textile fabric features a three-layer structure: an inner hydrophobic and fast-conducting layer, a middle layer with an irregular cross-section hydrophilic core, and an outer layer of regenerated cellulose fiber/cotton blend hydrophilic layer. A moisture gradient transport structure is formed by point-like hot-melt bonding. The inner and outer layers have a large difference in water contact angle. The middle layer fiber surface is grafted with chitosan-polyethylene glycol graft copolymer, and the outer layer is composite with sodium polyacrylate moisture-absorbing microcapsules.

Benefits of technology

It enables sweat to be quickly removed from the skin and transported outward, improving the moisture wicking rate and washability, maintaining the breathability and soft feel of the fabric, preventing sweat backflow and sticky, stuffy feeling, and has antibacterial and moisturizing functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060982A_ABST
    Figure CN123060982A_ABST
Patent Text Reader

Abstract

This invention discloses a textile fabric with moisture-absorbing properties and its preparation method, relating to the field of textile fabric technology. The textile fabric is composed of an inner layer, a middle layer, and an outer layer, sequentially stacked and bonded together by point-like hot-melt bonding, forming a moisture gradient transport structure with increasing hydrophilicity from the inner layer to the outer layer. The inner layer is a hydrophobic fast-conducting layer woven from hydrophobic synthetic fibers with an irregular cross-section, and the water contact angle of the inner layer is 95°~110°. The middle layer is an irregular cross-section hydrophilic core layer. This invention employs a three-layer point-like hot-melt bonding composite process, which, compared to traditional overall lamination and sewing composite processes, ensures a stable composite effect of the three-layer structure while retaining the fabric's excellent breathability and soft feel. It avoids the problems of stiffness, poor breathability, and skin-friendliness caused by overall bonding, balancing structural stability and wearing comfort.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile fabric technology, specifically to a textile fabric with moisture-absorbing properties and its preparation method. Background Technology

[0002] With the continuous development of textile technology and the improvement of people's living standards, consumers have increasingly higher requirements for the comfort and functionality of textile fabrics. Functional textile fabrics with moisture-wicking properties have been widely used in sportswear, underwear, and home textiles. During daily activities or exercise, the human body continuously secretes sweat. If the fabric cannot effectively and quickly wick away and evaporate the sweat from the skin's surface, the sweat will accumulate between the fabric and the skin, causing the clothing to feel sticky, stuffy, and damp. This not only significantly reduces wearing comfort but also easily breeds bacteria, causing skin discomfort. Therefore, functional fabrics that are highly efficient at wicking away moisture, quickly wicking away moisture, and are dry and breathable have become a key focus of industry research and development.

[0003] Most moisture-wicking textiles currently on the market are woven from a single hydrophilic fiber or undergo simple hydrophilic finishing processes, resulting in limited functionality and significant technical shortcomings. Existing conventional moisture-wicking fabrics largely rely on the fiber's inherent hydrophilic properties to passively absorb sweat, leading to low sweat transfer efficiency and an inability to achieve directional gradient sweat transfer. Sweat tends to remain trapped and flow back into the inner layers of the fabric, causing the skin-friendly layer to remain damp for extended periods, resulting in extremely poor drying performance. Furthermore, the moisture-wicking function of traditional fabrics is unstable; after repeated washing, the surface hydrophilic modified coating easily peels off, significantly reducing moisture absorption and wicking properties, and shortening their lifespan.

[0004] Existing technologies also include some multi-layer composite moisture-wicking fabrics, but these multi-layer structures often employ integral bonding and sewing methods, resulting in poor overall breathability, a stiff feel, and small differences in the hydrophilicity gradient between layers. This prevents the formation of a stable moisture transfer mechanism, allowing sweat to rely solely on natural diffusion, leading to a slow moisture wicking rate. Furthermore, conventional middle moisture-wicking layers are mostly composed of ordinary hydrophilic fibers without interconnected microporous moisture-wicking channels, limiting their moisture storage and wicking capabilities. The outer hydrophilic structure is often a simple fiber blend without an active moisture-absorbing and energy-storing structure, making it difficult to quickly capture and lock in sweat. This hinders the achievement of rapid moisture absorption, instantaneous moisture wicking, and long-lasting dryness, and easily leads to sweat back-permeation into the skin. The insufficient moisture absorption capacity of the outer layer makes it difficult to simultaneously meet the multiple requirements of efficient moisture absorption, rapid moisture wicking, long-lasting dryness, and washability. Therefore, this invention proposes a textile fabric with moisture-wicking function and its preparation method. Summary of the Invention

[0005] To solve the above-mentioned technical problems, the present invention provides a textile fabric with moisture-absorbing function and a method for preparing the same. This technical solution solves the problem that the outer layer has insufficient moisture absorption capacity and is difficult to meet the multiple usage requirements of efficient moisture absorption, rapid moisture wicking, long-lasting dryness and water resistance.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a textile fabric with moisture-absorbing function, wherein the textile fabric is composed of an inner layer, a middle layer and an outer layer stacked in sequence and bonded together by point-like hot melt bonding, forming a moisture gradient transport structure with increasing hydrophilicity along the direction from the inner layer to the outer layer. The inner layer is a hydrophobic fast-conducting layer, woven from hydrophobic synthetic fibers with irregular cross-sections, and the water contact angle of the inner layer is 95°~110°. The intermediate layer is a hydrophilic core layer with an irregular cross-section, woven from modified polyester fibers with a W-shaped or Y-shaped cross-section. The modified polyester fibers have axially extending microporous channels with a pore size of 0.5~2μm and a porosity of 8%~15%. The surface of the modified polyester fibers is grafted with chitosan-polyethylene glycol graft copolymer, and the grafting rate is 3%~6% based on the dry weight calculated after Soxhlet extraction purification. The outer layer is a hydrophilic layer made of regenerated cellulose fiber / cotton blend yarn, woven from a blend of regenerated cellulose fiber and cotton. The outer layer contains sodium polyacrylate moisture-absorbing microcapsules with a particle size of 15-35 μm, and the content of the sodium polyacrylate moisture-absorbing microcapsules is 5%-10% of the dry weight of the outer layer. The water contact angle of the outer layer is 20°-35°. The difference between the water contact angle of the inner layer and the water contact angle of the outer layer is not less than [value missing]. .

[0007] Preferably, the W-shaped or Y-shaped profiled modified polyester fiber in the intermediate layer has a single fiber linear density of 1.2~2.5 dtex and a profile degree of 0.35~0.55; the basis weight of the inner layer is 40~60 g / m². 2 The basis weight of the intermediate layer is 80~120g / m³. 2 The outer layer has a basis weight of 60~90g / m³. 2 .

[0008] Preferably, in the chitosan-polyethylene glycol graft copolymer, the degree of deacetylation of chitosan is 85%~95%, and the number average molecular weight of polyethylene glycol is 2000~6000; the content of the chitosan-polyethylene glycol graft copolymer in the intermediate layer is 3%~6% of the dry weight of the intermediate layer; and the water contact angle of the intermediate layer is 60°~75°.

[0009] Preferably, the regenerated cellulose fiber in the outer layer is one or a combination of Lyocell fiber, Modal fiber, or bamboo pulp fiber; the mass ratio of the regenerated cellulose fiber to cotton is 4:6 to 6:4; the sodium polyacrylate moisture-absorbing microcapsules form a core-shell structure with cross-linked chitosan as the wall material and cross-linked sodium polyacrylate as the core material.

[0010] Preferably, the adhesive points of the dotted hot melt adhesive are arranged in a regular array, the spacing between the adhesive points is 3~6mm, the area of ​​the adhesive points accounts for 8%~15% of the total area of ​​the fabric, and the hot melt adhesive used is a polyamide copolymer or polyester copolymer hot melt adhesive powder with a melting point of 120~140℃.

[0011] Preferably, the fabric has a moisture absorption rate of not less than 32% after 60 minutes at a temperature of 25°C and a relative humidity of 90%, and the water droplet diffusion time does not exceed 3 seconds.

[0012] A method for preparing a textile fabric with moisture-absorbing properties includes the following steps: S1 Inner Layer Preparation: Hydrophobic synthetic fibers with irregular cross-sections are processed into yarn through cleaning, combing, drawing, roving, and spinning processes, and then woven to obtain the inner layer fabric. Preparation of S2 intermediate layer modified fiber: W-shaped or Y-shaped cross-section polyester fibers are pretreated by low-temperature plasma and then impregnated in chitosan-polyethylene glycol graft copolymer solution. After impregnation, padding and drying, modified polyester fibers with a grafting rate of 3%~6% are obtained. Then, the intermediate layer fabric is obtained by spinning and weaving. S3 outer layer preparation: Sodium polyacrylate moisture-absorbing microcapsule dispersion is applied to regenerated cellulose fiber / cotton blended fabric, and the outer layer fabric is obtained by padding, microwave pre-drying and heat setting. S4 Composite Process: The inner layer fabric, the middle layer fabric, and the outer layer fabric are stacked sequentially and bonded together using a dot-matrix hot melt bonding process to obtain the textile fabric with moisture-absorbing function.

[0013] Preferably, in step S2, the low-temperature plasma pretreatment is carried out in an argon / oxygen mixed atmosphere, with a plasma power of 100~200W and a treatment time of 30~120s; the chitosan-polyethylene glycol graft copolymer solution has a mass concentration of 3%~6%, an impregnation temperature of 40~55℃, an impregnation time of 30~60min, two dips and two rolls, a roll residue of 75%~85%, and then drying at 90~110℃ for 3~8min.

[0014] Preferably, in step S3, the sodium polyacrylate hygroscopic microcapsule dispersion is prepared by interfacial polymerization, specifically as follows: a 1%~3% (w / w) chitosan-acetic acid aqueous solution is used as the aqueous phase, and a sodium acrylate aqueous solution containing N,N'-methylenebisacrylamide crosslinking agent is used as the core material precursor. The two phases are mixed and emulsified in the oil phase. An ammonium persulfate initiator is added, and the reaction is carried out at 65~75℃ for 2~4 hours. The temperature is then lowered to 35~45℃, and glutaraldehyde crosslinking agent is added in an amount of 10%~20% of the chitosan mass. The cross-linking reaction is carried out for 1.5 to 2.5 hours to solidify the chitosan wall material. The pH is then adjusted to 6.5 to 7.0 to obtain a core-shell structured microcapsule dispersion with cross-linked chitosan as the wall material, cross-linked sodium polyacrylate as the core material, and a particle size of 15 to 35 μm. The mass concentration of the dispersion is 8% to 12%, and the roll-out rate during padding is 70% to 80%. After padding, the microcapsule is first pre-dried by microwave at a power of 800 to 1200 W for 30 to 90 seconds, and then heat-set at 110 to 130 °C for 2 to 5 minutes.

[0015] Preferably, in step S4, the bonding temperature of the point-like hot melt bonding process is 130~150℃, the bonding pressure is 0.3~0.5MPa, the bonding time is 5~15s, the spacing between bonding points is 3~6mm, the bonding points are arranged in a square or rhomboid array, and the amount of hot melt adhesive powder applied is 8~12g / m 2 The area of ​​the bonding points accounts for 8% to 15% of the total area of ​​the fabric.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: The inner layer of this invention is a hydrophobic, fast-conducting layer with a water contact angle of 95°~110°, woven from hydrophobic synthetic fibers with an irregular cross-section. It provides excellent hydrophobic and moisture-wicking properties on the side in contact with the skin, effectively preventing the reverse penetration of sweat from the outer layer of the fabric and avoiding sweat sticking to the skin. Simultaneously, the difference in water contact angle between the inner and outer layers is not less than [value missing]. This creates a stable and powerful moisture transport drive, allowing sweat on the skin surface to quickly detach from the skin and be transported to the outside of the fabric, fundamentally eliminating the problems of sweat backflow, dampness, and stuffiness against the skin, and significantly improving the dryness of the skin.

[0017] The intermediate layer of this invention uses W-shaped or Y-shaped modified polyester fibers with an axially extended microporous channel structure, which greatly improves the sweat wicking and retention capacity. The micropore size is controlled at 0.5~2μm and the porosity is 8%~15%, which can form continuous capillary moisture-wicking channels. This can quickly receive the sweat wicked from the inner layer and diffuse it laterally and conduct it quickly to the outer layer, greatly improving the moisture wicking rate. At the same time, the fiber surface is grafted with chitosan-polyethylene glycol graft copolymer with a grafting rate of 3%~6%, which not only gives the intermediate layer excellent and long-lasting hydrophilic moisture-wicking properties, but also effectively improves the defects of traditional fiber hydrophilic modification that is easy to fall off and has rapid performance degradation, and improves the fabric's wash resistance. At the same time, the chitosan groups can give the fabric certain antibacterial and moisturizing auxiliary functions, improving the overall quality of the fabric.

[0018] The outer layer of this invention adopts a hydrophilic structure of regenerated cellulose fiber and cotton blend, and is compounded with 15~35μm sodium polyacrylate moisture-absorbing microcapsules. The microcapsule content is 5%~10% of the dry weight of the outer layer. Combined with a low water contact angle design of 20°~35°, the outer layer of the fabric has a super strong active moisture absorption, moisture locking and rapid evaporation ability.

[0019] This invention employs a three-layer structure dot-matrix hot-melt bonding composite process. Compared with the traditional overall film bonding and sewing composite process, it not only ensures the stable composite effect of the three-layer structure, but also retains the excellent breathability and soft feel of the fabric. It avoids the problems of stiff fabric, poor breathability, and skin-friendliness caused by overall bonding, and balances structural stability and wearing comfort. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the three-layer composite structure of the textile fabric of the present invention; Figure 2 This is a top view of the dot-shaped hot melt adhesive array of the present invention; Figure 3 This is a cross-sectional view of the W / Y irregular shape of the intermediate layer of the present invention; Figure 4 This is a schematic diagram of the outer microcapsule of the present invention and the water droplet with a contact angle gradient. Detailed Implementation

[0021] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.

[0022] The present invention provides a textile fabric with moisture-absorbing function, such as... Figure 1As shown, the structure is composed of an inner layer, a middle layer, and an outer layer, sequentially stacked and bonded together with point-like hot-melt adhesive. The hydrophilicity increases from the inner layer to the outer layer, forming a water gradient transport structure. The inner layer is a hydrophobic fast-conducting layer with a water contact angle θ1 of 95°~110°; the middle layer is a hydrophilic core layer with an irregular cross-section, woven from modified polyester fibers with a W-shaped or Y-shaped cross-section, with a water contact angle θ2 of 60°~75°; the outer layer is a hydrophilic layer made of regenerated cellulose fiber / cotton blend, with a water contact angle θ3 of 20°~35°; the difference in water contact angle between the inner and outer layers is Δθ = θ1 - θ3 ≥ . Figure 1 The arrows in the diagram indicate the directional gradient transport of sweat from the inner layer, through the capillary moisture-wicking channels of the middle layer, towards the outer layer. The "grafting" described in this invention includes a loading method where chitosan-PEG copolymers are chemically bonded to the fiber surface via a covalent cross-linking network, encompassing the cross-linking fixation loading of pre-synthesized grafted copolymers.

[0023] like Figure 2 As shown, the inner, middle, and outer layers are bonded together by a regularly arranged array of dot-shaped hot-melt adhesive points. These adhesive points are arranged in a square or rhomboid array, with a spacing s of 3-6 mm. The area of ​​the adhesive points accounts for 8%-15% of the total fabric area. Compared to traditional integral lamination bonding, the dot-array bonding ensures a stable three-layer structure while retaining large ventilation channels between the adhesive points, thus balancing structural stability, breathability, and a soft, skin-friendly feel.

[0024] like Figure 3 As shown, the modified polyester fiber in the middle layer has a W-shaped or Y-shaped cross-section, and the fiber interior has axially extending microporous channels with a pore size d of 0.5~2μm and a micropore porosity ε of 8%~15%. The fiber surface is uniformly grafted with chitosan-polyethylene glycol graft copolymer with a grafting rate G of 3%~6%. The synergistic effect of the W / Y shaped cross-section and the axial micropores forms a three-dimensional capillary moisture-wicking channel with a high specific surface area.

[0025] Pre-synthesis of chitosan-polyethylene glycol graft copolymer (carbodiimide coupling method): Chitosan with a degree of deacetylation of 85%–95% was dissolved in a 2%–4% (v / v) dilute acetic acid aqueous solution at a chitosan to polyethylene glycol mass ratio of 1:1 to prepare a 1.5%–3% (w / w) chitosan-acetic acid solution; an equal mass of terminally carboxyl-terminated monocarboxyl polyethylene glycol (number average molecular weight 2000–6000) was added and stirred until homogeneous; EDC·HCl (the amount added was equal to the molar amount of PEG-COOH) was then added. Use 1.2~1.5 times) and NHS (1.0~1.2 times the molar amount of PEG-COOH) as coupling agents, adjust the pH to 5.0~6.0, and react at 40~50℃ in the dark for 3~5h; after the reaction, precipitate with cold ethanol (4℃), filter, wash 3 times with deionized water to remove residual coupling agent, dissolve the purified chitosan-PEG graft copolymer in dilute acetic acid aqueous solution to prepare graft copolymer impregnation solution with pH=5.0~6.0 and mass concentration of 3%~6%; Impregnation loading: Citric acid (5%~10% of the chitosan-PEG graft copolymer mass) is added as a crosslinking agent to the above-mentioned graft copolymer impregnation solution and stirred until completely dissolved; modified polyester fibers with W-shaped or Y-shaped cross sections, containing axially extended microporous channels and pretreated by low-temperature plasma are placed in the above-mentioned impregnation solution and impregnated at 40~55℃ for 30~60 min, followed by two dips and two nips, with a roll-off rate of 75%~85%, then dried at 90~110℃ for 3~8 min to remove moisture, and then baked at 150~160℃ for 2~4 min for curing. In the carbodiimide coupling reaction, EDC activates the carboxyl group at the end of PEG-COOH to form an O-acylisourea active intermediate. This intermediate is converted into a stable NHS ester active intermediate in the presence of NHS, and then reacts with the primary amino group (-NH2) on the chitosan molecular chain. Nucleophilic substitution reaction is carried out to form amide bonds (—CO—NH—) covalently linked to pre-synthesize chitosan-PEG graft copolymer. During impregnation and drying, the residual amino groups on the chitosan chain segments and the active groups such as carboxyl groups (—COOH) and hydroxyl groups (—OH) generated by low-temperature plasma activation on the surface of polyester fibers first form hydrogen bonds and electrostatic adsorption, achieving initial loading. In the baking and curing stage, the three carboxyl groups of citric acid undergo amidation reaction with the primary amino groups (—NH2) on the chitosan molecular chain and esterification reaction with the hydroxyl groups (—OH) on the surface of polyester fibers under high temperature drive, forming a three-dimensional covalent cross-linked network with citric acid as the bridging center. This allows the chitosan-PEG graft copolymer to be firmly bound to the fiber surface and the inner wall of the microporous channel through a composite loading mechanism of "hydrogen bond adsorption + citric acid cross-linking covalent bonding", achieving a grafting rate of 3%~6%. Set up grafted modified fiber test samples and blank control samples of the same batch of ungrafted fibrils. The mass of each sample is 1.0000~2.0000g, and there are no less than 3 sets of parallel samples.

[0026] The grafted fiber samples were subjected to Soxhlet reflux extraction with a mixed solvent of ethanol / water (volume ratio 1:1) for 6-8 hours to remove the physically adsorbed free copolymers. After extraction, the samples were thoroughly washed with deionized water until the washing solution was neutral, and then vacuum dried at 60°C to constant weight. The difference between two consecutive weighings was no more than 0.0002 g.

[0027] like Figure 4 As shown, the outer layer is composed of a blend of regenerated cellulose fibers (one or more of Lyocell fibers, Modal fibers, or bamboo pulp fibers) and cotton, with a blending mass ratio of 4:6 to 6:4. The outer layer contains uniformly composited sodium polyacrylate moisture-absorbing microcapsules with a particle size of 15-35 μm. The microcapsules use cross-linked chitosan as the wall material and cross-linked sodium polyacrylate as the core material, forming a "core-shell" structure. The microcapsule content is 5% to 10% of the dry weight of the outer layer. After sweat reaches the outer layer, it is first rapidly spread through the continuous capillary network of the regenerated cellulose fiber / cotton blended yarn, and then actively adsorbed and locked by the sodium polyacrylate core. The typical gradient of contact angles θ1=102°, θ2=67°, and θ3=27° (Δθ=75°≥60°) provides a continuous chemical potential driving force for the unidirectional transport of sweat from the inside to the outside.

[0028] Main raw materials and equipment raw material Inner layer hydrophobic synthetic fiber: cross-shaped cross-section polypropylene fiber (PP, 1.4dtex×38mm) or cross-shaped cross-section polyester fiber (PET, 1.5dtex×38mm), from a chemical fiber company in Jiangsu Province; Intermediate layer profiled polyester fiber: W-shaped or Y-shaped profiled polyester fiber (PET, 1.2~2.5dtex), profile degree 0.35~0.55, with axially extending microporous channels inside, micropore diameter 0.5~2μm, micropore porosity 8%~15%, customized by a functional fiber company in Jiangsu. The intermediate layer profiled polyester fiber is prepared by blend spinning-stretching and setting-porogen dissolution method, and the final porosity is precisely controlled by adjusting the stretching ratio and dissolution process parameters. Typical parameter combinations and corresponding measured porosity results are shown in Table 1.

[0029] Table 1 Table 1 shows that for every 0.3-fold increase in the stretching ratio, the porosity decreases by approximately 1-2 percentage points (due to the highly oriented and refined micro-regions of the island phase, some micropores become closed or semi-closed after dissolution); for every 10°C increase in the setting temperature, the porosity decreases by approximately 0.5-1 percentage points (due to the increased densification of the marine matrix, leading to an increase in micropore closure rate); when the dissolution time is less than 50 minutes, dissolution is insufficient and the porosity is low, while extending it to more than 65 minutes does not significantly improve the porosity. The preferred parameter combination for this invention is a stretching ratio of 2.0-2.5 times, a setting temperature of 160-180°C, and a dissolution time of 55-65 minutes, corresponding to an open-pore porosity of 8%-15%.

[0030] Types and proportions of pore-forming agents Pore-forming system: conventional PET (marine phase, continuous phase) + water-soluble modified polyester (island phase, dispersed phase); Pore-forming agent: Boiling water soluble modified polyester (intrinsic viscosity 0.65~0.75 dL / g, melting point 220~230℃); Mass ratio: Conventional PET : Water-soluble modified polyester = 60~70 : 30~40; The process involves slicing and drying, melt blending and spinning, stretching and setting, followed by micropore dissolution. The theoretical porosity of the water-soluble modified polyester island phase after subsequent boiling water dissolution is close to its mass percentage (30%~40%). However, due to the high stretching ratio during melt spinning, the island phase micro-regions are highly oriented and elongated. Furthermore, stretching and setting further densifies the PET island phase matrix, causing some micropores to remain closed or semi-closed after dissolution. The actual open porosity is lower than the theoretical value. By adjusting process parameters such as stretching ratio, setting temperature, and dissolution time, the final open porosity is precisely controlled at 8%~15%.

[0031] The leaching medium was deionized water (boiling water); the bath ratio was 1:15~1:20 (fiber:water); the temperature was 95~100℃; the time was 55~65min; the post-treatment involved thorough washing with deionized water until neutral, followed by vacuum drying at 60℃ to constant weight. The final modified polyester fiber had a micropore porosity of 8%~15%.

[0032] Melt spinning process: The screw temperature is set as follows: feeding section 265~275℃, compression section 275~285℃, metering section 280~290℃; spinning box temperature 278~288℃; the spinneret adopts W-shaped or Y-shaped irregular cross-section spinnerets (matching the cross-sectional shape of the target fiber). The W-shaped spinneret consists of 4 slits arranged symmetrically in a central direction, with an angle of 90° between adjacent slits; the Y-shaped spinneret consists of 3 slits arranged symmetrically in a central direction, with an angle of 120° between adjacent slits; the width of a single slit is 0.08~0.15mm, the slit length is 0.6~1.2mm, the slit length-to-width ratio is 6~10:1, the total number of spinnerets is 200~400, and the length-to-diameter ratio is 3~5:1; the melt pressure is 1.5~3.0MPa; the side blowing temperature is 20~30℃, and the air velocity is 0.3~0.8m / s; The melt extrusion rate is 8~15 g / (min·hole), the side blowing angle is 15°~30° with the fiber bundle (to ensure uniform cooling of each arm of the irregular cross-section and avoid cross-section deformation), and the winding speed is 800~1500 m / min, to obtain PET / water-soluble modified polyester island-type nascent fiber; the irregularity is controlled by adjusting the ratio of melt extrusion rate to winding speed. When the extrusion rate decreases, the residence time of the melt in the spinneret is extended and the mold is filled more fully, thus improving the irregularity; when the winding speed increases, the axial stretch ratio of the melt after the fine flow out of the hole increases, the edges of the irregular cross-section are easily rounded, and the irregularity tends to decrease; when the winding speed is 1000 m / min and the extrusion rate is 10 g / (min·hole), the fiber irregularity is about 0.42 (W-shaped), which is in the range of 0.35~0.55.

[0033] Stretching and setting process: A two-step stretching + heat setting process is adopted; the first stretching ratio is 1.8~2.5 times, and the first stretching temperature is 75~85℃; the second stretching ratio is 2.0~3.0 times, and the second stretching temperature is 100~120℃; the heat setting temperature is 160~190℃, and the setting time is 10~30s. High stretching ratio causes the island phase microregions to be highly oriented and elongated along the fiber axis, forming a quasi-one-dimensional nanochannel precursor; the higher the stretching ratio, the finer the cross-section of the island phase microregions, and the smaller and more uniform the micropore size and distribution after dissolution; if the setting temperature is too high, the marine matrix will be over-densified, resulting in an increased micropore closure rate; if the setting temperature is too low, the internal stress of the fiber will not be fully eliminated, and the micropores will easily collapse and deform during the subsequent dissolution process.

[0034] Table 2 shows a customized project of a functional fiber company in Jiangsu.

[0035] Table 2 Chitosan: Degree of deacetylation 85%~95%, viscosity-average molecular weight 5.0×10⁻⁶ 5 A biotechnology company in Shandong; Polyethylene glycol (PEG): Number average molecular weight M n=2000~6000 (PEG-2000, PEG-4000, PEG-6000), Aladdin reagent; Sodium acrylate: CP grade, content ≥98%, Sinopharm Group; N,N'-Methylenebisacrylamide (MBA): Crosslinking agent, CP grade, Sinopharm Group; Ammonium persulfate (APS): Initiator, AR grade, Sinopharm Group; Glacial acetic acid, sodium hydroxide, Span 80, and liquid paraffin: all AR grade, produced by Sinopharm Group; Waterborne polyurethane (WPU) adhesive: Aliphatic waterborne polyurethane dispersion, solid content 40%, particle size ≤0.5μm, pH 6.5~8.0, used for microcapsule immobilization; Outer layer regenerated cellulose fibers: Lyocell fiber (1.33dtex×38mm), Modal fiber (1.3dtex×38mm), bamboo pulp fiber (1.5dtex×38mm), from a new materials company in Jiangsu Province; Cotton fiber: Xinjiang long-staple cotton, fiber length 31mm; Hot melt adhesive powder: Copolyamide (Co-PA) hot melt adhesive powder or copolyester (Co-PES) hot melt adhesive powder, melting point 120~140℃, particle size 80~200μm, from a German adhesive company.

[0036] equipment Low-temperature plasma processing equipment: Radio frequency capacitively coupled plasma (RF-CCP) reactor, radio frequency power 0~500W, gas path: argon, oxygen; Dipping and rolling mill: Small sample two-dipping and two-rolling mill; Interfacial polymerization reactor: 5L three-port reactor with stirring, temperature control, and pH meter; Homogenizer: Speed ​​0~15000 r / min; Microwave pre-drying equipment: power 0~2000W, industrial microwave tunnel oven; Dot-shaped hot melt adhesive machine: Powder dot transfer coating adhesive machine, with formula / diamond array coating roller, screen mesh number 40~100 mesh, working width 1600mm; One-way moisture conduction tester: MMT moisture management tester (AATCC 195 / GB / T 21655.2-2019); Contact angle measuring instrument: JC2000D contact angle measuring instrument, 5μL deionized water droplet; Electronic balance, textile washing color fastness tester (GB / T 8629-2017 4N program), scanning electron microscope (SEM), Fourier transform infrared spectrometer (FTIR), etc.

[0037] Performance testing methods Water contact angle: According to FZ / T 01102-2015 "Determination of contact angle of textiles - water droplet method", 5μL deionized water droplet, test at room temperature; take the initial contact angles θ1, θ2, θ3 of the inner layer, middle layer and outer layer; 60-minute moisture absorption rate: Referring to the moisture absorption rate test principle in GB / T 21655.1-2008 "Evaluation of moisture absorption and quick-drying properties of textiles - Part 1: Single-item combination test method", the moisture absorption rate was measured under the following conditions: first, the sample was equilibrated at (20±2)℃ and (65±3)%RH for 24 hours and weighed m0; then, it was exposed at (25±1)℃ and (90±2)%RH for 60 minutes and weighed m60. Moisture absorption rate = (m60-m0) / m0×100%; Water diffusion time: According to GB / T 21655.1-2008, 5μL of water is dropped onto the inner layer of the body, and a stopwatch is used to record the time required for the water droplet to completely penetrate. One-way Transport Index (OWT): The One-way Transport Index of fabrics is tested using an MMT moisture management tester according to GB / T 21655.2-2019. Washing durability: Perform 30 standard washes according to GB / T 8629-2017 4N procedure (40℃, phosphate-free detergent, hanging to dry is considered one cycle). Measure OWT before and after washing, and calculate OWT retention rate = OWT 30 / OWT0×100%; Air permeability: according to GB / T 5453-1997, pressure difference 200Pa; Moisture permeability: According to GB / T 12704.2-2009, inverted cup method, (38±1)℃, (50±2)%RH; Fiber cross-section and micropore channels: SEM was used to observe the W / Y profile of the intermediate layer fiber, the internal micropore channels, and the distribution and particle size of the outer layer microcapsules; Fourier transform infrared spectroscopy (FTIR) was used to compare and characterize the original polyester fiber, pure chitosan, pure PEG, and modified grafted fiber. By observing the shift of characteristic absorption peaks, the formation of covalent grafted chemical bonds between chitosan and PEG, the formation of covalent grafted chemical bonds between chitosan and PEG was verified, proving that the graft copolymer was successfully loaded onto the surface of the polyester fiber and clarifying the changes in chemical structure after modification.

[0038] Grafting rate: Grafting rate test: calculated as (m1-m0) / m0×100%, where m0 is the oven-dry weight of the same batch of fibers after plasma pretreatment and purification by Soxhlet extraction, and m1 is the oven-dry weight of the modified fibers after impregnation and drying and purification by Soxhlet extraction; Soxhlet extraction conditions: using a mixed solvent of ethanol / water (volume ratio 1:1), reflux extraction for 6-8 hours, followed by thorough washing with deionized water until the washing solution is neutral, and vacuum drying at 60℃ to constant weight. FTIR characteristic peak (3400 cm⁻¹) -1 A broad peak of —NH2 / —OH at 1650 cm⁻¹ -1 Amide I band, 1100cm -1 The PEG ether bond peak is used as a qualitative confirmation of successful grafting and is not included in the quantitative calculation of grafting rate. Microcapsule particle size: measured using a laser particle size analyzer (Malvern Mastersizer 3000) D 50 .

[0039] Example 1 (W-shaped irregular cross section + PEG-4000) S1 Inner Layer Preparation The yarn is made from cross-shaped polypropylene fiber (1.4 dtex × 38 mm), processed through cleaning, carding, drawing, roving, and spinning to produce 14.6 tex pure PP yarn. It is woven on a plain weave with a warp / weft density of 280 / 220 (ends / 10 cm), resulting in a weight of 50 g / m². 2 The inner layer of the fabric. The water contact angle of this inner layer was tested to be θ1 = 102°, which falls within the range of 95° to 110° (corresponding to...). Figure 1 , Figure 4 (Note θ1 in the middle).

[0040] Preparation of S2 intermediate layer modified fiber Low-temperature plasma pretreatment: W-shaped polyester fibers (1.65 dtex, irregularity 0.42, micropore diameter d=1.2 μm, micropore porosity ε=12%) were placed in a radio frequency capacitively coupled plasma (RF-CCP) reactor and a mixed gas with a volume ratio of Ar:O2=8:2 was introduced. The gas flow rate was 30 sccm, the working pressure was 20 Pa, the radio frequency power was 150 W, and the pretreatment time was 90 s to obtain surface-activated W-shaped polyester fibers. Preparation of chitosan-polyethylene glycol graft copolymer impregnation solution (pre-synthesis via carbodiimide coupling method): Chitosan with a degree of deacetylation of 92% was dissolved in a 1.5% (w / w) aqueous acetic acid solution to obtain a 4% (w / w) chitosan-acetic acid solution; an equal mass of PEG-4000 (carboxyl-terminated monocarboxyl PEG-COOH, Mn=4000) was added and stirred until homogeneous; EDC·HCl (1.3 times the molar amount of PEG-COOH) and NHS (equal to the molar amount of PEG-COOH) were added. Using 1.1 times the molar amount of H as a coupling agent, the pH was adjusted to 5.5, and the reaction was carried out at 45°C in the dark for 4 hours. After the reaction, the mixture was precipitated with cold ethanol (4°C), filtered, and washed three times with deionized water to remove residual coupling agent. The purified chitosan-PEG graft copolymer was then dissolved in dilute acetic acid aqueous solution to prepare a graft copolymer impregnation solution with pH=5.5 and a mass concentration of 5%. Citric acid was added to the above impregnation solution as a crosslinking agent (the amount used was 8% of the mass of chitosan-PEG graft copolymer), and stirred until completely dissolved. Impregnation-Pan-Drying: The fibers obtained from S2 were impregnated in the solution at 45℃ for 45 min, followed by two impregnations and two pans, with a padding rate of 80% (based on the oven-dry weight of the fibers). They were then dried at 100℃ for 5 min to remove moisture, and subsequently baked at 155℃ for 3 min to cure, allowing citric acid to form a covalently cross-linked network with the chitosan amino groups and the hydroxyl groups on the fiber surface. The grafting rate was measured to be G=3.2% by weighing. Grafting reaction mechanism: In the carbodiimide coupling reaction, EDC activates the carboxyl group at the end of PEG-COOH to form an O-acyl isourea active intermediate. This intermediate is converted into a stable NHS ester active intermediate in the presence of NHS, and then undergoes a nucleophilic substitution reaction with the primary amino group (—NH2) on the chitosan molecular chain to form an amide bond (—CO—NH—) covalently linked, thereby obtaining the chitosan-PEG graft copolymer. During the impregnation and drying process, the residual amino group on the chitosan chain and the active groups such as carboxyl groups (—COOH) and hydroxyl groups (—OH) generated on the surface of the polyester fiber by low-temperature plasma activation first form hydrogen bonds and electrostatic adsorption, achieving initial loading. Subsequently, in the baking and curing stage at 150~160℃, citric acid added to the impregnation solution (at an amount of 8% of the mass of the chitosan-PEG graft copolymer) acts as a preservative. The multi-carboxyl crosslinking agent, under high temperature driving, undergoes amidation reaction with the primary amino group (-NH2) on the chitosan molecular chain and esterification reaction with the hydroxyl group (-OH) on the polyester fiber surface, forming a three-dimensional covalent crosslinking network with citric acid as the bridging center. This allows the chitosan-PEG graft copolymer to be firmly bound to the fiber surface and the inner wall of the microporous channel through a composite loading mechanism of "hydrogen bond adsorption + citric acid crosslinking covalent bonding", rather than simple physical adsorption. In this composite loading mechanism, hydrogen bonding provides initial adsorption positioning, while citric acid crosslinking covalent bonding provides long-term water wash resistance stability. The two work together to ensure that the grafted material is not easily detached after repeated washing. The grafting rate is precisely controlled within the range of 3% to 6% by adjusting the plasma activation power, processing time, impregnation solution concentration, and citric acid dosage. In this example, the measured grafting rate G=3.2%. Grafting rate: calculated as (m1-m0) / m0×100%, where m0 is the oven-dry weight of the same batch of fibers after plasma pretreatment and purification by Soxhlet extraction, and m1 is the oven-dry weight of the modified fibers after impregnation and drying and purification by Soxhlet extraction. The Soxhlet extraction conditions are: using a mixed solvent of ethanol / water (volume ratio 1:1), reflux extraction for 6-8 hours, followed by thorough washing with deionized water until the washing liquid is neutral, and vacuum drying at 60℃ to constant weight (the difference between two adjacent weighings should not exceed 0.0002g). The test standard is uniformly "the calculated dry weight after Soxhlet extraction purification", that is, only the mass of the grafted copolymer with covalent bonding and strong chemical adsorption is included, while the mass of the free copolymer with physical adsorption is excluded, to ensure the accuracy and repeatability of the grafting rate value.

[0041] Spinning and weaving: The modified W-shaped profiled polyester fiber is processed into 19.7 tex yarn through cleaning, carding, drawing, roving, and spinning. It is then woven using a double-sided weft knitting structure to achieve a weight of 100 g / m². 2 The intermediate layer fabric; the water contact angle of this intermediate layer was tested to be θ2=67°, which is within the range of 60°~75° (corresponding to...). Figure 1 , Figure 4 (θ2 annotation in the middle) SEM observation revealed that the cross-section of the intermediate fiber exhibited a complete W-shaped four-lobed profile, and micropores with a diameter of approximately 1.2 μm could be clearly observed along the axial direction within the fiber (corresponding to...). Figure 3 The W-shaped microporous structure shown); 3400 cm⁻¹ in FTIR. -1 A broad peak of —NH2 / —OH at 1650 cm⁻¹ -1 Amide I band and 1100cm -1 The characteristic ether bond peaks of PEG were all clearly observed, confirming that the chitosan-PEG graft copolymer had been successfully grafted onto the surface of the polyester fiber.

[0042] S3 outer layer preparation Preparation of chitosan-sodium polyacrylate core-shell microcapsule dispersion (interfacial polymerization method): 100 mL of a 2% (w / w) chitosan-acetic acid aqueous solution (containing 2.0 g chitosan) was used as the aqueous phase. 20 g sodium acrylate and 0.6 g N,N'-methylenebisacrylamide (MBA) were dissolved in 80 mL of deionized water to prepare an aqueous solution for the core material precursor. The two aqueous phases were combined and stirred (the total volume of the combined aqueous phase was approximately 180 mL). The solution was then added dropwise to the liquid paraffin oil phase at a constant temperature of 25-30 °C. The mass concentration of Span 80 in the oil phase was 2% of the oil phase weight (i.e., 2.0 g Span 80 per 100 mL of liquid paraffin). The volume ratio of the aqueous phase to the oil phase was 1:3 (180 mL aqueous phase : 540 mL oil phase). The mixture was homogenized and emulsified at 10000 r / min for 5 min (homogenization temperature controlled at 25-30 °C) to obtain a W / O emulsion. The mixture was transferred to a three-necked reactor, protected with nitrogen, and 0.2 g of ammonium persulfate (APS) was added as an initiator. The reaction was carried out at 70°C for 3 hours. After the reaction, the pH of the emulsion was adjusted to 5.5–6.0 with acetic acid. A glutaraldehyde crosslinking agent solution (25% by mass, 12%–18% of the chitosan mass) was slowly added dropwise, and the reaction was carried out at 40°C for 2 hours to ensure the chitosan wall material was fully crosslinked and cured. Insufficient glutaraldehyde would result in insufficient chitosan crosslinking, leading to partial dissolution and loss of the wall material during subsequent demulsification and washing. Excessive glutaraldehyde would cause over-crosslinking and brittleness of the wall material, affecting the flexibility and abrasion resistance of the microcapsules after application. After crosslinking, the pH was adjusted to 6.8, followed by demulsification, centrifugation, and washing. The product was then redispersed in deionized water to obtain a core-shell structured microcapsule dispersion with a chitosan-glutaraldehyde crosslinked network as the wall material and crosslinked sodium polyacrylate as the core material. Figure 4(Schematic diagram of microcapsule structure); The cross-linking and curing mechanism of chitosan wall material is as follows: the primary amino group (-NH2) on the chitosan molecular chain reacts with the aldehyde group (-CHO) of glutaraldehyde to form a Schiff base reaction, resulting in a -N=CH- covalent bond. This forms a stable three-dimensional cross-linked network between the chitosan molecular chains, thereby firmly encapsulating the sodium polyacrylate core material inside the cross-linked chitosan wall material, giving the microcapsules a water-washable and abrasion-resistant structural stability; the D of the microcapsules was measured by a laser particle size analyzer. 50 =22μm, located in the 15~35μm range; it is prepared into an application solution with a mass concentration of 10%; Impregnation-microwave pre-drying-heat setting: The obtained 10% microcapsule dispersion was mixed with waterborne polyurethane (WPU) adhesive at a mass ratio of 100:4 (WPU solid content 40%, the effective concentration of WPU in the application solution after addition is about 1.5%), and stirred evenly to prepare a composite application solution; Lyocell fiber / cotton blended fabric (Lyocell:cotton = 5:5, 14.6 tex, plain weave, weight 75 g / m2) was immersed in the composite application solution, dipped and rubbed twice, with a roll-off rate of 75% (based on the dry weight of the fabric), then microwave pre-dried at 1000W for 60s, and finally heat-set at 120℃ for 3min. During the heat setting process, WPU crosslinks at the fiber surface and microcapsule interface to form a flexible polyurethane film with a thickness of approximately 0.5~2μm. This film mechanically encapsulates and anchors the microcapsules to the fiber surface and interfiber spaces. Simultaneously, the residual amino groups of the crosslinked chitosan wall material and the hydroxyl groups on the surface of the regenerated cellulose fibers form hydrogen bonds at 120℃, constructing a dual fixation system of "WPU film-forming mechanical anchoring + crosslinked chitosan wall material hydrogen bond synergy". The gravimetric method determined that the microcapsule content in the outer layer was 8% of the dry weight of the outer layer. The water contact angle θ3 of this outer layer was measured to be 27°, falling within the 20°~35° range (corresponding to...). Figure 1 , Figure 4 (Note: θ3 in the text).

[0043] S4 Composite Process The inner, middle, and outer fabric layers obtained from S1, S2, and S3 are stacked sequentially from the skin-facing side outwards and fed into a powder-dot transfer coating type dot hot melt adhesive machine in a square array with a dot spacing s=4mm and a dot diameter of 1.4mm. Co-PA hot melt adhesive powder with a melting point of 130℃ is used, applied at a rate of 10g / m². 2 The bonding temperature was 140℃, the bonding pressure was 0.4MPa, and the bonding time was 10s; the area of ​​the bonding points accounted for approximately 9.6% of the total fabric area, falling within the range of 8% to 15% (corresponding to...). Figure 2 The adhesive array shown.

[0044] Performance testing: The difference in contact angle between the inside and outside of the body is Δθ = θ1 - θ3 = 102° - 27° = 75° ≥ 60°; 60-minute moisture absorption rate: 38% (≥32%); Water diffusion time: 1.8s (≤3s); Initial unidirectional transmission index OWT0 = 462% (≥400%); OWT after 30 washes 30 =393%, retention rate OWT 30 / OWT0=85% (≥80%) Breathability: 320mm / s; Moisture permeability: 12800g / (m 2 ·24h); Graft retention rate after washing: The intermediate layer fabric of Example 1 was washed 30 times according to the GB / T 8629-2017 4N procedure. The grafting rate was tested by weighing method (based on dry weight after Soxhlet extraction purification). After washing, the grafting rate G30=2.8%, and the graft retention rate G30 / G0=2.8% / 3.2%=87.5%. This shows that after citric acid crosslinking and curing, the graft copolymer still maintains a retention rate of 87.5% after repeated washing, which corresponds to the OWT retention rate of 85%. This proves that the covalent crosslinking network effectively improves the wash fastness of the graft. Microcapsule mass retention rate: After 30 washes, SEM observation showed that the microcapsules were still evenly distributed on the surface and in the gaps of the outer fiber layer, and no large-area detachment was observed; the microcapsule mass retention rate measured by the weight difference method was 82%, which corresponds to the OWT retention rate of 85%, proving that the WPU film-forming and fixation system effectively ensures the water wash fastness of the microcapsules.

[0045] Example 2 (Y-shaped cross-section + PEG-6000) S1 Inner Layer Preparation The yarn is made of cross-section polyester (1.5 dtex × 38 mm), processed through carding, drawing, roving, and spinning to produce 14.6 tex PET yarn. It is then woven on a plain weave machine to a weight of 55 g / m². 2 The inner layer of the fabric. The water contact angle of the inner layer was tested and found to be θ1 = 108°, which is within the range of 95° to 110°.

[0046] Preparation of S2 intermediate layer modified fiber Plasma pretreatment: Y-shaped cross-section polyester fiber (1.85dtex, irregularity 0.50, micropore diameter d=0.8μm, micropore porosity ε=10%), Ar:O2=7:3, working pressure 15Pa, power 180W, treatment time 60s; Solution preparation (pre-synthesis via carbodiimide coupling method): Chitosan with a degree of deacetylation of 88% was dissolved in a 2% (w / w) aqueous acetic acid solution to prepare a 3.5% (w / w) chitosan-acetic acid solution; an equal mass of PEG-6000 (carboxyl-terminated monocarboxyl PEG-COOH, M...) was added. n =6000), stir evenly; add EDC·HCl (1.3 times the molar amount of PEG-COOH) and NHS (1.1 times the molar amount of PEG-COOH) as coupling agents, adjust the pH to 5.5, and react at 45℃ in the dark for 4h; after the reaction, precipitate with cold ethanol (4℃), filter, wash 3 times with deionized water to remove residual coupling agent, dissolve the purified chitosan-PEG graft copolymer in dilute acetic acid aqueous solution to prepare a graft copolymer impregnation solution with pH=5.5 and mass concentration of 6%; Impregnation-Pan-Drying: Citric acid (6% of the chitosan-PEG graft copolymer mass) was added to the graft copolymer impregnation solution and stirred to dissolve. The fibers were impregnated at 50℃ for 60 min, followed by two impregnations and two pans, with a padding rate of 78% (based on the oven-dry weight of the pretreated fibers). The fibers were first dried at 105℃ for 6 min to remove moisture, and then baked at 155℃ for 3 min to cure. The modified fibers after impregnation and drying were then refluxed in a Soxhlet extractor for 6-8 h to remove the physically adsorbed free chitosan-PEG copolymer. After extraction, the fibers were thoroughly washed with deionized water until the washing solution was neutral, and then vacuum dried at 60℃ to constant weight. Based on the dry weight after Soxhlet extraction purification, the grafting rate G was calculated to be 3.8% by weighing. Spinning and weaving: Produced into 19.7 tex yarn, double-sided weft knitted, weight 110 g / m² 2 The intermediate layer of the fabric was tested; the water contact angle of the intermediate layer was θ2=70°, which is within the range of 60°~75°.

[0047] S3 outer layer preparation Microcapsule preparation (interfacial polymerization method, same principle as in Example 1): The concentration of chitosan aqueous phase was adjusted to 2.5%, the concentration of sodium acrylate core material precursor was increased to 22% (w / w), the amount of MBA was 3% of the mass of the core material precursor, the emulsification speed was 12000 r / min, the reaction temperature was 72℃, and the reaction time was 3.5 h, finally obtaining D 50 Core-shell microcapsules with a diameter of 28 μm were prepared into an application solution with a mass concentration of 12%. Core-shell structure formation mechanism: In the W / O emulsion system, chitosan molecular chains simultaneously contain hydrophilic amino (-NH2) and hydroxyl (-OH) groups as well as hydrophobic N-acetyl groups, exhibiting amphiphilic characteristics. During emulsification, they spontaneously migrate and accumulate at the water-oil interface, reducing interfacial tension. Simultaneously, sodium acrylate and MBA crosslinking agent dissolve inside the water droplet, serving as core material precursors. The reaction consists of two stages: In the first stage, APS initiates the polymerization of sodium acrylate at 70℃, forming a crosslinked sodium acrylate polymer network (core material) inside the water droplet. In the second stage, after cooling to 40℃, glutaraldehyde is added. Glutaraldehyde undergoes a Schiff base crosslinking reaction with the chitosan molecules enriched in the interfacial region, forming a chitosan-glutaraldehyde crosslinked network wall material on the outer layer of the water droplet. Because the two stages of the reaction are spatially separated—polymerization occurs within the water droplet itself, while crosslinking is concentrated in the interfacial region—a core-shell structure is formed with sodium acrylate as the core and crosslinked chitosan as the wall.

[0048] Outer fabric: Lyocell:Modal:Cotton blended yarn = 2:2:6 (by weight), 14.6 tex, plain weave, 80 g / m² 2 ; Patch-microwave pre-baking-heat setting: The obtained 12% microcapsule dispersion was mixed with waterborne polyurethane (WPU) adhesive at a mass ratio of 100:3 (WPU solid content 40%, effective WPU concentration in the application solution after addition is approximately 1.2%), and stirred evenly; the roll-off rate was 72% (based on the absolute dry weight of the fiber), microwave pre-baking was performed at 1200W for 45s, and heat setting was carried out at 125℃ for 4min. During the heat setting process, WPU crosslinked to form a film that fixed the microcapsules. The microcapsules accounted for 9% of the dry weight of the outer layer by weighing; the water contact angle θ3 of the outer layer was tested to be 25°, which is within the range of 20°~35°.

[0049] S4 Composite Process A diamond-shaped array was used, with a bonding point spacing of s=5mm and a bonding point diameter of 1.9mm. Co-PES hot melt adhesive powder with a melting point of 135℃ was applied at a rate of 11g / m². 2 The bonding temperature was 145℃, the pressure was 0.45MPa, and the time was 12s; the area of ​​the bonding points accounted for η≈11.4%.

[0050] Performance testing: The difference in contact angle between the inside and outside of the body is Δθ = 108° - 25° = 83° ≥ 60°; 60-minute moisture absorption rate: 41%; Water droplet diffusion time: 1.5s; OWT0=485%; After 30 washes, OWT30 = 399%, retention rate 82%; Breathability: 305mm / s; Moisture permeability: 13200g / (m2 •24h).

[0051] Comparative Example 1 It adopts a three-layer nonwoven needle-punching composite process, with the inner layer being ordinary circular cross-section polyester needle-punched nonwoven fabric (50g / m²). 2 (No hydrophobic finishing applied), the middle layer is ordinary circular cross-section polyester needle-punched nonwoven fabric (100g / m²). 2 Ungrafted chitosan-PEG), outer layer is Lyocell / cotton needle-punched nonwoven fabric (80g / m²). 2 (The three layers are composited by an integral needle punching process, without point-like hot melt bonding, chemical modification or microcapsules are introduced, and the effect of "contact angle decreasing sequentially" is only formed by the fiber thickness gradient (Δθ is not quantified).

[0052] Performance testing: θ1=88°, θ3=45°, Δθ=43° (<60°); 60min moisture absorption rate=25%; OWT0=320%, OWT after 30 washes 30 =176%, OWT retention rate =55% (<80%).

[0053] Conclusion: Due to the lack of W / Y irregular shape + microporous channels, lack of chitosan-PEG graft modification, lack of core-shell microcapsules, and Δθ below 60°, the gradient driving force is insufficient, resulting in significantly lower moisture conduction rate and moisture absorption rate than the present invention, and poor washability.

[0054] Comparative Example 2 Chitosan-PEG-1500 graft copolymer was directly applied to ordinary circular cross-section polyester knitted fabric (single-layer structure, basis weight 220g / m²). 2 ), and sodium polyacrylate powder (non-core-shell microcapsules, D) prepared by reverse suspension polymerization. 50 (≈50μm) is sprayed with adhesive onto the same layer of fabric surface, without a gradient layer, and without distinguishing between inside and outside.

[0055] Performance testing: Single-sided measurement θ=55°; 60-minute moisture absorption rate = 48% (large total moisture absorption but bidirectional permeation); OWT0 = 180% (<400%, not unidirectional moisture conduction); microcapsule powder detachment occurred after 10 washes, and OWT0 decreased after 30 washes. 30 =71%, retention rate ≈39%.

[0056] Comparative Example 2 used sodium polyacrylate powder directly sprayed onto the fabric surface, without employing a core-shell microcapsule structure or a water-based polyurethane film-forming fixation system and a cross-linked chitosan wall material hydrogen bond synergistic fixation mechanism. Functional loading was achieved solely through physical adhesion. While this method could achieve some moisture absorption in the initial stage, the lack of chemical bonding, film coating, and wall material hydrogen bond between the functional particles and the fiber interface resulted in extremely weak interfacial adhesion. Under washing and friction, particle aggregation and significant detachment occurred, with noticeable detachment appearing after 10 washes. After 30 washes, the microcapsule mass retention rate was only about 15%, ultimately leading to a rapid decline in moisture management performance. In contrast, Example 1 of this invention employed a dual fixation system of "WPU film-forming mechanical anchoring + cross-linked chitosan wall material hydrogen bond synergy," achieving a microcapsule mass retention rate of 82% after 30 washes, fully demonstrating the synergistic effect of the core-shell microcapsule structure and the dual fixation system.

[0057] Comparative Example 3 The W-shaped cross-section modified polyester fiber in the middle layer of Example 1 was replaced with a circular cross-section modified polyester fiber (also grafted with chitosan-PEG-4000, with a grafting rate of 3.2%), and other process parameters were completely consistent with those of Example 1.

[0058] Performance testing: 60-minute moisture absorption rate = 35%; water droplet diffusion time = 2.6s; OWT0 = 385% (<400%); OWT after 30 washes 30 =300%, retention rate =78%.

[0059] Conclusion: Simply replacing the W-shaped profile with a circular cross-section reduced OWT0 from 462% to 385% (a decrease of approximately 17%), and extended the water diffusion time from 1.8s to 2.6s, demonstrating that the combination of the W / Y profile and axial microporous channels significantly contributes to the capillary moisture conduction rate and OWT.

[0060] Comparative Example 4 The microcapsule dispersion in the outer layer impregnation-microwave pre-drying-heat setting process of Example 1 was omitted (only water was used for impregnation), and other process parameters were completely consistent with those of Example 1. The content of outer layer microcapsules was 0%.

[0061] Performance testing: 60-minute moisture absorption rate = 24% (<32%); drip diffusion time = 2.2s; OWT0 = 418%; OWT after 30 washes 30 =339%, retention rate =81%.

[0062] Conclusion: By omitting the sodium polyacrylate core-shell microcapsules, the moisture absorption rate at 60 min decreased from 38% to 24%, which is lower than the lower limit of 32% required by the claim, proving that the outer sodium polyacrylate core-shell microcapsules play a key role in the high moisture absorption rate and active moisture-locking ability of the fabric.

[0063] Comparative Example 5 (W-shaped irregular cross section + no grafting modification) The chitosan-PEG grafting modification step of the intermediate layer in Example 1 is omitted (the chitosan-PEG graft copolymer solution is not impregnated in S2, and deionized water is used instead of impregnation). The intermediate layer still uses W-shaped cross-section polyester fiber (1.65 dtex, irregularity 0.42, micropore diameter d=1.2μm, micropore porosity ε=12%). Other process parameters (including three-layer structure, point-like hot melt adhesive composite, application of outer microcapsules, etc.) are completely consistent with those in Example 1.

[0064] Performance testing: 60-minute moisture absorption rate = 33%; water droplet diffusion time = 2.9s; OWT0 = 350%; OWT after 30 washes 30 =265%, OWT retention rate =76%.

[0065] Conclusion: By retaining the W-shaped cross-section and microporous channel structure but omitting the chitosan-PEG grafting modification, OWT0 decreased from 462% in Example 1 to 350% (a decrease of 24.2%), the water diffusion time increased from 1.8s to 2.9s, the 60-min moisture absorption rate decreased from 38% to 33%, and the OWT retention rate decreased from 85% to 76%. This demonstrates that the chitosan-PEG grafting modification has a significant independent contribution to the hydrophilic and moisture-wicking properties and water-washing resistance of the intermediate layer.

[0066] To verify the synergistic effect of the intermediate layer's W / Y shaped cross-section and chitosan-PEG grafting modification, performance benchmarks for each feature when applied individually were established by combining Comparative Example 3 (circular cross-section + grafting modification) and Comparative Example 5 (W-shaped cross-section + no grafting modification), and synergistic analysis was performed: OWT Collaborative Validation (Note: Comparative Example 1 uses a three-layer nonwoven needle-punching composite process, which has a different microstructure than the woven / weft knitting + dot-shaped hot-melt composite process in the embodiments of this invention. The following independent contribution decomposition and collaborative gain analysis are approximate estimates based on this benchmark): Comparative Example 5 (W-shaped irregular shape + no grafting) OWT0=350%, representing the benchmark value of the contribution of W / Y irregular cross section + microporous channel alone (an improvement of 30 percentage points compared to Comparative Example 1's OWT0=320%); Comparative Example 3 (circular cross section + grafting modification) OWT0=385%, representing the benchmark value of the contribution of grafting modification alone (an improvement of 65 percentage points compared to Comparative Example 1); The linear superposition of the two is expected to result in OWT0=320+30+65=415%. In Example 1 (W-shaped profile + graft modification), the measured OWT0 = 462%, significantly exceeding the expected value of 415% for linear superposition, with a synergistic gain of 47 percentage points. This demonstrates that the combination of W / Y profile + microporous channels and chitosan-PEG graft modification produces a super-superposition synergistic effect. This synergistic effect originates from the high specific surface area three-dimensional capillary channels provided by the W / Y profile + microporous structure, which makes the loading of the graft copolymer on the fiber surface more uniform and firm. At the same time, the graft modification endows the microporous channel walls with durable hydrophilic properties. The two work synergistically to greatly improve capillary moisture wicking efficiency and long-term stability.

[0067] Synergistic verification of water diffusion time: The water diffusion time of Comparative Example 5 was 2.9s (2.7s shorter than 5.6s of Comparative Example 1), and 2.6s of Comparative Example 3 (3.0s shorter); The measured water diffusion time of Example 1 was 1.8s, which was significantly better than either of the individual feature schemes (2.6s, 2.9s), proving that the two features have a positive synergistic effect in accelerating water penetration.

[0068] Table 3 below is a performance comparison table between the examples and the comparative examples.

[0069] Table 3 As can be seen from Examples 1, 2 and Comparative Example 1, by adopting the combination scheme of the present invention of "W / Y irregular shape + axial micropore + chitosan-PEG grafting + core-shell microcapsule + dot-like hot melt adhesive + Δθ≥60°", the OWT0 reached 462% and 485% respectively, which is significantly higher than the 320% of Comparative Example 1 (CN119749022A represents the closest prior art); and after 30 washes, the OWT retention rate was ≥82%, which is significantly better than the 55% of Comparative Example 1, verifying that the initial moisture wicking performance and water wash resistance of the present invention are significantly improved.

[0070] As shown in Example 1 and Comparative Example 2, although Comparative Example 2 also introduced chitosan-PEG graft copolymer and sodium polyacrylate functional agent, due to the lack of a three-layer gradient structure, core-shell microcapsule design, and point-like hot-melt adhesive composite, its OWT was only 180%, which is a typical bidirectional diffusion fabric and cannot achieve unidirectional directional transmission; moreover, after 30 washes, a large amount of powder was shed, and the OWT retention rate was only 39%, proving that chemical modifiers alone cannot replace the gradient layer structure and microcapsule process. The data intuitively demonstrate the synergistic gain of multiple features: under the complete synergistic system, Example 1 OWT0=462%, which is 44.4% higher than Comparative Example 1 (without any core feature); the OWT retention rate after 30 washes was 85%, which is 30 percentage points higher than the 55% of Comparative Example 1 (relative improvement of 54.5%); the moisture absorption rate at 60 min was 38%, which is 52% higher than Comparative Example 1; and the water droplet diffusion time was shortened by 67.9%. Relying solely on ordinary fiber needle-punched composites, without gradient driving force, capillary moisture wicking, long-lasting hydrophilicity, and active moisture locking, the sweat transmission power is insufficient, channels are lacking, moisture absorption capacity is low, and washability is poor. All core performance characteristics are comprehensively degraded, proving that a complete set of distinguishing features are indispensable.

[0071] As can be seen from Example 1 and Comparative Example 3, after replacing the W-shaped irregular cross-section of the middle layer with a circular cross-section, OWT0 decreased by 17% and the water droplet diffusion time increased by 44%, proving that the combination of W / Y irregular shape + axial micropores plays a decisive role in the capillary moisture wicking rate of the fabric, which is the key technical feature that distinguishes this invention from the circular cross-section core layer scheme.

[0072] As shown in Example 1 and Comparative Example 5, after retaining the W-shaped cross-section and microporous channels but omitting the chitosan-PEG grafting modification, OWT0 decreased from 462% to 350% (a decrease of 24.2%), the water diffusion time increased from 1.8s to 2.9s (an increase of 61.1%), and the OWT retention rate decreased from 85% to 76%. This demonstrates that chitosan-PEG grafting modification has a significant independent contribution to moisture conduction rate, hydrophilic durability, and water washability. Further comparison of synergistic effects: the linear superposition of Comparative Example 5 (W-shaped + no grafting, OWT0=350%) and Comparative Example 3 (circular + grafting, OWT0=385%) expected OWT0=415%, while the measured OWT0 of Example 1 was 462%, exceeding the linear superposition expectation by 47 percentage points. This confirms a significant synergistic gain between the W / Y shaped cross-section and microporous channels and the chitosan-PEG grafting modification, with the combined effect being superior to the simple superposition of the individual contributions.

[0073] As can be seen from Example 1 and Comparative Example 4, when sodium polyacrylate core-shell microcapsules are missing, the moisture absorption rate at 60 min decreases from 38% to 24% (below the lower limit of 32%), proving that the active moisture absorption and moisture retention capacity of the outer microcapsules is a necessary condition for the present invention to achieve a moisture absorption rate of ≥32%.

[0074] In summary, the six core distinguishing technical features of this invention do not work independently, but rather form a five-in-one synergistic system of gradient driving force, capillary moisture-wicking channels, durable hydrophilic modification, outer active moisture-locking, and breathable composite structure. The absence of any one feature will break the overall moisture-wicking closed loop, and all performance indicators will decrease significantly and simultaneously. Inner layer hydrophobic high contact angle + outer layer extremely low contact angle (Δθ≥60°): This creates a continuous unidirectional water chemical potential difference, providing the basic driving force for the directional transport of sweat; without this gradient difference, sweat diffuses bidirectionally and is very easy to re-permeate back into the skin. The middle layer features a W / Y shaped cross-section with axially extending micropores, which amplifies the capillary effect, quickly receives and laterally disperses sweat, and acts as a carrier for gradient dynamics. The circular cross-section lacks three-dimensional capillary channels, resulting in a significant decrease in moisture wicking rate. Chitosan-polyethylene glycol covalent grafting modification (grafting rate 3%~6%): imparts stable hydrophilic properties to the intermediate layer, solves the problem of traditional coating peeling off after washing, and maintains capillary moisture wicking ability for a long time; the performance of physical coating modification drops sharply after washing. Cross-linked chitosan wall material with sodium polyacrylate core-shell moisture-absorbing microcapsules: The outer layer actively captures and locks in sweat, increasing the total moisture absorption capacity of the fabric and quickly evaporating the sweat; without microcapsules, the total moisture absorption of the fabric will not meet the standard. Three-layer dot-matrix hot-melt array composite: balances interlayer bonding strength and breathable channels, ensuring the gradient structure remains intact and is not blocked by the coating; overall coating / needling will block capillary channels and weaken the one-way moisture-wicking effect; Multi-layer fiber basis weight, fiber linear density, micropore size, and microcapsule particle size parameters are matched within a range: the capillary force, moisture absorption capacity, and hydrophobic resistance of each layer are precisely matched to form a continuous and unobstructed sweat transmission link of "skin → inner layer → middle layer → outer layer". If the parameters deviate from the range, the synergistic effect will fail.

[0075] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A textile fabric with moisture-absorbing properties, characterized in that, The textile fabric is made by sequentially stacking an inner layer, a middle layer and an outer layer and bonding them together with point-like hot melt adhesive, forming a water gradient transport structure with increasing hydrophilicity along the direction from the inner layer to the outer layer. The inner layer is a hydrophobic fast-conducting layer, woven from hydrophobic synthetic fibers with irregular cross-sections, and the water contact angle of the inner layer is 95°~110°. The intermediate layer is a hydrophilic core layer with an irregular cross-section, woven from modified polyester fibers with a W-shaped or Y-shaped cross-section. The modified polyester fibers have axially extending microporous channels with a pore size of 0.5~2μm and a porosity of 8%~15%. The surface of the modified polyester fibers is grafted with chitosan-polyethylene glycol graft copolymer, and the grafting rate is 3%~6% based on the dry weight calculated after Soxhlet extraction purification. The outer layer is a hydrophilic layer made of regenerated cellulose fiber / cotton blend yarn, woven from a blend of regenerated cellulose fiber and cotton. The outer layer contains sodium polyacrylate moisture-absorbing microcapsules with a particle size of 15-35 μm, and the content of the sodium polyacrylate moisture-absorbing microcapsules is 5%-10% of the dry weight of the outer layer. The water contact angle of the outer layer is 20°-35°. The difference between the water contact angle of the inner layer and the water contact angle of the outer layer is not less than [value missing]. .

2. The textile fabric with moisture-absorbing function according to claim 1, characterized in that, The modified polyester fiber of the intermediate layer with a W-shaped or Y-shaped cross-section has a single fiber linear density of 1.2~2.5 dtex and a shape degree of 0.35~0.55; the basis weight of the inner layer is 40~60 g / m². 2 The basis weight of the intermediate layer is 80~120g / m³. 2 The outer layer has a basis weight of 60~90g / m³. 2 .

3. The textile fabric with moisture-absorbing function according to claim 1, characterized in that, In the chitosan-polyethylene glycol graft copolymer, the degree of deacetylation of chitosan is 85%~95%, and the number average molecular weight of polyethylene glycol is 2000~6000; the content of the chitosan-polyethylene glycol graft copolymer in the intermediate layer is 3%~6% of the dry weight of the intermediate layer; and the water contact angle of the intermediate layer is 60°~75°.

4. The textile fabric with moisture-absorbing function according to claim 1, characterized in that, The regenerated cellulose fiber in the outer layer is one or a combination of Lyocell fiber, Modal fiber, or bamboo pulp fiber; the mass ratio of the regenerated cellulose fiber to cotton is 4:6 to 6:4; the sodium polyacrylate moisture-absorbing microcapsules use cross-linked chitosan as the wall material and cross-linked sodium polyacrylate as the core material to form a core-shell structure.

5. The textile fabric with moisture-absorbing function according to claim 1, characterized in that, The adhesive points of the dotted hot melt adhesive are arranged in a regular array, with a spacing of 3-6 mm between adhesive points. The area of ​​the adhesive points accounts for 8%-15% of the total area of ​​the fabric. The hot melt adhesive used is a polyamide copolymer or polyester copolymer hot melt adhesive powder with a melting point of 120-140℃.

6. The textile fabric with moisture-absorbing function according to claim 1, characterized in that, The fabric has a moisture absorption rate of no less than 32% after 60 minutes at a temperature of 25°C and a relative humidity of 90%, and the water droplet diffusion time does not exceed 3 seconds.

7. A method for preparing a textile fabric with moisture-absorbing function as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1 Inner Layer Preparation: Hydrophobic synthetic fibers with irregular cross-sections are processed into yarn through cleaning, combing, drawing, roving, and spinning processes, and then woven to obtain the inner layer fabric. Preparation of S2 intermediate layer modified fiber: W-shaped or Y-shaped cross-section polyester fibers are pretreated by low-temperature plasma and then impregnated in chitosan-polyethylene glycol graft copolymer solution. After impregnation, padding and drying, modified polyester fibers with a grafting rate of 3%~6% are obtained. Then, the intermediate layer fabric is obtained by spinning and weaving. S3 outer layer preparation: Sodium polyacrylate moisture-absorbing microcapsule dispersion is applied to regenerated cellulose fiber / cotton blended fabric, and the outer layer fabric is obtained by padding, microwave pre-drying and heat setting. S4 Composite Process: The inner layer fabric, the middle layer fabric, and the outer layer fabric are stacked sequentially and bonded together using a dot-matrix hot melt bonding process to obtain the textile fabric with moisture-absorbing function.

8. The method for preparing a textile fabric with moisture-absorbing function according to claim 7, characterized in that, In step S2, the low-temperature plasma pretreatment is carried out in an argon / oxygen mixed atmosphere, with a plasma power of 100~200W and a treatment time of 30~120s; the chitosan-polyethylene glycol graft copolymer solution has a mass concentration of 3%~6%, an impregnation temperature of 40~55℃, an impregnation time of 30~60min, two dips and two rolls, a roll residue of 75%~85%, and then drying at 90~110℃ for 3~8min.

9. The method for preparing a textile fabric with moisture-absorbing function according to claim 7, characterized in that, In step S3, the sodium polyacrylate hygroscopic microcapsule dispersion is prepared by interfacial polymerization. Specifically, a 1%–3% (w / w) chitosan-acetic acid aqueous solution is used as the aqueous phase, and an aqueous solution of sodium acrylate containing N,N'-methylenebisacrylamide crosslinking agent is used as the core material precursor. The two phases are mixed and emulsified in the oil phase. Ammonium persulfate initiator is added, and the reaction is carried out at 65–75°C for 2–4 hours. The temperature is then lowered to 35–45°C, and glutaraldehyde crosslinking agent is added at an amount of 10%–20% of the chitosan mass. The chitosan wall material is cured by cross-linking reaction for 1.5-2.5 hours, and the pH is adjusted to 6.5-7.0 to obtain a core-shell structured microcapsule dispersion with cross-linked chitosan as the wall material, cross-linked sodium polyacrylate as the core material, and a particle size of 15-35 μm. The mass concentration of the dispersion is 8%-12%, and the roll-off rate is 70%-80% during rolling. After rolling, the microcapsule is first pre-dried by microwave at a power of 800-1200W for 30-90s, and then heat-set at 110-130℃ for 2-5 minutes.

10. A method for preparing a textile fabric with moisture-absorbing function according to claim 7, characterized in that, In step S4, the bonding temperature of the dot-matrix hot melt bonding process is 130~150℃, the bonding pressure is 0.3~0.5MPa, the bonding time is 5~15s, the spacing between bonding points is 3~6mm, the bonding points are arranged in a square or diamond array, and the amount of hot melt adhesive powder applied is 8~12g / m 2 The area of ​​the bonding points accounts for 8% to 15% of the total area of ​​the fabric.

Citation Information

Patent Citations

  • Triple gradient structure one-way moisture conduction non-woven composite fabric and preparation method thereof

    CN119749022A