Cobalt sulfide powder materials and their polymorphism control methods
By employing hydrothermal reaction and annealing methods, the problem of inconsistent cobalt sulfide synthesis was solved, enabling efficient control of multiple cobalt sulfide crystal forms within the same system, thereby reducing synthesis costs and equipment requirements.
Patent Information
- Application Number
- CN202611120903.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-27
- Publication Date
- 2026-11-10
AI Technical Summary
The existing methods for synthesizing cobalt sulfide catalysts are not standardized, resulting in high costs for using precious metals, difficulty in synthesizing Co9S8 and low raw material utilization. Furthermore, different cobalt sulfides require different equipment for synthesis, making it impossible to control the crystal form in the same system.
A hydrothermal reaction combined with annealing was used to synthesize CoS2, Co3S4, Co4S3 and Co9S8 by controlling the annealing temperature, time and whether alkaline substances were added, thereby regulating the crystal form of cobalt sulfides. A unified equipment and solvent system were used.
This method enables efficient and low-cost control of the crystal forms of different cobalt sulfides within the same synthesis system, simplifying the synthesis process and reducing the cost of using precious metal catalysts.
Smart Images

Figure CN123062011A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of inorganic functional material synthesis, specifically relating to a cobalt sulfide powder material and its polymorph control method. Background Technology
[0002] Electrolysis of water for hydrogen production boasts high hydrogen production efficiency and purity, making it a green hydrogen production method for the efficient utilization of renewable energy in the future. Currently, precious metal-based catalysts (such as Pt, Ir, and Ru) used in water electrolysis for hydrogen production are scarce and expensive. Non-precious metal catalysts, due to their lower cost, abundant reserves, and tunable electronic structure, have the potential to replace precious metal-based catalysts. Among them, cobalt sulfides, due to their variable valence states, readily undergo redox reactions, exhibit excellent OER or HER catalytic activity in alkaline media, have low overpotentials, and good conductivity, thus being considered promising catalysts for water electrolysis.
[0003] Currently studied cobalt sulfides include CoS2, Co3S4, Co4S3, and Co9S8. CoS2 has been extensively studied due to its excellent metallic properties and intrinsic catalytic activity; however, CoS2 has relatively few exposed active sites, making it difficult to achieve the catalytic activity required for practical applications. Co3S4, with its spinel structure, has a higher Co content... 3+ And Co 3+ Due to their low coordination number and high H2O molecule adsorption energy, cobalt sulfides are considered active centers for electrochemical water oxidation and have attracted the attention of researchers in recent years. Some researchers have sulfided Co3O4 to obtain Co3S4 water electrolysis catalysts, which can achieve hydrogen evolution and oxygen evolution reactions under the same environment. The presence of Co-Co bonds in Co9S8 gives it metallic or conductive behavior and influences its nearest neighboring sulfide atoms through bond coupling, thereby improving its conductivity and affecting its electrochemical activity. Furthermore, cobalt sulfides have wide applications in photocatalysis, battery electrode materials (lithium-ion, sodium-ion, lithium-sulfur), thermal battery cathode materials, and magnetic materials.
[0004] Common synthesis methods include high-temperature solid-phase sulfidation, hydrothermal methods, solvothermal methods, and template methods. However, these methods often only synthesize cobalt sulfides with a specific crystal form. For example, Co9S8 single crystals can be synthesized via hydrothermal reduction using CoSO4·7H2O, Na2SO3, and N2H4·H2O, or Co9S8-C composites can be prepared using CoCl2, thiourea, citric acid, etc., through freeze-drying and calcination with NaCl molten salt. High-temperature solid-phase / sulfidation is a classic process for synthesizing CoS2, producing high-purity products, but it consumes a lot of energy, and the sulfur powder sublimates at high temperatures, resulting in low utilization. Using thiourea as a sulfur source, a one-step hydrothermal method can be used to in-situ sulfidate cobalt foam to synthesize Co4S3@Co composite electrocatalytic materials, but it is difficult to obtain pure Co4S3 powder materials. Using cobalt acetate, thioacetamide, etc., as raw materials, and with the assistance of triethylenediamine, a polyhedral Co3S4 material was synthesized via a hydrothermal method. Cubic Co3S4 nanocrystals can also be prepared using CoCl2·6H2O, thiourea, and other raw materials via ultrasonic spray pyrolysis. In summary, there are many different methods for preparing various types of cobalt sulfides, making it difficult to synthesize them conveniently within a unified synthetic system.
[0005] In summary, the existing technologies suffer from the aforementioned technical problems, leading to the following drawbacks: 1. The catalytic materials are mostly precious metals, resulting in excessively high usage costs; 2. Co9S8 is difficult to synthesize, and direct sulfidation in a tube furnace results in low raw material utilization; 3. Different cobalt sulfides in the existing technologies employ different preparation methods and synthesis systems, leading to inconsistent equipment. Therefore, the current methods for preparing cobalt sulfides are not universally applicable, and there are problems such as the inability to easily control the crystal form within the same system. Summary of the Invention
[0006] This invention provides a cobalt sulfide powder material and a method for controlling its polymorphism. The preparation method does not require complex structural compounds or surfactants, is low in cost, and has a simple and easy preparation process.
[0007] One objective of this invention is to provide a method for controlling the polymorphism of cobalt sulfides, comprising the following steps: Step 1: The cobalt source and the sulfur source are subjected to a hydrothermal reaction in a solvent to obtain the cobalt sulfide precursor; Step 2: Anneal the cobalt sulfide precursor obtained in Step 1 in a protective atmosphere. By controlling the annealing conditions, cobalt sulfide powder materials with different crystal forms are obtained. The annealing conditions include: annealing temperature, annealing time, and the presence of alkaline substances in the annealing system.
[0008] As a preferred embodiment, in step one, the cobalt source is cobalt nitrate and the sulfur source is thiourea.
[0009] As a preferred embodiment, in step one, the solvent is deionized water; or a mixed solution of deionized water and ammonia. When deionized water is used as the solvent, the resulting precursor is CoS2; When a mixture of deionized water and ammonia is used as a solvent, the resulting precursor is Co3S4.
[0010] As a preferred embodiment, in step two, when there is no alkaline substance in the annealing system, the cobalt sulfide product is cobalt tetrasulfide.
[0011] As a preferred embodiment, in step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
[0012] As a preferred embodiment, in step two, when an alkaline substance is present in the annealing system, the cobalt sulfide product is cobalt octasulfide; and the alkaline substance is KOH.
[0013] As a preferred embodiment, in step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
[0014] As a preferred embodiment, in step one, the temperature of the hydrothermal reaction is 180~220 ℃, and the holding time is 7~12 h.
[0015] As a preferred embodiment, in step one, the molar ratio of cobalt to sulfur is 1:3 to 1:9.
[0016] The second objective of this invention is to provide a cobalt sulfide powder material prepared by any of the above-described control methods, wherein the cobalt sulfide powder material is Co4S3 or Co9S8.
[0017] In the method for controlling the crystal form of cobalt sulfide and its crystal structure in this invention, cobalt nitrate and thiourea are first dissolved sequentially in deionized water and stirred until homogeneous. The solution is then transferred to a micro-magnetically stirred high-pressure vessel with real-time temperature and pressure display. The vessel is kept at a set temperature for a certain time. After the reaction is complete, the vessel is cooled to room temperature and then opened. The solution is filtered, and the precipitate is centrifuged, washed, and dried to obtain CoS2 powder. Similarly, cobalt nitrate and thiourea are dissolved sequentially in deionized water containing an appropriate amount of ammonia and stirred until homogeneous. The same hydrothermal process is then used to obtain Co3S4 powder. Direct heating of the Co3S4 powder obtained above in a tube furnace yields Co4S3 powder. Adding KOH (not mixed with the raw materials, but placed in different positions within the tube furnace) during heating yields Co9S8 powder.
[0018] The present invention has at least the following beneficial effects: This invention optimizes the crystal form control method by stabilizing the synthesis of Co9S8 in a tube furnace using a KOH atmosphere. Various cobalt sulfides can be prepared under a unified synthesis system, using standardized equipment and a hydrothermal system. Subsequent direct heating or heating with KOH can directly control the crystal form of the product. In this crystal form control method, CoS2 and Co3S4 can be prepared via a one-step hydrothermal method. Co3S4 can then be directly heated or heated under alkaline conditions to prepare Co4S3 and Co9S8, respectively. This not only solves the problems of complex surface morphology and composition of cobalt disulfide composite powder materials and long synthesis processes, but also realizes a method for controlling different crystal forms of cobalt sulfide powders under the same synthesis system. The crystal form control method of this invention has high synthesis efficiency, low cost, and a simple and easy-to-implement process. The raw materials required for this invention are simple and readily available, with low cost and a short process flow, enabling the control of the crystal form of multiple cobalt sulfides within a unified process framework. The various cobalt sulfides produced in this method, when used as catalysts, have a lower cost than precious metal catalysts. Attached Figure Description
[0019] Figure 1 This is a process flow diagram for preparing various cobalt sulfide materials according to the present invention; Figure 2 Here is a SEM image of the CoS2 powder synthesized in Example 1; Figure 3 The XRD pattern of the synthesized CoS2 powder in Example 1: The horizontal axis of the XRD pattern is the 2θ angle (in °), and the vertical axis is the diffraction intensity; Figure 4 SEM image of Co3S4 powder synthesized in Example 2; Figure 5 The image shows the XRD pattern of the Co3S4 powder synthesized in Example 2. Figure 6 SEM image of Co4S3 powder synthesized in Example 3; Figure 7 The image shows the XRD pattern of the Co4S3 powder synthesized in Example 3. Figure 8 SEM image of Co9S8 powder synthesized in Example 4; Figure 9 The image shows the XRD pattern of the Co9S8 powder synthesized in Example 4. Figure 10 Here is a SEM image of the synthesized powder from Comparative Example 1; Figure 11 The image shows the XRD pattern of the synthesized powder in Comparative Example 1. Figure 12 Here is a SEM image of the synthesized powder from Comparative Example 2; Figure 13 The image shows the XRD pattern of the synthesized powder in Comparative Example 2. Figure 14 Here is a SEM image of the synthesized powder from Comparative Example 3; Figure 15 The image shows the XRD pattern of the synthesized powder in Comparative Example 3. Figure 16 Here is a SEM image of the synthesized powder from Comparative Example 4; Figure 17 The image shows the XRD pattern of the synthesized powder in Comparative Example 4. Figure 18 Here is a SEM image of the synthesized powder from Comparative Example 5; Figure 19 The XRD pattern of the synthesized powder in Comparative Example 5 is shown. Figure 20 Here is a SEM image of the synthesized powder from Comparative Example 6; Figure 21 The XRD pattern of the synthesized powder in Comparative Example 6 is shown. Figure 22 Here is a SEM image of the synthesized powder from Comparative Example 7; Figure 23 The XRD pattern of the synthesized powder in Comparative Example 7 is shown. Figure 24 Here is a SEM image of the synthesized powder from Comparative Example 8; Figure 25 The XRD pattern of the synthesized powder in Comparative Example 8; Detailed Implementation
[0020] To make the technical means, creative features, objectives, and beneficial effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.
[0021] In addition, to better illustrate the present invention, numerous specific details are given in the following detailed embodiments. Those skilled in the art should understand that the present invention can be implemented even without certain specific details. In other embodiments, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the main points of the present invention.
[0022] This embodiment provides a method for controlling the crystal form of cobalt sulfide, including the following steps: Step 1: The cobalt source and the sulfur source are subjected to a hydrothermal reaction in a solvent to obtain the cobalt sulfide precursor; Step 2: Anneal the cobalt sulfide precursor obtained in Step 1 in a protective atmosphere. By controlling the annealing conditions, cobalt sulfide powder materials with different crystal forms are obtained. The annealing conditions include: annealing temperature, annealing time, and the presence of alkaline substances in the annealing system.
[0023] Preferably, in step one, the cobalt source is cobalt nitrate and the sulfur source is thiourea.
[0024] Preferably, in step one, the solvent is deionized water; or a mixed solution of deionized water and ammonia; when the solvent is deionized water, the cobalt sulfide precursor of the hydrothermal reaction product is CoS2; when the solvent is a mixed solution of deionized water and ammonia, the cobalt sulfide precursor of the hydrothermal reaction product is Co3S4.
[0025] Preferably, in step two, when there are no alkaline substances in the annealing system, the cobalt sulfide product is cobalt tetrasulfide.
[0026] Preferably, in step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
[0027] Preferably, in step two, when an alkaline substance is present in the annealing system, the cobalt sulfide product is cobalt octasulfide; and the alkaline substance is KOH.
[0028] Preferably, in step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
[0029] Preferably, in step one, the temperature of the hydrothermal reaction is 180~220 ℃, and the holding time is 7~12 h.
[0030] Preferably, in step one, the molar ratio of cobalt to sulfur is 1:3 to 1:9.
[0031] This embodiment also provides a cobalt sulfide powder material prepared according to the above-described control method, wherein the cobalt sulfide powder material is Co4S3 or Co9S8.
[0032] This invention involves dissolving cobalt nitrate and thiourea separately in deionized water, stirring until fully dissolved, and then transferring the solution to a hydrothermal reactor (a micro-magnetically stirred high-pressure reactor). The reactor is held at a set temperature for a certain time, and the hydrothermal product is centrifuged, washed, and dried to obtain cobalt disulfide powder. Adding an appropriate amount of ammonia to the initial mixed solution and then hydrothermally synthesizing it yields cobalt tetrasulfide powder. The aforementioned cobalt tetrasulfide powder can be directly heated in a tube furnace under inert gas protection to synthesize cobalt trisulfide powder. Adding KOH powder to the aforementioned cobalt tetrasulfide powder and heating it in a tube furnace under inert gas protection yields cobalt octasulfide powder (the annealing treatment involves heating the cobalt sulfide precursor and KOH together in a protective atmosphere, without direct contact between the cobalt sulfide precursor and KOH). This invention not only solves the problems of complex surface morphology and composition of cobalt disulfide composite powder materials and long synthesis process, but also provides a method for controlling cobalt sulfide powders of different crystal forms under the same synthesis system. The method has high synthesis efficiency, low cost and simple and easy control process.
[0033] Example 1
[0034] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.524 g of thiourea (CH4N2S), dissolve them in 80 mL of deionized water, and obtain a pink solution after magnetic stirring. Transfer the mixed solution to a 200 mL hydrothermal reactor with a polytetrafluoroethylene liner, control the hydrothermal synthesis temperature at 200 °C, and maintain the temperature for 8 h. After the reactor cools to room temperature, centrifuge (8000 r·min) to obtain the final product. -1 The precipitate was obtained by centrifugation for 5 min, and washed four times with ethanol and deionized water, respectively. After centrifugation and washing, the precipitate was placed in a forced-air drying oven and dried at 60 °C for 12 h to obtain CoS2 powder material.
[0035] Example 2
[0036] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.524 g of thiourea (CH4N2S) and dissolve them in a mixed solution consisting of 75 mL of deionized water and 5 mL of ammonia water (mass concentration 25-28%). After magnetic stirring, a blue solution is obtained. Transfer the mixed solution to a 200 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene. Control the hydrothermal synthesis temperature at 180 °C and maintain the temperature for 8 h. After the reactor cools to room temperature, the precipitate obtained after the reaction is centrifuged (8000 r min). -1 The precipitate was washed four times with ethanol and deionized water, respectively, and centrifuged for 5 min. After centrifugation, the precipitate was placed in a drying oven and dried at 60°C for 12 h to obtain Co3S4 powder material.
[0037] Example 3
[0038] The Co3S4 obtained in Example 2 was heated in a tube furnace with nitrogen as a protective atmosphere and held at 500°C for 2 hours. Then it was cooled to room temperature to obtain Co4S3 powder material.
[0039] Example 4
[0040] The Co3S4 obtained in Example 2 was heated together with 3 g of KOH powder in a tube furnace. The Co3S4 powder and KOH powder were placed on different magnetic boats, and argon was used as the protective atmosphere. The furnace was kept at 600 °C for 1 h to obtain Co9S8 powder material.
[0041] Example 5
[0042] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.786 g of thiourea (CH4N2S), dissolve them in 80 mL of deionized water, and obtain a pink solution after magnetic stirring. Transfer the mixed solution to a 200 mL hydrothermal reactor with a polytetrafluoroethylene liner, control the hydrothermal synthesis temperature at 220 °C, and maintain the temperature for 7 h. After the reactor cools to room temperature, centrifuge (8000 r·min) to obtain the final product. -1 The precipitate was obtained by centrifugation for 5 min, and washed four times with ethanol and deionized water, respectively. After centrifugation and washing, the precipitate was placed in a forced-air drying oven and dried at 60 °C for 12 h to obtain CoS2 powder material.
[0043] Example 6
[0044] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.786 g of thiourea (CH4N2S) and dissolve them in a mixed solution consisting of 75 mL of deionized water and 5 mL of ammonia water (mass concentration 25-28%). After magnetic stirring, a blue solution is obtained. Transfer the mixed solution to a 200 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene. Control the hydrothermal synthesis temperature at 200 °C and maintain the temperature for 7 h. After the reactor cools to room temperature, the precipitate obtained after the reaction is centrifuged (8000 r min). -1 The precipitate was washed four times with ethanol and deionized water, respectively, and centrifuged for 5 min. After centrifugation, the precipitate was placed in a drying oven and dried at 60°C for 12 h to obtain Co3S4 powder material.
[0045] Example 7
[0046] The Co3S4 obtained in Example 6 was heated in a tube furnace with nitrogen as a protective atmosphere and held at 600°C for 1 h, and then cooled to room temperature to obtain Co4S3 powder material.
[0047] Example 8
[0048] The Co3S4 obtained in Example 6 was heated together with 5 g of KOH powder in a tube furnace. The Co3S4 powder and KOH powder were placed on different magnetic boats, and argon was used as the protective atmosphere. The furnace was kept at 500 °C for 3 h to obtain Co9S8 powder material.
[0049] Example 9
[0050] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.262 g of thiourea (CH4N2S), dissolve them in 80 mL of deionized water, and obtain a pink solution after magnetic stirring. Transfer the mixed solution to a 200 mL hydrothermal reactor with a polytetrafluoroethylene liner, control the hydrothermal synthesis temperature at 180 °C, and maintain the temperature for 12 h. After the reactor cools to room temperature, centrifuge (8000 r·min) to obtain the final product. -1 The precipitate was obtained by centrifugation for 5 min, and washed four times with ethanol and deionized water, respectively. After centrifugation and washing, the precipitate was placed in a forced-air drying oven and dried at 60 °C for 12 h to obtain CoS2 powder material.
[0051] Example 10
[0052] Accurately weigh 0.334 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.262 g of thiourea (CH4N2S) and dissolve them in a mixed solution consisting of 75 mL of deionized water and 5 mL of ammonia water (mass concentration 25-28%). After magnetic stirring, a blue solution is obtained. Transfer the mixed solution to a 200 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene. Control the hydrothermal synthesis temperature at 220 °C and maintain the temperature for 12 h. After the reactor cools to room temperature, the precipitate obtained after the reaction is centrifuged (8000 r min). -1 The precipitate was washed four times with ethanol and deionized water, respectively, and centrifuged for 5 min. After centrifugation, the precipitate was placed in a drying oven and dried at 60°C for 12 h to obtain Co3S4 powder material.
[0053] Example 11
[0054] The Co3S4 obtained in Example 10 was heated in a tube furnace with nitrogen as a protective atmosphere and held at 550°C for 3 h. Then it was cooled to room temperature to obtain Co4S3 powder material.
[0055] Example 12
[0056] The Co3S4 obtained in Example 10 was heated together with 4 g of KOH powder in a tube furnace. The Co3S4 powder and KOH powder were placed on different magnetic boats, and argon was used as the protective atmosphere. The furnace was kept at 550 °C for 2 h to obtain Co9S8 powder material.
[0057] Comparative Example 1 The preparation method and conditions were the same as in Example 1. The only difference in Comparative Example 1 was that the amount of thiourea CH4N2S added was changed to 0.087 g. The powder material obtained in Comparative Example 1 showed extremely poor crystallinity according to XRD analysis, and was not a cobalt sulfide.
[0058] Comparative Example 2 The preparation method and conditions were the same as in Example 2. The only difference in Comparative Example 2 was that the amount of thiourea CH4N2S added was changed to 0.087 g. The powder material obtained in Comparative Example 2 showed very poor crystallinity and indistinct phases according to XRD analysis.
[0059] Comparative Example 3 The powder material obtained in Comparative Example 2 was heated in a tube furnace using nitrogen as a protective atmosphere and held at 500 °C for 2 h, then cooled to room temperature to obtain the product powder material. XRD analysis showed that the powder was composed of cobalt trisulfide and cobalt trioxide, with the oxide phase being more prominent.
[0060] Comparative Example 4 The powder material obtained in Comparative Example 2 was heated together with 3 g of KOH powder in a tube furnace. The raw material powder and KOH powder were placed on different magnetic boats, and argon was used as a protective atmosphere. The furnace was heated at 600 °C for 1 h to obtain the product powder material. However, XRD analysis showed that the powder was mainly cobalt cobaltate, with very little cobalt octasulfide.
[0061] Comparative Example 5 The preparation method and conditions were the same as in Example 1. The only difference in Comparative Example 5 was that the amount of thiourea CH4N2S added was changed to 0.029 g. XRD analysis of the powder material obtained in Comparative Example 5 revealed that the powder had extremely poor crystallinity and was not a cobalt sulfide.
[0062] Comparative Example 6 The preparation method and conditions were the same as in Example 2. The only difference in Comparative Example 6 was that the amount of thiourea CH4N2S added was changed to 0.029 g. XRD analysis of the powder material obtained in Comparative Example 6 revealed that the main phase was cobalt tetroxide, with a small amount of cobalt tetrasulfide also present.
[0063] Comparative Example 7 The powder material obtained in Comparative Example 6 was heated in a tube furnace using nitrogen as a protective atmosphere and held at 500 °C for 2 h, followed by cooling to room temperature to obtain the product powder material. XRD analysis showed that the main phase of the powder was cobalt tetroxide.
[0064] Comparative Example 8 The powder material obtained in Comparative Example 6 was heated together with 3 g of KOH powder in a tube furnace. The raw material powder and KOH powder were placed on different magnetic boats, and argon was used as the protective atmosphere. The furnace was heated at 600 °C for 1 h to obtain the product powder material. XRD analysis showed that the main phase of the powder was cobalt cobaltate, with a small content of cobalt octasulfide.
[0065] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for controlling the polymorphism of cobalt sulfides, characterized in that: Includes the following steps: Step 1: The cobalt source and the sulfur source are subjected to a hydrothermal reaction in a solvent to obtain the cobalt sulfide precursor; Step 2: Anneal the cobalt sulfide precursor obtained in Step 1 in a protective atmosphere. By controlling the annealing conditions, cobalt sulfide powder materials with different crystal forms are obtained. The annealing conditions include: annealing temperature, annealing time, and the presence of alkaline substances in the annealing system.
2. The method for controlling the polymorphism of cobalt sulfides according to claim 1, characterized in that: In step one, the cobalt source is cobalt nitrate and the sulfur source is thiourea.
3. The method for controlling the polymorphism of cobalt sulfides according to claim 1, characterized in that: In step one, the solvent is deionized water; or a mixed solution of deionized water and ammonia. When deionized water is used as the solvent, the resulting precursor is CoS2; When a mixture of deionized water and ammonia is used as a solvent, the resulting precursor is Co3S4.
4. The method for controlling the polymorphism of cobalt sulfides according to claim 3, characterized in that, In step two, when there is no alkaline substance in the annealing system, the cobalt sulfide product is cobalt tetrasulfide.
5. The method for controlling the polymorphism of cobalt sulfides according to claim 4, characterized in that, In step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
6. The method for controlling the polymorphism of cobalt sulfides according to claim 3, characterized in that, In step two, when an alkaline substance is present in the annealing system, the cobalt sulfide product is cobalt octasulfide; the alkaline substance is KOH.
7. The method for controlling the polymorphism of cobalt sulfides according to claim 6, characterized in that, In step two, the annealing temperature is 500~600 ℃, the annealing time is 1~3 h, and the protective atmosphere is argon or nitrogen.
8. The method for controlling the polymorphism of cobalt sulfides according to any one of claims 1 to 7, characterized in that, In step one, the temperature of the hydrothermal reaction is 180~220 ℃, and the holding time is 7~12 h.
9. The method for controlling the polymorphism of cobalt sulfides according to any one of claims 1 to 7, characterized in that, In step one, the molar ratio of cobalt to sulfur is 1:3 to 1:
9.