A method for preparing a wrinkled hierarchical porous SAPO-11 molecular sieve and its application

By preparing a wrinkled, hierarchical porous SAPO-11 molecular sieve and loading it with Pt metal, the problem of micropore limitation in SAPO-11 molecular sieve was solved, significantly improving the alkane isomerization performance and meeting the upgrade requirements of gasoline standards.

CN123061972APending Publication Date: 2026-11-10HENAN INST OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611123154.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The narrow micropores of existing SAPO-11 molecular sieves restrict the diffusion of isomeric intermediates, resulting in low selectivity and yield of isoalkanes, making it difficult to meet the requirements of automotive gasoline standards for reducing olefins and aromatics.

Method used

KCC-1 with a specific fold spacing was used as a silicon source and hard template agent. A folded hierarchical porous SAPO-11 molecular sieve was prepared by combining in-situ hydrothermal method. The folded structure was precisely controlled by adjusting the synthesis parameters of KCC-1 to construct a micro-mesoporous composite structure. Pt metal was loaded as a catalyst.

Benefits of technology

It significantly improved the catalytic activity and isomer yield of alkane isomerization, with an increase of 10.6%~23.4% in n-decane conversion, 5.7%~8.0% in isomer selectivity, and 17.0%~33.9% in isomer yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061972A_ABST
    Figure CN123061972A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a wrinkled hierarchical porous SAPO-11 molecular sieve and its application. The preparation process uses KCC-1, with controllable wrinkle spacing, as both a silicon source and a hard template agent. A combined in-situ hydrothermal method is used to construct the wrinkled hierarchical porous SAPO-11 molecular sieve. By adjusting the synthesis parameters of KCC-1, the wrinkled structure is precisely controlled, thereby achieving directional control over the microstructure and pore structure of the SAPO-11 molecular sieve. The hierarchical porous SAPO-11 prepared by this invention possesses a microporous-mesoporous composite pore structure, exhibiting a wrinkled morphology, and a particle size between 250 and 700 nm. After loading Pt metal onto it to prepare a bifunctional catalyst, it can significantly promote the generation and diffusion of isomer intermediates, improve the catalytic activity and isomer yield of alkane isomerization, thereby improving the octane number of gasoline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of molecular sieve catalysis technology, specifically relating to a method for preparing a wrinkled hierarchical porous SAPO-11 molecular sieve and its application. Background Technology

[0002] Under the dual constraints of "dual carbon" targets and energy security, my country's gasoline standards have fully entered the China VI era, setting strict limits on the content of aromatics and olefins. Traditional processes relying on catalytic reforming and catalytic cracking to increase octane number are facing a structural contradiction between "reducing olefins and aromatics" and "maintaining octane number." Alkane hydroisomerization technology, which can convert low-octane n-alkanes into high-octane isoalkanes, has become a key technological approach for refineries to upgrade oil product quality.

[0003] The development of highly efficient catalysts is the core of alkane isomerization technology. Currently, bifunctional catalysts combining molecular sieve acidic supports and metals are commonly used. The pore structure of the support is a key factor affecting the activity and isomer selectivity of alkane isomerization reactions. Among them, SAPO-11 molecular sieve, with its one-dimensional straight-channel structure, is an excellent support for alkane isomerization catalysts. However, its narrow micropores (0.39 × 0.63 nm) restrict the diffusion of isomer intermediates, resulting in low selectivity and yield of isomerized alkanes.

[0004] To overcome the aforementioned diffusion limitations, constructing hierarchical porous SAPO-11 molecular sieves with micro-mesoporous composite structures has become a research hotspot. Morphology control is one of the important strategies for improving the pore structure of molecular sieves. In recent years, wrinkled nanoparticles have attracted much attention due to their three-dimensional open framework structure and high mesopore volume, which can significantly promote the diffusion of reactants and products. For example, literature (Fuel 2024, 361:130644) discloses the preparation of a wrinkled hierarchical porous TS-1@KCC-1 composite using a seed-assisted strategy and its application in hydrodesulfurization reaction. Patent documents CN202411694810.1 and CN202411694804.6 respectively disclose methods for preparing mesoporous-microporous composite molecular sieves with Y or Beta molecular sieves as the core and KCC-1 as the shell, aiming to improve diffusion performance and hydrocracking efficiency. Although the above-mentioned wrinkled composite has more mesopores and a larger specific surface area than conventional molecular sieves, its molecular sieve core itself does not have a wrinkled morphology. The improvement of its pore structure mainly depends on the shell KCC-1, and the diffusion enhancement effect is still quite limited.

[0005] Current research has attempted to use KCC-1 as a silicon source and hard template agent to prepare hierarchical porous SAPO-11 molecular sieves with a wrinkled morphology via in-situ hydrothermal synthesis, effectively improving the diffusion limitation of SAPO-11 molecular sieve micropores. However, the synthesis conditions of KCC-1 in this work are relatively simple, and no technical approach has been explored to directionally optimize the pore structure and alkane isomerization performance of SAPO-11 by controlling the wrinkled structure of KCC-1. Summary of the Invention

[0006] To overcome the aforementioned technical problems, this invention provides a method for preparing a pleated hierarchical porous SAPO-11 molecular sieve. This method uses KCC-1, with controllable pleat spacing, as both a silicon source and a hard template agent, combined with an in-situ hydrothermal method to construct the hierarchical porous SAPO-11 molecular sieve. By precisely controlling the synthesis parameters of KCC-1, its pleated structure can be controlled, thereby achieving directional control over the microstructure and pore structure of the SAPO-11 molecular sieve. The prepared hierarchical porous SAPO-11 possesses a microporous-mesoporous composite pore structure, exhibiting a pleated morphology, and its particle size is between 250 and 700 nm. After loading it with Pt metal to prepare a bifunctional catalyst, it can significantly promote the generation and diffusion of isomer intermediates, improve the catalytic activity and isomer yield of alkane isomerization, thereby improving the octane number of gasoline.

[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0008] A method for preparing a wrinkled hierarchical porous SAPO-11 molecular sieve, the specific preparation steps of which are as follows:

[0009] Step S1: Add aluminum source and phosphorus source to deionized water and stir at 20~50℃ for 0.5~3.5h to obtain aluminum phosphorus precursor solution, wherein the aluminum source is one or more of aluminum isopropoxide, boehmite and aluminum nitrate nonahydrate; and the phosphorus source is one or more of phosphoric acid, phosphorous acid and ammonium phosphate.

[0010] Step S2: Add KCC-1 with a specific wrinkle spacing and a structure directing agent to the aluminum phosphate precursor solution obtained in step S1, and stir at 20~50℃ for 2~4h to obtain a homogeneous gel, wherein KCC-1 serves as both a silicon source and a hard template agent, and the structure directing agent is one or more of di-n-propylamine and diisopropylamine.

[0011] Step S3: The homogeneous gel obtained in step S2 is transferred to a reaction vessel and crystallized at 180-220℃ for 24-48 h. The resulting product is then washed, dried, and calcined to obtain a hierarchical porous SAPO-11 molecular sieve with a wrinkled morphology. The particle size is 250-700 nm, and the BET specific surface area is 250-350 m². 2 / g, mesopore volume is 0.25~0.50cm³ 3 / g.

[0012] Furthermore, the specific preparation process of KCC-1 in step S2 is as follows: a silicon source, a surfactant, a co-surfactant, an alkali source, an oil phase, and deionized water are mixed, and a microemulsion is formed by adjusting the oil-water ratio, the amount of surfactant added, and / or the amount of co-surfactant added; the microemulsion is then stirred at 30~70℃ for 12~36h, and the resulting product is washed and dried sequentially to obtain KCC-1 with a specific fold spacing;

[0013] The silicon source is one or more of tetraethyl silicate, silica sol, and silica fume; the alkali source is one or more of sodium hydroxide, urea, and ammonia; the surfactant is one or more of tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, and octadecyltrimethylammonium bromide; the co-surfactant is one or more of n-pentanol, n-butanol, and isoamyl alcohol; the oil phase is one or more of cyclohexane, n-hexane, and n-heptane; the drying temperature is 80~120℃, and the drying time is 24~48h.

[0014] Furthermore, the molar ratio of the silicon source, surfactant, co-surfactant, alkali source, oil phase and deionized water is (1.0~1.2):(0.1~0.3):(1.0~1.5):(0.5~1.0):(20~25):(110~120). By changing the oil-water ratio, the amount of surfactant added and / or the amount of co-surfactant added, a series of KCC-1 with different wrinkled structures can be obtained.

[0015] Furthermore, the wrinkle spacing of KCC-1 in step S2 is 5~150nm, and the wrinkle spacing refers to the average distance between adjacent wrinkle peaks on the outer surface of the sphere in the scanning electron microscope image.

[0016] Furthermore, the molar ratio of the aluminum source, phosphorus source, KCC-1, structure directing agent and deionized water is (0.6~1.0):(1.5~2.5):(0.2~0.6):(1.0~1.6):(40~60).

[0017] Furthermore, in step S3, the drying temperature is 80~120℃ and the drying time is 24~48h; the calcination temperature is 500~650℃ and the calcination time is 4~8h.

[0018] The present invention also provides an alkane hydroisomerization catalyst, which is prepared by loading the metal active component Pt onto the wrinkled hierarchical porous SAPO-11 molecular sieve obtained by the above method. This catalyst effectively promotes the generation and diffusion of isomer intermediates, reduces the occurrence of cracking side reactions, and significantly improves the catalytic activity and isomer yield of alkane isomerization.

[0019] Furthermore, the loading of the metal active component Pt in the alkane hydroisomerization catalyst is 0.1 wt.% to 0.6 wt.%.

[0020] This invention provides the application of the aforementioned pleated hierarchical porous SAPO-11 molecular sieve as a support for supporting metal Pt catalysts in the catalytic hydroisomerization reaction of alkane.

[0021] Furthermore, the alkane hydroisomerization reaction specifically refers to the hydroisomerization reaction of n-decane, and the specific reaction conditions are: reaction temperature of 280~400℃, reaction pressure of 1.5~2.5MPa, and n-decane mass hourly space velocity of 1.0~40h⁻¹. -1 The volume ratio of hydrogen to n-decane is (200~600):1.

[0022] Compared with the prior art, the beneficial effects and advantages of the present invention are as follows:

[0023] This invention utilizes KCC-1 with a specific fold spacing as both a silicon source and a hard template agent. By controlling the synthesis parameters of KCC-1, its fold structure can be manipulated. Combined with an in-situ hydrothermal synthesis process, the directional and precise construction of the microstructure and pore structure of SAPO-11 molecular sieves can be achieved. Furthermore, using folded hierarchical porous SAPO-11 as a support, and employing an equal-volume impregnation method to load metal active components, the conversion rate and isomer yield in the hydroisomerization reaction of n-decane are increased by 10.6%~23.4% and 17.0%~33.9%, respectively, compared to conventional microporous SAPO-11. The supported catalyst prepared by this invention effectively promotes the generation and diffusion of isomer intermediates, reduces the occurrence of cracking side reactions, and significantly improves the catalytic activity and isomer yield of alkane isomerization. Attached Figure Description

[0024] Figure 1 The X-ray diffraction patterns of the molecular sieves prepared in Examples 1, 2 and Comparative Example 1 are shown.

[0025] Figure 2 Scanning electron microscope (SEM) images of the molecular sieves prepared in Examples 1, 2 and Comparative Example 1.

[0026] Figure 3 The N2 adsorption-desorption isotherms of the molecular sieves prepared in Examples 1, 2 and Comparative Example 1 are shown. Detailed Implementation

[0027] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments, but this should not be construed as limiting the invention. Unless otherwise specified, the technical means used in the following embodiments are conventional means well known to those skilled in the art, and the materials, reagents, etc. used in the following embodiments are commercially available unless otherwise specified.

[0028] Example 1

[0029] (1) Dissolve 5.0g hexadecyltrimethylammonium bromide and 3.0g urea in 150.0g deionized water, then add 136.5g cyclohexane and 6.1g n-butanol and stir to mix; then add 15.0g tetraethyl silicate to the above solution and mix, and stir the mixed solution at 70℃ for 24h; finally, wash the obtained product and dry it at 90℃ for 12h to obtain KCC-1 nanoparticles.

[0030] (2) 12.2g of phosphoric acid and 8.1g of boehmite were added to 40.0g of deionized water and stirred in a water bath at 35℃ for 3h to make them uniformly mixed; then 4.5g of the KCC-1 nanoparticles prepared above were added and stirred for 2h, followed by 6.8g of di-n-propylamine and stirred for 1h to obtain a homogeneous gel; finally, the homogeneous gel was placed in a reaction vessel and crystallized at 200℃ for 24h.

[0031] (3) The product obtained above was filtered with deionized water and dried at 120°C for 12 hours. The product was placed in a muffle furnace and heated to 600°C for 6 hours at a heating rate of 2°C / min. Finally, a wrinkled hierarchical porous SAPO-11 molecular sieve was obtained, which was denoted as WS-11-1.

[0032] The X-ray diffraction pattern of the wrinkled, hierarchical porous SAPO-11 molecular sieve is shown below. Figure 1 Scanning electron microscope image (see) Figure 2 Left, see N2 adsorption-desorption isotherm diagram. Figure 3 .

[0033] Example 2

[0034] The amount of n-butanol added in Example 1 was changed to 7.6g, and the remaining steps were completely consistent with Example 1, resulting in a wrinkled hierarchical porous SAPO-11 molecular sieve, denoted as WS-11-2.

[0035] The X-ray diffraction pattern of the wrinkled, hierarchical porous SAPO-11 molecular sieve is shown below. Figure 1 Scanning electron microscope image (see) Figure 2 On the right, see the N2 adsorption-desorption isotherm diagram. Figure 3 .

[0036] Example 3

[0037] The amount of n-butanol added in Example 1 was changed to 9.1g, and the remaining steps were completely consistent with Example 1, resulting in a wrinkled hierarchical porous SAPO-11 molecular sieve, denoted as WS-11-3.

[0038] Example 4

[0039] The amount of n-butanol added in Example 1 was changed to 10.7g, and the remaining steps were completely consistent with Example 1, resulting in a wrinkled hierarchical porous SAPO-11 molecular sieve, denoted as WS-11-4.

[0040] Example 5

[0041] The amount of n-butanol added in Example 1 was changed to 12.2g, and the remaining steps were completely the same as in Example 1, resulting in a wrinkled hierarchical porous SAPO-11 molecular sieve, denoted as WS-11-5.

[0042] Comparative Example 1

[0043] (1) 12.2g of phosphoric acid and 8.1g of boehmite were added to 40.0g of deionized water and stirred in a water bath at 35°C for 3h to make them uniformly mixed; then tetraethyl silicate (about 4.7g) with the same amount of silicon as KCC-1 in Example 1 was added and stirred for 2h, followed by 6.8g of di-n-propylamine and stirred for 1h to obtain a homogeneous gel; finally, the homogeneous gel was placed in a reaction vessel and crystallized at 200°C for 24h.

[0044] (2) The product obtained above was filtered with deionized water and dried at 120°C for 12 hours. The product was placed in a muffle furnace and calcined at 600°C for 6 hours at a heating rate of 2°C / min. Finally, conventional microporous SAPO-11 molecular sieve was obtained, which was denoted as TS-11.

[0045] The X-ray diffraction pattern of the microporous SAPO-11 molecular sieve is shown below. Figure 1 See the N2 adsorption-desorption isotherm diagram. Figure 3 .

[0046] Catalytic performance evaluation:

[0047] The wrinkled hierarchical porous SAPO-11 molecular sieves prepared in Examples 1, 2, 3, 4 and 5, and the conventional microporous SAPO-11 molecular sieve prepared in Comparative Example 1 were pressed into tablets and sieved to 20-40 mesh. Chloroplatinic acid solution was added dropwise to the above particles using the equal volume impregnation method. After standing at room temperature for 24-48 h, drying at 100-120℃ for 12-24 h, and calcining at 400-500℃ for 3-6 h, a Pt / SAPO-11 catalyst with a metal active component Pt content of 0.5 wt.% was obtained.

[0048] Using n-decane model oil as raw material, the performance of the Pt / SAPO-11 catalyst prepared above in the alkane isomerization reaction was evaluated. The reaction temperature was 340℃, the reaction pressure was 1.5 MPa, and the mass hourly space velocity (HHSV) was 4.0 h⁻¹. -1 The volume ratio of hydrogen to n-decane was 400, and the evaluation results are shown in Table 1.

[0049] Table 1. Results of the hydroisomerization of n-decane using the catalysts corresponding to Examples 1-5 and Comparative Example 1 under the same reaction conditions.

[0050] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Conversion rate (%) 78.0 80.2 87.0 83.0 82.2 70.5 Isomer selectivity (%) 93.9 94.2 95.9 95.1 94.8 88.8 Isomer yield (%) 73.2 75.5 83.4 78.9 77.9 62.6

[0051] Table 2. Pore structure parameters of the carriers corresponding to Examples 1, 2 and Comparative Example 1

[0052] catalyst <![CDATA[BET specific surface area (m 2 g -1 )]]> <![CDATA[External specific surface area (m 2 g -1 )]]> <![CDATA[Mesopore volume (cm 3 g -1 )]]> Example 1 279 205 0.31 Example 2 283 235 0.33 Comparative Example 1 191 50 0.08

[0053] Analysis results

[0054] The performance of n-decane hydroisomerization under the same reaction conditions was compared and analyzed in Examples 1, 2, 3, 4, 5, and Comparative Example 1, and the results are shown in Table 1. As can be seen from the table, compared with the catalyst in Comparative Example 1, the n-decane conversion rate of the catalysts in Examples 1-5 of this invention is increased by approximately 10.6%-23.4%, the isomer selectivity is increased by approximately 5.7%-8.0%, and the isomer yield is increased by approximately 17.0%-33.9%. Since the prepared Pt / SAPO-11 series catalysts all have the same metal active component loading, the alkane isomerization performance of the catalysts is mainly affected by the physicochemical properties of the molecular sieves prepared in Examples 1-5 and Comparative Example 1. The SAPO-11 series molecular sieves prepared in Examples 1-5 of this invention exhibit a wrinkled morphology, and their particle size is controlled between 250-700 nm. On the one hand, this exposes more active sites for alkane isomerization reactions; on the other hand, it gives them a high mesopore volume, which can promote the formation and diffusion of isomer intermediates and reduce the occurrence of cracking side reactions. Therefore, the catalysts obtained by loading metal active components onto molecular sieves prepared in Examples 1-5 can effectively promote the generation and diffusion of isomer intermediates, reduce the occurrence of cracking side reactions, and significantly improve the catalytic activity and isomer yield of alkane isomerization.

[0055] The embodiments described above are merely preferred embodiments of the present invention, and not all feasible embodiments of the present invention. Any obvious modifications made by those skilled in the art without departing from the essence of the present invention should be considered to be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a wrinkled, hierarchical porous SAPO-11 molecular sieve, characterized in that... The specific preparation steps are as follows: Step S1: Add aluminum source and phosphorus source to deionized water and stir at 20~50℃ for 0.5~3.5h to obtain aluminum phosphorus precursor solution, wherein the aluminum source is one or more of aluminum isopropoxide, boehmite and aluminum nitrate nonahydrate; and the phosphorus source is one or more of phosphoric acid, phosphorous acid and ammonium phosphate. Step S2: Add KCC-1 with a specific wrinkle spacing and a structure directing agent to the aluminum phosphate precursor solution obtained in step S1, and stir at 20~50℃ for 2~4h to obtain a homogeneous gel, wherein KCC-1 serves as both a silicon source and a hard template agent, and the structure directing agent is one or more of di-n-propylamine and diisopropylamine. Step S3: The homogeneous gel obtained in step S2 is transferred to a reaction vessel and crystallized at 180-220℃ for 24-48 h. The resulting product is then washed, dried, and calcined to obtain a hierarchical porous SAPO-11 molecular sieve with a wrinkled morphology. The particle size is 250-700 nm, and the BET specific surface area is 250-350 m². 2 / g, mesopore volume is 0.25~0.50cm³ 3 / g; The specific preparation process of KCC-1 is as follows: a silicon source, a surfactant, a co-surfactant, an alkali source, an oil phase and deionized water are mixed, and a microemulsion is formed by adjusting the oil-water ratio, the amount of surfactant added and / or the amount of co-surfactant added; the microemulsion is then stirred at 30~70℃ for 12~36h, and the resulting product is washed and dried in sequence to obtain KCC-1 with a specific fold spacing. Wherein, the silicon source is one or more of tetraethyl silicate, silica sol, and fumed silica; the alkali source is one or more of sodium hydroxide, urea, and ammonia; the surfactant is one or more of tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, and octadecyltrimethylammonium bromide; the co-surfactant is one or more of n-pentanol, n-butanol, and isoamyl alcohol; and the oil phase is one or more of cyclohexane, n-hexane, and n-heptane.

2. The method for preparing the wrinkled hierarchical porous SAPO-11 molecular sieve according to claim 1, characterized in that: The wrinkle spacing of KCC-1 in step S2 is 5~150nm. The wrinkle spacing refers to the average distance between adjacent wrinkle peaks on the outer surface of the sphere in the scanning electron microscope image.

3. The method for preparing the wrinkled hierarchical porous SAPO-11 molecular sieve according to claim 1, characterized in that: The molar ratio of the aluminum source, phosphorus source, KCC-1, structure guiding agent and deionized water is (0.6~1.0):(1.5~2.5):(0.2~0.6):(1.0~1.6):(40~60).

4. The method for preparing the wrinkled hierarchical porous SAPO-11 molecular sieve according to claim 1, characterized in that: The drying temperature during the preparation of KCC-1 is 80~120℃, and the drying time is 24~48h.

5. The method for preparing the wrinkled hierarchical porous SAPO-11 molecular sieve according to claim 1, characterized in that: The molar ratio of silicon source, surfactant, co-surfactant, alkali source, oil phase and deionized water is (1.0~1.2):(0.1~0.3):(1.0~1.5):(0.5~1.0):(20~25):(110~120). By changing the oil-water ratio, the amount of surfactant added and / or the amount of co-surfactant added, a series of KCC-1 with different wrinkled structures can be obtained.

6. The method for preparing the wrinkled hierarchical porous SAPO-11 molecular sieve according to claim 1, characterized in that: The drying temperature in step S3 is 80~120℃, and the drying time is 24~48h; the calcination temperature is 500~650℃, and the calcination time is 4~8h.

7. A catalyst for the hydroisomerization of alkane, characterized in that: The catalyst is prepared by loading the active metal component Pt onto a wrinkled hierarchical porous SAPO-11 molecular sieve obtained by any one of claims 1 to 6. This catalyst can effectively promote the generation and diffusion of isomer intermediates, reduce the occurrence of cracking side reactions, and significantly improve the catalytic activity and isomer yield of alkane isomerization.

8. The alkane hydroisomerization catalyst according to claim 7, characterized in that: The loading of the active metal component Pt in the alkane hydroisomerization catalyst is 0.1 wt.% to 0.6 wt.%.

9. The application of the wrinkled hierarchical porous SAPO-11 molecular sieve prepared by any one of claims 1 to 6 as a support for loading the active metal component Pt in the catalytic hydroisomerization reaction of alkane.

10. The application according to claim 9, characterized in that: The alkane hydroisomerization reaction specifically refers to the hydroisomerization reaction of n-decane, and the specific reaction conditions are: reaction temperature of 280~400℃, reaction pressure of 1.5~2.5MPa, and n-decane mass hourly space velocity of 1.0~40h⁻¹. -1 The volume ratio of hydrogen to n-decane is (200~600):1.

Citation Information

Patent Citations

  • Y / KCC-1 Mesoporous-Microporous Composite Molecular Sieve and Its Preparation, Hydrocracking Catalyst and Its Preparation and Application

    CN119500236B

  • Beta / KCC-1 mesoporous composite molecular sieve and its preparation, hydrocracking catalyst and its preparation and application

    CN119524922B