Oxygen-enriched vacancy cadmium sulfide quantum dot / tin oxide hollow microsphere gas sensitive material and preparation method and application thereof

By preparing oxygen-vacancy-rich cadmium sulfide/tin oxide hollow microsphere gas-sensitive materials, the problems of insufficient sensitivity and poor stability of SnO2 gas-sensitive materials in the detection of n-butanol were solved, achieving detection effects with high sensitivity, low temperature response and good selectivity.

CN123061997APending Publication Date: 2026-11-10SHANGHAI UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611080896.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing SnO2 gas-sensitive materials suffer from insufficient sensitivity, poor selectivity, large temperature drift interference, and poor long-term stability in n-butanol detection. Furthermore, the CdS quantum dot modification process has failed to achieve precise optimization and optimal matching of the material's gas-sensitive performance.

Method used

Nanocarbon sphere templates were prepared by hydrothermal method to form carbon sphere@tin oxide core-shell structure. After removing the carbon template by high-temperature calcination, cadmium sulfide quantum dots were loaded to construct oxygen-vacancy-rich cadmium sulfide/tin oxide hollow microsphere gas-sensitive materials. The electronic structure was optimized by DFT theoretical calculation.

Benefits of technology

The material exhibits high sensitivity, low-temperature response, good selectivity, and long-term stability, significantly improving the detection performance of n-butanol with a response value of 385 and excellent long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061997A_ABST
    Figure CN123061997A_ABST
Patent Text Reader

Abstract

The application relates to an oxygen-enriched-vacancy cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material and a preparation method and application thereof, and belongs to the technical field of semiconductor gas-sensitive material preparation. The method is to combine liquid deposition to form a heterojunction by synthesizing hollow SnO2 nano microspheres through a carbon template method. The successful construction of the CdS / SnO2 heterojunction is systematically verified through a series of characterization means. The variation law of differential charge density distribution and oxygen atom adsorption energy is revealed through theoretical calculation, and the essential reason for the performance optimization of the material is clarified in combination with a gas-sensitive sensing mechanism. Through the deep coupling of material design and mechanism research, a practical potential n-butanol sensing material is developed, and a new research strategy is provided for the research and development of similar gas-sensitive materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor gas-sensitive material preparation technology, specifically to a cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material rich in oxygen vacancies, its preparation method, and its application. Background Technology

[0002] Real-time monitoring of volatile organic compounds (VOCs) is of great significance in environmental safety, industrial production, and health protection. Among them, n-butanol, a commonly used industrial solvent, is flammable and irritating to humans; long-term exposure can easily cause respiratory damage. Rapid and sensitive detection of n-butanol is crucial for safe production and environmental remediation. Metal-oxide-semiconductor (MOS) gas sensors are widely used in VOCs detection due to their advantages such as rapid response, low cost, and simple structure. Tin oxide (SnO2), as a classic n-type semiconductor material, possesses advantages such as good chemical stability and high sensitivity, making it an important research subject for gas-sensitive materials.

[0003] However, pure SnO2 gas-sensitive materials suffer from problems such as high operating temperature, poor selectivity, insufficient surface active sites, and low oxygen vacancy defect content, limiting their practical applications. To improve the gas-sensitive performance of SnO2, existing research mainly employs modification strategies such as morphology control, elemental doping, and heterostructure construction. Quantum dots (QDs), as zero-dimensional semiconductor materials, possess size effects, high specific surface area, abundant surface defects, and tunable band structures, making them ideal modification materials for enhancing the gas-sensitive performance of MOS devices. Among them, cadmium sulfide (CdS) has a narrow quantum band gap, high electron mobility, and energy level matching with SnO2, enabling the formation of n-node heterojunctions. This effectively controls the interface electron distribution, increases oxygen vacancy defects, reduces the material band gap, and improves electron transition efficiency, thereby significantly enhancing the material's response performance to VOCs. Sao et al. prepared CdS-SnO2 composite films by colloidal deposition, which showed an ultra-high response to 10 ppm nitrogen dioxide at a low temperature of 90℃, with a response value as high as 2800. The excellent performance was attributed to the construction of the n-nanocomposite thin film and the increase of oxygen vacancies (Sao AK, Sharma A, Verma M, et al. Development of CdS-SnO2 hybridnanocomposite thin films for trace level detection of NO2 gas[J]. Sensors and Actuators B:Chemical,2023,392:134198). Wang et al. prepared a SnO2 hollow cubic structure assembled from ultrathin nanorods. After modification with CdS quantum dots, the response value to 100 ppm n-butanol reached 320 at 240℃. The narrow bandgap effect promoted electronic transitions and significantly improved the sensing sensitivity (Wang Y, Zeng Y, Wang L, et al. Ultrathin nanorod-assembled SnO2 hollow cubes for high sensitive n-butanol detection[J]. Sensors and Actuators B: Chemical, 2019, 283: 693-704). In summary, through reasonable structural design and composition modification, the comprehensive performance of SnO2 gas-sensitive materials has been significantly improved.

[0004] Currently, preliminary progress has been made in the research of CdS quantum dot-modified SnO2-based gas-sensitive materials, which can effectively improve the inherent defects of single SnO2 materials such as low gas-sensing responsivity and poor selectivity. However, existing research still faces several key technical bottlenecks, failing to achieve precise optimization and optimal matching of the material's gas-sensing performance. Regarding quantum dot loading control, existing studies mostly use empirical loading ratios to prepare modified materials, and the quantitative correlation between CdS quantum dot loading and the specific surface area, number of active sites, and carrier transport efficiency of SnO2 hollow microspheres has not yet been clarified. At the interface structure control level, the bonding mode, contact tightness, and control mechanism of the interface charge transfer channel between CdS and SnO2 heterojunctions are still unclear. Most modification processes only achieve simple physical recombination, failing to construct stable and efficient covalently bonded heterojunctions, resulting in severe interface charge recombination losses and high charge transport resistance, significantly reducing the material's gas-sensing response speed and recovery characteristics. At the level of defect regulation mechanism, existing studies have not clarified the types, concentrations and distribution patterns of defects such as oxygen vacancies and lattice defects induced by CdS quantum dot modification in SnO2 hollow microspheres. This makes it impossible to achieve precise and controllable construction of surface defects, and difficult to optimize the gas adsorption and activation capacity and electron transport performance of material surfaces through defect engineering. It also fails to address practical problems such as insufficient sensitivity, large temperature drift interference and poor long-term stability in the detection of n-butanol VOCs. Summary of the Invention

[0005] To address at least one of the practical problems in existing n-butanol VOCs detection methods, such as insufficient sensitivity, large temperature drift interference, and poor long-term stability, this invention provides an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material, its preparation method, and its application. This invention relies on a precise modification strategy of CdS quantum dots to directionally control the surface defect state and electronic band structure of SnO2 hollow microspheres, constructing a highly stable and highly active heterojunction gas-sensitive material. This has significant theoretical research value and engineering application value for achieving high-precision, rapid, and stable detection of VOCs gases such as n-butanol.

[0006] This invention uses urea as a carbon source and prepares carbon nanospheres as templates via a hydrothermal method. Sodium stannate is then used as a tin source, and a tin oxide precursor is uniformly coated onto the surface of the carbon nanospheres via a hydrothermal reaction, forming a carbon nanosphere@tin oxide core-shell structure. Subsequently, the carbon template is removed by high-temperature calcination, yielding SnO2 hollow microspheres with a high specific surface area. Cadmium sulfide (CdS) quantum dots are then uniformly loaded onto the surface of the SnO2 hollow microspheres via a simple hydrothermal method, ultimately obtaining an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material (CdS / SnO2). The quantum dot loading of the CdS / SnO2 hollow microsphere gas-sensitive material prepared by this invention significantly reduces the band gap of the composite material and increases the number of oxygen vacancy defects on its surface, resulting in a greater number of electron transitions during the gas-sensitive reaction and greatly improving the efficiency of the gas-sensitive reaction. Furthermore, the formation of a heterojunction between CdS quantum dots and SnO2 effectively improves electron transfer at the composite material interface, broadens the electron depletion layer, and enhances the detection sensitivity of the composite material for the target gas. Simultaneously, DFT calculations further confirm that the surface charge density of the material increases after CdS quantum dot compositing, leading to increased adsorption energy for oxygen atoms and thus improving the detection sensitivity of the composite material for the target gas. The method of this invention features a simple and mild preparation process, combining template-based hollow structure construction with quantum dot surface modification to simultaneously optimize the material's microstructure and regulate its electronic structure. The oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material prepared by this method for n-butanol detection exhibits advantages such as low operating temperature, high sensitivity, good selectivity, and strong long-term stability.

[0007] The objective of this invention can be achieved through the following technical solutions: One objective of this invention is to provide a method for preparing oxygen-vacant cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material, comprising the following steps: a. Place urea, sodium stannate, and carbon ball template in an ethanol-water solution and ultrasonically stir to obtain a uniformly dispersed mixed solution of carbon ball template; b. Transfer the mixed solution obtained in step a to a high-pressure reactor and heat it to react; c. After the reaction is complete, allow it to cool naturally, separate the black solid by centrifugation, wash and dry to obtain carbon sphere / tin oxide precursor material; d. After grinding the carbon ball / tin oxide precursor material obtained in step c evenly, place it in a crucible and calcine it in a muffle furnace to remove the carbon ball template. After calcination, allow it to cool naturally to room temperature to obtain tin oxide hollow microspheres (SnO2). e. Disperse the tin oxide hollow microspheres obtained in step d in an anhydrous ethanol solution of cadmium acetate, stir, filter and wash to obtain an intermediate tin oxide hollow microsphere loaded with cadmium ions; f. The intermediate obtained in step e is dispersed in an anhydrous ethanol solution of sodium sulfide, stirred and reacted. After the solution turns yellow, it is washed, filtered, and dried to obtain oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere composite gas-sensitive material (CdS / SnO2).

[0008] Furthermore, in step a, at least one of the following conditions is satisfied: (1) The dosage relationship between urea, sodium stannate and carbon ball template is (1.500~3.500 g): (0.100~0.500 g):0.120 g; (2) In the aqueous ethanol solution, the volume ratio (V / V) of ethanol to water is (1:1)~(1:3); (3) The duration of ultrasound was 0.5~1.5 h; (4) The stirring time is 20~40 min.

[0009] Furthermore, in step b, at least one of the following conditions must be met: (1) The temperature for heating the reaction is 150~190℃; (2) The reaction time for the heating reaction is 24~48 h; (3) The high-pressure reactor is a high-pressure reactor with a polytetrafluoroethylene liner.

[0010] Furthermore, in step c, at least one of the following conditions is satisfied: (1) The centrifugation speed is 6000~10000 rpm, and the centrifugation time is 3~5 min; (2) Washing and drying: Wash with anhydrous ethanol 3 to 5 times, put the obtained solid product into a vacuum oven to dry at a temperature of 50 to 70°C for 5 to 8 hours.

[0011] Furthermore, in step d, the muffle furnace calcination conditions are as follows: the temperature is increased to 300-500℃ at a rate of 2-8℃ / min, and calcined at this temperature for 3-9 h.

[0012] Furthermore, in step e, at least one of the following conditions is satisfied: (1) The ratio of SnO2, cadmium acetate, and anhydrous ethanol solution is 0.1 g : 0.4 g : (10~30 mL); (2) The stirring rate is 300~700 r / min, and the stirring time is 50~150 s; (3) Wash with methanol 1 to 3 times.

[0013] Furthermore, in step f, at least one of the following conditions is satisfied: (1) The concentration of sodium sulfide in the anhydrous ethanol solution of sodium sulfide is 0.05~0.20 mol / L, and the solution volume is 10~30 mL; (2) The stirring reaction rate is 300~700 r / min, and the stirring time is 100~300 s; (3) Wash with methanol 1 to 3 times; (4) The drying temperature is 40~80℃ and the drying time is 7~12 h.

[0014] The second objective of this invention is to provide an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material, characterized in that it is prepared by the method described above.

[0015] The third objective of this invention is the application of a gas-sensitive material containing oxygen-vacancy-rich cadmium sulfide quantum dots / tin oxide hollow microspheres as described above. This gas-sensitive material is used as a gas sensor device for detecting volatile organic gases and is suitable for detecting trace gases in complex environments. The volatile organic gases include, but are not limited to, n-butanol, methanol, ethanol, or ethylene glycol.

[0016] Compared with the prior art, the present invention has the following advantages: (1) The present invention adopts a preparation process combining hard template method and liquid phase deposition method. The whole process is mild, simple and highly controllable. First, SnO2 hollow microspheres are synthesized using carbon spheres as templates, and then CdS quanta are loaded by room temperature liquid phase deposition method. No high temperature, high pressure or complex equipment is required. The process has good repeatability and is easy to scale up.

[0017] (2) This invention achieves controllable gradient of CdS quantum dot loading by adjusting the concentration of cadmium acetate precursor. Two groups of samples were prepared, one with optimal loading SnO2 / CdS-2 and the other with excessive loading SnO2 / CdS-3. The microscopic differences caused by different loading were intuitively distinguished by TEM, XRD, BET and XPS characterization. At the same time, the gas-sensing performance changes were corresponded to the CdS quantum dot loading in the optimal range, taking into account high specific surface area, sufficient heterogeneous interface and high oxygen vacancy concentration.

[0018] (3) The present invention employs a two-step room temperature liquid phase deposition method, first adsorbing Cd 2+ In-situ generation of CdS quantum dots was then used to achieve a tightly bonded heterointerface between CdS and SnO2. HRTEM lattice fringe patterns confirmed the formation of a continuous and complete SnO2 / CdS heterointerface. UV-Vis diffuse reflectance spectroscopy demonstrated that the heterointerface synergistically reduced the band gap, significantly lowered the electronic transition energy barrier, and improved the carrier migration rate during the gas-sensitive reaction. (4) The CdS quantum dot modification method of the present invention can simultaneously induce a large number of oxygen vacancy defects on SnO2 substrate, and a large number of active adsorbed oxygen sites promote the redox reaction of n-butanol, and finally achieve an ultra-high response value of 385 under the conditions of 240℃ and 100 ppm n-butanol. Attached Figure Description

[0019] Figure 1 This is a high-resolution transmission electron microscope (HRTEM) image of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of the present invention. Figure 2 The images show the lattice fringe pattern, high-resolution transmission electron microscopy (HRTEM) image, and energy dispersive spectroscopy (EDS) image of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of this invention. Figure 3 The high-resolution X-ray photoelectron spectroscopy (XPS) spectrum of the oxygen 1s orbital (XPS O 1s) of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of this invention is shown below. Figure 4 The diagram shows the concentration response characteristics of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of this invention to different concentrations of n-butanol at 240°C. Figure 5 The selectivity test diagram of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of the present invention for n-butanol under the condition of 100 ppm mixed gas is shown. Figure 6 This is a stability test diagram of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of the present invention against 100 ppm n-butanol gas. Figure 7 This is a differential charge diagram of the heterostructure of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of the present invention. Detailed Implementation

[0020] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0021] Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this invention. Unless otherwise specified, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0022] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0023] This invention provides a method for preparing oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive materials, comprising the following steps: a. Place urea, sodium stannate, and carbon ball template in an ethanol-water solution and ultrasonically stir to obtain a uniformly dispersed mixed solution of carbon ball template; b. Transfer the mixed solution obtained in step a to a high-pressure reactor and heat it to react; c. After the reaction is complete, allow it to cool naturally, separate the black solid by centrifugation, wash and dry to obtain carbon sphere / tin oxide precursor material; d. After grinding the carbon ball / tin oxide precursor material obtained in step c evenly, place it in a crucible and calcine it in a muffle furnace to remove the carbon ball template. After calcination, allow it to cool naturally to room temperature to obtain tin oxide hollow microspheres (SnO2). e. Disperse the tin oxide hollow microspheres obtained in step d in an anhydrous ethanol solution of cadmium acetate, stir, filter and wash to obtain an intermediate tin oxide hollow microsphere loaded with cadmium ions; f. The intermediate obtained in step e is dispersed in an anhydrous ethanol solution of sodium sulfide, stirred and reacted. After the solution turns yellow, it is washed, filtered, and dried to obtain oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere composite gas-sensitive material (CdS / SnO2).

[0024] In step a of some embodiments of the present invention, at least one of the following conditions is satisfied: (1) The ratio of urea, sodium stannate and carbon sphere template is (1.500~3.500 g): (0.100~0.500 g): 0.120 g; urea is used as a hydrolysis-release alkali source, and if the amount is too low, the system OH -Insufficient supply leads to incomplete hydrolysis of sodium stannate, resulting in a thin and discontinuous Sn(OH)4 coating on the carbon sphere surface. After calcination, the hollow sphere shell is incomplete, with a significant loss of pores. Excessive urea usage rapidly generates large amounts of tin hydroxide precipitates, which detach from the carbon template and aggregate freely, preventing the formation of the core-shell precursor. When sodium stannate usage is below 0.100 g, the tin precursor coating on the carbon sphere surface is too thin, making the SnO2 shell prone to collapse and breakage after high-temperature decarburization. When sodium stannate usage exceeds 0.500 g, the coating is too thick, leading to densification of the microsphere shell after calcination, a significant decrease in specific surface area, blockage of internal gas diffusion channels, and reduced gas-sensitive activity. Fixing the carbon template at 0.120 g as a supporting framework, the synergistic ratio of the three raw materials yields a carbon@Sn(OH)4 core-shell precursor with uniform shell thickness and a complete structure, laying the structural foundation for the subsequent preparation of porous hollow SnO2 microspheres.

[0025] (2) In the ethanol-water solution, the volume ratio (V / V) of ethanol to water is (1:1) to (1:3). Water is the ionization medium for tin source hydrolysis. Ethanol can reduce solvent polarity, slow down the instantaneous precipitation of Sn(OH)4, and inhibit random particle aggregation. If the proportion of ethanol is too high (i.e., less than 1:1), the solvent polarity is too low, the hydrolysis of tin ions is hindered, the coating reaction is slow, and the coating of carbon spheres is uneven. If the proportion of ethanol is too low (i.e., greater than 1:3), the system polarity is too strong, a large amount of tin hydroxide is precipitated instantaneously, the free precipitation increases, a large amount of Sn(OH)4 detaches from the carbon template, and cannot uniformly coat to form a core-shell structure. It can be seen that when the volume ratio of ethanol to water is in the range of 1:1 to 1:3, the hydrolysis rate and particle dispersion can be balanced, so that the tin precursor can uniformly and completely coat the carbon spheres, and a core-shell precursor with uniform morphology can be obtained.

[0026] (3) The ultrasonic time is 0.5~1.5 h. The purpose of ultrasonication is to break up the carbon ball agglomerates and achieve uniform dispersion of carbon template in alcohol-water system, so as to ensure that tin precursor synchronously coats all carbon balls. If the ultrasonic time is less than 0.5 h, the carbon balls will stack and agglomerate, and some carbon particles will not be able to contact the tin source, resulting in a large difference in coating thickness. If the ultrasonic time exceeds 1.5 h, the long-term ultrasonic impact will destroy the carbon ball skeleton, the template will break, and ultimately it will be impossible to form complete hollow microspheres.

[0027] (4) The stirring time is 20-40 min. If the stirring time is less than 20 min, the sodium stannate, urea and carbon balls will be mixed unevenly, the local metal ion concentration will be unbalanced and the coating will be uneven; if the stirring time exceeds 40 min, the continuous fluid shear force will peel off the thin layer of nascent tin hydroxide on the surface of the carbon balls, resulting in a defective shell. This range can achieve complete dispersion of carbon balls and uniform mixing of all components, ensuring that the subsequent coating process is carried out synchronously.

[0028] In step b of some embodiments of the present invention, at least one of the following conditions is satisfied: (1) The heating reaction temperature is 150~190℃ and the reaction time is 24~48 h, which is suitable for the slow hydrolysis deposition of tin source on the carbon template surface and the complete growth of Sn(OH)4 shell. When the temperature is below 150℃ and the time is less than 24 h, the activation energy of the hydrolysis reaction is insufficient, the growth rate of tin hydroxide is extremely slow, the coating layer on the surface of carbon spheres is thin and the crystallinity is poor, and the hollow spheres are prone to collapse after calcination; when the temperature is above 190℃ and the reaction time exceeds 48 h, the hydrolysis rate is too fast, a large amount of tin hydroxide is released, and the maturation is intensified, the shell grains are coarse, the porosity disappears, and the specific surface area of ​​the material is sharply reduced. The range of 150~190℃ and 24~48 h can realize the uniform growth of tin precursor on the carbon template surface layer by layer, forming a continuous core-shell precursor with appropriate thickness, which provides an ideal precursor framework for porous hollow SnO2 microspheres after calcination.

[0029] (3) The high-pressure reactor is a high-pressure reactor with a polytetrafluoroethylene liner.

[0030] In step c of some embodiments of the present invention, at least one of the following conditions is satisfied: (1) The centrifugation speed is 6000~10000 rpm, and the centrifugation time is 3~5 min; (2) Washing and drying: Wash with anhydrous ethanol 3 to 5 times, put the obtained solid product into a vacuum oven to dry at a temperature of 50 to 70°C for 5 to 8 hours.

[0031] In step d of some embodiments of the present invention, the muffle furnace calcination conditions are as follows: heating to 300-500°C at a rate of 2-8°C / min, and calcining at this temperature for 3-9 hours. This synergistically achieves complete thermal decomposition of the carbon template, transformation of the Sn(OH)4 crystalline phase into porous SnO2, and maintenance of the integrity of the hollow microsphere framework. A heating rate below 2°C / min results in excessive time consumption and low production efficiency; a heating rate above 8°C causes the carbon template to decompose rapidly, releasing a large amount of gas that breaks through the uncured SnO2 shell, shattering the hollow structure. Calcination temperatures below 300°C and holding times less than 3 hours result in incomplete carbon template decomposition, residual carbon impurities clogging the pores, and insufficient decrystallization of tin hydroxide, leading to low crystallinity and scarce oxygen vacancies. Calcination temperatures above 500°C and holding times exceeding 9 hours cause high-temperature sintering and growth of SnO2 grains, mesopore collapse, densification of the hollow sphere shell, a significant decrease in specific surface area, and annihilation of oxygen vacancies, weakening the subsequent CdS quantum dot loading sites and gas-sensitive activity. The carbon template can be completely removed at 300~500℃ for 3~9 h, generating porous, defect-rich hollow SnO2 microspheres.

[0032] In step e of some embodiments of the present invention, at least one of the following conditions is satisfied: (1) The ratio of SnO2, cadmium acetate, and anhydrous ethanol solution is 0.1 g : 0.1~1.0 g : (10~30 mL); 10~30 mL of ethanol solvent can fully disperse the hollow microspheres and avoid particle agglomeration; if the ethanol is less than 10 mL, the powder concentration is too high, SnO2 will stack, and Cd will... 2+ Only the outer layer of microspheres is adsorbed; when ethanol exceeds 30 mL, Cd 2+ If the concentration is too low, the quantum dot loading will be insufficient, resulting in a sparse number of heterojunctions. Fixing with 0.4 g of cadmium acetate can ensure the optimal loading ratio of CdS quantum dots for subsequent application.

[0033] (2) The stirring rate is 300~700 r / min, and the stirring time is 50~150 s; (3) Wash with methanol 1 to 3 times.

[0034] In step f of some embodiments of the present invention, at least one of the following conditions is satisfied: (1) The concentration of sodium sulfide in the anhydrous ethanol solution is 0.05~0.20 mol / L, and the solution volume is 10~30 mL. When the concentration is below 0.05 mol / L, the Cd source is insufficient, the quantum dots are sparse, the number of n heterojunctions is small, and the oxygen vacancy enhancement is limited. When the concentration is above 0.20 mol / L, a large number of CdS nucleates instantaneously in local areas, resulting in quantum agglomeration, grain growth, loss of quantum confinement effect, and blockage of SnO2 mesoporous channels. 10~30 mL of solvent can achieve complete dispersion of hollow microspheres and ensure uniform loading of quantum dots throughout the entire domain.

[0035] (2) The stirring reaction rate is 300~700 r / min, and the stirring time is 100~300 s; (3) Wash with methanol 1 to 3 times; (4) The drying temperature is 40~80℃ and the drying time is 7~12 h.

[0036] Example 1 This embodiment provides a method for preparing oxygen-vacant cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material, including the following steps: a. Weigh 2.572 g of urea, 0.300 g of sodium stannate, and 0.120 g of carbon sphere template sequentially and place them into 80 mL of a mixed solution of ethanol and water. Sonicate for 1 h and stir for 30 min to obtain a uniformly dispersed mixed solution of carbon sphere template. The preparation method of the carbon ball template is as follows: 9.3g of sucrose is dissolved in 200 mL of deionized water, 0.05g of NaOH is added, and the mixture is stirred for 1 h. 80 mL of the solution is taken and transferred to a 100 mL polytetrafluoroethylene-lined reactor. The mixture is hydrothermally reacted at 180℃ for 12 h. The product is washed three times by centrifugation with deionized water and dried overnight at 60℃. The dried black solid is then thoroughly ground to obtain the carbon ball template. In a mixed solution of ethanol and water, the volume ratio of ethanol to water is 1:2. b. Transfer the mixed solution obtained in step a to a 100 ml high-pressure reactor and hydrothermally heat it at 170 °C for 36 h; c. After the reaction is complete, allow it to cool naturally, separate the black solid by centrifugation, wash and dry with ethanol solution to obtain carbon sphere / tin oxide precursor material; wherein, the centrifugation speed is 6000~10000 rpm, the centrifugation time is 3~5 min; the washing and drying are as follows: wash with anhydrous ethanol 3~5 times, and place the obtained solid product in a vacuum oven to dry at a temperature of 50~70℃ for 5~8 h.

[0037] d. After grinding the carbon ball / tin oxide precursor material obtained in step c evenly, place it in a crucible, put it in a muffle furnace, heat it to 400°C at a rate of 5°C / min in an air atmosphere, and keep it at this temperature for 6 h to remove the carbon ball template. After calcination, let it cool naturally to room temperature to obtain tin oxide hollow microspheres. e. Weigh 0.1 g of the hollow tin oxide microspheres obtained in step d and disperse them in 20 ml of anhydrous cadmium acetate solution. After stirring, filter and wash to obtain the cadmium ion-loaded hollow tin oxide microsphere intermediate. The concentration of cadmium acetate in the anhydrous cadmium acetate solution is 0.075 mol / L. The stirring rate is 300~700 r / min and the stirring time is 50~150 s. Washing is performed 1~3 times with methanol.

[0038] f. Disperse the intermediate obtained in step e in 20 ml of anhydrous ethanol solution of sodium sulfide, stir for 180 s, and after the solution turns yellow, wash with methanol solution, filter, and dry to obtain oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere composite gas-sensitive material; wherein, the concentration of sodium sulfide in the anhydrous ethanol solution of sodium sulfide is 0.1 mol / L; the stirring rate is 300~700 r / min, the stirring time is 100~300 s; washing is performed with methanol 1~3 times; the drying temperature is 40~80℃, and the drying time is 7~12 h.

[0039] To verify the successful synthesis of the cadmium sulfide (CdS) quantum dot modified tin oxide (SnO2) hollow microsphere composite gas-sensitive material in this invention, its morphology and composition were characterized.

[0040] Figure 1 The high-resolution transmission electron microscope (HRTEM) image of the CdS / SnO2 composite gas-sensitive material confirms that the material is composed of hollow microspheres with uniformly loaded quantum dots on the surface. This hollow structure has both a high specific surface area and open gas diffusion channels, which is beneficial to the adsorption and diffusion of target gas during the gas sensing process.

[0041] Figure 2 The images show the lattice fringes, high-resolution transmission electron microscopy (HRTEM) image, and energy dispersive spectroscopy (EDS) image of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of this invention. Analysis of the lattice fringes revealed the formation of a tin oxide / cadmium sulfide heterojunction on the tin oxide surface, which promotes electron transfer and electronic structure rearrangement, facilitating the gas-sensitive reaction. The images also show a uniform distribution of Sn, O, Cd, and S elements on the sample surface, confirming the successful synthesis of the CdS / SnO2 composite gas-sensitive material.

[0042] Figure 3 The image shows the high-resolution X-ray photoelectron spectroscopy (XPS) spectrum of the oxygen 1s orbital (O 1s) of the CdS / SnO2 composite gas-sensitive material prepared in Example 1 of this invention. The suitable composite ratio of CdS / SnO2 results in a high specific surface area and numerous surface oxygen vacancies. Analysis revealed that the oxygen vacancy content of the CdS / SnO2 composite gas-sensitive material is 22%, which is one of the reasons why the sensor prepared from this sample exhibits the highest gas-sensing performance. Application Example 1 To verify the gas-sensing performance of the CdS / SnO2 composite gas-sensing material obtained in Example 1, this application example fabricated a gas sensor device, including the following steps: Add 4 mg of the CdS / SnO2 composite gas-sensitive material obtained in Example 1 to an agate mortar, add an appropriate amount of ethanol, grind evenly and mix into a paste. Apply the paste evenly to the surface of an Al2O3 ceramic tube with a spatula to form a sensitive film of suitable thickness. Transfer the coated ceramic tube to a 60°C forced-air drying oven and dry for 2 hours. Then, use a soldering iron to solder the Pt wires at both ends of the ceramic tube to a metal base. Finally, pass a heating wire through the ceramic tube and solder it in place to complete the fabrication of the gas sensor device.

[0043] Gas-sensing performance testing The prepared device was inserted into the test circuit board and aged at 300℃ for 48 hours on an aging bench. Then, testing was conducted using the WS-30A gas-sensitive testing system. The testing system reflects the resistive characteristics of the gas-sensitive element by measuring the voltage change across a load resistor connected in series with it. During testing, the circuit board was first inserted, the load resistor was selected, the power was turned on, and the measurement and heating voltages were set. After the element's resistance in air stabilized, the gas distribution chamber was closed. The n-butanol liquid to be tested was injected into the evaporator, and the evaporator and fan were turned on to ensure uniform gas diffusion. After the voltage stabilized, the chamber door was opened, the gas dissipated, and the voltage returned to its initial level, completing one test cycle.

[0044] Test results: Figure 4 The response curves of CdS / SnO2 to different concentrations of n-butanol at 240℃ are shown. The material responds well to n-butanol in the range of 300 ppb to 100 ppm, and the response value increases with increasing concentration. Figure 5 The selectivity of CdS / SnO2 to a 100 ppm mixed gas at 240℃ was tested, and its response to n-butanol was significantly higher than that to interfering gases such as ethanol and acetone. Figure 6 For the long-term stability test of CdS / SnO2 against 100 ppm n-butanol, the initial response value reached 385 at 240℃, and the response fluctuation was less than 20% after 35 days, indicating that the sensor has excellent sensitivity, selectivity and long-term stability.

[0045] Figure 7 The differential charge diagram for the CdS / SnO2 heterostructure is shown. Yellow represents increased charge density, and blue represents decreased charge density. It can be seen that at the cadmium sulfide-tin oxide heterostructure interface, the tin oxide side is blue, while the cadmium sulfide side is yellow. This indicates that the charge density increases on the cadmium sulfide side and decreases on the tin oxide side, with electrons transferring from the tin oxide side to the cadmium sulfide side. This results in a higher charge density on the cadmium sulfide surface, which is beneficial for increasing the surface depletion layer and facilitating gas-sensitive reactions. The theoretical calculations above reveal, at the atomic scale, the interfacial charge transfer mechanism of the SnO2-CdS heterostructure and its regulatory effect on gas-sensitive performance: 1. Compared to a pure tin oxide surface, the cadmium sulfide / tin oxide composite structure is more conducive to oxygen atom adsorption, which will benefit the adsorption of oxygen species on the material surface. 2. The heterostructure interface induces electron migration from SnO2 to CdS, increasing the surface charge density of the composite material, which also benefits the adsorption of surface oxygen species and the gas-sensitive reaction. The charge redistribution resulting from the recombination of cadmium sulfide quantum dots optimizes the surface depletion layer and charge density, which is beneficial for improving the response to n-butanol.

[0046] Example 2 The process of this embodiment is basically the same as that of Embodiment 1, except that in step e, the concentration of cadmium acetate in the anhydrous ethanol solution of cadmium acetate is 0.15 mol / L.

[0047] Application Example 2 To verify the gas-sensing performance of the CdS / SnO2 composite gas-sensitive material obtained in Example 2, a gas sensor device was fabricated in this application example. The fabrication and performance testing process of the gas sensor device were the same as in Application Example 1. The CdS / SnO2 composite gas-sensitive material prepared using the process described in this application example was tested for gas-sensing performance, exhibiting excellent gas-sensing properties. The test results show that the response of CdS / SnO2 to different concentrations of n-butanol at 240℃ increases with increasing concentration. In the test of a mixed gas of 100 ppm at 240℃, the material's response to n-butanol was significantly higher than its response to other gases, indicating that it has excellent selectivity for n-butanol.

[0048] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material, characterized in that, Includes the following steps: a. Place urea, sodium stannate, and carbon ball template in an ethanol-water solution and ultrasonically stir to obtain a uniformly dispersed mixed solution of carbon ball template; b. Transfer the mixed solution obtained in step a to a high-pressure reactor and heat it to react; c. After the reaction is complete, allow it to cool naturally, separate the black solid by centrifugation, wash and dry to obtain carbon sphere / tin oxide precursor material; d. After grinding the carbon ball / tin oxide precursor material obtained in step c evenly, place it in a crucible and calcine it in a muffle furnace to remove the carbon ball template. After calcination, allow it to cool naturally to room temperature to obtain tin oxide hollow microspheres. e. Disperse the tin oxide hollow microspheres obtained in step d in an anhydrous ethanol solution of cadmium acetate, stir, filter and wash to obtain an intermediate of tin oxide hollow microspheres loaded with cadmium ions; f. The intermediate obtained in step e is dispersed in an anhydrous ethanol solution of sodium sulfide, stirred and reacted. After the solution turns yellow, it is washed, filtered, and dried to obtain a cadmium sulfide quantum dot / tin oxide hollow microsphere composite gas-sensitive material with oxygen-vacancy sites.

2. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step a, at least one of the following conditions must be met: (1) The dosage relationship between urea, sodium stannate and carbon ball template is (1.500~3.500 g): (0.100~0.500 g):0.120 g; (2) In the aqueous ethanol solution, the volume ratio (V / V) of ethanol to water is (1:1)~(1:3); (3) The duration of ultrasound was 0.5~1.5 h; (4) The stirring time is 20~40 min.

3. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step b, at least one of the following conditions must be met: (1) The temperature for heating the reaction is 150~190℃; (2) The reaction time for the heating reaction is 24~48 h; (3) The high-pressure reactor is a high-pressure reactor with a polytetrafluoroethylene liner.

4. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step c, at least one of the following conditions must be met: (1) The centrifugation speed is 6000~10000 rpm, and the centrifugation time is 3~5 min; (2) Washing and drying: Wash with anhydrous ethanol 3 to 5 times, put the obtained solid product into a vacuum oven to dry at a temperature of 50 to 70°C for 5 to 8 hours.

5. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step d, the muffle furnace calcination conditions are as follows: the temperature is increased to 300-500℃ at a rate of 2~8℃ / min, and calcined at this temperature for 3~9 h.

6. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step e, at least one of the following conditions must be met: (1) The ratio of the amounts of tin oxide hollow microspheres, cadmium acetate, and anhydrous ethanol solution is 0.1g:(0.1~1.0g):(10~30mL); (2) The stirring rate is 300~700 r / min, and the stirring time is 50~150 s; (3) Wash with methanol 1 to 3 times.

7. The method for preparing an oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material according to claim 1, characterized in that, In step f, at least one of the following conditions must be met: (1) The concentration of sodium sulfide in the anhydrous ethanol solution of sodium sulfide is 0.05~0.20 mol / L, and the solution volume is 10~30mL; (2) The stirring reaction rate is 300~700 r / min, and the stirring time is 100~300 s; (3) Wash with methanol 1 to 3 times; (4) The drying temperature is 40~80℃ and the drying time is 7~12 h.

8. A cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material rich in oxygen vacancies, characterized in that, It is prepared by the preparation method described in any one of claims 1-7.

9. An application of the oxygen-vacancy-rich cadmium sulfide quantum dot / tin oxide hollow microsphere gas-sensitive material as described in claim 8, characterized in that, This gas-sensitive material is used in gas sensor devices to detect volatile organic gases.