A solid waste-based modified concrete and its preparation method
By using solid waste materials and hydrophobic nano-magnesium oxide modification in concrete, the problems of insufficient compressive strength and durability of recycled concrete are solved, the overall performance of concrete is improved, and the recycling and reuse of solid waste is realized.
Patent Information
- Application Number
- CN202611290047.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-10
AI Technical Summary
Existing recycled concrete lacks sufficient compressive strength and durability, failing to meet the standards for high-performance concrete.
Solid waste materials are used to replace silicate cement, and hydrophobic nano-magnesium oxide is added for modification. By preparing a polymer structure of hydrophobic nano-magnesium oxide, the crack resistance and hydrophobicity of concrete are enhanced.
It improves the compressive strength, impermeability, frost resistance and crack resistance of concrete, realizes the recycling and reuse of solid waste materials, and reduces production costs.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of concrete technology, specifically relating to a solid waste-based modified concrete and its preparation method. Background Technology
[0002] Concrete (abbreviated as "concrete") is an engineering composite material made by binding aggregates together with cementing materials. The most common type is cement concrete, which uses cement as the cementing material, sand and stone as aggregates, and water (with admixtures and additives added) to be mixed and hardened in proportion. Concrete has the advantages of readily available raw materials, low cost, and simple production process. It also has the characteristics of high compressive strength, excellent durability, and a wide range of strength grades. Its performance can be customized and adjusted according to needs to adapt to different engineering scenarios. In addition to its large-scale use in various civil engineering projects, it can also be applied to special fields such as shipbuilding, machinery industry, marine development, and geothermal engineering. As one of the most consumed artificial building materials in the world, concrete has a very large annual consumption. At the same time, the carbon dioxide emissions from traditional concrete production are relatively large. In order to reduce carbon emissions at the production end, methods such as reducing the amount of clinker and replacing raw materials with industrial waste are usually adopted to adapt to the current "dual carbon" development goals of the concrete industry.
[0003] Industrial solid waste refers to fly ash, steel slag, red mud, coal gangue, smelting slag, chemical slag, oily sludge, etc. generated in industrial production. Using solid waste in concrete can not only consume a large amount of solid waste, significantly reduce the land occupation and environmental pollution caused by solid waste landfill, but also replace some cement and natural sand and gravel, reduce the exploitation of natural resources, reduce carbon emissions from cement production, and promote the development of the concrete industry towards a green and low-carbon direction. In particular, the cost of solid waste raw materials is much lower than that of cement, which can significantly reduce the overall production cost of concrete. With reasonable proportioning, the impermeability, carbonation resistance, frost resistance and corrosion resistance of concrete can be improved, resulting in solid waste-based concrete with excellent comprehensive performance.
[0004] Chinese patent application CN202610802260.3 discloses a recycled concrete and its preparation method. The raw materials of the recycled concrete include cement, coarse and fine aggregates, recycled aggregates, modified magnesium oxide powder, water, water-reducing agent and carbon dioxide solution. The modified magnesium oxide powder includes three activity levels: high, medium and low, which play a role in the mixing stage, curing stage and long-term service stage, respectively, to achieve early strength improvement, mid-term strengthening and crack self-repair. This method promotes the efficient utilization of recycled aggregates and the reduction of carbon dioxide emissions. However, the compressive strength and durability of this recycled concrete are insufficient and cannot meet the standards of high-performance concrete. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing technologies by providing a solid waste-based modified concrete and its preparation method. The solid waste-based modified concrete provided by this invention uses solid waste materials to replace silicate cement, realizing the recycling and reuse of solid waste materials. At the same time, hydrophobic nano-magnesium oxide is added to modify the concrete, resulting in solid waste-based modified concrete with good mechanical properties, impermeability, durability and crack resistance.
[0006] The technical solution adopted by the present invention to achieve the above objectives is as follows: A solid waste-based modified concrete, comprising the following components by weight: 30-40 parts silicate cement; 40-50 parts solid waste material; 20-25 parts fly ash; 12-15 parts limestone; 8-10 parts hydrophobic nano-magnesium oxide; and 3-5 parts alkali activator.
[0007] Furthermore, the solid waste material is composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:1.5-2:0.5-1.
[0008] Furthermore, the alkaline activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1-1.2.
[0009] Furthermore, the hydrophobic nano-magnesium oxide is prepared by the following method: S1. Add nano-magnesium oxide to a 60-70 wt% ethanol solution, stir until homogeneous, slowly add vinyltrimethoxysilane, adjust the pH to 6.0-6.5, place at 40-50℃, stir and react for 5-6 hours to obtain alkenylated nano-magnesium oxide. S2. Add alkenylated magnesium oxide to deionized water and stir until homogeneous. Add acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphonic acid. Under nitrogen protection, place at 70-80℃, add initiator, and continue stirring for 4-5 hours to obtain hydrophobic nano-magnesium oxide.
[0010] Further, in step S1, the mass ratio of nano-magnesium oxide to vinyltrimethoxysilane is 1:0.05-0.08.
[0011] Further, in step S2, the mass ratio of acrylic acid, acrylamide, styrene, allylpyrene phenylphosphonic acid, and alkenylated nano-magnesium oxide is 1:1.5-2:0.5-0.8:0.8-1:3-5.
[0012] Further, the amount of initiator used in step S2 is 0.2-0.3% of the total mass of acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphonic acid; the initiator is ammonium persulfate.
[0013] Furthermore, the allylpyrene phenylphosphonic acid is prepared by the following method: (1) Add 1-pyrenebutanol and triethylamine to anhydrous chloroform, stir until homogeneous, slowly add allyl glycidyl ether, place at 50-60℃ and stir for 4-5 h to obtain allyl pyrene alcohol; (2) Add 4-aminophenyl phosphate and N,N'-carbonyldiimidazole to acetonitrile, place at room temperature and stir for 6-7 h, then add allylpyrene alcohol, place at 70-80℃ and continue stirring for 5-6 h to obtain allylpyrene phenyl phosphate.
[0014] Further, the molar ratio of 1-pyrenebutanol, allyl glycidyl ether, and triethylamine in step (1) is 1:1.1-1.2:1.1-1.2.
[0015] Further, in step (2), the molar ratio of 4-aminophenyl phosphate, N,N'-carbonyldiimidazole and allylpyrene is 1:1.1-1.2:1.1-1.2.
[0016] The present invention also provides a method for preparing solid waste-based modified concrete, comprising the following steps: according to the mass ratio, silicate cement, solid waste materials, fly ash, limestone, hydrophobic nano magnesium oxide and alkali activator are mixed evenly to obtain solid waste-based modified concrete.
[0017] The present invention has the following beneficial effects: To obtain solid waste-based modified concrete with good comprehensive performance, this invention uses 1-pyrenebutanol as a raw material, which is reacted sequentially with allyl glycidyl ether, 4-aminophenyl phosphate, and N,N'-carbonyldiimidazole to prepare allylpyrene phenyl phosphate containing pyrene, phosphate, and allyl groups in its structure. This invention also uses vinyltrimethoxysilane to modify nano-magnesium oxide, introducing vinyl groups onto the surface of the nano-magnesium oxide. Furthermore, a polymer is formed by polymerizing the vinyl groups with acrylic acid, acrylamide, styrene, and allylpyrene phenyl phosphate, further introducing a polymer structure containing carboxyl groups, rigid benzene rings, pyrene groups, and phosphate groups onto the surface of the nano-magnesium oxide. The nano-magnesium oxide, through hydration, generates magnesium hydroxide, resulting in volume expansion that can compensate for the shrinkage stress of concrete, inhibit crack formation, and exert a certain anti-cracking effect. Nanostructures can effectively fill micropores, reduce porosity, and enhance the density of concrete, thus improving its compressive strength, impermeability, and freeze-thaw resistance. The carboxyl and phosphate groups in the polymer structure can strongly coordinate with calcium ions in the hydration products, enhancing the bonding force between hydrophobic nano-magnesium oxide and other concrete components. This helps reduce shrinkage stress concentration, improves the uniformity of shrinkage stress distribution, and further enhances the crack resistance of concrete. The hydrophobic rigid benzene rings, the pyrene groups containing rigid conjugated planar structures, and the strong hydrophobic properties of the polymer structure impart strong hydrophobicity to concrete, effectively reducing its absorption of moisture and corrosive ions from the environment. This further improves the impermeability and durability of concrete, and also helps enhance its mechanical properties.
[0018] The solid waste-based modified concrete provided by this invention replaces silicate cement with solid waste materials, realizing the recycling and reuse of solid waste materials. At the same time, hydrophobic nano-magnesium oxide is added to modify the concrete, resulting in solid waste-based modified concrete with good mechanical properties, impermeability, durability and crack resistance. Detailed Implementation
[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0020] The raw materials used in this invention are all commercially available products, including limestone (CAS number 1317-65-3), sodium hydroxide (CAS number 1310-73-2), sodium silicate (CAS number 1344-09-8), nano magnesium oxide (CAS number 1309-48-4), vinyltrimethoxysilane (CAS number 2768-02-7), acrylic acid (CAS number 79-10-7), acrylamide (CAS number 79-06-1), and styrene (CAS number 100). -42-5; Ammonium persulfate CAS No. 7727-54-0; 1-Pyrenebutanol CAS No. 67000-89-9; Allyl glycidyl ether CAS No. 106-92-3; 4-Aminophenyl phosphate CAS No. 52331-30-3; N,N'-carbonyldiimidazole CAS No. 530-62-1; Triethylamine CAS No. 121-44-8; Acetonitrile CAS No. 75-05-8; Chloroform CAS No. 67-66-3.
[0021] Example 1 This embodiment provides a method for preparing allylpyrene phenylphosphonic acid:
[0022] (1) Add 25.0g of 1-pyrenebutanol and 10.1g of triethylamine to 500mL of anhydrous chloroform, stir well, slowly add 11.4g of allyl glycidyl ether, place at 60℃ and stir for 4.5h. After the reaction is complete, remove the anhydrous chloroform, extract, concentrate and dry to obtain 29.4g of allyl pyrene; wherein the molar ratio of 1-pyrenebutanol, allyl glycidyl ether and triethylamine is 1:1.1:1.1; Allylpyrene: ESI (m / z): 389.5 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 8.31-8.34 (m, 1H), 8.03-8.08 (m, 4H), 7.87-7.91 (m, 2H), 7.70-7.74 (m, 2H), 6.07-6.10 (m, 1H), 5.77 (s, 1H), 5.34-5.38 (m, 2H), 4.00-4.04 (m, 3H), 3.63-3.66 (m, 2H), 3.35-3.38 (m, 4H), 3.07-3.10 (m, 2H), 1.52-1.58 (m, 4H); (2) Add 13.0 g of 4-aminophenyl phosphate and 12.3 g of N,N'-carbonyldiimidazole to 500 mL of acetonitrile, stir at room temperature for 7 h, then add 29.4 g of allylpyrene alcohol, stir at 80 °C for 6 h. After the reaction is complete, remove anhydrous chloroform, extract, concentrate and dry to obtain 34.5 g of allylpyrene phenyl phosphate; wherein the molar ratio of 4-aminophenyl phosphate, N,N'-carbonyldiimidazole and allylpyrene alcohol is 1:1.1:1.1; Allylpyrene phenylphosphonic acid: ESI (m / z): 604.6 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 9.88 (s, 1H), 8.32-8.35 (m, 1H), 8.04-8.08 (m, 4H) , 7.88-7.92 (m, 2H), 7.71-7.74 (m, 2H), 7.56 (d, J=8.4Hz, 2H), 7.38 (d, J=8.4Hz, 2H) , 6.08-6.11 (m, 1H), 5.34-5.37 (m, 2H), 5.07-5.10 (m, 1H), 4.20 (s, 2H), 4.02-4.05 ( m, 2H), 3.71-3.75 (m, 2H), 3.38-3.42 (m, 4H), 3.08-3.11 (m, 2H), 1.53-1.58 (m, 4H).
[0023] Example 2 This embodiment provides a solid waste-based modified concrete, which comprises the following components by weight: 40 parts silicate cement; 50 parts solid waste material; 23 parts fly ash; 15 parts limestone; 10 parts hydrophobic nano-magnesium oxide; and 5 parts alkali activator. The solid waste material is composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:2:1. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.2.
[0024] Hydrophobic nano-magnesium oxide was prepared by the following method: S1. Add nano-magnesium oxide to a 70wt% ethanol solution, stir until homogeneous, slowly add vinyltrimethoxysilane, adjust the pH to 6.5, place at 40℃, stir and react for 6 hours. After the reaction is complete, filter, wash and dry to obtain alkenylated nano-magnesium oxide; wherein the mass ratio of nano-magnesium oxide to vinyltrimethoxysilane is 1:0.08. S2. Add alkenylated magnesium oxide to deionized water and stir until homogeneous. Add acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. Under nitrogen protection, place at 80°C, add initiator, and continue stirring for 4 hours. After the reaction is complete, filter, wash, and dry to obtain hydrophobic nano-magnesium oxide. The mass ratio of acrylic acid, acrylamide, styrene, allylpyrene phenylphosphic acid, and alkenylated nano-magnesium oxide is 1:2:0.7:1:5. The amount of initiator is 0.3% of the total mass of acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. The initiator is ammonium persulfate.
[0025] This embodiment also provides a method for preparing solid waste-based modified concrete, including the following steps: according to the mass ratio, silicate cement, solid waste materials, fly ash, limestone, hydrophobic nano magnesium oxide, and alkali activator are mixed evenly to obtain solid waste-based modified concrete.
[0026] Example 3 This embodiment provides a solid waste-based modified concrete, which comprises the following components by weight: 35 parts silicate cement; 45 parts solid waste materials; 20 parts fly ash; 13 parts limestone; 9 parts hydrophobic nano-magnesium oxide; and 4 parts alkali activator. The solid waste materials are composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:1.8:0.7. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.1.
[0027] Hydrophobic nano-magnesium oxide was prepared by the following method: S1. Add nano-magnesium oxide to a 65wt% ethanol solution, stir until homogeneous, slowly add vinyltrimethoxysilane, adjust the pH to 6.2, place at 45℃, stir and react for 5.5h. After the reaction is complete, filter, wash and dry to obtain alkenylated nano-magnesium oxide; wherein the mass ratio of nano-magnesium oxide to vinyltrimethoxysilane is 1:0.06. S2. Add alkenylated magnesium oxide to deionized water and stir until homogeneous. Add acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. Under nitrogen protection, place at 75°C, add initiator, and continue stirring for 4.5 hours. After the reaction is complete, filter, wash, and dry to obtain hydrophobic nano-magnesium oxide. The mass ratio of acrylic acid, acrylamide, styrene, allylpyrene phenylphosphic acid, and alkenylated nano-magnesium oxide is 1:1.8:0.5:0.9:4. The amount of initiator is 0.25% of the total mass of acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. The initiator is ammonium persulfate.
[0028] This embodiment also provides a method for preparing solid waste-based modified concrete, including the following steps: according to the mass ratio, silicate cement, solid waste materials, fly ash, limestone, hydrophobic nano magnesium oxide, and alkali activator are mixed evenly to obtain solid waste-based modified concrete.
[0029] Example 4 This embodiment provides a solid waste-based modified concrete, which comprises the following components by weight: 30 parts silicate cement; 40 parts solid waste materials; 25 parts fly ash; 12 parts limestone; 8 parts hydrophobic nano-magnesium oxide; and 3 parts alkali activator. The solid waste materials are composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:1.5:0.5. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.
[0030] Hydrophobic nano-magnesium oxide was prepared by the following method: S1. Add nano-magnesium oxide to a 60wt% ethanol solution, stir until homogeneous, slowly add vinyltrimethoxysilane, adjust the pH to 6.0, place at 50℃, stir and react for 5 hours. After the reaction is complete, filter, wash and dry to obtain alkenylated nano-magnesium oxide; wherein the mass ratio of nano-magnesium oxide to vinyltrimethoxysilane is 1:0.05. S2. Add alkenylated magnesium oxide to deionized water and stir until homogeneous. Add acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. Under nitrogen protection, place at 70°C, add initiator, and continue stirring for 5 hours. After the reaction is complete, filter, wash, and dry to obtain hydrophobic nano-magnesium oxide. The mass ratio of acrylic acid, acrylamide, styrene, allylpyrene phenylphosphic acid, and alkenylated nano-magnesium oxide is 1:1.5:0.8:0.8:3. The amount of initiator is 0.2% of the total mass of acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphic acid. The initiator is ammonium persulfate.
[0031] This embodiment also provides a method for preparing solid waste-based modified concrete, including the following steps: according to the mass ratio, silicate cement, solid waste materials, fly ash, limestone, hydrophobic nano magnesium oxide, and alkali activator are mixed evenly to obtain solid waste-based modified concrete.
[0032] Comparative Example 1 This embodiment provides a solid waste-based modified concrete, which comprises the following components by weight: 40 parts silicate cement; 50 parts solid waste material; 23 parts fly ash; 15 parts limestone; 10 parts alkenylated nano-magnesium oxide; and 5 parts alkali activator. The solid waste material is composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:2:1. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.2.
[0033] The alkenylated nano-magnesium oxide was prepared by the following method: the same as step S1 in Example 2.
[0034] This comparative example also provides a method for preparing solid waste-based modified concrete that is the same as in Example 2.
[0035] Comparative Example 2 This embodiment provides a solid waste-based modified concrete, which comprises the following components by weight: 40 parts silicate cement; 50 parts solid waste material; 23 parts fly ash; 15 parts limestone; 10 parts nano-magnesium oxide; and 5 parts alkali activator. The solid waste material is composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:2:1. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.2.
[0036] This comparative example also provides a method for preparing solid waste-based modified concrete that is the same as in Example 2.
[0037] Comparative Example 3 This embodiment provides a solid waste-based modified concrete, which includes the following components by weight: 40 parts silicate cement; 50 parts solid waste materials; 23 parts fly ash; 15 parts limestone; and 5 parts alkali activator. The solid waste materials are composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:2:1. The alkali activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1.2.
[0038] This comparative example also provides a method for preparing solid waste-based modified concrete that is the same as in Example 2.
[0039] Test case Performance tests were conducted on the solid waste-based modified concrete provided in Examples 2 to 4 and Comparative Examples 1 to 3. Mechanical performance tests were conducted according to GB / T 50081-2019 standard, measuring 28-day compressive strength; water absorption tests were conducted according to SL 352-2020 standard, measuring 48-hour water absorption rate; water contact angle tests were performed using a contact angle measuring instrument and the water droplet method on the concrete contact surface; freeze-thaw performance tests were conducted according to GB / T 50082-2009 standard, measuring the freeze-thaw resistance grade; crack resistance tests were conducted using a crack-resistant plate test, measuring the total crack area per unit area. The results are shown in Table 1.
[0040] Table 1
[0041] As shown in Table 1, the solid waste-based modified concrete provided in Examples 2 to 4 of this invention exhibits high compressive strength, low water absorption, large contact angle, high frost resistance, and small crack area, indicating that the solid waste-based modified concrete provided by this invention possesses excellent mechanical properties, impermeability, durability, and crack resistance. Compared with Comparative Examples 1 to 3, Example 2 of this invention's solid waste-based modified concrete includes hydrophobic nano-magnesium oxide in its composition. The structure of this hydrophobic nano-magnesium oxide comprises nano-magnesium oxide and a polymer formed by the polymerization of its surface vinyl groups with acrylic acid, acrylamide, styrene, and allylpyrene phenyl phosphate. The polymer structure includes carboxyl groups, rigid benzene rings, pyrene groups, and phosphate groups. The nano-magnesium oxide hydrates to generate magnesium hydroxide, resulting in volume expansion, which can compensate for the shrinkage stress of the concrete, inhibit crack formation, and play a certain role in... The nanostructure of the polymer effectively fills micropores, reduces porosity, and enhances the density of concrete, thus improving its compressive strength, impermeability, and freeze-thaw resistance. The carboxyl and phosphate groups in the polymer structure strongly coordinate with calcium ions in the hydration products, enhancing the bonding force between hydrophobic nano-magnesium oxide and other concrete components. This helps reduce shrinkage stress concentration, improves the uniformity of shrinkage stress distribution, and further enhances the crack resistance of concrete. The hydrophobic rigid benzene ring, the pyrene group with a rigid conjugated planar structure and strong hydrophobic properties in the polymer structure impart strong hydrophobicity to the concrete, effectively reducing its absorption of moisture and corrosive ions from the environment. This further improves the impermeability and durability of the concrete, and also contributes to improving its mechanical properties.
[0042] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus; although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A solid waste-based modified concrete, characterized in that, The solid waste-based modified concrete comprises the following components by weight: 30-40 parts silicate cement; 40-50 parts solid waste materials; 20-25 parts fly ash; 12-15 parts limestone; 8-10 parts hydrophobic nano magnesium oxide; and 3-5 parts alkali activator. The hydrophobic nano-magnesium oxide was prepared by the following method: S1. Add nano-magnesium oxide to a 60-70 wt% ethanol solution, stir until homogeneous, slowly add vinyltrimethoxysilane, adjust the pH to 6.0-6.5, place at 40-50℃, stir and react for 5-6 hours to obtain alkenylated nano-magnesium oxide. S2. Add alkenylated magnesium oxide to deionized water and stir until homogeneous. Add acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphonic acid. Under nitrogen protection, place at 70-80℃, add initiator, and continue stirring for 4-5 hours to obtain hydrophobic nano-magnesium oxide.
2. The solid waste-based modified concrete according to claim 1, characterized in that, The mass ratio of nano-magnesium oxide and vinyltrimethoxysilane in step S1 is 1:0.05-0.
08.
3. The solid waste-based modified concrete according to claim 1, characterized in that, The mass ratio of acrylic acid, acrylamide, styrene, allylpyrene phenylphosphonic acid, and alkenylated nano-magnesium oxide in step S2 is 1:1.5-2:0.5-0.8:0.8-1:3-5.
4. The solid waste-based modified concrete according to claim 1, characterized in that, The amount of initiator used in step S2 is 0.2-0.3% of the total mass of acrylic acid, acrylamide, styrene, and allylpyrene phenylphosphoric acid; the initiator is ammonium persulfate.
5. The solid waste-based modified concrete according to claim 1, characterized in that, The allylpyrene phenylphosphonic acid is prepared by the following method: (1) Add 1-pyrenebutanol and triethylamine to anhydrous chloroform, stir until homogeneous, slowly add allyl glycidyl ether, place at 50-60℃ and stir for 4-5 h to obtain allyl pyrene alcohol; (2) Add 4-aminophenyl phosphate and N,N'-carbonyldiimidazole to acetonitrile, place at room temperature and stir for 6-7 h, then add allylpyrene alcohol, place at 70-80℃ and continue stirring for 5-6 h to obtain allylpyrene phenyl phosphate.
6. The solid waste-based modified concrete according to claim 5, characterized in that, The molar ratio of 1-pyrenebutanol, allyl glycidyl ether, and triethylamine in step (1) is 1:1.1-1.2:1.1-1.
2.
7. The solid waste-based modified concrete according to claim 5, characterized in that, The molar ratio of 4-aminophenyl phosphate, N,N'-carbonyldiimidazole and allylpyrene in step (2) is 1:1.1-1.2:1.1-1.
2.
8. The solid waste-based modified concrete according to claim 1, characterized in that, The solid waste material is composed of granulated blast furnace slag, steel slag, and silica fume in a mass ratio of 6:1.5-2:0.5-1.
9. The solid waste-based modified concrete according to claim 5, characterized in that, The alkaline activator is composed of sodium hydroxide and sodium silicate in a mass ratio of 1:1-1.
2.
10. A method for preparing solid waste-based modified concrete as described in any one of claims 1-9, characterized in that, The process includes the following steps: according to the mass ratio, silicate cement, solid waste materials, fly ash, limestone, hydrophobic nano magnesium oxide, and alkali activator are mixed evenly to obtain solid waste-based modified concrete.
Citation Information
Patent Citations
Smelting process
CA100425A
Structure preserving paint
CA106923A
Devices, systems, and methods for delivering fluid to tissue
CA2768027A1
Rail member for mounting sinuously corrugated wire springs
CA530621A
Feeder for perforating machine
CA67663A