Adsorption method and application of vanadium in wastewater from gamma-iron oxide-modified corn stalk carbon recovery wastewater

By modifying corn stalk carbon composite materials with gamma iron oxide, the problem of unrecovered vanadium resources in vanadium-containing wastewater treatment was solved, achieving efficient vanadium adsorption and low-cost modification of the electrode for all-vanadium redox flow batteries, thus improving resource utilization efficiency.

CN123062035APending Publication Date: 2026-11-10HUAZHONG AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611497027.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, vanadium resources cannot be effectively recovered and utilized after the treatment of vanadium-containing wastewater. Traditional carbon-based adsorption materials have insufficient adsorption capacity, and the modification cost of all-vanadium redox flow battery electrodes is high and the process is complex.

Method used

Gamma-FeO-modified corn stalk carbon was prepared by in-situ chemical co-precipitation. By uniformly loading γ-Fe2O3 onto the surface of activated corn stalk carbon, the high specific surface area of ​​activated corn stalk carbon and the high activity of γ-Fe2O3 were combined to achieve efficient adsorption of vanadium ions. The adsorbed material was then applied to the electrode of an all-vanadium redox flow battery.

Benefits of technology

This improved the adsorption capacity of vanadium ions, enabled the recycling of vanadium resources, reduced the preparation cost of electrode materials, simplified the process flow, and improved resource utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a method for vanadium adsorption in wastewater recovery using gamma-FeO-modified corn stalk carbon and its application. The invention employs an in-situ chemical co-precipitation method to prepare γ-Fe₂O₃-modified corn stalk carbon. Under acidic conditions, the prepared γ-Fe₂O₃-modified corn stalk carbon adsorbs and removes vanadium from water. The vanadium-adsorbed composite material is then loaded onto a graphite felt electrode and applied to a vanadium redox flow battery system, where its electrochemical performance is tested. This invention achieves efficient enrichment and recycling of vanadium resources in vanadium-containing wastewater by combining adsorption recovery with energy device applications. While reducing environmental pollution from vanadium-containing wastewater, it also realizes the transformation of vanadium resources from pollutant treatment to energy storage material reuse, providing a new technical approach for the development of vanadium redox flow battery electrode materials and the green recycling of vanadium resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of vanadium-containing wastewater treatment and energy materials technology, specifically to a method for adsorbing vanadium in corn stalk carbon recovery wastewater modified with gamma iron oxide and its application. Background Technology

[0002] Vanadium is an important strategic metal resource, widely used in metallurgy, chemical industry, and new energy storage due to its excellent redox properties and high energy storage activity. Among these, vanadium redox flow batteries (VRFBs) are considered a key technology for large-scale energy storage due to their high safety, long cycle life, and scalable capacity. However, with the increasing demand for vanadium resources and the expansion of related industrial production, the amount of vanadium-containing wastewater generated in ore smelting, vanadium slag treatment, and energy chemical processes is also increasing. Since vanadium has a certain degree of biotoxicity, direct discharge of vanadium-containing wastewater without effective treatment poses potential harm to the ecological environment and human health. Therefore, achieving efficient removal and resource recovery of vanadium from vanadium-containing wastewater is of great significance.

[0003] Currently, the main methods for treating vanadium pollution in water bodies include chemical precipitation, membrane separation, ion exchange, solvent extraction, and adsorption. Among these, adsorption is widely used in the treatment of heavy metal wastewater due to its advantages such as simple operation, high treatment efficiency, wide applicability, and low energy consumption. Existing adsorption materials mainly include activated carbon, carbon nanomaterials, metal oxides, layered materials, and composite adsorption materials. However, traditional carbon-based adsorption materials often suffer from insufficient surface active sites, limited selective adsorption capacity for vanadium ions, and low adsorption capacity.

[0004] Current vanadium-containing wastewater treatment technologies mostly focus on pollutant removal, while the adsorbed vanadium resources are typically treated as waste residue, failing to achieve further utilization of vanadium and resulting in resource waste. Vanadium redox flow batteries, as an important application area for vanadium resources, usually require electrode material modification to improve electrochemical reactivity. Existing electrode modification methods often employ precious metals, carbon nanomaterials, or other functional materials, which suffer from complex preparation processes, high costs, and insufficient resource utilization efficiency. Therefore, developing a novel material and method that can simultaneously achieve vanadium pollution control in water, vanadium resource recovery, and energy storage device applications is of great value for promoting the recycling of vanadium resources.

[0005] Gamma-Fe2O3 possesses high surface activity, abundant oxygen functional groups, and excellent metal ion adsorption capacity. Combining it with activated corn stalk carbon materials, which have high specific surface area, stable structure, and are widely available, holds promise for enhancing the adsorption capacity of vanadium ions and giving the adsorbent material the potential for further application in energy devices. However, existing research on the use of γ-Fe2O3-modified corn stalk carbon materials for the adsorption and recovery of vanadium-containing wastewater, and further on the application of the adsorbed vanadium-based composite materials in all-vanadium redox flow battery electrode systems, is limited.

[0006] Therefore, there is an urgent need to develop a composite material with a simple preparation process, high vanadium adsorption efficiency, and the ability to recycle vanadium resources, as well as its application methods. Summary of the Invention

[0007] The purpose of this invention is to address the problems in the existing technology, such as the failure to effectively recover and utilize vanadium resources after the treatment of vanadium-containing wastewater, the insufficient adsorption capacity of traditional carbon-based adsorption materials, and the high cost and complex process of electrode modification for all-vanadium redox flow batteries. This invention provides a method for adsorbing vanadium in wastewater from gamma oxidation (iron (γ-Fe2O3) modified corn straw carbon recovery wastewater) and its application, thereby achieving an effective combination of vanadium-containing wastewater treatment and vanadium resource energy storage utilization.

[0008] To achieve the above objectives, the technical solution designed by the present invention is as follows: This invention provides a method for adsorbing vanadium from wastewater in corn stalk carbon recovery by modifying it with gamma-iron oxide, comprising the following steps: (1) Activated corn stalk carbon, ferrous chloride, and ferric chloride are mixed to obtain a mixture. The mixture is dissolved in deionized water and ultrasonically dispersed to obtain a dispersion. Among them, ferrous chloride contains Fe 2+ Fe with ferric chloride 3+ The molar ratio is 1:1~3; (2) Heat and stir the dispersion, then add ammonia water dropwise to the dispersion to adjust the pH of the dispersion to alkaline (so that iron hydroxide is deposited in situ on the surface of the corn stalk carbon), continue stirring and then cool to obtain a liquid containing solid precipitate; (3) The feed solution is repeatedly filtered and washed with deionized water until the filtrate after washing is neutral, and a solid precipitate is collected; the solid precipitate is calcined and cooled to room temperature to obtain gamma iron oxide modified corn straw carbon. (4) Add gamma iron oxide-modified corn straw carbon to a vanadium-containing wastewater solution. Under acidic conditions, the vanadium in the vanadium-containing wastewater solution is adsorbed. After solid-liquid separation, the obtained solid is dried to obtain a vanadium-loaded composite material.

[0009] Furthermore, in step (1), the ratio of the total mass of ferrous chloride and ferric chloride to the mass of activated corn stalk carbon is 1:1~5.

[0010] Furthermore, in step (1), the activated corn stalk carbon is prepared by the following steps: a. Crush and sieve the corn stalks to obtain corn stalk powder; b. Add corn stalk powder to hydrochloric acid and stir to acid wash, then wash with deionized water until neutral, dry, and obtain pretreated biomass; c. The pretreated biomass was heated to 700℃ under an inert atmosphere for carbonization, and then cooled to obtain corn straw carbon; d. Grind and mix corn stalk carbon with KOH, heat to 800°C under an inert atmosphere for activation, and cool to obtain the activated product, wherein the activation temperature is higher than the carbonization temperature; e. Add the activated product to hydrochloric acid, stir and acid wash, then wash with deionized water until neutral, and dry to obtain activated corn stalk carbon.

[0011] Furthermore, in step c, the inert atmosphere is argon, the heating rate is 3℃ / min, the isothermal carbonization time is 1h, and the furnace is naturally cooled to room temperature. In step d, the mass ratio of corn stalk carbon to KOH is 1:1, the inert atmosphere is argon, the heating rate is 3℃ / min, and the activation time is 1h.

[0012] Furthermore, in step b, the mass fraction of hydrochloric acid is 10%, the pickling time is 12 hours, and the drying temperature is 80°C. In step e, the hydrochloric acid has a mass fraction of 10%, and the drying temperature is 80°C.

[0013] Furthermore, in step (2), the concentration of ammonia is 0.01~1 mol / L, and the pH is adjusted to 8~14.

[0014] Furthermore, in step (3), the calcination temperature is 200~1000℃ and the heating rate is 1~10℃ / min.

[0015] Furthermore, in step (4), the acidic conditions are pH 1 to 6; the concentration of vanadium in the vanadium-containing wastewater solution is 50 mg / L to 1000 mg / L.

[0016] Furthermore, in step (4), the adsorption time is 0.25~48h and the adsorption temperature is 15~55℃.

[0017] The present invention also provides an application of the vanadium-loaded composite material obtained by the above method in the preparation of an all-vanadium redox flow battery.

[0018] This invention also provides a method for preparing an all-vanadium redox flow battery, comprising the following steps: a. Load the vanadium-loaded composite material obtained by the above method onto graphite felt to obtain a vanadium-loaded composite electrode; b. Using the vanadium-loaded composite electrode as the electrode, assemble it with a separator, bipolar plate and current collector, and inject vanadium-containing electrolyte to obtain a full vanadium redox flow battery.

[0019] Further, in step a, the vanadium-loaded composite electrode is obtained by dispersing the vanadium-loaded composite material in a Nafion solution, ultrasonically dispersing it to obtain an impregnation solution, immersing the graphite felt in the impregnation solution and drying it, and repeating the immersion and drying operation until the impregnation solution is completely absorbed.

[0020] Furthermore, the loading of vanadium-loaded composite material on the graphite felt is 5 mg to 500 mg.

[0021] The beneficial effects of this invention are: 1. This invention uses an in-situ chemical coprecipitation method to prepare γ-Fe2O3 modified corn straw carbon, so that γ-Fe2O3 is uniformly loaded on the surface of activated corn straw carbon, which increases the active adsorption sites on the material surface and improves the adsorption capacity of the composite material for vanadium ions in water.

[0022] 2. This invention utilizes activated corn stalk carbon as a carrier, which not only has a large specific surface area and good structural stability, but also has a wide range of raw material sources and low cost, which is conducive to the large-scale preparation of adsorption materials.

[0023] 3. This invention combines vanadium adsorption and recovery in the treatment of vanadium-containing wastewater with the application of vanadium redox flow batteries, avoiding the problem of vanadium resources being discarded as pollutants in traditional wastewater treatment. It realizes the transformation of vanadium from pollution control to energy material utilization, and improves resource utilization efficiency.

[0024] 4. The vanadium-loaded composite material prepared by the present invention after vanadium adsorption can be directly used as a modified material for the electrode of vanadium redox flow battery, reducing the additional processing steps in the traditional electrode material preparation process, and providing a new technical solution for developing low-cost, high-performance vanadium redox flow battery electrode materials.

[0025] 5. The method of the present invention has a simple process flow, mild operating conditions, good environmental adaptability and application promotion value, and can be used in the treatment of vanadium-containing industrial wastewater and the recycling of vanadium resources. Attached Figure Description

[0026] Figure 1 Scanning electron microscope images of γ-Fe2O3@KOH-CSC and γ-Fe2O3@KOH-CSC(V) obtained in Example 1; Among them, (a) is a scanning electron microscope image of gamma iron oxide modified corn straw carbon γ-Fe2O3@KOH-CSC; (b) is a scanning electron microscope image of the vanadium-loaded composite material γ-Fe2O3@KOH-CSC(V); Figure 2 X-ray diffraction patterns of the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF obtained in Example 2 and the blank graphite felt electrode; Figure 3 Scanning electron microscope images of the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF obtained in Example 2 and the blank graphite felt electrode; Among them, (a) is a scanning electron microscope image of a blank graphite felt; (b) is a scanning electron microscope image of the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF; Figure 4 Scanning electron microscope images of the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF obtained in Example 2, and its distribution of carbon, iron, oxygen and vanadium elements; Among them, (a) is a scanning electron microscope image of a vanadium-loaded composite electrode; (b) is a map showing the distribution of carbon elements; (c) is a map showing the distribution of iron. (d) is a map showing the distribution of oxygen; (e) is a distribution map of vanadium; Figure 5 The rate performance diagrams show the vanadium redox flow batteries assembled from the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF obtained in Example 2 and the blank graphite felt electrode, respectively. Wherein, (a) is 100 mA cm -2 Charge-discharge curves of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF and blank graphite felt electrode at current density; (b) 200 mA cm -2 Charge-discharge curves of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF and blank graphite felt electrode at current density; (c) is 300 mA cm -2 Charge-discharge curves of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF and blank graphite felt electrode at current density; Figure 6 The cycling performance of all-vanadium redox flow batteries assembled with the vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF obtained in Example 2 and a blank graphite felt electrode are shown in the figure. Among them, (a) is 150 mA cm -2 Charge-discharge curves of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF and blank graphite felt electrode at the first and 50th cycles under the current density; (b) is 150 mA cm -2 Capacity retention rates of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF and blank graphite felt electrode at current density. Detailed Implementation

[0027] The present invention will now be described in further detail with reference to specific embodiments, so that those skilled in the art can understand it.

[0028] Example 1 1. A method for preparing activated corn straw carbon (KOH-CSC), comprising the following steps: a. Cut commercially available corn stalks into 2-4cm long pieces, crush them with a high-speed grinder, pass them through a 100-mesh sieve, collect the sieve material, and obtain corn stalk powder; b. Add the powder obtained in step a to 10% hydrochloric acid and stir magnetically for 12 hours; then repeatedly filter and wash with deionized water until the filtrate is neutral; finally dry in an 80℃ forced-air drying oven to obtain pretreated biomass. c. Place the biomass obtained in step b in a tube furnace, raise the temperature to 700°C at a rate of 3°C / min under argon protection, carbonize at a constant temperature for 1 hour, and allow it to cool naturally to room temperature with the furnace to obtain corn stalk carbon (CSC). d. Grind and mix the corn stalk carbon obtained in step c with KOH at a mass ratio of 1:1, transfer the mixture to a tube furnace, raise the temperature to 800℃ at a heating rate of 3℃ / min under argon protection, keep it at the temperature for 1 hour, cool it to room temperature and take it out to obtain the activated product. e. To remove residual activator and potassium salt, the activated product obtained in step d is added to 10% hydrochloric acid and magnetically stirred for acid washing. Then, it is repeatedly filtered and washed with deionized water until the filtrate is neutral. It is then dried in an 80°C forced-air drying oven to obtain activated corn stalk carbon (KOH-CSC).

[0029] 2. A method for adsorbing vanadium into wastewater from corn stalk carbon recovery by modifying it with gamma-iron oxide, comprising the following steps: (1) Weigh 1g of activated corn stalk carbon (KOH-CSC). Based on a molar ratio of ferrous ions in ferrous chloride to ferric ions in ferric chloride of 1:2, weigh 0.378g of ferrous chloride and 1.614g of ferric chloride hexahydrate. The total mass of ferrous chloride and ferric chloride is 1.992g, and the mass ratio of ferrous chloride to corn stalk carbon is 1.99:1. (2) Mix corn stalk carbon, ferrous chloride and ferric chloride to obtain a mixture, dissolve the mixture in 120 mL of deionized water, and ultrasonically disperse at 70 °C for 15 min to obtain a dispersion; (3) Heat and stir the dispersion at 80°C for 30 min, then add 150 mL of 0.5 mol / L ammonia water dropwise to the dispersion using a peristaltic pump to adjust the pH of the dispersion to 10.0 to 11.0. At this time, iron hydroxide is deposited in situ on the surface of corn straw carbon, and the system changes from brownish-yellow to black. Continue stirring for 45 min and then cool naturally to room temperature to obtain a liquid containing solid precipitate. (4) The liquid containing the solid precipitate was repeatedly filtered and washed with deionized water until the filtrate was neutral. The solid precipitate was collected. The solid precipitate was placed in a muffle furnace and calcined at 250°C at a rate of 3°C / min under air atmosphere and kept at the temperature for 1 hour. After cooling to room temperature, gamma iron oxide modified corn straw carbon γ-Fe2O3@KOH-CSC was obtained. (5) Measure 25 mL of vanadium-containing wastewater solution with a vanadium concentration of 300 mg / L and place it in an Erlenmeyer flask. Add 25 mg of the above-mentioned gamma iron oxide modified corn straw carbon. Adjust the pH of the system to 4.0 with 1 mol / L hydrochloric acid. After sealing with a sealing film, place the flask in a horizontal shaker and shake for 24 h at 25 °C and 180 r / min. After the adsorption is completed, perform solid-liquid separation using an aqueous filter membrane with a pore size of 0.45 μm. Dry the obtained solid in an 80 °C forced-air drying oven for 12 h to obtain the vanadium-loaded composite material γ-Fe2O3@KOH-CSC(V).

[0030] The vanadium removal rate was determined to be 62.0% under these conditions, with a corresponding equilibrium adsorption capacity of 186 mg / g.

[0031] Example 2 A method for preparing an all-vanadium redox flow battery includes the following steps: (1) Preparation of vanadium-loaded composite electrode: Weigh 25 mg γ-Fe2O3@KOH-CSC(V), disperse it in 5 mL of 0.1% Nafion solution, sonicate for 30 min to obtain a dispersion, then immerse the graphite felt in the above dispersion and dry it completely in an 80℃ forced-air drying oven. Repeat the above steps until all the dispersion is completely absorbed, and finally prepare the vanadium-loaded composite electrode (γ-Fe2O3@KOH-CSC(V)-GF).

[0032] (2) Battery assembly: The vanadium redox flow cell mainly consists of a battery separator, electrode frame, and graphite felt electrode GF (thickness 4.35mm, 3) from the inside out. The assembly consists of a 3cm bipolar plate, a sealing ring, a current collector, an insulating gasket, and a clamp. The separator is a Nafion 212 membrane; the electrode frame is made of black fluororubber; the bipolar plate is a high-purity graphite plate with internally etched serpentine channels; the current collector is a gold-plated copper plate; and the clamp is made of aluminum alloy. During single-cell assembly, all components are tightened together with an inside angle wrench using uniform and consistent force. Both the positive and negative electrolytes are 30mL of 1.7MV solution. 3+ / VO 2+ +3 M H2SO4. Before testing, nitrogen gas is continuously introduced into the negative electrode electrolyte tank for 10 minutes to prevent V during charging and discharging. 2+ The electrolyte is oxidized and then the negative electrode electrolyte tank is sealed. The electrolyte is then pumped through the single cell at a flow rate of 40 mL / min using a peristaltic pump to obtain a vanadium redox flow battery.

[0033] The above performance tests of the all-vanadium redox flow battery: Single-cell performance was tested using the Newway Battery Testing System (CT 4008 T-5V / 6A). Rate performance testing was conducted with current densities ranging from 100-300 mA cm⁻¹. -2 Cyclic performance test current density is 150 mA cm⁻¹ -2 Voltage range: 0.8-1.65V.

[0034] 1. Scanning electron microscopy characterization of gamma-FeO modified corn straw carbon γ-Fe2O3@KOH-CSC and vanadium-loaded composite material γ-Fe2O3@KOH-CSC(V) Depend on Figure 1 (a) It can be seen that before adsorption, the surface of γ-Fe2O3@KOH-CSC is rough and granular, and the carbon matrix surface is covered with a large number of fine particles, indicating that γ-Fe2O3 has been successfully loaded onto the KOH-CSC surface. The introduction of γ-Fe2O3 particles increases the surface roughness and active sites of the material, while the material still retains a certain porosity and crack structure, which is conducive to the diffusion and contact of vanadium during the adsorption process.

[0035] Depend on Figure 1 (b) It can be seen that after vanadium adsorption, the particle aggregation and covering phenomenon on the sample surface is more obvious, and some pores are filled or covered, indicating that vanadium is enriched and fixed on the material surface and in the pores.

[0036] 2. X-ray diffraction characterization of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF Depend on Figure 2It can be seen that both the blank graphite felt electrode and the vanadium-loaded composite electrode exhibit broad and diffuse diffraction peaks near 2θ≈22°, which belong to the graphite-like (002) crystal plane. The vanadium-loaded composite electrode also shows characteristic diffraction peaks near 35.6° and 62.9°, corresponding to the (311) and (440) crystal planes of γ-Fe2O3, respectively. The vanadium-loaded composite electrode did not show obvious diffraction peaks of new crystalline vanadium compounds, indicating that vanadium may not exist in the form of a large amount of crystalline vanadium oxide or iron vanadate precipitation, but rather in a highly dispersed surface-bound state or amorphous vanadium oxide species fixed on the material surface.

[0037] 3. Scanning electron microscopy characterization of vanadium-loaded composite electrode γ-Fe2O3@KOH-CSC(V)-GF Depend on Figure 3 (a) It can be seen that the original graphite felt is composed of a large number of interlaced carbon fibers with relatively smooth fiber surfaces. The fibers form an open three-dimensional network structure, which is conducive to electrolyte flow and ion transport; however, its surface roughness is low and the effective active sites are limited.

[0038] Depend on Figure 3 (b) It can be seen that after loading γ-Fe2O3@KOH-CSC(V), a large number of granular and flaky deposits appeared on the surface of the graphite felt fibers, and the surface became significantly rougher, indicating that γ-Fe2O3@KOH-CSC(V) was successfully loaded onto the surface of the graphite felt fibers. At the same time, the composite electrode still maintains the original interwoven fiber structure, and the pores between the fibers are not completely blocked, indicating that the loading process introduces active components while preserving the three-dimensional conductive framework and electrolyte transport channels of the graphite felt.

[0039] 4. Energy dispersive spectroscopy (EDS) characterization of vanadium-loaded composite electrode γ-Fe₂O₃@KOH-CSC(V)-GF The vanadium-loaded composite electrode was tested using an energy dispersive spectroscopy (EDS) instrument paired with a scanning electron microscope.

[0040] Depend on Figure 4 As shown in (b)~(e), C element is widely distributed throughout the region, indicating that graphite felt and carbon-based materials still constitute the main structure of the composite electrode; Fe and O elements are clearly distributed in the loading region on the fiber surface, proving that γ-Fe2O3 has been successfully introduced into the graphite felt surface; V element is uniformly distributed in the loading region, indicating that γ-Fe2O3@KOH-CSC(V) has been successfully fixed on the surface of the composite electrode.

[0041] 5. Rate performance testing of vanadium redox flow batteries Depend on Figure 5 It can be seen that at 100, 200, and 300 mA cm -2At the specified current density, all vanadium redox flow batteries assembled using the γ-Fe2O3@KOH-CSC(V)-GF composite electrode prepared in this invention exhibit lower polarization voltage and higher discharge capacity.

[0042] 6. Cyclic performance testing of vanadium redox flow batteries Depend on Figure 6 It can be seen that the vanadium redox flow battery assembled with the γ-Fe2O3@KOH-CSC(V)-GF composite electrode prepared in the example maintains a high discharge capacity, with a capacity retention rate of 51.5% after 100 cycles.

[0043] This invention improves the adsorption and enrichment capacity of vanadium ions in water by constructing γ-Fe2O3-modified corn straw carbon composite material, and further applies the adsorbed and recovered vanadium-containing composite material to the electrode system of vanadium redox flow battery, thereby achieving an effective combination of vanadium-containing wastewater treatment and vanadium resource energy storage and utilization, and thus improving the efficiency of vanadium resource recycling.

[0044] All other parts not described in detail are existing technologies. Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for adsorbing vanadium from wastewater in corn stalk carbon recovery by modifying it with gamma-iron oxide, characterized in that, Includes the following steps: (1) Activated corn stalk carbon, ferrous chloride, and ferric chloride are mixed to obtain a mixture. The mixture is dissolved in deionized water and ultrasonically dispersed to obtain a dispersion. Among them, ferrous chloride contains Fe 2+ Fe with ferric chloride 3+ The molar ratio is 1:1~3; (2) Heat and stir the dispersion, then add ammonia water dropwise to the dispersion to adjust the pH of the dispersion to alkaline, continue stirring and then cool to obtain a liquid containing solid precipitate; (3) The liquid containing solid precipitate was repeatedly filtered and washed with deionized water until the filtrate was neutral. The solid precipitate was collected. The solid precipitate was calcined and cooled to room temperature to obtain gamma iron oxide modified corn straw carbon. (4) Add gamma iron oxide-modified corn straw carbon to a vanadium-containing wastewater solution. Under acidic conditions, the vanadium in the vanadium-containing wastewater solution is adsorbed. After solid-liquid separation, the obtained solid is dried to obtain a vanadium-loaded composite material.

2. The adsorption method according to claim 1, characterized in that, In step (1), the ratio of the total mass of ferrous chloride and ferric chloride to the mass of activated corn stalk carbon is 1:1~5.

3. The adsorption method according to claim 1, characterized in that, In step (1), the activated corn stalk carbon is prepared by the following steps: a. Crush and sieve the corn stalks to obtain corn stalk powder; b. Add corn stalk powder to hydrochloric acid and stir to acid wash, then wash with deionized water until neutral, dry, and obtain pretreated biomass; c. The pretreated biomass was heated to 700℃ under an inert atmosphere for carbonization, and then cooled to obtain corn straw carbon; d. Grind and mix corn stalk charcoal with KOH, heat to 800℃ under an inert atmosphere for activation, and obtain the activated product after cooling; e. Add the activated product to hydrochloric acid, stir and acid wash, then wash with deionized water until neutral, and dry to obtain activated corn stalk carbon.

4. The adsorption method according to claim 1, characterized in that, In step c, the inert atmosphere is argon, the heating rate is 3℃ / min, the isothermal carbonization time is 1h, and the furnace is naturally cooled to room temperature. In step d, the mass ratio of corn stalk carbon to KOH is 1:1, the inert atmosphere is argon, the heating rate is 3℃ / min, and the activation time is 1h.

5. The method for preparing activated corn straw carbon according to claim 3 or 4, characterized in that, In step b, the mass fraction of hydrochloric acid is 10%, the pickling time is 12 h, and the drying temperature is 80℃. In step e, the hydrochloric acid has a mass fraction of 10%, and the drying temperature is 80°C.

6. The adsorption method according to claim 1, characterized in that, In step (2), the concentration of ammonia is 0.01~1mol / L, and the pH is adjusted to 8~14; in step (3), the calcination temperature is 200~1000℃, and the heating rate is 1~10℃ / min.

7. The adsorption method according to claim 1, characterized in that, In step (4), the acidic conditions are pH 1 to 6; the concentration of vanadium in the vanadium-containing wastewater solution is 50 mg / L to 1000 mg / L; the adsorption time is 0.25 to 48 h; and the adsorption temperature is 15 to 55 °C.

8. The application of the vanadium-loaded composite material obtained by the method of claim 1 in the preparation of an all-vanadium redox flow battery.

9. A method for preparing an all-vanadium redox flow battery, characterized in that: Includes the following steps: a. Load the vanadium-loaded composite material obtained by the method described in claim 1 onto a graphite felt to obtain a vanadium-loaded composite electrode; b. Using the vanadium-loaded composite electrode as the electrode, assemble it with a separator, bipolar plate and current collector, and inject vanadium-containing electrolyte to obtain a full vanadium redox flow battery.

10. The preparation method according to claim 9, characterized in that: In step a, the vanadium-loaded composite electrode is prepared by dispersing the vanadium-loaded composite material in a Nafion solution, ultrasonically dispersing it to obtain an impregnation solution, immersing the graphite felt in the impregnation solution and drying it, and repeating the immersion and drying operation until the impregnation solution is completely absorbed to obtain the vanadium-loaded composite electrode; wherein, the loading amount of the vanadium-loaded composite material on the graphite felt is 5mg~500mg.