A method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials

By employing a process flow of crushing and grinding, combined magnetic and gravity separation for enrichment, impurity removal, and granulation, drying, and preheating, the application problem of low-grade iron-containing raw materials in hydrogen-based reduction was solved. Iron oxide powder suitable for fluidized bed hydrogen reduction was prepared, improving iron recovery rate and reducing energy consumption, and expanding the raw material sources for iron-based fuel recycling.

CN123062009APending Publication Date: 2026-11-10SHAANXI LANJI COAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611510118.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies cannot effectively utilize low-grade iron-containing solid waste such as red mud, steel slag, steel rolling mill iron oxide scale, and iron-containing dust to prepare iron oxide powder suitable for direct hydrogen-based reduction. These technologies suffer from problems such as low iron content, fine particle size, and high content of alkali metals and sulfur and phosphorus impurities, making them unsuitable for direct hydrogen-based reduction.

Method used

The process involves crushing and grinding, combined magnetic and gravity separation for enrichment, impurity removal, granulation, and drying and preheating. This includes two-stage magnetic separation, differentiated impurity removal methods, granulation, and drying and preheating. The aim is to prepare spherical particles with a particle size of 50-200 μm, a compressive strength of not less than 10 N/particle, and an abrasion index of not more than 5%, which meet the requirements of fluidized bed hydrogen reduction.

Benefits of technology

It achieves the tiered enrichment and impurity control of low-grade iron-containing raw materials, reduces fine powder entrainment loss, improves iron recovery rate, reduces energy consumption, and expands the raw material sources for iron-based fuel recycling, thus possessing the benefits of resource recycling and carbon emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062009A_ABST
    Figure CN123062009A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials. The method uses one or more of the following as raw materials: red mud, steel slag, rolled iron oxide scale, or iron-containing dust. The raw materials are crushed and ground to a particle size of no more than 0.1 mm, then enriched by a two-stage magnetic separation combined with gravity separation using a shaking table or spiral chute to remove siliceous aluminum gangue. Impurities are then removed by calcification transformation—water washing and dealkalization, acid leaching, or oxidative roasting, depending on the source, to ensure that the mass fractions of sulfur, phosphorus, and alkali metal oxides are no higher than 0.05%, 0.03%, and 0.2%, respectively. 0.5%–3.0% binder is added to the purified material for granulation, resulting in spherical particles with a particle size of 50–200 μm. These particles are then dried and preheated at 200–400 °C to obtain iron oxide powder for hydrogen reduction with a Fe2O3 mass fraction of no less than 85%. This powder can be mixed with recycled iron oxide at a mass ratio of 1:9 to 9:1 for hydrogen-based reduction to produce fuel iron powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical raw material pretreatment and solid waste resource utilization technology, specifically to a method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials such as red mud, steel slag, steel rolling mill iron oxide scale or iron-containing dust and sludge. The obtained iron oxide powder is suitable for hydrogen-based direct reduction to produce fuel iron powder and iron-based fuel recycling systems. Background Technology

[0002] Hydrogen-based direct reduction is an important technological path for achieving deep decarbonization in the steel industry. In recent years, iron-based fuel recycling using metallic iron powder as an energy carrier has attracted attention: iron powder is burned to generate iron oxide and release heat, and the combustion products are recovered and then reduced back to metallic iron powder by hydrogen, thus achieving a carbon-free energy cycle. This cycle imposes strict requirements on the iron oxide raw materials entering the hydrogen reduction unit: First, the Fe2O3 content must be maintained at a high level, otherwise the cycle ratio will increase, and energy consumption and costs will increase significantly; Second, the particle size must be suitable for the fluidized bed reactor and have sufficient compressive strength and wear resistance to avoid fine powder entrainment and bed loss; Third, the sulfur and phosphorus content must be strictly controlled to prevent the generation of harmful sulfur and phosphorus-containing gases during reduction and combustion, corrosion of equipment, and deterioration of product quality; Fourth, the alkali metal oxide content must be strictly limited, otherwise it is easy to cause particle adhesion, ring formation, or even loss of flow in the fluidized bed.

[0003] Meanwhile, the annual generation and stockpiling of iron-containing solid wastes such as red mud, steel slag, rolled iron oxide scale, and iron-containing dust are enormous, posing significant environmental risks. Current utilization methods mainly involve them as building material raw materials, roadbed materials, and sintering or blast furnace feedstocks, resulting in low added value. Furthermore, due to their fine particle size, high alkali content, and complex impurity distribution, they cannot be directly used as raw materials for hydrogen reduction. Existing sorting and purification methods for these solid wastes primarily aim to prepare iron-containing materials for blast furnaces or sintering. These methods suffer from coarse particle size, and the control indicators for sulfur, phosphorus, and alkali metals do not match the requirements for hydrogen-based reduction. Moreover, they do not consider the strength and abrasion behavior of granulated particles under fluidized conditions, and lack dedicated pretreatment processes for iron oxide powder used in hydrogen reduction.

[0004] Therefore, there is an urgent need to provide a method for preparing iron oxide powder that meets the requirements of hydrogen reduction in terms of grade, particle size, strength and impurity content from low-grade iron-containing raw materials. Summary of the Invention Technical problems to be solved

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials. This method solves the problem that low-grade iron-containing raw materials such as red mud, steel slag, steel rolling mill iron oxide scale, and iron-containing dust cannot be directly used for hydrogen-based reduction due to their low iron content, fine particle size, and high content of impurities such as alkali metals, sulfur, and phosphorus. Furthermore, the method enables the obtained iron oxide powder to be adapted to the fluidized bed hydrogen reduction process in terms of particle size, strength, and impurity content. Technical solution

[0006] To achieve the above objectives, the present invention adopts the following technical solution: a method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials, comprising the steps of crushing and grinding the raw materials, combined magnetic separation and gravity separation enrichment, impurity removal, granulation, and drying and preheating, as detailed below: S1 Crushing and Grinding: Low-grade iron-containing raw material (10) is fed into the crushing and grinding unit (1), crushed and ground to a particle size of no more than 0.1 mm, so that the iron-containing minerals and gangue are fully liberated. The low-grade iron-containing raw material is one or more of red mud, steel slag, steel rolling mill iron oxide scale or iron-containing dust. S2 Combined magnetic and gravity separation enrichment: The grinding product is fed into the combined magnetic and gravity separation enrichment unit (2), first undergoing two stages of magnetic separation with a weak magnetic induction intensity of 0.3~0.6 T and a strong magnetic induction intensity of 0.8~1.2 T, and then undergoing gravity separation on a shaking table or a spiral chute to remove the low-density siliceous aluminum gangue, thus obtaining the enriched material. S3 Impurity Removal: The enriched material is sent to the impurity removal unit (3), and one or more of the following sub-units are selected according to the source of the raw material: water washing and dealkali removal sub-unit (3a), acid leaching sub-unit (3b), or oxidative roasting sub-unit (3c) for treatment, so that the mass fraction of sulfur in the material is not higher than 0.05%, the mass fraction of phosphorus is not higher than 0.03%, and the total mass fraction of alkali metal oxides is not higher than 0.2%. After solid-liquid separation and washing in the filtration and washing unit (11), the impurity-removed material is obtained. When the raw material is red mud, a calcification-washing dealkalization process is adopted, and the Na2O mass fraction in the dealkalized material is not higher than 0.2%. When the raw material is steel slag or iron-containing dust, acid leaching is carried out using a 5%~15% hydrochloric acid or sulfuric acid solution, with a liquid-solid mass ratio of 3:1~8:1, a leaching temperature of 60~90 ℃, and a leaching time of 30~120 min. When the raw material is rolled iron oxide scale or carbon-containing dust, oxidative roasting is adopted, with a temperature of 600~900 ℃, a holding time of 30~90 min, and an atmosphere of air or oxygen-enriched air to remove sulfur, carbon, and residual organic matter. S4 Granulation: Add 0.5%~3.0% (by dry weight) of binder to the purified material, and granulate in granulation unit (4) using a disc granulator or spray granulation tower to obtain spherical particles with a particle size of 50~200 μm; the binder is bentonite, carboxymethyl cellulose, or polyvinyl alcohol aqueous solution. The compressive strength of the obtained spherical particles is not less than 10 N / particle, and the wear index is not higher than 5%, to meet the wear resistance requirements in the fluidized bed reduction process. S5 Drying and Preheating: The spherical particles are dried and preheated to 200~400 ℃ in the drying and preheating unit (5) to obtain Fe2O3 with a mass fraction of not less than 85% and a BET specific surface area of ​​0.5~5 m².2 / g of iron oxide powder for hydrogen reduction; the heat source for drying and preheating is the waste heat from hydrogen reduction tail gas or the waste heat from iron powder boiler flue gas.

[0007] Further, the prepared iron oxide powder for hydrogen reduction and the recycled iron oxide recovered from the iron powder combustion products are mixed in the batching and mixing unit (8) at a mass ratio of 1:9 to 9:1 and then fed into the hydrogen reduction unit (6); the recycled iron oxide is obtained by magnetic separation of the combustion products of the iron powder combustion and energy utilization unit (7) through the recycled iron oxide recovery unit (9), and the hydrogen reduction unit (6) is a fluidized bed reduction reactor. Beneficial effects

[0008] Compared with the prior art, the present invention has the following beneficial effects: 1. By combining two-stage magnetic separation and gravity separation for enrichment, strong magnetic iron minerals can be preferentially recovered under low magnetic field strength, weak magnetic iron-containing phases can be recovered under high magnetic field strength, and low-density siliceous aluminum gangue can be removed by gravity separation, thus achieving the stepwise enrichment of low-grade raw materials and simultaneously improving iron recovery rate and enrichment ratio. 2. Different purification routes are adopted according to the source of raw materials, namely calcification transformation-water washing dealkalization, acid leaching or oxidative roasting, so that sulfur, phosphorus and alkali metal oxides are reduced to below 0.05%, 0.03% and 0.2% respectively. This can effectively avoid the generation of harmful gases, equipment corrosion and adhesion loss in the fluidized bed during hydrogen reduction and iron powder combustion. 3. By granulation and drying preheating, fine particles are transformed into spherical particles with a particle size of 50~200 μm, a compressive strength of not less than 10N / particle, and an abrasion index of not more than 5%, which meets the requirements of fluidized bed for particle size and abrasion resistance, and significantly reduces the loss of fine powder entrainment. 4. The heat source for drying and preheating is taken from the waste heat of hydrogen reduction tail gas or the waste heat of iron powder boiler flue gas, realizing the cascade utilization of heat within the system and reducing energy consumption in the pretreatment process. 5. The obtained iron oxide powder can be mixed with recycled iron oxide recovered from iron powder combustion products in any proportion, allowing low-grade iron-containing solid waste to directly enter the iron-based fuel cycle, reducing the cost of hydrogen reduction raw materials, expanding the raw material sources for the iron-based fuel cycle, and achieving both resource recycling and carbon emission reduction benefits. Attached Figure Description

[0009] Figure 1 This is a schematic diagram of the process flow for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials according to the present invention.

[0010] Figure 2 This is a schematic diagram of the impurity removal route of the impurity removal unit in this invention, which sorts the raw materials according to their source.

[0011] Explanation of reference numerals in the attached diagram: 1. Crushing and grinding unit; 2. Magnetic separation-gravity separation combined enrichment unit; 3. Impurity removal unit; 3a. Water washing and dealkalization sub-unit; 3b. Acid leaching sub-unit; 3c. Oxidative roasting sub-unit; 4. Granulation unit; 5. Drying and preheating unit; 6. Hydrogen reduction unit; 7. Iron powder combustion and energy utilization unit; 8. Batching and mixing unit; 9. Circulating iron oxide recovery unit; 10. Low-grade iron-containing raw material; 11. Filtration and washing unit. Detailed Implementation

[0012] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Example 1 (using red mud as raw material)

[0013] Bayer red mud was used as a low-grade iron-containing raw material (10), with a total iron content of about 30% to 35% and a Na2O content of about 6% to 8%. Red mud was crushed and ground in crushing and grinding unit (1) to a particle size of no more than 0.1 mm (more than 90% of which were -0.074 mm); it was then fed into magnetic separation-gravity separation combined enrichment unit (2), where it was subjected to weak magnetic separation with a magnetic induction intensity of 0.45 T and strong magnetic separation with a magnetic induction intensity of 1.0 T in sequence, and then the silica-alumina gangue was removed by shaking table gravity separation to obtain enriched material; the enriched material was sent to impurity removal unit (3), where calcium additives were added to carry out calcification transformation (850 ℃, 60 min, air atmosphere) to convert soluble sodium into a sparingly soluble sodium-containing phase, and then washed with water to remove alkali until the Na2O mass fraction was no more than 0.2%, and then separated and washed by filtration and washing unit (11) to obtain impurity-free material; 1.5% bentonite by dry weight was added to the impurity-free material, and granulation was carried out in a disc granulator to obtain spherical particles with a particle size of 80~150 μm; and then dried and preheated in drying and preheating unit (5) at 300 ℃. The iron oxide powder for hydrogen reduction was obtained by drying and preheating at ℃. Example 2 (using steel slag and iron-containing dust as raw materials)

[0014] The converter steel slag and iron-containing dust were mixed at a mass ratio of 7:3 to form a low-grade iron-containing raw material (10). The raw material was crushed and ground to a particle size of no more than 0.1 mm. In the magnetic separation-gravity separation combined enrichment unit (2), 0.5 T weak magnetic separation and 1.1 T strong magnetic separation were carried out in sequence. Then, the silica-alumina gangue was removed by gravity separation through a spiral chute to obtain enriched material. The enriched material was sent to the acid leaching subunit (3b) and leached at 80 °C for 60 min with a mass concentration of 10% hydrochloric acid solution at a liquid-solid mass ratio of 5:1 to remove phosphorus and some alkali metals. The material was washed to neutrality through the filtration and washing unit (11) to obtain impurity-free material. 2.0% polyvinyl alcohol aqueous solution (dry basis mass) was added to the impurity-free material and granulated by spray granulation tower to obtain spherical particles with a particle size of 60~120 μm. The material was dried and preheated at 350 °C in the drying and preheating unit (5) to obtain iron oxide powder for hydrogen reduction. Example 3 (using rolled iron oxide scale as raw material)

[0015] Iron oxide scale from steel rolling mills was used as a low-grade iron-containing raw material (10), which was crushed and ground to a particle size of no more than 0.1 mm. In the magnetic separation-gravity separation combined enrichment unit (2), 0.4 T weak magnetic separation and 0.9 T strong magnetic separation were carried out in sequence, followed by gravity separation on a shaking table to obtain enriched material. The enriched material was sent to the oxidation roasting subunit (3c) and oxidized and roasted at 800 ℃ for 60 min in an air atmosphere to remove residual oil, carbon and sulfur, and obtain impurity-free material. 1.0% bentonite by dry weight was added to the impurity-free material, and granulation was carried out in a disc granulator to obtain spherical particles with a particle size of 100~180 μm. The waste heat of hydrogen reduction tail gas was used in the drying and preheating unit (5) to oxidize the material at 250 ℃. The iron oxide powder for hydrogen reduction is obtained by drying and preheating at ℃. The obtained iron oxide powder and the recycled iron oxide recovered by the recycled iron oxide recovery unit (9) are mixed in the batching and mixing unit (8) at a mass ratio of 1:1 and then sent to the fluidized bed hydrogen reduction unit (6) for hydrogen reduction to obtain metallic iron powder. The metallic iron powder is burned and released heat in the iron powder combustion and energy utilization unit (7) to recover the recycled iron oxide.

[0016] The main performance indicators of the iron oxide powder for hydrogen reduction obtained in the above embodiments are shown in Table 1. Table 1. Main process parameters and product indicators of the examples Example raw material Impurity removal methods <![CDATA[Fe2O3(%)]]> S(%) P(%) <![CDATA[Na2O+K2O(%)]]> 1 Red mud Calcification Transformation—Water Washing and Dealkalization 88.5 0.030 0.020 0.15 2 Steel slag + iron-containing dust and sludge Hydrochloric acid leaching (10%) 90.2 0.020 0.015 0.12 3 Iron oxide scale from rolled steel Oxidative roasting (800 ℃) 93.6 0.010 0.020 0.08 Note: The indicators listed in the table are representative results obtained under the above process conditions. The compressive strength is not less than 10 N / particle and the wear index is not higher than 5%, which meets the requirements of fluidized bed hydrogen reduction.

[0017] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention. The method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials provided by the present invention has wide-ranging raw material sources, smooth process integration, and can be coupled with iron-based fuel cycle systems, thus possessing good industrial applicability.

Claims

1. A method for preparing iron oxide powder for hydrogen reduction from low-grade iron-containing raw materials, characterized in that, Includes the following steps: S1. The low-grade iron-containing raw material is crushed and ground to a particle size of no more than 0.1 mm. The low-grade iron-containing raw material is one or more of red mud, steel slag, steel rolling mill iron oxide scale or iron-containing dust and sludge. S2 performs a combination of magnetic and gravity separation to enrich the grinding products, resulting in enriched material. S3 performs impurity removal treatment on the enriched material, wherein the impurity removal treatment is one or more of water washing and dealkalization, acid leaching or oxidative roasting, so that the mass fraction of sulfur in the material is not higher than 0.05%, the mass fraction of phosphorus is not higher than 0.03%, and the total mass fraction of alkali metal oxides is not higher than 0.2%. S4 Add a binder to the purified material and granulate it to obtain spherical particles with a particle size of 50~200 μm; S5. The spherical particles are dried and preheated to 200~400 °C to obtain iron oxide powder for hydrogen reduction with a Fe2O3 mass fraction of not less than 85%.

2. The method according to claim 1, characterized in that, The magnetic separation in step S2 is a two-stage magnetic separation. The first stage is a weak magnetic separation with a magnetic induction intensity of 0.3~0.6 T, and the second stage is a strong magnetic separation with a magnetic induction intensity of 0.8~1.2 T. The gravity separation is a shaking table gravity separation or a spiral chute gravity separation, used to remove low-density silica-alumina gangue.

3. The method according to claim 1, characterized in that, In step S3, when the low-grade iron-containing raw material is red mud, a calcification transformation-water washing dealkalization process is adopted, and the mass fraction of Na2O in the dealkalized material is not higher than 0.2%.

4. The method according to claim 1, characterized in that, The oxidative roasting in step S3 is carried out at a temperature of 600~900℃, for a holding time of 30~90 min, and in an atmosphere of air or oxygen-enriched air, in order to remove sulfur, carbon and residual organic matter from the raw materials.

5. The method according to claim 1, characterized in that, The acid leaching in step S3 uses a hydrochloric acid or sulfuric acid solution with a mass concentration of 5% to 15%, a liquid-solid mass ratio of 3:1 to 8:1, a leaching temperature of 60 to 90 ℃, and a leaching time of 30 to 120 min.

6. The method according to claim 1, characterized in that, The binder mentioned in step S4 is bentonite, carboxymethyl cellulose, or polyvinyl alcohol aqueous solution, and the amount added is 0.5% to 3.0% of the dry basis material mass; the granulation equipment is a disc granulator or a spray granulation tower.

7. The method according to claim 6, characterized in that, The spherical particles obtained in step S4 have a compressive strength of not less than 10 N / particle and an abrasion index of not more than 5% to meet the abrasion resistance requirements in the fluidized bed reduction process.

8. The method according to claim 1, characterized in that, The heat source for drying and preheating in step S5 is the waste heat from hydrogen reduction tail gas or the waste heat from iron powder boiler flue gas, and the BET specific surface area of ​​the obtained iron oxide powder for hydrogen reduction is 0.5~5m². 2 / g.

9. The method according to claim 1, characterized in that, The prepared iron oxide powder for hydrogen reduction is mixed with recycled iron oxide recovered from iron powder combustion products at a mass ratio of 1:9 to 9:1 and then fed into the hydrogen reduction unit.

10. The method according to claim 9, characterized in that, The circulating iron oxide is obtained by magnetic separation of the iron powder combustion products, and the hydrogen reduction unit is a fluidized bed reduction reactor.