Method for preparing high-purity gallium oxide by gallium extraction from bayer process mother liquor

By using LSC-600 chelating resin adsorption and enhanced water washing, the problems of high energy consumption and long process in the Bayer process for gallium extraction from mother liquor were solved, achieving efficient preparation of high-purity gallium oxide, reducing energy consumption and improving gallium recovery rate and product purity.

CN123061998APending Publication Date: 2026-11-10CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611565500.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies for gallium extraction from Bayer process mother liquor involve long processes, high energy consumption, low electrolysis efficiency, and significant gallium loss. Furthermore, the desorption process lacks selectivity for separating impurities such as aluminum, iron, and vanadium, which affects product purity.

Method used

LSC-600 chelating resin was used for dynamic adsorption, combined with enhanced water washing, acid desorption, iron removal and neutralization precipitation steps, and impurities were removed by pulping and washing to directly prepare high-purity gallium oxide, skipping the electrolysis process. The high selective adsorption characteristics and physical removal mechanism of chelating resin were utilized to reduce energy consumption and improve purity.

Benefits of technology

It achieves efficient preparation of high-purity gallium oxide, reduces overall energy consumption by more than 50%, achieves gallium recovery rate of 70%~75%, and product purity ≥99.9%. It simplifies the process flow and avoids the increase in energy consumption and gallium loss caused by electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061998A_ABST
    Figure CN123061998A_ABST
Patent Text Reader

Abstract

The application discloses a method for preparing high-purity gallium oxide by Bayer mother liquor gallium extraction, and the method comprises the following steps: after the Bayer seed mother liquor is pretreated by filtration, the gallium is adsorbed and enriched through an LSC-600 chelating resin adsorption column; 4-6 BV of deionized water is used to intensively wash the saturated resin; an acid solution is used to desorb the saturated resin after the intensive washing, so that a gallium-rich desorption solution is obtained, and the mass ratio of Al / Ga is less than 0.1; the pH of the gallium-rich desorption solution is adjusted to 2.5-3.5, so that Fe 3+ is precipitated and removed by filtration; the filtrate after the iron removal is adjusted to pH 7.0-8.0, so that the gallium and the trace amount of aluminum remaining in the solution are co-precipitated in the form of hydroxide; the co-precipitate is sufficiently pulped and washed by deionized water; after the washing, the precipitate is dried and calcined to obtain high-purity β-Ga2O3 product. The method has the advantages of short process, simple operation and low cost, and the purity of the obtained gallium oxide can reach more than 99.9%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydrometallurgy and rare dispersed metal extraction technology, specifically relating to a method for preparing high-purity gallium oxide from Bayer process mother liquor. Background Technology

[0002] Gallium is an important rare and dispersed metal widely used in semiconductors, optoelectronics, integrated circuits, 5G communications, and new energy fields. With the rapid development of the information industry and artificial intelligence technology, gallium's strategic importance as a core material for third- / fourth-generation semiconductors is increasingly prominent. Gallium typically does not form independent deposits in nature, but is mainly found as an associated mineral in bauxite, lead-zinc ore, and coal mines. The seed mother liquor from the Bayer process for alumina production is an important source of gallium, with a gallium content generally ranging from 0.1 to 0.3 g / L.

[0003] Currently, industrial methods for extracting gallium from Bayer process mother liquor mainly include chemical precipitation, solvent extraction, ion exchange, and electrochemical methods. Among these, ion exchange (resin adsorption) has become the mainstream industrial technology for gallium extraction due to its advantages such as high selectivity, short process, and no pollution to the main process. A typical ion exchange gallium extraction process is as follows: mother liquor → resin adsorption → water washing → desorption → impurity removal → electrolysis → metallic gallium. This method uses chelating resin to selectively adsorb gallium, then uses a desorbent to elute gallium from the resin, obtaining a gallium-rich desorbent solution, which is then purified and electrolyzed to obtain the metallic gallium product. However, existing technologies still have the following problems: (1) The end product of the traditional process is metallic gallium, which requires an electrolysis process. This process has high energy consumption and the electrolysis process requires high purity of the desorption solution. Impurities (especially vanadium) can cause electrode burns and reduce electrolysis capacity.

[0004] (2) When preparing gallium oxide from metallic gallium, the metallic gallium needs to be remelted and oxidized, which increases the additional energy consumption and gallium loss.

[0005] (3) In the process of removing impurities from the desorption solution, existing methods mostly use a single precipitation or extraction operation, which is not selective enough for separating coexisting impurities such as aluminum, iron, and vanadium, thus affecting the purity of the final product.

[0006] Therefore, developing a short-process method that can directly prepare high-purity gallium oxide from Bayer process mother liquor without electrolysis is of great significance for reducing energy consumption, reducing gallium loss, and simplifying the process. Summary of the Invention

[0007] The purpose of this invention is to provide a method for preparing high-purity gallium oxide by extracting gallium from mother liquor using the Bayer process, in order to solve the problems of long process flow, high energy consumption, low electrolysis efficiency, and large gallium loss in the prior art.

[0008] To achieve the above objectives, the present invention provides a method for preparing high-purity gallium oxide from Bayer process mother liquor, specifically comprising the following steps: (1) Raw material pretreatment: The seed mother liquor from the Bayer process of alumina production is filtered or pretreated by sedimentation to remove suspended solid particles and obtain pretreated mother liquor.

[0009] (2) Resin Adsorption: The pretreated mother liquor is dynamically adsorbed through an adsorption column packed with LSC-600 chelating resin, allowing gallium ions or gallium complex ions to be adsorbed onto the resin. The adsorbed mother liquor is returned to the seed mother liquor storage tank of the Bayer process production system, mixed with fresh mother liquor, and then used for alumina production. Since the LSC-600 chelating resin does not introduce new impurities into the mother liquor, the return of the adsorbed liquid to the main process does not affect the quality of alumina products or normal production. The LSC-600 chelating resin is a chelating resin with a amine oxime functional group on its backbone. The adsorption temperature is 25~45℃, and the influent flow rate is 2~10 BV / h. The adsorption endpoint is defined as the gallium concentration in the effluent reaching 5%~10% of the initial concentration. The single-column adsorption rate is approximately 85%~88%.

[0010] Preferably, the adsorption column adopts a dual-column series connection or an intermittent dynamic column flow method, and the bottom of the resin column is intermittently backflushed during the adsorption process to prevent resin layer blockage. When a dual-column series connection is used, the total adsorption rate can reach over 95%.

[0011] (3) Enhanced washing: The saturated resin is washed with water to remove the mother liquor entrained on the resin surface and in the pores. The washing water volume is 4-6 BV, and the washing flow rate is 1-3 BV / h. The washing endpoint is defined as the Al concentration in the effluent being below 50 mg / L, or by online conductivity monitoring, where the conductivity of the effluent drops to a stable low value, or by measuring the pH of the effluent, where the pH drops to 7-8, which is considered the washing endpoint. This invention significantly increases the water washing volume (traditionally 2-3 BV), thus fully removing impurities such as aluminum and sodium from the mother liquor entrained in the resin at the source. It should be noted that the LSC-600 amine oxime chelating resin has a high selective adsorption capacity for gallium, but a very low chemical adsorption capacity for aluminum. Therefore, the main source of aluminum impurities in the desorption solution is the mother liquor remaining in the resin pores, rather than the chelation adsorption of aluminum by the resin. The enhanced washing solution (effluent) is mainly composed of diluted sodium aluminate solution with extremely low gallium content (<5 mg / L), and can be combined with the post-adsorption solution and returned to the Bayer process system. Preferably, the washing solution is partially reused in the enhanced washing process of the next batch of resin after simple filtration to reduce the amount of fresh deionized water used.

[0012] (4) Acid desorption: The washed saturated resin is desorbed using an acidic desorbent, allowing the gallium adsorbed on the resin to enter the desorption solution, resulting in a gallium-rich desorption solution. The acidic desorbent is one or more of sulfuric acid, hydrochloric acid, or nitric acid, with an acid concentration of 0.1~3 mol / L. The desorption temperature is 0~30℃, and the desorption time is 20~60 min. Preferably, a two-stage desorption method is used, with the secondary desorption solution serving as the acid for the next cycle.

[0013] (5) Iron removal: Slowly add 1-4 mol / L NaOH solution to the gallium-rich desorption solution to adjust the pH to 2.5-3.5, so that Fe 3+ It precipitates as Fe(OH)3, and is removed by filtration after standing for 1-2 hours. Within this pH range, Al... 3+ and Ga 3+ Only trace amounts of precipitate remain in the filtrate.

[0014] (6) Neutralization and precipitation: Slowly add 1-4 mol / L NaOH solution to the filtrate after iron removal to adjust the pH to 7.0-8.0, so that gallium and trace amounts of residual aluminum in the solution co-precipitate as hydroxides. The precipitation temperature is room temperature to 50℃, and the aging time is 1-4 h. After solid-liquid separation, a mixed hydroxide precipitate is obtained.

[0015] (7) Slurry washing: The mixed hydroxide precipitate is thoroughly slurried and washed with deionized water. The precipitate and deionized water are mixed at a solid-liquid ratio of 1:3 to 1:5, stirred for 10 to 30 minutes, and then filtered. This process is repeated 3 to 5 times. The washing endpoint is when the Al concentration in the wash solution is below 10 mg / L and no SO4 is detected by BaCl2 solution. 2- (If using a sulfuric acid system) or using AgNO3 to detect the absence of Cl - (If a hydrochloric acid system is used). This step uses a pulping and washing method to thoroughly wash away soluble aluminates, sodium salts, and other impurities that were carried into the filter cake during co-precipitation. Since aluminum impurities are mainly carried in the form of soluble salts rather than existing in large quantities in the precipitate as Al(OH)3, pulping and washing can remove them efficiently. The pulping and washing liquid contains a small amount of soluble sodium salts (Na2SO4 or NaCl) and trace amounts of Al, Na, V, etc., which can be combined with the water washing liquid and returned to the Bayer process system. The accumulated salts are then discharged through the existing salt removal process of the Bayer process (such as evaporation and crystallization). Preferably, the final pulping and washing liquid is directly reused for the initial pulping and washing of the next batch of precipitate, further reducing the amount of fresh water used and wastewater discharged.

[0016] (8) Dry the washed precipitate at 80~120℃ for 2~6 h. Place the dried hydroxide in a muffle furnace, heat it to 700~800℃ at 5℃ / min, hold it at that temperature in air for 0.5~2 h, and then cool it to room temperature with the furnace to obtain a high-purity gallium oxide product. The high-purity gallium oxide product is of the β-Ga2O3 crystal form with a purity ≥99.9% (3N), and can be used as a high-purity raw material in the fields of semiconductor materials, optoelectronic materials, etc.

[0017] This invention addresses the problems of long process flow, high energy consumption, and low electrolysis efficiency in the existing Bayer process for gallium extraction from mother liquor, and provides a short-process method for preparing high-purity gallium oxide. This invention significantly reduces impurities such as aluminum and sodium entrained in the desorption solution by strengthening the water washing step. It utilizes the highly selective adsorption characteristics of gallium by a amine oxime chelating resin, combined with the physical removal mechanism of co-precipitated impurities through pulping and washing. While skipping the electrolysis step (avoiding electrode burn caused by vanadium and saving approximately 5%~10% of gallium oxide loss during smelting), the overall energy consumption is expected to be reduced by more than 50% compared to the traditional electrolysis-smelting route, with a total recovery rate of 70%~75%. The obtained β-Ga2O3 product has a purity ≥99.9%, and the aluminum-containing filtrate and washing liquid can be recycled back to the Bayer process system, achieving efficient recovery and high-value utilization of gallium resources. Attached Figure Description

[0018] Figure 1 This is a flowchart of the method for preparing high-purity gallium oxide from mother liquor using the Bayer process, as described in this invention. Detailed Implementation

[0019] The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that the following embodiments are only used to illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention.

[0020] Example 1 A mother liquor from the Bayer process of an alumina plant was used as raw material. The mother liquor contained 252 mg / L gallium, 170 g / L caustic soda, and 90 g / L Al₂O₃. The mother liquor was pretreated by pressure filtration to remove suspended solids before use. 500 mL of LSC-600 chelating resin was packed into an ion exchange column (3 cm inner diameter, 12:1 height-to-diameter ratio). The pretreated mother liquor was passed through the resin column at a flow rate of 4 BV / h for dynamic adsorption at 30℃. Breakthrough was considered achieved when the gallium concentration in the effluent reached 8% of the initial concentration, and the feed was stopped. The gallium adsorption rate was measured to be 92.5%. After adsorption saturation, the resin was washed with 5 BV of deionized water at a flow rate of 2 BV / h. The Al concentration in the effluent was measured every 30 min during washing. Washing was stopped when the Al concentration in the effluent dropped to 35 mg / L (approximately 2.5 h in total), at which point the pH of the effluent was 7.6. Using 1.0 mol / L H₂SO₄ solution as the desorbent, the washed saturated resin was desorbed at a flow rate of 3 BV / h at 25℃ for 30 min. The eluent was collected. Analysis showed that the gallium concentration in the eluent was 1.7 g / L, the Al concentration was 0.16 g / L (Al / Ga = 0.094), the Fe concentration was 0.08 g / L, and the V concentration was 0.12 g / L, with a desorption rate of 91.0%. 2 mol / L NaOH solution was slowly added dropwise to the gallium-rich eluent, and the pH was adjusted to 3.0 under stirring. After standing for 1 h, the Fe(OH)₃ precipitate was removed by filtration. The Fe concentration in the filtrate after iron removal was 0.005 g / L. 2 mol / L NaOH solution was then slowly added dropwise to the filtrate after iron removal, and the pH was adjusted to 7.5. The filtrate was aged at room temperature with stirring for 2 h, resulting in a grayish-white hydroxide precipitate. The precipitate was separated by vacuum filtration. The resulting precipitate was mixed with deionized water at a solid-liquid ratio of 1:4, stirred for 15 min, and then filtered. The pulping and washing process was repeated four times. After the fourth wash, the Al concentration in the eluent was 6 mg / L, and no SO4 was detected by BaCl2. 2- The washed precipitate was dried in an oven at 105°C for 4 hours. The dried hydroxide was then placed in a muffle furnace and heated to 700-800°C at a rate of 5°C / min, held at this temperature in air for 0.5-2 hours, and then cooled to room temperature with the furnace to obtain white gallium oxide powder. Preferably, the calcination temperature was 700-750°C, and the calcination time was 0.5-1 hours. Calcination was carried out in air, which has advantages over inert atmospheres in terms of lower equipment requirements, higher operational safety, and lower production costs. XRD analysis identified it as β-Ga₂O₃, and ICP-OES analysis showed a purity of 99.93%. Based on the total gallium content in the mother liquor, the overall recovery rate from the mother liquor to the gallium oxide product was 72.5%.

[0021] Example 2 The mother liquor from the Bayer process was used as raw material, containing 170 mg / L gallium, 160 g / L caustic soda, and 85 g / L Al₂O₃. The mother liquor was pretreated by vacuum filtration and then set aside. 1 L of LSC-600 chelating resin was packed into an ion exchange column. The pretreated mother liquor was subjected to dynamic adsorption at a flow rate of 6 BV / h at 40℃. The single-column gallium adsorption rate was measured to be 85.2%. After adsorption saturation, the column was washed with 6 BV of deionized water at a flow rate of 1.5 BV / h until the Al concentration in the effluent reached 28 mg / L. The washed saturated resin was then desorbed with 1.5 mol / L HCl solution at 15℃ for 40 min, and the eluent was collected. Analysis revealed that the gallium concentration in the desorption solution was 1.5 g / L, the Al concentration was 0.12 g / L (Al / Ga = 0.080), the Fe concentration was 0.06 g / L, and the V concentration was 0.09 g / L, with a desorption rate of 92.0%. The pH of the gallium-rich desorption solution was adjusted to 3.2 by slowly adding 2 mol / L NaOH solution, and the solution was allowed to stand for 1.5 h before filtration to remove iron. The pH was then adjusted to 7.8 by further adding 2 mol / L NaOH solution, and the solution was aged at 40℃ for 3 h to form a hydroxide precipitate. After filtration, the precipitate was slurried and washed five times at a solid-liquid ratio of 1:5 until the Al concentration in the washings was 5 mg / L. An AgNO3 test was performed to detect the absence of Cl. - After washing, the precipitate was dried at 110℃ for 3 h, then calcined at 750℃ for 1 h with a temperature increase of 5℃ / min to obtain the β-Ga2O3 product. The purity was determined to be 99.95%, and the total recovery rate was 70.8%.

[0022] Example 3 The mother liquor from the Bayer process was used as raw material, containing 210 mg / L gallium, 175 g / L caustic soda, and 95 g / L Al₂O₃. The mother liquor was pretreated by vacuum filtration and then used for further processing. Two ion exchange columns were connected in series (each packed with 500 mL of LSC-600 resin) for continuous dynamic adsorption at a flow rate of 5 BV / h and an adsorption temperature of 35℃. During adsorption, the bottom of the resin columns was backflushed for 30 s every 1 h to prevent resin blockage. The single-column gallium adsorption rate was 87.0%, and the total adsorption rate of the two-column system was 96.5%. After adsorption saturation, the column was washed with 5.5 BV of deionized water until the Al concentration in the effluent reached 42 mg / L. Desorption was then performed with 0.8 mol / L H₂SO₄ at 20℃ for 45 min, using 3 BV of desorbent, and the eluent was collected. The desorption solution contained 1.6 g / L Ga, 0.14 g / L Al (Al / Ga = 0.088), 0.09 g / L Fe, and 0.10 g / L V, with a single desorption rate of 91.5%. The pH was adjusted to 2.8 with 3 mol / L NaOH, and after iron removal and filtration, the pH was further adjusted to 7.2 with 2 mol / L NaOH, and the mixture was aged for 3 h. The precipitate was slurried and washed three times at a 1:3 solid-liquid ratio, yielding an Al concentration of 7 mg / L in the washings. The precipitate was dried at 105 °C for 3 h, then calcined at 700 °C for 0.5 h with a heating rate of 8 °C / min to obtain β-Ga₂O₃ powder. The purity was 99.94%, and the total recovery rate was 73.8%.

[0023] Comparative Example 1 (Traditional washing volume, without enhancement) The same raw materials and operating conditions as in Example 1 were used, the only difference being that the water washing volume after adsorption saturation was 2 BV (instead of the 4-6 BV of this invention) in the conventional process. After washing, the Ga concentration in the desorption solution was 2.0 g / L, and the Al concentration was 0.92 g / L (Al / Ga = 0.46). After iron removal, co-precipitation, pulping, and washing were performed under the same conditions. The resulting precipitate, after calcination, had a gallium oxide purity of 97.2%, which did not meet the requirement of high-purity gallium oxide (≥99.9%).

[0024] Comparative Example 2 (Traditional Electrolysis Process) A traditional process of "resin adsorption—acid desorption—neutralization precipitation—alkali dissolution—impurity removal—electrolysis" was used to treat an equal volume of Bayer process mother liquor. The desorbed solution underwent neutralization precipitation, alkali dissolution, and impurity removal before electrolysis (electrolysis voltage 3.5 V, current density 500 A / m³). 2 The electrolysis time was 12 hours, the current efficiency was 80%, and the power consumption per kilogram of gallium was approximately 9.5 kWh. The obtained metallic gallium was then smelted and oxidized to prepare gallium oxide, with a gallium loss of approximately 7.2% during the smelting and oxidation process. The overall recovery rate from the mother liquor to gallium oxide was 65%–70%, lower than the 70.8%–73.8% of the present invention.

[0025] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing high-purity gallium oxide from mother liquor using the Bayer process, characterized in that, The method includes the following steps: (1) The seed mother liquor in the Bayer process of alumina production is filtered or pretreated by sedimentation to remove suspended solid particles and obtain pretreated mother liquor; (2) The pretreated mother liquor is dynamically adsorbed through an adsorption column filled with LSC-600 chelating resin, so that gallium ions or gallium complex ions are adsorbed onto the resin. (3) Use water to wash the saturated resin to remove the mother liquor entrained on the resin surface and in the pores. The amount of water used for washing is 4~6 BV. (4) Use an acidic desorbent to desorb the saturated resin after strengthening and washing, so that the gallium adsorbed on the resin enters the desorption solution to obtain a gallium-rich desorption solution. (5) Add alkaline solution to the gallium-rich desorption solution to adjust the pH to 2.5-3.5, so that Fe 3+ The iron was precipitated as Fe(OH)3, removed by filtration, and the filtrate after iron removal was obtained. (6) Add alkaline solution to the filtrate after iron removal to adjust the pH to 7.0~8.0 so that gallium and the aluminum remaining in the solution co-precipitate in the form of hydroxides, and obtain mixed hydroxide precipitate by solid-liquid separation; (7) Wash the mixed hydroxide precipitate thoroughly with deionized water 3 to 5 times to remove the entrained soluble aluminum salts, sodium salts and other impurities; (8) After washing, the precipitate is dried and then calcined at 700~800℃ for 0.5~2 h to obtain high-purity gallium oxide product.

2. The method according to claim 1, characterized in that, In step (2), the LSC-600 chelating resin is a chelating resin with a amine oxime functional group on its backbone; the adsorption temperature is 25~45℃ and the influent flow rate is 2~10 BV / h.

3. The method according to claim 1, characterized in that, In step (3), the washing flow rate of the enhanced washing is 1~3 BV / h, and the washing endpoint is when the Al concentration in the effluent is less than 50 mg / L, or the conductivity of the effluent drops to a stable low value, or the pH of the effluent is 7~8.

4. The method according to claim 1, characterized in that, The acidic desorbent is one or more of sulfuric acid, hydrochloric acid, or nitric acid, with an acid concentration of 0.1~3 mol / L; the desorption temperature is 0~30℃, and the desorption time is 20~60 min.

5. The method according to claim 1, characterized in that, In step (6), the alkaline solution is a NaOH solution with a concentration of 1~4 mol / L; the pH is adjusted by slow dripping and thorough stirring; the precipitation temperature is room temperature to 50℃; and the aging time is 1~4 h.

6. The method according to claim 1, characterized in that, In step (7), the pulping and washing process involves mixing the precipitate with deionized water at a solid-liquid ratio of 1:3 to 1:5, stirring for 10 to 30 minutes, and then filtering. This process is repeated 3 to 5 times. The washing endpoint is defined as an Al concentration in the wash solution below 10 mg / L and the absence of SO4 detected by BaCl2 solution. 2- Alternatively, AgNO3 can be used to detect the absence of Cl. - .

7. The method according to claim 1, characterized in that, In step (8), the drying temperature is 80~120℃ and the drying time is 2~6 h; calcination is carried out in an air atmosphere and the heating rate is 2~10 ℃ / min.

8. The method according to claim 1, characterized in that, The high-purity gallium oxide product is in the β-Ga2O3 crystal form with a purity ≥99.9%.

9. The method according to claim 1, characterized in that, The adsorption liquid of step (2) is returned to the Bayer process production system for recycling; the enhanced washing liquid of step (3) is partially reused in the enhanced washing process of step (3) after simple filtration, and the remainder is returned to the Bayer process system; the last washing water in the pulping and washing liquid of step (7) is reused in the pulping and washing process of the next batch of step (7), and the rest is returned to the Bayer process system.