A grouting and curing material and method for fluidized solidified soil based on polyurethane-water glass composite grout.
By combining polyurethane-water glass composite grout with modified filler additives, an organic-inorganic cross-linked structure is formed, which solves the problems of insufficient pore filling and low early strength of fluidized solidified soil. This achieves high-strength, low-cost fluidized solidified soil treatment effect and expands its application range in engineering.
Patent Information
- Application Number
- CN202611326271.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-29
- Publication Date
- 2026-11-10
AI Technical Summary
Existing fluidized solidified soil grouting materials suffer from problems such as insufficient pore filling, shrinkage cracking, low early strength, high cost of single chemical grouts, weak interfacial bonding, and poor adaptability. In particular, conventional polyurethane-water glass grouts have failed to effectively solve the problems under the characteristics of high water content and fine particles with large pores.
A two-component grouting matrix based on polyurethane-water glass composite grout is adopted, combined with modified filler admixtures, including fly ash, nano silica and polypropylene fiber. Through layered grouting and intermittent grouting process, an organic-inorganic interpenetrating network cross-linked structure is formed to fill the internal pores of the fluidized solidified soil, improve early strength and shear strength, and repair shrinkage defects through secondary grouting.
It significantly improves the overall density and long-term mechanical stability of fluidized solidified soil, reduces material costs, and is suitable for roadbed backfilling, soft foundation pits, and reinforcement projects of fluidized solidified soil in water conservancy reservoir areas, solving the problems of insufficient pore filling and weak interfacial bonding.
Smart Images

Figure CN123062229A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a grouting and solidification material and method for fluidized solidified soil based on polyurethane-water glass composite slurry. It belongs to the technical fields of resource utilization and disposal of solid waste in geotechnical engineering and solidification treatment of fluidized solidified soil. Background Technology
[0002] With the continuous expansion of domestic infrastructure projects, water conservancy and hydropower projects, and urban underground space development, a large amount of fine-grained, high-moisture soil, such as excavated soil, river dredging silt, and lake sediment, is generated during construction. Traditional methods of transporting and landfilling these materials consume land resources and easily cause water and soil pollution. Resource-based preparation of fluidized bed solidified soil for backfilling has become an important treatment approach. Fluidized bed solidified soil is a high-moisture-content backfill soil formed by mixing solid waste such as excavated soil, silt, and lake sediment with a small amount of cement and solidifying agent. It is widely used in projects such as excavated soil backfilling, highway subgrade, and reservoir backfilling. Fluidized bed solidified soil has high natural porosity, high moisture content, and large compression deformation. Under the action of superstructure loads, it is prone to engineering disasters such as uneven settlement, localized liquefaction, and surface cracking. Therefore, grouting technology is commonly used in engineering projects for its solidification and seepage prevention.
[0003] Currently, grouting and solidification materials for fluidized solidified soil are mainly divided into two categories: inorganic cement-based grouting materials and organic chemical grouting materials. A detailed analysis follows: 1. Cement-based grouting: While the raw materials are inexpensive and the aggregate has good long-term stability, the large particle size of the solid particles inside the grout makes it difficult to penetrate the micron-sized pores within the fluidized, solidified soil. The cement hydration and hardening process involves significant volume shrinkage, leading to new shrinkage cracks in the soil after grouting, reducing the overall reinforcement effect. Furthermore, the slow early hydration rate of cement results in low 24-hour compressive strength of the reinforced soil, failing to meet the time-sensitive requirements of rapid traffic opening and quick backfilling of foundation pits. Although clay-cement composite grout improves fluidity, the cohesion of the aggregate is relatively low, limiting the improvement in shear strength.
[0004] 2. Single organic polymer curing agents (pure polyurethane, acrylate, epoxy resin): The curing system has low viscosity and good dispersibility when mixed with fine-grained soil, and can penetrate into the tiny pores of the soil. However, the unit price of pure organic curing materials is high, and the cost of using them in large-scale sludge treatment projects is difficult to control. The bonding strength between the polymer curing product and soil particles is weak, and the slurry-soil interface is prone to debonding and strength reduction under long-term dynamic load and groundwater soaking environment. The single polyurethane curing system is brittle after curing, and the soil is prone to brittle cracking failure under load.
[0005] 3. Water glass grout: It has good injectability and low cost, but low stone formation rate and serious long-term erosion. It is only suitable for temporary seepage prevention and cannot be used as a permanent soil reinforcement material.
[0006] 4. Conventional Polyurethane-Water Glass Two-Liquid System: Existing research confirms that mixing polyurethane and water glass can form an organic-inorganic interpenetrating network cross-linked structure, balancing toughness and compressive strength. However, existing two-liquid systems have not been modified to address the high water content, fine particle size, and large porosity characteristics of fluidized solidified soil. Direct mixing with silt has certain drawbacks: First, the reaction rate after mixing the two liquids is difficult to control, leading to rapid gelation when mixed with high-water-content soil, resulting in localized clumping and uneven solidification. Second, the system lacks ultrafine fillers, leaving a large number of interconnected pores within the solidified soil, resulting in significant compression deformation. Third, there is a lack of standardized graded mixing and segmented curing processes, and no unified operating procedures exist between indoor samples and on-site in-situ construction, leading to large variations in solidification effects. Furthermore, existing formulations do not incorporate industrial solid waste fillers, resulting in higher overall material costs, and there is a lack of specialized grouting construction techniques suitable for layered, thick-layer backfilling of fluidized solidified soil.
[0007] Existing solidified soil mixing processes are mostly designed for single cement solidification systems, only setting up single mixing and one-time addition of solidifying agent, without considering the rapid cross-linking reaction characteristics of polyurethane-water glass two-component systems. Mixing large quantities of soil and solidifying slurry at one time can easily cause local premature gelation and uneven mixing. At the same time, existing solidification and curing methods only involve simple film covering for moisture retention, without setting up a secondary control step of intermittent addition of solidifying slurry. The shrinkage pores inside the soil cannot be filled a second time, resulting in insufficient long-term stability of the solidified soil. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a grouting and curing material and method for fluidized solidified soil based on polyurethane-water glass composite grout, so as to solve the technical problems of insufficient pore filling, shrinkage cracking, low early strength, high cost of single chemical grout, weak interfacial bonding, and insufficient pore filling and poor adaptability of conventional polyurethane-water glass grout.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A fluidized solidified soil grouting and curing material based on polyurethane-water glass composite grout is made from a two-component grouting matrix and modified filler additives. The two-component grouting matrix is composed of component A and component B. Component A is prepared by mixing liquid sodium silicate, glycerol, and dibutyltin dilaurate. Component B is a mixture of polymeric MDI (polymethylene polyphenyl isocyanate), polyether polyol, chlorinated paraffin, and dioctyl phthalate (DOP). The modified filler additive is selected from any one or a mixture of three of fly ash, nano silica, and polypropylene fiber.
[0010] Preferably, the modified filler additive is selected from any one of fly ash, nano-silica, and polypropylene fiber.
[0011] Further preferred, the amounts of each raw material, by weight, are as follows: Component A: 120 parts liquid sodium silicate, 2 parts glycerol, 0.4 parts dibutyltin dilaurate; Component B: 108 parts of polymeric MDI, 12 parts of polyether polyol, 15.5 parts of chlorinated paraffin, and 8 parts of dioctyl phthalate; Modified filler additives: 0-6 parts fly ash, or 0-6 parts nano silica, or 0-2 parts polypropylene fiber.
[0012] Preferably, the modified filler additive is made by mixing fly ash, nano-silica, and polypropylene fiber.
[0013] Further preferred, the amounts of each raw material, by weight, are as follows: Component A: 120 parts liquid sodium silicate, 2 parts glycerol, 0.4 parts dibutyltin dilaurate; Component B: 108 parts of polymeric MDI, 12 parts of polyether polyol, 15.5 parts of chlorinated paraffin, and 8 parts of dioctyl phthalate; Modified filler additives: 3 parts fly ash, 3 parts nano silica, and 1 part polypropylene fiber.
[0014] Preferably, the modulus of the liquid sodium silicate is 2.23 to 3.33, more preferably 2.68, and the polyether polyol is polyether polyol-210N.
[0015] The aforementioned curing method for a fluidized solidified soil grouting and curing material based on polyurethane-water glass composite slurry includes the following steps: S1. Prepare component A and component B separately; S2. The modified filler additive is uniformly incorporated into component A to obtain modified solution A; S3. Mix the modified liquid A and component B at a volume ratio of 1:1 and stir to obtain a composite slurry; S4. The composite grout is injected into the fluid soil to be solidified using a layered grouting method to complete the grouting and obtain an indoor precast solidified soil sample or an on-site in-situ solidified soil body; S5. Cover with film and seal, then intermittently replenish with slurry for curing.
[0016] Preferably, in step S1, the preparation method of component A is as follows: glycerol and dibutyltin dilaurate are added sequentially to liquid sodium silicate, and the mixture is stirred at a constant speed for 5 minutes at room temperature (25°C) to obtain a uniform and stable component A.
[0017] Preferably, in step S1, the preparation method of component B is as follows: polymeric MDI, polyether polyol, chlorinated paraffin, and dioctyl phthalate are mixed under light-protected conditions and stirred at room temperature for 8 minutes to obtain a homogeneous solution without layering or precipitation, which is component B.
[0018] Preferably, in step S2, the preparation method of the modified liquid A is as follows: the modified filler additive is added to component A in portions, and the mixture is first stirred at a low speed of 80 r / min for 3 min for pre-dispersion, and then the speed is increased to 250 r / min for high-speed stirring for 7 min. The total stirring time is not less than 10 min. After stirring, the mixture is allowed to stand for 2 min to eliminate fiber agglomeration and nanofiller aggregation, ensuring that the filler is completely suspended and dispersed in the water glass system without any visible flocs or precipitates.
[0019] Preferably, the specific method for step S3 is as follows: Pour the modified liquid A and component B into a mixing container simultaneously, and stir at 300 r / min for 20 seconds. It should be noted that the mixture must be combined with the soil within 10 minutes after stirring; if the ambient temperature at the construction site is higher than 30℃, an additional 1g of glycerol can be added to liquid A to extend the workable window of the slurry.
[0020] Preferably, step S4 includes indoor pre-prepared sample conditions and on-site in-situ curing conditions, as detailed below: (1) Indoor precast sample working conditions: S4.1.1 Pretreatment: Silt and slag raw materials are screened to remove large stones, plant roots and stems, and the natural moisture content of the soil is measured. The amount of water added to the soil is adjusted according to the target fluidity. S4.1.2 Premixed soil: Weigh the soil after sieving and pour it into a vertical mixer, mix, and evenly loosen the soil particles; S4.1.3 Staged slurry addition and mixing: The composite slurry is added in stages to obtain a fluid mixture; S4.1.4 Molding and standing: The mixed fluid mixture is immediately poured into a standard mold, vibrated to eliminate large air bubbles inside, and indoor precast solidified soil samples are obtained. (2) On-site in-situ curing conditions: S4.2.1 Soil pretreatment: The in-situ silt and slag were crushed using an excavator, and the crushed soil was obtained. S4.2.2 Initial pre-mixing: The crushed soil material is put into the mixing machine; S4.2.3 Segmented grouting and mixing: The composite grout is sprayed evenly into the soil in several stages to obtain fluidized solidified soil; S4.2.4 Layered paving: The mixed fluidized solidified soil is spread and backfilled in layers to obtain in-situ solidified soil on site.
[0021] In a further preferred embodiment, in step S4.1.1, the silt and slag raw materials are passed through a 5mm standard geotextile sieve, large clumps of soil are manually broken up, and the materials are spread on a tray to air dry naturally or dried in a low-temperature oven. The materials are then sprayed in small amounts multiple times using a spray bottle, thoroughly mixed, and then sealed and left to stand for 12 hours to ensure uniform moisture content within the soil.
[0022] In a further preferred embodiment, in step S4.1.2, the mixing conditions are: dry mixing at 100 r / min for 2 min; during the mixing process, the lid is opened intermittently for observation, and dry soil clumps adhering to the barrel wall are manually scraped off to ensure that the soil is loose and free of agglomeration.
[0023] In a further preferred embodiment, in step S4.1.3, the total amount of composite slurry required is calculated based on 12% of the soil mass in step S4.1.2, and added slowly in two batches. The first batch of composite slurry, accounting for 60% of the total volume, is added and mixed at a stirring speed of 150 r / min for 3 minutes. The second batch of composite slurry is added, and the stirring speed is increased to 200 r / min and mixed continuously for 5 minutes until the mixture is in a uniform self-leveling flow state, with no dry soil clumps and no slurry stratification or floating slurry, thus obtaining a fluid mixture.
[0024] In a further preferred embodiment, in step S4.1.4, the inner wall of the mold is cleaned, and a thin layer of release jelly is applied evenly to prevent the hardened soil from sticking to the mold; the sample is placed stably on the low-frequency vibration table, the vibration frequency is 50Hz, and the vibration is continued for 1 minute.
[0025] In a further preferred embodiment, in step S4.2.1, the crushed particle size is controlled to be ≤5cm; if the soil moisture content is higher than 60%, dry slag soil with a mass ratio of 10-20% is pre-mixed to adjust the moisture content.
[0026] In a further preferred embodiment, in step S4.2.2, the filling volume of a single mixing bin does not exceed 70% of the rated volume of the equipment, and the loose soil is mechanically dry-mixed for 1 minute.
[0027] More preferably, in step S4.2.3, the amount of the composite slurry used is 8-15% of the total mass of the soil, with the upper limit for high moisture content silt and the lower limit for low moisture content slag.
[0028] More preferably, in step S4.2.3, the composite slurry is sprayed evenly three times, and after each spray, it is continuously mixed for 4 minutes, with a total mixing time of not less than 12 minutes.
[0029] In a further preferred embodiment, in step S4.2.4, the thickness of a single layer is controlled to be ≤20cm. After the current layer is vibrated and compacted and the surface layer has initially set (30min after paving), the next layer of soil is mixed and paved.
[0030] Preferably, step S5 includes indoor small-scale sample curing and solidification methods and on-site large-area in-situ solidification soil curing methods, as follows: (1) Indoor small sample curing and solidification method: Indoor precast solidified soil sample is molded, the surface is covered with waterproof plastic film, grouting is applied 3 times during the total curing period, the mold is removed after curing, and the sample is left to stand at room temperature for 24 hours to complete stable curing. (2) On-site large-area in-situ solidified soil curing method: After each layer of in-situ solidified soil is laid and vibrated, a geomembrane is immediately laid to cover it, and the soil is grouted 3 times during the overall site curing cycle.
[0031] For further optimization, the specific methods are as follows: (1) Indoor small sample curing and solidification method: After the indoor precast solidified soil sample is installed and vibrated, the surface is immediately covered with a waterproof plastic film and completely sealed. It is cured in sections at room temperature of 25℃. Every 12 hours, the film is lifted and composite slurry is added to the tiny pores on the surface of the sample in small amounts multiple times using a drip pipe. The amount of slurry added at one time does not exceed 0.5% of the total mass of the soil. The slurry is added continuously for 3 times, and the total curing and solidification cycle is 48 hours. After curing, the mold is removed and the sample is left to stand at room temperature for 24 hours to complete the stable curing. (2) On-site large-area in-situ solidified soil curing method: After each layer of the in-situ solidified soil is laid and vibrated, it is immediately covered with a geomembrane to isolate air and moisture evaporation. The edges of the membrane are covered with soil and compacted to seal. Every 24 hours, solidified grout is added to the shallow pores of the soil through a pre-embedded small grouting hose. The grouting is repeated 3 times. The overall site curing cycle is 7 days. During the curing period, heavy vehicles and large machinery are prohibited from entering the site for compaction. After the curing is completed, subsequent construction such as roadbed filling and dam foundation backfilling can be carried out.
[0032] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a grouting and curing material and method for fluidized solidified soil based on polyurethane-water glass composite grout. It is made from a two-component grouting matrix and a modified filler admixture. The two-component grouting matrix consists of component A and component B. Component A is a mixture of liquid sodium silicate, glycerol, and dibutyltin dilaurate; component B is a mixture of polymeric MDI, polyether polyol, chlorinated paraffin, and dioctyl phthalate (DOP). The modified filler admixture is selected from any one or a mixture of three of fly ash, nano-silica, and polypropylene fiber. This invention, through the synergistic effect of the organic-inorganic crosslinked matrix and the multi-component modified filler, meets the requirements for fluidized soil curing while fully filling the internal pores of the fluidized solidified soil, significantly improving the early strength, shear strength, and impermeability of the soil, reducing soil compression deformation. It is compatible with layered grouting and intermittent grouting processes for backfilling projects with fluidized solidified soil of different thicknesses. The material incorporates industrial solid waste fly ash, making it environmentally friendly and with a lower overall cost.
[0033] The functions of each raw material in this invention are as follows: 1. Component A (water glass base liquid): The main material is liquid sodium silicate with a modulus of 2.68. Glycerol is used as a plasticizer to extend the working time of the slurry. Dibutyltin dilaurate (DBTDL) is used as a crosslinking catalyst to regulate the reaction rate between polyurethane and silicate and balance the gel time and curing strength.
[0034] 2. Component B (Polyurethane-based liquid): Polymerized MDI is the core reaction raw material, polyether polyol-210N regulates the toughness of the solidified body; chlorinated paraffin is flame-retardant modified to be suitable for underground closed foundation pit engineering; dioctyl phthalate (DOP) further reduces the viscosity of the slurry and improves the deep permeability of the soil.
[0035] 3. Modified filler admixture: a compound of fly ash, nano-silica, and polypropylene fiber. Fly ash, an industrial solid waste, fills the pores and undergoes a pozzolanic reaction in an alkaline water glass environment, increasing the density of the stone mass; nano-silica acts as nucleation sites, promoting uniform cross-linking of the organic-inorganic network and reducing solidification shrinkage; the three-dimensional distribution of polypropylene fiber inhibits the propagation of microcracks within the soil, improving the ductility and shear strength of the solidified body.
[0036] The curing mechanism of this invention is as follows: 1. Organic-inorganic cementitious skeleton formation mechanism: The isocyanate groups of polyurethane component B and the hydroxyl groups of water glass in component A undergo covalent bonding, generating organic polymer chain segments and inorganic silicon-oxygen cementitious skeleton on the surface of soil particles. This quickly wraps and binds the soil particles, forming an integral composite soil with load-bearing capacity in a short time, achieving early high-strength curing.
[0037] 2. Pore filling mechanism: Fly ash fills medium-sized pores in the soil, nano-silica fills micro-pores, and polypropylene fibers form a spatial support skeleton. The three types of fillers fill the pores at all levels in the soil in layers, which greatly reduces the compression deformation of the solidified soil, while inhibiting the volume shrinkage caused by the solidification reaction and avoiding the formation of new through-cracks.
[0038] 3. Mechanism of secondary grouting for pore repair: During the segmented curing stage, solidified grout is intermittently added to replenish the tiny pores inside the soil caused by deformation and shrinkage. The solidified grout undergoes a mineralization reaction again, filling the pore defects a second time, further improving the compactness, impermeability and long-term mechanical stability of the solidified soil.
[0039] 4. Strengthening mechanism of grout-soil interface: Nano-silica enhances the adsorption and adhesion force between the solidified grout and soil particles. Fly ash undergoes a volcanic ash hydration reaction in an alkaline environment to generate hydration gel products, which fill the gaps at the grout-soil interface and prevent interface bonding failure and rapid strength decay under load.
[0040] This invention has the following advantages: 1. Compared to traditional single-cement solidification materials, the polyurethane-water glass composite slurry of this invention contains no coarse solid particles and has a lower bulk viscosity, enabling it to fully penetrate the micropores of fluidized solidified soil, completely encapsulating fine soil particles and resulting in a wider cementation distribution range. The reaction rate after mixing the two components is much faster than the cement hydration process, rapidly generating a high-strength cemented skeleton under the same curing period, effectively improving the early compressive and shear strength of the solidified soil.
[0041] 2. Compared with pure polyurethane and acrylate single organic curing agents, water glass as the main inorganic substrate significantly reduces the procurement and construction costs of grout raw materials; on the other hand, nano silica and fly ash fillers can strengthen the bonding between the grout and soil, reducing the problems of debonding and subsequent strength reduction of pure organic materials after immersion in water; this curing grout is low in toxicity, has no highly alkaline leachate, and the cured product has strong resistance to groundwater corrosion.
[0042] 3. Based on conventional unmodified polyurethane-water glass, this composite grout is combined with fly ash, nano-silica, and polypropylene composite fillers, along with a graded mixing and intermittent grouting solidification process. The multi-component fillers fill the pores of the soil in layers, and the intermittent grouting repairs the solidification shrinkage defects, significantly improving the overall density and long-term deformation stability of the fluidized solidified soil. This greatly enhances the in-situ solidification treatment effect of silt and slag, expanding the application prospects and scope of this composite grout in various fluidized solidified soil projects.
[0043] In summary, the composite slurry of this invention has excellent fluidity and can uniformly penetrate high-moisture-content, large-pore fluidized solidified soil. After solidification, the soil exhibits high early strength, small compression deformation, and significantly improved shear and impermeability. The use of industrial solid waste fly ash reduces material costs. It is suitable for roadbed backfilling, soft foundation pits, and reinforcement of fluidized solidified soil in water conservancy reservoir areas. Attached Figure Description
[0044] Figure 1 Diagram of component A solution; Figure 2 Diagram of component B solution; Figure 3 This is a diagram of the clay sample from Comparative Example 1. Figure 4 This is a sample image of the cement-cured specimen from Comparative Example 2. Figure 5 This is a sample image of the cured polyurethane-water glass composite slurry from Example 1; Figure 6 This is a diagram showing the failure of the clay sample in the direct shear test of Comparative Example 1. Figure 7 This is a failure diagram of the direct shear test specimen of cement-cured sample in Comparative Example 2; Figure 8 This is a direct shear test specimen failure diagram of the cured polyurethane-water glass composite slurry with the optimal mix ratio in Example 1; Figure 9 This is a diagram showing the results of the direct shear test on clay samples from Comparative Example 1. Figure 10 The graph shows the results of the direct shear test on the cement-cured sample of Comparative Example 2. Figure 11 This is a graph showing the direct shear test results of the cured polyurethane-water glass composite slurry sample from Example 1. Detailed Implementation
[0045] The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be noted that the following description is only for explaining the present invention and does not limit its content.
[0046] The polymeric MDI involved in this invention was purchased from Wanhua, brand name PM200; Polyether polyol-210N, purchased from Runhong Chemical; Fly ash, GB / T 1596-2017 standard Class F fly ash, dried at 105℃ for 2 hours and passed through a 0.075mm sieve before use; Nano-silica, purity ≥99.8%, vacuum packaged for single use only after opening; Polypropylene fiber, specifically 6mm chopped polypropylene monofilament fiber, with a molecular weight of 200,000 to 300,000 polypropylene. Before use, the fiber bundles should be manually kneaded and broken up.
[0047] Example 1: A curing method for a fluidized solidified soil grouting and curing material based on polyurethane-water glass composite slurry includes the following steps: Step S1: Prepare grouting matrix components A and B separately, specifically including: Step S1.1: Prepare a component A solution containing sodium silicate, glycerol, and dibutyltin dilaurate, specifically including: Step S1.1.1: Select an electronic balance with an accuracy of 0.01g, take a clean 500mL transparent plastic stirring beaker, tare and zero it, weigh 120g of industrial liquid sodium silicate with a modulus of 2.68 and pour it into the beaker; Step S1.1.2: Take a 10mL disposable plastic dropper and take 2.00g of glycerol and 0.40g of dibutyltin dilaurate (DBTDL) liquid catalyst, and slowly drip them in layers along the inner wall of the beaker; Step S1.1.3: Set the stirrer to a constant speed of 120 r / min and start the stirring timer for 5 minutes. During the first 2 minutes of stirring, the sodium silicate and additives will initially mix, and the liquid will show slight milky white flocculent matter, which is a normal mixing reaction phenomenon. After stirring for 3 minutes, the flocculent matter will gradually dissipate. By the end of the 5-minute stirring cycle, the liquid must reach a uniform, transparent, and light yellow state, with no layering, no floating oil droplets, and no white silicate precipitate at the bottom of the cup. If white flocculent matter or hard precipitate at the bottom still exists after 5 minutes of stirring, the stirring time should be extended by 3 minutes and visually inspected again. If the standard is still not met, the batch of material should be discarded and re-weighed and prepared. Step S1.1.4: If the prepared component A solution is not used immediately, place it in a light-proof plastic container, seal it, and let it stand at room temperature for 24 hours. If the storage time exceeds 24 hours, open the container and visually inspect it. If there is no stratification or bottom sediment, stir it again at 120 rpm for 2 minutes before use. If a grayish-white hard silicate precipitate appears at the bottom of the container and the liquid surface is turbid and stratified, it is determined that the sodium silicate hydrolysis has failed, and the entire container of liquid must be discarded. Do not dilute with water or reuse it after stirring. Collect the failed liquid and dispose of it properly. Do not pour it out at will. The prepared component A solution should be... Figure 1 As shown; Step S1.2 involves preparing a component B solution containing polymeric MDI, polyether polyol-210N, chlorinated paraffin flame retardant, and dioctyl phthalate (DOP) plasticizer, specifically including the following steps: Step S1.2.1: Using an electronic balance with an accuracy of 0.01g, weigh out 108g of polymeric MDI, 12.00g of polyether polyol-210N, 15.50g of chlorinated paraffin flame retardant, and 8g of dioctyl phthalate (DOP) plasticizer, and pour them all into a light-proof container and stir. Step S1.2.2: Polymerized MDI is prone to reacting with moisture in the air and becoming ineffective. The weighing time should be strictly controlled within 30 seconds. After weighing, immediately tighten the sealing cap of the raw material container. Step S1.2.3: Set the stirring speed to 180 r / min and stir continuously for 8 min. In the first 3 min of stirring, there is slight stratification between polyurethane polyol and polymeric MDI, which is a normal phenomenon due to the difference in raw material density. After stirring for 6 min, the solution is completely mixed. After the 8 min stirring cycle, the liquid is a uniform brown transparent oily liquid with no suspended solid particles and no viscous sediment at the bottom of the tank. Step S1.2.4: Immediately after stirring, replace the matching light-proof rubber sealing cap, wrap with waterproof tape to isolate air and moisture, store at room temperature away from light, shelf life 7 days; before use, open the cap and observe. If white flocculent hydrolysis precipitate or a skin forms on the liquid surface, it indicates deterioration due to contact with moisture, the entire container should be discarded. Do not mix with solution A. The prepared component B solution is as follows: Figure 2 As shown; Step S2 involves preparing modified solution A, specifically including the following steps: Step S2.1: Keep the prepared component A solution in a 500mL stirring beaker. Dry the fly ash in a 105℃ oven for 2 hours to remove moisture and cool it to room temperature before use. The nano silica is vacuum-packed and used once opened to avoid moisture absorption and agglomeration. Rub and break up the polypropylene fiber to remove any sticky fiber bundles. Step S2.2: For the first feeding, add 1g of fly ash, 1g of nano silica, and 0.3g of polypropylene fiber. Set the mixer to low speed of 80r / min and continue stirring for 3min to break up large clumps of fiber. Once no centimeter-sized fiber flocs are visible to the naked eye, the next feeding can begin. Step S2.3: For the second feeding, add 1g of fly ash, 1g of nano silica, and 0.3g of polypropylene fiber. Maintain a low speed of 80r / min for 2min to break up the secondary agglomerated particles. During the stirring process, the agitator should be kept close to the liquid surface to prevent the filler from floating on the liquid surface and not being able to wet it. Step S2.4: For the third feeding, add the remaining 1g fly ash, 1g nano silica, and 0.4g polypropylene fiber, increase the stirring speed to 250r / min and stir at high speed for 7min, with a total stirring time of no less than 10min. Step S2.5: After stirring, turn off the equipment and let it stand for 2 minutes to eliminate the tiny air bubbles introduced by stirring. Hold the beaker and observe it from the side with light: there should be no white agglomerates inside the liquid, no floating fiber flocs on the surface, and no gray fly ash accumulation or sediment at the bottom of the beaker. The three types of fillers should be completely uniform. If local filler accumulation or white agglomerates are found during light observation, the high-speed stirring at 250 r / min should be restarted for 3 minutes, and the mixture should be allowed to stand again for re-inspection until it meets the standard. Unqualified modified liquid A should not be allowed to enter the composite slurry mixing process. Step S3 involves preparing the composite slurry, specifically including the following steps: Step S3.1: Use a graduated measuring cup to measure the modified liquid A and polyurethane base liquid B, strictly control the volume ratio to 1:1, and the error should not exceed ±5mL; use a 250mL measuring cup in the laboratory and a graduated plastic storage container on the construction site. Excessive deviation in the ratio will directly affect the gelation time and curing strength. Step S3.2: Pour the modified solution A and component B into the stirring beaker simultaneously. Set the stirring speed to 300 r / min and stir continuously for 20 seconds. Stop the machine immediately after stirring is complete. Do not set the stirring time too long, as long-term high-speed stirring will shorten the effective mixing time. After stirring, the slurry should be a uniform light brownish-yellow homogeneous mixture with no oil-water separation and no white silicate precipitates. Step S3.3: After mixing is completed, start the timer. The effective mixing time of the slurry is 10 minutes. It must be completely mixed with the soil within 10 minutes. If it exceeds 10 minutes, gel particles will appear inside the slurry, and it will lose its self-flowing mixing performance. It is forbidden to add water or add new slurry to dilute and reuse it. It should be discarded directly. Step S3.4: High temperature conditions (ambient temperature > 30℃): Add an additional 1g of glycerol during the preparation of component A solution and stir simultaneously to extend the gelation time of the slurry, which can extend the window period to 15min; Low temperature conditions (ambient temperature < 10℃): Increase the amount of DBTDL catalyst to 0.6g during the preparation of component A solution to accelerate the reaction and avoid the slurry solidification rate being too slow and the early strength being insufficient at low temperatures; If the slurry quickly clumps together and gel blocks appear after mixing, it indicates that the temperature control is improper or the ratio is unbalanced. Stop using it immediately, clean the stirring container and prepare the slurry again.
[0048] Step S4 involves two stratified grouting methods under different working conditions, specifically including the following steps: Step S4.1: Working Condition 1 (Indoor Precast Fluidized Solidified Soil); Step S4.1.1: Collect dredged silt and construction waste from the river channel. Manually break up large clumps of soil. For silt with high moisture content, allow it to air dry naturally. For silt with low moisture content, spray it in small amounts multiple times using a small sprayer. After each spray, thoroughly mix the soil. Seal it in a plastic bag and let it stand for 12 hours to ensure uniform internal moisture without any dry-wet stratification. After pretreatment, pass the soil through a 5mm standard geotextile sieve. Manually remove hard impurities such as stones, plant roots, and shells, leaving only the fine-grained soil that passes through the sieve for later use. Take a 20g soil sample and determine its natural moisture content using the drying method. This will be used as the basis for calculating the slurry dosage. The standard solidification slurry dosage is 12% of the dry weight of the soil. Step S4.1.2: Weigh 1000g of sieved standard soil material, set the rotation speed to 100r / min, and dry mix for 2min; during the mixing process, open the lid intermittently to observe, and manually scrape off any dry soil clumps adhering to the barrel wall to ensure that the soil material is loose and free of agglomeration; Step S4.1.3: Calculate the total amount of composite grout based on 12% of the dry soil mass. Divide the grout into two portions using a measuring cylinder and add them slowly. The first portion accounts for 60% of the total grout, and the second portion accounts for the remaining 40%. This avoids rapid local solidification when adding grout all at once. First, slowly pour 60% of the grout along the wall of the cylinder and mix continuously at 150 r / min for 3 minutes. Most of the soil particles will be initially moistened to form a wet mud ball. Then, pour in the remaining 40% of the grout and increase the speed to 200 r / min and mix continuously for 5 minutes. After mixing, the mixture should have no dry soil core, no surface slurry, and no localized gel lumps, which means it meets the solidification test standard. Step S4.1.4: Clean the inner wall of the mold, apply a thin, even layer of release jelly to prevent the hardened soil from sticking to the mold; place the sample stably on the low-frequency vibration table, vibrate at a frequency of 50 Hz, and vibrate continuously for 1 minute; after the slurry no longer produces continuous large bubbles and the surface is smooth, turn off the equipment, and the prepared sample meets the test requirements; Step S4.2: Working Condition 2 (On-site solidification of silt); Step S4.2.1: Excavate and crush the stockpiled silt and original excavated soil in the foundation pit, and pre-transfer the dry excavated soil to the site for layered pre-mixing. The dry excavated soil content (by mass) should be controlled at 10% to 20%. Step S4.2.2: The crushed and water-adjusted soil is transported to the mixing machine for mixing. The filling volume of the mixing bin in a single batch shall not exceed 70% of the rated volume of the equipment. Step S4.2.3: Prepare sufficient composite slurry on site in advance, and dispense it into graduated measuring storage buckets. Set the total slurry usage according to 8%~15% of the dry weight of the soil. Take 12%~15% of the mass of high-moisture silt and 8%~10% of the mass of hard, low-moisture slag. Divide the total amount into three equal parts for spraying. Spray 1 / 3 of the slurry in the first round and mix continuously for 4 minutes. Spray 1 / 3 of the slurry in the second round and mix for another 4 minutes. Spray the remaining slurry in the third round and mix for 4 minutes. The total mixing time for the three rounds shall not be less than 12 minutes. Step S4.2.4: The mixed fluidized solidified soil is transported to the backfilling work surface and spread in layers. The thickness of each layer is strictly controlled to be ≤20cm. After the layer is vibrated and compacted and the surface is initially set (30min after spreading), the next layer of soil can be mixed and spread.
[0049] Step S5 involves curing the fluidized solidified soil, which specifically includes the following steps: Step S5.1: Working Condition 1 (Indoor Precast Fluidized Solidified Soil); Step S5.1.1: After the sample is vibrated, immediately lay a waterproof plastic film to cover the surface of the mold and place it in a 25℃ constant temperature standard curing chamber to avoid moisture evaporation causing the sample surface to dry and crack. Step S5.1.2: Perform a timed grouting operation every 12 hours for a total of 3 times. Take the sample out of the curing box, use a 5mL plastic dropper to draw up the solidified grout, and drip it into the surface of the sample in small amounts at multiple points to shrink the fine pores. The total amount of grouting in a single operation should be less than 0.5% of the total mass of the soil. After the grouting is completed, immediately re-cover and seal the sample and put it back into the curing box. Step S5.1.3: After 48 hours of curing, the sample is taken out and left to stand for 24 hours before conducting uniaxial and direct shear mechanical property tests. If the film breaks and water is lost during the curing process, or if a through-crack appears on the surface of the sample, the sample is discarded and a new sample is prepared and cured. Step S5.2: Working Condition Two (On-site In-situ Sludge Solidification); Step S5.2.1: After each layer is laid and vibrated, immediately lay the geomembrane. The overlap width between membranes should be ≥20cm. Excavate shallow trenches around the working surface, backfill with in-situ native soil and compact the edges of the membrane to prevent the surface from losing water quickly and causing through dry cracks. Step S5.2.2: Embed 8mm inner diameter plastic grouting hoses in each soil layer, with one end of the hose extending to the reserved grouting port on the outside of the working surface, and the pipe opening is temporarily sealed; later grouting is carried out through the embedded pipeline to inject grout into the shallow pores of the soil under low pressure. Step S5.2.3: Grouting should be carried out every 24 hours for three consecutive times. Remove the plug at the pipe opening, slowly inject the composite grout, and stop grouting when the grout seeps out of the gaps in the soil under the membrane. Seal the pipe opening. After the three grouting operations are completed, cut off the exposed hose and continue to cover the geomembrane until the end of the 7-day total maintenance cycle.
[0050] Step S5.2.4: The overall curing period is 7 days. Excavators, dump trucks and other heavy machinery are strictly prohibited from entering the work surface for compaction. After the curing period is over, the surface solidified soil must be intact without large-area cracks and the strength must meet the standards before subsequent engineering procedures such as roadbed filling, dam foundation backfilling and soil covering can be carried out.
[0051] The sample obtained under working condition 1 is shown below. Figure 5 .
[0052] Example 2: The modified filler additive in step S2 is nano-silica, corresponding to test sample numbers 6, 7, 11, and 14 in Table 1.
[0053] The rest is the same as in Example 1.
[0054] Example 3: The modified filler additive in step S2 is fly ash, corresponding to test sample numbers 3, 9, 10, and 17 in Table 1.
[0055] The rest is the same as in Example 1.
[0056] Example 4: The modified filler additive in step S2 is polypropylene fiber, corresponding to test sample numbers 2, 4, 15, and 16 in Table 1.
[0057] The rest is the same as in Example 1.
[0058] Comparative Example 1: The sample material was pure clay (containing gravel), taken from the Lannihuwan Remediation Project in Yiyang City, Hunan Province. The sample was not cured with a curing slurry, i.e., it was in its original state. Figure 3 ).
[0059] Comparative Example 2: The sample is a cement-cured sample ( Figure 4The sample was prepared by curing with cement slurry. The cement used was purchased K1340 cement ash, which can be sieved through a 1340-mesh sieve, with a fineness D90 (the particle size corresponding to 90% of the cumulative particle size distribution of the sample, i.e., 90% of the particles are smaller than the standard particle size). After the sample was prepared, the surface was covered with a moisturizing film and left to stand in a curing chamber for 24 hours before demolding. It was then marked and cured in a constant temperature and humidity environment (temperature 25℃, humidity 90%) until the predetermined age (28 days).
[0060] Table 1. Orthogonal Experiment Table for Raw Materials
[0061] Performance testing: The following performance tests were conducted on the samples treated in Examples 1-4 and Comparative Examples 1-2, in accordance with the "Test Method for Compression Properties of Plastics", "Standard for Geotechnical Test Methods" (GB / T50123-2019) and "Standard for Test Methods for Engineering Rock Mass" (GB / T50266-2013).
[0062] 1. Average setting time test of polyurethane-water glass, the test results are shown in Table 2.
[0063] Table 2 Average setting time of polyurethane-water glass
[0064] As shown in Table 2, among all additives, the experimental groups with added polypropylene fibers (e.g., groups 4 and 16) exhibited the shortest setting time. This indicates that polypropylene fibers not only act as a reinforcing agent in the slurry system but also significantly accelerate the curing reaction. This is because polypropylene fibers have a large specific surface area, which significantly enhances the friction between fibers and between fibers and slurry particles during slurry flow, thereby increasing the slurry viscosity. The dosage of nano-silica and fly ash had little effect on flow and setting time. The experimental results show that increasing the catalyst mass has the most significant effect on regulating the setting rate. Increasing the plasticizer content, however, prolongs the final setting time of the slurry.
[0065] 2. The uniaxial compressive strength test of polyurethane-water glass is shown in Table 3.
[0066] Table 3 Uniaxial compressive strength of polyurethane-water glass
[0067] The uniaxial strength analysis in Table 3 shows that the order of influence of the four factors on material strength is: catalyst mass (B) > water glass modulus (A) > plasticizer mass (C) > admixture type (D). Catalyst mass (factor B) is the core factor affecting strength. Its difference is as high as 26.72, far exceeding that of other factors. Data shows that as the catalyst mass increases from 0.1 to 0.4, the average strength increases significantly from 21.83 MPa to 48.55 MPa. This indicates that the catalyst plays a key role in the reaction process, significantly accelerating material hardening and enhancing structural density.
[0068] 3. The shear strength test results for the control sample are shown in Table 4. The failure diagram of the direct shear test specimen is shown below. Figures 6-8 The experimental results are shown in the figure. Figures 9-11 .
[0069] Table 4. Shear strength test of control samples
[0070] Table 4 shows that, under the same vertical stress conditions, the peak shear stress of cement and polyurethane / clay samples is higher than that of clay samples, but the increase is more significant when the shear stress is lower. Specifically, at 100 kPa, the maximum horizontal shear stress of the cement-aggregate sample is 2981.93 kPa, at 200 kPa it is 3123.10 kPa, at 300 kPa it is 3228.50 kPa, and at 400 kPa it is 3424.58 kPa. At 100 kPa, the maximum horizontal shear stress of the polyurethane water glass sample is 3683.96 kPa, at 200 kPa it is 3885.03 kPa, at 300 kPa it is 4032.24 kPa, and at 400 kPa it is 4358.37 kPa. Comparing the reinforcement effects, at 100 kPa, the maximum shear stress of the cement sample increased by 503.92%, while that of the polyurethane water glass sample increased by 646.10%; at 200 kPa, the maximum shear stress of the cement sample increased by 404.10%, while that of the polyurethane water glass sample increased by 526.98%; at 300 kPa, the maximum shear stress of the cement sample increased by 355.93%, while that of the polyurethane water glass sample increased by 469.42%; at 400 kPa, the maximum shear stress of the cement-aggregate sample increased by 315.15%, while that of the polyurethane water glass sample increased by 428.34%. These data show that the maximum shear stress of the polyurethane water glass sample is greater than that of the cement sample under different vertical stress conditions, demonstrating the superior performance of polyurethane water glass in curing.
[0071] 4. Uniaxial compressive strength test
[0072] Example 1 and Comparative Example 2: Uniaxial compressive strength tests on specimens of different ages. The test results are shown in Table 5.
[0073] Table 5 Uniaxial compressive strength test of specimens at different ages
[0074] Table 5 shows that the uniaxial compressive strength of both cement-based and polyurethane-water glass-based solidified bodies increases with the extension of curing age. Cement-based solidified bodies have lower early-stage strength but a higher rate of strength increase in later stages; polyurethane-water glass-based solidified bodies can achieve rapid strength growth within a short period. The compressive strength of cement-based samples after 1 day of curing is only 4.5 MPa, indicating a low strength level; with continuous hydration, the compressive strength reaches 14.5 MPa after 7 days of curing, an increase of approximately 222.2% compared to the 1-day strength. In contrast, polyurethane-water glass samples exhibit certain early-strength characteristics, reaching a compressive strength of 15.2 MPa after 1 day of curing, which is higher than the compressive strength of cement-based crushed stone solidified bodies after 7 days of curing. However, with the curing age increasing to 7 days, the strength increase of polyurethane-water glass samples is only about 11.2%, and its compressive strength growth curve rapidly flattens after 1 day.
[0075] In summary, the polyurethane-water glass composite fluidized bed curing slurry preparation process of this invention uses 2.68 modulus water glass and polymeric MDI polyurethane to form a cementing matrix; it is compounded with three types of modified fillers—fly ash, nano-silica, and polypropylene fiber—to fill the multi-level pores of the soil. The nanomaterials enhance the bonding strength of the slurry-soil interface, the fly ash utilizes industrial solid waste to reduce the overall material cost, and the polypropylene fiber constructs a supporting skeleton, effectively inhibiting the formation of microcracks due to curing shrinkage. Compared to traditional ordinary cement-based fluidized bed curing materials, cement-cured particles are large and cannot fill the fine pores inside silt and slag, resulting in low early mechanical strength and significant volume shrinkage during hydration and hardening, which easily leads to the formation of through-seepage cracks. The composite slurry of this invention has low viscosity, excellent mixing performance, and can uniformly wet the fine pores of soil with high water content. It is generally low in toxicity, produces no strongly alkaline leachate, and has minimal pollution to groundwater and the surrounding soil environment. After curing, the soil compression deformation is reduced. Compared to pure polyurethane and single-organic chemical curing grouts, pure organic materials have high raw material costs, weak interfacial adhesion between cementing products and soil particles, and are prone to interfacial debonding and continuous strength decay after long-term immersion in groundwater. This invention introduces low-cost water glass and solid waste fly ash to replace part of the organic components, significantly reducing the cost of engineering materials. Compared to existing research schemes related to polyurethane-water glass grouting with only single-component modification, most existing technologies only add a single modifying agent, lack a mixing operation process that distinguishes between indoor samples and in-situ on-site conditions, and do not set up an intermittent grouting and curing process. The shrinkage pores generated during curing cannot be filled and repaired a second time. This invention improves the short-term curing efficiency, long-term mechanical stability, and impermeability of soil.
[0076] While the specific embodiments of the present invention have been described above in conjunction with the accompanying drawings, this is not intended to limit the scope of protection of the present invention. Based on the technical solutions of the present invention, various modifications or variations that can be made by those skilled in the art without creative effort are still within the scope of protection of the present invention.
Claims
1. A grouting and solidification material for fluidized solidified soil based on polyurethane-water glass composite slurry, characterized in that, It is made from a two-component grouting matrix and modified filler additives, wherein the two-component grouting matrix is composed of component A and component B; wherein... Component A is prepared by mixing liquid sodium silicate, glycerol, and dibutyltin dilaurate. Component B is made from a mixture of polymeric MDI, polyether polyol, chlorinated paraffin, and dioctyl phthalate. The modified filler additive is selected from any one or a mixture of three of fly ash, nano silica, and polypropylene fiber.
2. The curing method for a fluidized solidified soil grouting and curing material based on polyurethane-water glass composite slurry as described in claim 1, characterized in that, Includes the following steps: S1. Prepare component A and component B separately; S2. The modified filler additive is uniformly incorporated into component A to obtain modified solution A; S3. Mix the modified liquid A and component B at a volume ratio of 1:1 and stir to obtain a composite slurry; S4. The composite grout is injected into the fluid soil to be solidified using a layered grouting method to complete the grouting and obtain an indoor precast solidified soil sample or an on-site in-situ solidified soil body; S5. Cover with film and seal, then intermittently replenish with slurry for curing.
3. The curing method according to claim 2, characterized in that, In step S1, the preparation method of component A is as follows: glycerol and dibutyltin dilaurate are added sequentially to liquid sodium silicate, and the mixture is stirred at room temperature and at a constant speed for 5 minutes to obtain a uniform and stable component A.
4. The curing method according to claim 2, characterized in that, In step S1, the preparation method of component B is as follows: polymeric MDI, polyether polyol, chlorinated paraffin, and dioctyl phthalate are mixed under light-protected conditions and stirred at room temperature for 8 minutes to obtain a homogeneous solution without layering or precipitation, which is component B.
5. The curing method according to claim 2, characterized in that, In step S2, the modified solution A is prepared by adding the modified filler additive to component A in portions, first stirring at a low speed of 80 r / min for 3 min for pre-dispersion, then increasing the speed to 250 r / min for 7 min for high-speed stirring, with a total stirring time of not less than 10 min; after stirring, let stand for 2 min to eliminate fiber agglomeration and nanofiller aggregation, ensuring that the filler is completely suspended and dispersed in the water glass system, with no visible flocs or precipitates.
6. The curing method according to claim 2, characterized in that, The specific method for step S3 is as follows: pour the modified solution A and component B into a stirring container at the same time, and stir at 300 r / min for 20 seconds.
7. The curing method according to claim 2, characterized in that, Step S4 includes indoor pre-prepared sample conditions and on-site in-situ curing conditions, as detailed below: (1) Indoor precast sample working conditions: S4.1.1 Pretreatment: Silt and slag raw materials are screened to remove large stones, plant roots and stems, and the natural moisture content of the soil is measured. The amount of water added to the soil is adjusted according to the target fluidity. S4.1.2 Premixed soil: Weigh the soil after sieving and pour it into a vertical mixer, mix, and evenly loosen the soil particles; S4.1.3 Staged slurry addition and mixing: The composite slurry is added in stages to obtain a fluid mixture; S4.1.4 Molding and standing: The mixed fluid mixture is immediately poured into a standard mold, vibrated to eliminate large air bubbles inside, and indoor precast solidified soil samples are obtained. (2) On-site in-situ curing conditions: S4.2.1 Soil pretreatment: Excavators are used to break up in-situ silt and stockpile slag, and then break it up to obtain broken soil material; S4.2.2 Initial pre-mixing: The crushed soil material is put into the mixing machine; S4.2.3 Segmented grouting and mixing: The composite grout is sprayed evenly into the soil in several stages to obtain fluidized solidified soil; S4.2.4 Layered paving: The mixed fluidized solidified soil is spread and backfilled in layers to obtain in-situ solidified soil on site.
8. The curing method according to claim 2, characterized in that, Step S5 includes methods for curing and solidifying small indoor samples and methods for curing large-area in-situ solidified soil, as detailed below: (1) Indoor small sample curing and solidification method: Indoor precast solidified soil sample is molded, the surface is covered with waterproof plastic film, grouting is applied 3 times during the total curing period, the mold is removed after curing, and the sample is left to stand at room temperature for 24 hours to complete stable curing. (2) On-site large-area in-situ solidified soil curing method: After each layer of in-situ solidified soil is laid and vibrated, a geomembrane is immediately laid to cover it, and the soil is grouted 3 times during the overall site curing cycle.