A rapid high-strength phosphate two-component spraying material for tunnel primary support and a construction method thereof
By forming a magnesium silicate transition layer and a discontinuous island copolymer coordination layer on the surface of lightly calcined magnesium oxide, combined with phosphate activating components, the problems of low early strength of traditional shotcrete and easy clogging of magnesium phosphate materials are solved, realizing rapid hardening and high strength of tunnel initial support materials, which are suitable for rapid support of tunnel surrounding rock.
Patent Information
- Application Number
- CN202611509418.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional cement-based shotcrete has problems such as slow early strength development, large rebound loss, a lot of dust and poor adhesion to the rock surface in the initial support of tunnels. Magnesium phosphate cementitious materials are prone to concentrated heat release and blockage. Existing retarders reduce the early hardening speed and increase the limitations of material composition and environmental applicability.
By employing sequential surface regulation of lightly calcined magnesium oxide to form a magnesium silicate transition layer and a discontinuous island-shaped carboxyl-functionalized styrene-acrylate copolymer coordination layer, combined with dipotassium hydrogen phosphate and potassium dihydrogen phosphate activation components, a MgKPO4·6H2O crystal framework and a hydrated magnesium silicate gel phase are formed. By controlling the reaction window and the magnesium silicate hydration reaction, rapid hardening and high strength are achieved.
It provides a suitable spraying time, and the material hardens rapidly after initial setting. It has high compressive strength, flexural strength, impermeability and frost resistance, and has good adhesion to the rock surface. It is suitable for rapid initial support of the surrounding rock after tunnel blasting.
Smart Images

Figure REF-OBJ-1790567422642-000001 
Figure REF-OBJ-1790567422642-000002
Abstract
Description
Technical Field
[0001] This application belongs to the field of lightweight building materials, specifically relating to a rapid high-strength phosphate two-component spraying material for tunnel initial support and its construction method. Background Technology
[0002] After tunnel excavation, especially blasting, the exposed surrounding rock is prone to instability due to unloading, fissure expansion, groundwater seepage, or localized rockfall. In such cases, an initial support layer needs to be applied immediately. Traditional cement-based shotcrete generally suffers from slow early strength development, high rebound loss, excessive dust, and poor adhesion between the sprayed layer and damp rock surfaces, failing to provide reliable support for the unstable surrounding rock in the short term. Adding accelerators to traditional cement-based shotcrete can effectively reduce setting time, but this may also lead to uneven slurry dispersion, decreased later strength, and deterioration of durability. Magnesium phosphate cementitious materials are often used in tunnel repair and rapid support due to their advantages of rapid setting, high early strength, and good adhesion to rock surfaces. However, the high reactivity of lightly calcined magnesium oxide makes it prone to concentrated heat release and instantaneous setting upon contact with acidic phosphates and water. This not only results in insufficient spraying time but also causes agglomeration, adhesion, and blockage in the delivery pipeline and even inside the nozzle. Existing solutions typically involve adding boric acid or borate to slow down the setting process. However, these retarders primarily inhibit the entire reaction system, thereby reducing the early hardening rate of the material and increasing limitations on material composition and environmental applicability.
[0003] While treating lightly calcined magnesium oxide with a continuous, dense, inert coating can reduce its surface reaction rate, insufficient coating cannot effectively slow down the setting rate. Excessive coating reduces the active sites participating in the early reaction, hindering rapid hardening after initial setting. Furthermore, hardened bodies formed solely by magnesium phosphate crystals still contain pores and weak interfaces between crystals, making it difficult to achieve the required high flexural strength, impermeability, and freeze-thaw durability.
[0004] If the dry powder and liquid are mixed before being transported during the spraying process, the phosphate gelation reaction may occur prematurely, leading to increased transport resistance. Using ordinary nozzles to directly add liquid may result in insufficient wetting of the dry powder, uneven component distribution, and high spray rebound rate. Therefore, it is necessary to propose a two-component phosphate spraying material and its application method that can regulate the reaction sequence of lightly calcined magnesium oxide while ensuring uniform wetting, rapid hardening, low rebound, high bond strength, and long-term durability. Summary of the Invention
[0005] To address the aforementioned deficiencies, this application provides the following technical solution: a rapid high-strength phosphate two-component spraying material for tunnel initial support, comprising separately stored dry powder component A and liquid activation component B; The A dry powder component, by weight, includes: 55-75 parts of sequentially surface-modified lightly calcined magnesium oxide, 10-22 parts of reactive silicon source, 8-18 parts of acicular silicate minerals, 15-30 parts of fine aggregate, 0.6-1.8 parts of microfiber toughening component, and 0.2-1.0 parts of rheological building block component; The liquid activation component B comprises, by weight, 20 to 32 parts of dipotassium hydrogen phosphate, 2 to 8 parts of potassium dihydrogen phosphate, 30 to 55 parts of water, and 0.05 to 0.30 parts of defoamer; The sequential surface-controlled light-burned magnesium oxide includes a light-burned magnesium oxide particle core, a magnesium silicate transition layer formed on the surface of the light-burned magnesium oxide particle core, and a carboxyl-functionalized styrene-acrylate copolymer coordination layer formed on the outside of the magnesium silicate transition layer; the carboxyl-functionalized styrene-acrylate copolymer coordination layer is distributed in a discontinuous island shape, and forms a reaction window on the particle surface of the sequential surface-controlled light-burned magnesium oxide that is not covered by the carboxyl-functionalized styrene-acrylate copolymer coordination layer.
[0006] Furthermore, the sequentially surface-controlled lightly calcined magnesium oxide is prepared using the following method: M1: Add 3 to 8 parts of water glass (based on solids) to every 100 parts of light-burned magnesia. Spray the water glass solution onto the surface of the fluidized light-burned magnesia, mix, and then dry. M2: The dried lightly calcined magnesium oxide is heat-treated at 260℃~340℃ for 30min~90min to allow the silicate components in the water glass to react with the surface of the lightly calcined magnesium oxide particles to form the magnesium silicate transition layer. M3: Add 0.5 to 2.5 parts (based on solids) of carboxyl-functionalized styrene-acrylate copolymer to 100 parts of lightly calcined magnesium oxide with the magnesium silicate transition layer. Spray the carboxyl-functionalized styrene-acrylate copolymer emulsion into the lightly calcined magnesium oxide with the magnesium silicate transition layer, and add deionized water to adjust the solid content of the resulting coating slurry to 45 wt% to 60 wt%. At 20°C to 35°C, with a stirring paddle tip linear velocity of 0.3 m / s to 1... Low-shear coating was performed at 0 m / s for 10 to 30 minutes; then the resulting coated slurry was spray-dried at an inlet air temperature of 140°C to 180°C, an outlet air temperature of 70°C to 90°C, and an atomization pressure of 0.25 MPa to 0.60 MPa to obtain sequentially surface-controlled lightly calcined magnesium oxide with a moisture content of no more than 1.5 wt%, which caused the carboxyl-functionalized styrene-acrylate copolymer to form a coordination layer with a discontinuous island distribution on the outside of the magnesium silicate transition layer.
[0007] Furthermore, the MgO content in the lightly calcined magnesium oxide is not less than 85 wt%, the median particle size D50 is 10 μm to 45 μm, and the citric acid activation time is 40 s to 120 s; the water glass modulus used to form the magnesium silicate transition layer is 2.0 to 3.2; and the acid value of the carboxyl-functionalized styrene-acrylate copolymer is 20 mg KOH / g to 80 mg KOH / g. The magnesium silicate transition layer has a coverage rate of 80% to 98% on the surface of the lightly calcined magnesium oxide particles, and the carboxyl-functionalized styrene-acrylate copolymer coordination layer has a coverage rate of 35% to 70% on the surface of the magnesium silicate transition layer.
[0008] Further, the weight ratio of dipotassium hydrogen phosphate to potassium dihydrogen phosphate is 1:(0.08-0.30), the pH value of the B liquid activation component at 20°C is 7.6-8.5, the B liquid activation component does not contain boric acid or borate, and the defoamer is one or at least two of the following: polydimethylsiloxane emulsion defoamer, polyether-modified polysiloxane defoamer, polyoxypropylene glycerol ether defoamer, and mineral oil defoamer.
[0009] Furthermore, the reactive silicon source comprises silica fume and spray-dried nano-silica, wherein the weight ratio of silica fume to spray-dried nano-silica is 1:(0.10-0.40); the median particle size D50 of the silica fume is 0.10μm-1.00μm, and the silica content is not less than 90wt%; the spray-dried nano-silica is obtained by spray drying colloidal silica with a primary particle size of 5nm-30nm.
[0010] Further, the acicular silicate mineral is wollastonite, and the aspect ratio of the wollastonite is 8-20; the microfiber toughening component is composed of polyvinyl alcohol fiber and basalt fiber in a weight ratio of 1:(0.2-0.6), the length of the polyvinyl alcohol fiber is 6mm-12mm, and the length of the basalt fiber is 3mm-6mm; the rheological building block is composed of starch ether and attapulgite in a weight ratio of 1:(2-6).
[0011] Further, the A dry powder component and the B liquid activation component are mixed at a weight ratio of 1:(0.35~0.55); after mixing, the lightly calcined magnesium oxide at the reaction window first reacts with dipotassium hydrogen phosphate and potassium dihydrogen phosphate from the B liquid activation component to form a crystal framework with MgKPO4·6H2O as the main crystal phase; the lightly calcined magnesium oxide in the region covered by the carboxyl-functionalized styrene-acrylate copolymer coordination layer participates in the reaction after the coordination layer is gradually dissociated; the magnesium silicate transition layer and the reactive silicon source jointly participate in the magnesium silicate hydration reaction, forming a hydrated magnesium silicate gel phase between the MgKPO4·6H2O crystal framework.
[0012] Furthermore, the initial setting time of the mixture of the A dry powder component and the B liquid activating component is 6 min to 15 min, and the time interval from reaching the initial setting state to reaching the final setting state is no more than 5 min; the compressive strength after 1 hour of hardening is no less than 30 MPa, the compressive strength after 24 hours of hardening is no less than 45 MPa, the compressive strength after 28 days of hardening is no less than 60 MPa, the flexural strength after 28 days of hardening is no less than 6.0 MPa, the 24-hour tensile bond strength with the rock substrate is no less than 1.0 MPa, the impermeability grade is no less than P8, and the freeze-thaw resistance grade is no less than F300.
[0013] This application also provides a construction method for the above-mentioned rapid high-strength phosphate two-component spraying material for tunnel initial support, including the following steps: S1: Add dry powder component A to a closed dry powder spraying equipment, and fluidize and pneumatically convey dry powder component A through a material-carrying airflow, while conveying liquid activating component B to a nozzle with an annular liquid outlet. S2: The B liquid activating component forms an annular liquid curtain from the annular liquid outlet, and the A dry powder component conveyed by pneumatic conveying passes through the annular liquid curtain. The collision between the A dry powder component and the annular liquid curtain completes the particle wetting and initial dispersion. S3: The secondary atomized airflow in the nozzle is used to shear and disperse the wetted material to form a phosphate spraying mixture; S4: The phosphate spraying mixture is sprayed onto the exposed surrounding rock surface, the surface of the reinforcing mesh, or around the steel arch frame after tunnel blasting, forming an initial support layer for the tunnel in layers.
[0014] Further, in step S1, the conveying rate of dry powder component A is 15 kg / min to 35 kg / min, the material airflow pressure is 0.35 MPa to 0.65 MPa, and the conveying pressure of liquid activating component B is 0.40 MPa to 0.80 MPa; in step S2, the width of the annular liquid outlet is 0.5 mm to 1.5 mm, and the collision angle between the movement direction of dry powder component A and the annular liquid curtain is 30° to 60°; in step S4, the distance between the nozzle and the sprayed surface is 0.8 m to 1.3 m, the spray angle is 75° to 90°, the single-layer spray thickness is 20 mm to 50 mm, and the spray rebound rate is not higher than 10%.
[0015] The technical solution of this application has the following beneficial effects: This application achieves a reaction window by sequentially forming a magnesium silicate transition layer and a discontinuously distributed carboxyl-functionalized styrene-acrylate copolymer coordination layer on the surface of lightly calcined magnesium oxide particles. The region not covered by the coordination layer forms a reaction window, allowing the lightly calcined magnesium oxide at the window to preferentially react with dipotassium hydrogen phosphate and potassium dihydrogen phosphate. The region covered by the coordination layer participates in the reaction later after the coordination layer gradually dissociates, thereby suppressing concentrated exothermic reactions and instantaneous condensation. This allows for a suitable spraying time without the use of boric acid and borates, and enables the material to harden rapidly after reaching the initial setting state. The magnesium silicate transition layer also improves the bonding stability between the particle core and the outer layer material, while the liquid activation system composed of dipotassium hydrogen phosphate and potassium dihydrogen phosphate helps regulate the initial reaction environment. A reactive silicon source composed of silica fume and spray-dried nano-silica, along with the magnesium silicate transition layer, participates in the silicon reaction. The magnesium hydration reaction forms a hydrated magnesium silicate gel phase between the magnesium potassium phosphate crystal framework, thereby filling the pores and improving the compressive strength, impermeability, and frost resistance of the hardened body. Acicular silicate minerals, together with polyvinyl alcohol fibers and basalt fibers, play a bridging and crack-resistant role, which can improve the flexural strength of the sprayed layer and limit crack propagation. The rheological building block helps to improve the adhesion of the material and the stability of the sprayed layer. During construction, dry powder component A is pneumatically conveyed through the annular liquid curtain formed by liquid activating component B, so that the dry powder particles are wetted and initially dispersed by collision. Then, secondary atomized airflow is used for shear dispersion, which can reduce local dry powder agglomeration and nozzle accumulation. The resulting material has continuous spraying capability, low rebound rate, uniform layering performance, high interfacial bonding strength, and rapid load-bearing capacity. It is suitable for rapid initial support around the surrounding rock, steel mesh, and steel arch frame after tunnel blasting. Detailed Implementation
[0016] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0017] Example 1
[0018] This embodiment provides a fast-acting, high-strength phosphate two-component spraying material for tunnel initial support, comprising separately stored dry powder component A and liquid activating component B.
[0019] First, sequentially surface-controlled light-burned magnesium oxide (MgO) was prepared. The MgO used had an MgO content of 85 wt%, a median particle size (D50) of 28 μm, and a citric acid activation time of 120 s. 100 parts of MgO were placed in a fluidized bed coating apparatus, and a water glass solution with a modulus of 2.0 and a solid content of 30 wt% was sprayed onto the fluidized MgO surface, with 3 parts of water glass solids used. After spraying, mixing continued for 5 min, drying at 105 °C for 2 h, and then heat-treated at 300 °C for 90 min to form a magnesium silicate transition layer. Scanning electron microscopy combined with energy dispersive spectroscopy (EDS) analysis showed that the magnesium silicate transition layer covered 80% of the MgO particle core surface.
[0020] A carboxyl-functionalized styrene-acrylate copolymer emulsion with an acid value of 50 mg KOH / g and a solid content of 40 wt% was sprayed into lightly calcined magnesia with a magnesium silicate transition layer. The copolymer solids content was 1.5 parts, and deionized water was added to adjust the solid content of the slurry to 45 wt%. Coating was performed at 35°C with a low shear rate of 0.65 m / s at the impeller tip for 10 min, followed by spray drying at an inlet air temperature of 180°C, an outlet air temperature of 80°C, and an atomization pressure of 0.25 MPa. The resulting sequentially surface-controlled lightly calcined magnesia had a moisture content of 0.7 wt%, and the copolymer coordination layer exhibited a discontinuous island-like distribution, covering 50% of the magnesium silicate transition layer surface.
[0021] Component A, by weight, consists of 55 parts of sequentially surface-modified lightly calcined magnesia, 22 parts of reactive silicon source, 13 parts of wollastonite, 15 parts of washed silica sand, 1.8 parts of microfiber toughening component, and 0.6 parts of rheological building block component. The reactive silicon source comprises 20 parts of silica fume and 2 parts of spray-dried nano-silica in a weight ratio of 1:0.10; the median particle size (D50) of the silica fume is 1.00 μm, and the SiO2 content is 90 wt%; the primary particle size of the spray-dried nano-silica is 18 nm. The aspect ratio of wollastonite is 8. The median particle size (D50) of the washed silica sand is 0.30 mm. The microfiber toughening component consists of 9 mm long polyvinyl alcohol fibers and 3 mm long basalt fibers in a weight ratio of 1:0.6. The rheological building block component consists of starch ether and attapulgite in a weight ratio of 1:4. Mix the raw materials except for the microfiber toughening component for 5 minutes, then add the microfiber toughening component and mix at low speed for 3 minutes to obtain dry powder component A.
[0022] Liquid activating component B, by weight, consists of 25 parts dipotassium hydrogen phosphate, 2 parts potassium dihydrogen phosphate, 55 parts water, and 0.18 parts polydimethylsiloxane emulsion defoamer. The weight ratio of dipotassium hydrogen phosphate to potassium dihydrogen phosphate is 1:0.08. Dipotassium hydrogen phosphate and potassium dihydrogen phosphate are dissolved sequentially in water, and then the defoamer is added and stirred to disperse, yielding liquid activating component B, which is free of boric acid and borate and has a pH of 8.5 at 20°C.
[0023] This embodiment also provides a construction method for a rapid high-strength phosphate two-component spraying material for tunnel initial support, which includes the following steps S1-S4: S1: Add dry powder component A to a closed dry powder spraying equipment and pneumatically convey it at a conveying rate of 15 kg / min and a material airflow pressure of 0.50 MPa; send liquid activating component B into a nozzle with an annular outlet width of 1.0 mm at a conveying pressure of 0.80 MPa.
[0024] S2: The B liquid activating component forms an annular liquid curtain from the annular outlet, allowing the pneumatically conveyed A dry powder component to pass through the annular liquid curtain. The collision between the A dry powder component and the annular liquid curtain completes particle wetting and initial dispersion. The weight ratio of the A dry powder component to the B liquid activating component is 1:0.35, and the collision angle between the movement direction of the A dry powder component and the annular liquid curtain is 30°.
[0025] S3: After being wetted by the collision of the annular liquid curtain and atomized twice, a phosphate spraying mixture is formed.
[0026] S4: Apply the phosphate spraying mixture to the exposed surrounding rock surface after tunnel blasting. The distance between the nozzle and the sprayed surface is 1.3m, the spraying angle is 82°, and the thickness of a single layer is 20mm.
[0027] Testing revealed that the initial setting time of the sprayed mixture was 6 minutes, the final setting time was 10 minutes, and the time interval between initial and final setting was 4 minutes. The compressive strength after 1 hour of hardening was 38.6 MPa, after 24 hours it was 45.0 MPa, after 28 days it was 68.4 MPa, the flexural strength after 28 days it was 6.0 MPa, the 24-hour tensile bond strength with the rock substrate was 1.28 MPa, the impermeability grade was P8, the freeze-thaw resistance grade was F350, and the spraying rebound rate was 10.0%. X-ray diffraction analysis showed the formation of a MgKPO4·6H2O crystal framework in the hardened body, while infrared spectroscopy and scanning electron microscopy-energy dispersive spectroscopy indicated the presence of a hydrated magnesium silicate gel phase within the crystal framework.
[0028] Example 2
[0029] This embodiment provides a fast-acting, high-strength phosphate two-component spraying material for tunnel initial support, comprising separately stored dry powder component A and liquid activating component B.
[0030] The light-burned magnesia used had an MgO content of 90 wt%, a median particle size (D50) of 45 μm, and a citric acid activation time of 40 s. 100 parts of light-burned magnesia were placed in a fluidized bed coating apparatus, and a water glass solution with a modulus of 2.6 and a solid content of 30 wt% was sprayed onto the surface of the magnesia, with 5.5 parts of solid water glass used. After spraying, mixing continued for 5 min, drying at 105 °C for 2 h, and then heat-treated at 340 °C for 30 min to form a magnesium silicate transition layer with a surface coverage of 90%.
[0031] A carboxyl-functionalized styrene-acrylate copolymer emulsion with an acid value of 80 mg KOH / g and a solid content of 40 wt% was sprayed into lightly calcined magnesia with a magnesium silicate transition layer. The copolymer solids content was 0.5 parts, and deionized water was added to adjust the solid content of the slurry to 52 wt%. Coating was performed at 20°C with a low shear rate of 1.0 m / s at the impeller tip for 20 min, followed by spray drying at an inlet air temperature of 140°C, an outlet air temperature of 90°C, and an atomization pressure of 0.42 MPa. The resulting sequentially surface-controlled lightly calcined magnesia had a moisture content of 1.0 wt%, and the copolymer coordination layer exhibited a discontinuous island-like distribution with a surface coverage of 35%.
[0032] Component A, by weight, consists of 65 parts of sequentially surface-modified lightly calcined magnesia, 10 parts of reactive silicon source, 18 parts of wollastonite, 22 parts of basalt sand, 0.6 parts of microfiber toughening component, and 1.0 part of rheological building block component. The reactive silicon source comprises 8 parts of silica fume and 2 parts of spray-dried nano-silica in a weight ratio of 1:0.25; the median particle size (D50) of the silica fume is 0.10 μm, and the SiO2 content is 96 wt%; the primary particle size of the spray-dried nano-silica is 30 nm. The aspect ratio of wollastonite is 14. The median particle size (D50) of the basalt sand is 0.45 mm. The microfiber toughening component consists of 12 mm long polyvinyl alcohol fibers and 4.5 mm long basalt fibers in a weight ratio of 1:0.2. The rheological building block component consists of starch ether and attapulgite in a weight ratio of 1:2. Dry powder component A was prepared according to the dry mixing sequence of Example 1.
[0033] Liquid activation component B, by weight, consists of 20 parts dipotassium hydrogen phosphate, 6 parts potassium dihydrogen phosphate, 30 parts water, and 0.30 parts defoamer. The defoamer is composed of polyether-modified polysiloxane defoamer and polyoxypropylene glycerol ether defoamer in a weight ratio of 1:1. The weight ratio of dipotassium hydrogen phosphate to potassium dihydrogen phosphate is 1:0.30. Liquid activation component B, free of boric acid and borate, with a pH of 7.6 at 20°C, was prepared according to the dissolution sequence of Example 1.
[0034] This embodiment also provides a construction method for a rapid high-strength phosphate two-component spraying material for tunnel initial support, which includes the following steps S1-S4: S1: The conveying rate of dry powder component A is 25 kg / min, the material airflow pressure is 0.65 MPa, and liquid activating component B is sent into a nozzle with an annular outlet width of 1.5 mm at a conveying pressure of 0.40 MPa.
[0035] S2: The B liquid activating component forms an annular liquid curtain from the annular outlet, allowing the pneumatically conveyed A dry powder component to pass through the annular liquid curtain. The collision between the A dry powder component and the annular liquid curtain completes particle wetting and initial dispersion. The weight ratio of the A dry powder component to the B liquid activating component is 1:0.45, and the collision angle between the movement direction of the A dry powder component and the annular liquid curtain is 45°.
[0036] S3: After being wetted by the collision of the annular liquid curtain and atomized twice, a phosphate spraying mixture is formed.
[0037] S4: The formed phosphate spraying mixture is sprayed onto the surface of the steel mesh and the surrounding rock surface behind it. The distance between the nozzle and the sprayed surface is 0.8m, the spraying angle is 90°, and the thickness of a single layer is 35mm.
[0038] Testing revealed that the initial setting time of the sprayed mixture was 10 min, the final setting time was 15 min, and the time interval between initial and final setting was 5 min. The compressive strength after 1 hour of hardening was 35.4 MPa, after 24 hours it was 54.6 MPa, after 28 days it was 60.0 MPa, the flexural strength after 28 days it was 8.1 MPa, the 24-hour tensile bond strength with the rock substrate was 1.00 MPa, the impermeability grade was P12, the freeze-thaw resistance grade was F300, and the spraying rebound rate was 6.8%. A MgKPO4·6H2O crystal framework and a hydrated magnesium silicate gel phase distributed between the crystal framework were also detected in the hardened body.
[0039] Example 3
[0040] This embodiment provides a fast-acting, high-strength phosphate two-component spraying material for tunnel initial support, comprising separately stored dry powder component A and liquid activating component B.
[0041] The light-burned magnesia used had an MgO content of 93 wt%, a median particle size (D50) of 10 μm, and a citric acid activation time of 80 s. One hundred parts of light-burned magnesia were placed in a fluidized bed coating apparatus, and a water glass solution with a modulus of 3.2 and a solid content of 30 wt% was sprayed onto the surface of the magnesia, with 8 parts of solid water glass used. After spraying, mixing continued for 5 min, drying at 105 °C for 2 h, and then heat-treated at 260 °C for 60 min to form a magnesium silicate transition layer with a surface coverage of 98%.
[0042] A carboxyl-functionalized styrene-acrylate copolymer emulsion with an acid value of 20 mg KOH / g and a solid content of 40 wt% was sprayed into lightly calcined magnesia with a magnesium silicate transition layer. The copolymer solids content was 2.5 parts, and deionized water was added to adjust the solid content of the slurry to 60 wt%. Coating was performed at 28°C with a low shear rate of 0.3 m / s at the impeller tip for 30 min, followed by spray drying at an inlet air temperature of 160°C, an outlet air temperature of 70°C, and an atomization pressure of 0.60 MPa. The resulting sequentially surface-controlled lightly calcined magnesia had a moisture content of 1.5 wt%, and the copolymer coordination layer exhibited a discontinuous island-like distribution with a surface coverage of 70%.
[0043] Component A, by weight, consists of 75 parts of sequentially surface-modified lightly calcined magnesia, 14 parts of reactive silicon source, 8 parts of wollastonite, 30 parts of fine aggregate, 1.4 parts of microfiber toughening component, and 0.2 parts of rheological building block component. The reactive silicon source comprises 10 parts of silica fume and 4 parts of spray-dried nano-silica in a weight ratio of 1:0.40; the median particle size (D50) of the silica fume is 0.50 μm, and the SiO2 content is 93 wt%; the primary particle size of the spray-dried nano-silica is 5 nm. The aspect ratio of wollastonite is 20. The fine aggregate is composed of washed quartz sand and basalt sand in a weight ratio of 1:1, with a median particle size (D50) of 0.60 mm. The microfiber toughening component is composed of 6 mm long polyvinyl alcohol fibers and 6 mm long basalt fibers in a weight ratio of 1:0.4. The rheological building block component is composed of starch ether and attapulgite in a weight ratio of 1:6. Dry powder component A was prepared according to the dry mixing sequence of Example 1.
[0044] Liquid activation component B, by weight, consists of 32 parts dipotassium hydrogen phosphate, 8 parts potassium dihydrogen phosphate, 42 parts water, and 0.05 parts mineral oil-based defoamer. The weight ratio of dipotassium hydrogen phosphate to potassium dihydrogen phosphate is 1:0.25. Liquid activation component B, free of boric acid and borates, with a pH of 8.0 at 20°C, was prepared following the dissolution sequence in Example 1.
[0045] This embodiment also provides a construction method for a rapid high-strength phosphate two-component spraying material for tunnel initial support, which includes the following steps S1-S4: S1: The conveying rate of dry powder component A is 35 kg / min, the material airflow pressure is 0.35 MPa, and liquid activating component B is sent into a nozzle with an annular outlet width of 0.5 mm at a conveying pressure of 0.60 MPa.
[0046] S2: The B liquid activating component forms an annular liquid curtain from the annular outlet, and the A dry powder component conveyed by pneumatic conveying passes through the annular liquid curtain. The particle wetting and initial dispersion are completed by the collision between the A dry powder component and the annular liquid curtain. The weight ratio of the A dry powder component to the B liquid activating component is 1:0.5, and the collision angle between the movement direction of the A dry powder component and the annular liquid curtain is 60°.
[0047] S3: After being wetted by the collision of the annular liquid curtain and atomized twice, a phosphate spraying mixture is formed.
[0048] S4: Spray the formed phosphate spray mixture onto the area around the steel arch and the surrounding rock surface. The distance between the nozzle and the sprayed surface is 1.0m, the spray angle is 75°, and the thickness of a single layer is 50mm.
[0049] Testing revealed that the initial setting time of the sprayed mixture was 15 min, the final setting time was 18 min, and the time interval between initial and final setting was 3 min. The compressive strength after 1 hour of hardening was 30.0 MPa, after 24 hours it was 58.2 MPa, after 28 days it was 74.5 MPa, the flexural strength after 28 days it was 7.2 MPa, the 24-hour tensile bond strength with the rock substrate was 1.46 MPa, the impermeability grade was P10, the freeze-thaw resistance grade was F400, and the spraying rebound rate was 8.4%. A MgKPO4·6H2O crystal framework and a hydrated magnesium silicate gel phase distributed between the crystal framework were also detected in the hardened body.
[0050] Comparative Example 1 This comparative example is based on Example 2, with the only difference being that all the sequentially surface-controlled light-burned magnesium oxide in Example 2 was replaced with equal weight, from the same batch, and without water glass treatment or copolymer coating. All other raw material composition, dosage, preparation conditions, and construction parameters were the same as in Example 2. The light-burned magnesium oxide particles in this comparative example do not have a magnesium silicate transition layer or a discontinuous island copolymer coordination layer on their surface, and are used to investigate the effects of uncontrolled light-burned magnesium oxide on reaction rate, settling time, and concentrated exothermic reaction.
[0051] Comparative Example 2 This comparative example is based on Example 2, with the only difference being that after step M2 in the sequential surface-controlled preparation of light-burned magnesium oxide, step M3 is not performed. The light-burned magnesium oxide with the magnesium silicate transition layer is directly used to formulate dry powder component A. The composition, amount, preparation conditions, and construction parameters of the remaining raw materials are the same as in Example 2. This comparative example retains the magnesium silicate transition layer but does not have the carboxyl-functionalized styrene-acrylate copolymer coordination layer and the reaction window defined by it. It is used to investigate the effect of the discontinuous coordination structure of the outer layer on the reaction sequence and rapid hardening after initial setting.
[0052] Comparative Example 3 This comparative example is based on Example 2, with the only difference being that the reactive silicon source in Example 2 was completely replaced with an equal weight of crystalline quartz powder, and the crystalline quartz powder was graded and compounded to the same particle size distribution as the reactive silicon source in Example 2. All other raw material compositions, amounts, preparation conditions, and construction parameters were the same as in Example 2. This comparative example retains the magnesium silicate transition layer and the discontinuous island copolymer coordination layer, but does not include a reactive silicon source capable of participating in the magnesium silicate hydration reaction. This is used to investigate the effects of the hydrated magnesium silicate gel on relative pore filling, later-stage strength, impermeability, and freeze-thaw resistance.
[0053] Test Example 1: Reaction Time, Exothermic Behavior, and Mechanical Properties Test Materials from Examples 1-3 and Comparative Examples 1-3 were tested respectively. Comparative Example 1 was based on Example 2, except that the sequentially surface-controlled light-burned magnesium oxide was replaced with an equal amount of untreated light-burned magnesium oxide from the same batch. Comparative Example 2 was based on Example 2, except that the sequentially surface-controlled light-burned magnesium oxide was only processed in steps M1 and M2, without the addition of a carboxyl-functionalized styrene-acrylate copolymer coordination layer. Comparative Example 3 was based on Example 2, except that the reactive silicon source was replaced with an equal amount of crystalline quartz powder with the same particle size distribution.
[0054] Three independent batches of tests were conducted for each group. Setting time was determined using the penetration resistance method according to GB / T 50080-2016 "Standard for Test Methods of Performance of Ordinary Concrete Mixtures". After the sprayed material stabilized, samples of the mixture were continuously collected at the nozzle outlet. The moment of first contact between dry powder component A and liquid activating component B was taken as the starting point for timing. Penetration resistance was measured every 30 seconds. The time corresponding to a penetration resistance of 3.5 MPa was taken as the initial setting time, and the time corresponding to a penetration resistance of 28 MPa was taken as the final setting time. The difference between the final setting time and the initial setting time was calculated.
[0055] The hydration exothermic reaction was performed according to ASTM C1702. 15g samples were prepared according to the weight ratio of dry powder component A to liquid activating component B specified for each group. Isothermal conduction calorimetry was conducted at 20℃±0.1℃ for 72h. The time of occurrence of the main exothermic peak, the maximum heat flux, and the cumulative heat release after 2h after mixing were recorded. The heat flux and cumulative heat release were normalized to the mass of the cementitious material in dry powder component A.
[0056] Compressive strength specimens were prepared using 100mm×100mm×100mm cubic molds. The mixture was directly sprayed into the molds. Three specimens were prepared for each batch and at each age. The compressive strength was determined at 1h, 24h, and 28d according to GB / T50081-2019. For 28d flexural strength specimens, sprayed large plates were prepared according to Appendix B of JGJ / T 372-2016, and then cut into 75mm×125mm×600mm beam specimens according to Appendix E, with no fewer than three specimens per group. The arithmetic mean of the valid specimens was taken as the result.
[0057] Table 1. Results of reaction time, exothermic behavior, and mechanical properties.
[0058] As can be seen from Table 1, in Examples 1 to 3, the initial setting time was 6.0 min to 15.0 min, and the time difference between initial setting and final setting was in the range of 3.0 min to 5.0 min. That is, this application does not simply reduce the activity of lightly calcined magnesium oxide, but rather forms a reaction sequence with a longer spraying operation period and rapid hardening after initial setting. Furthermore, the 1-hour compressive strength in Examples 1 to 3 is greater than or equal to 30.0 MPa, the 24-hour compressive strength is greater than or equal to 45.0 MPa, the 28-day compressive strength is greater than or equal to 60.0 MPa, and the 28-day flexural strength is also greater than or equal to 6.0 MPa. In contrast, Comparative Example 1 did not perform surface conditioning on the lightly calcined magnesia, and the initial solidification time was only 1.5 min. The main exothermic peak was also brought forward to 2.2 min, and the maximum heat flux reached 16.4 mW / g. It has obvious characteristics of concentrated exothermic heat release and instantaneous solidification. Although its 1-hour compressive strength is very high, its 24-hour and 28-day compressive strengths are 43.8 MPa and 50.6 MPa, respectively. This indicates that the excessively fast reaction is not conducive to the uniform growth of the crystal skeleton and the development of later strength.
[0059] Comparative Example 2, with only a magnesium silicate transition layer, showed an increased initial setting time from 1.5 min to 4.2 min and a decreased maximum heat flux from 16.4 mW / g to 10.9 mW / g, indicating that the magnesium silicate transition layer could slow down the initial reaction on the surface of lightly calcined magnesium oxide; however, its initial setting time was still below 6.0 min, suggesting that simply setting the magnesium silicate transition layer could not provide a sufficient spraying operation window. Example 2, with the further addition of a discontinuous island-shaped copolymer coordination layer, showed an increased initial setting time to 10.0 min and a decreased maximum heat flux to 6.8 mW / g, indicating that the reaction window and the area covered by the coordination layer together formed a spatial partitioning reaction effect.
[0060] Comparative Example 3 retained the sequential surface-controlled calcined magnesia, so its condensation time and the time of the exothermic peak were similar to those of Example 2. However, after replacing the reactive silicon source with crystalline quartz powder, its 28-day compressive strength and flexural strength decreased to 52.8 MPa and 4.8 MPa, respectively. This indicates that the sequential surface-controlled structure is mainly used to regulate the reaction sequence of calcined magnesia and phosphate, while the reactive silicon source mainly participates in the subsequent hydration reaction of magnesium silicate and improves the continuity between crystal frameworks. The two play different but complementary roles.
[0061] In summary, this application constructs a sequential surface regulation structure by sequentially forming a magnesium silicate transition layer and a copolymer coordination layer with discontinuous island distribution on the surface of lightly calcined magnesium oxide particles, and utilizing the regions not covered by the copolymer coordination layer to form reaction windows. Without using boric acid and borates, it effectively suppresses concentrated exothermics and instantaneous solidification of lightly calcined magnesium oxide, while retaining sufficient early reaction sites. This allows the material to possess advantages such as workability, rapid hardening after initial setting, early load-bearing capacity, and later strength development, resulting in technical effects distinct from simply slowing setting or reducing the activity of magnesium oxide.
[0062] Test Example 2: Spray coating performance, interface bonding and durability test Spraying tests were conducted using Examples 1-3 and Comparative Examples 1-3, respectively. Each group underwent three independent sprayings, with an ambient temperature of 20℃±2℃. The feed rate of dry powder component A was uniformly 25 kg / min, the material-carrying airflow pressure was 0.50 MPa, the feed pressure of liquid activating component B was 0.60 MPa, the width of the annular liquid outlet was 1.0 mm, the collision angle between the movement direction of dry powder component A and the annular liquid curtain was 45°, the distance between the nozzle and the sprayed surface was 1.0 m, the spray angle was 90°, and the single-layer spray thickness was 40 mm. Examples 1-3 were supplied according to their respective specified weight ratio of dry powder component A to liquid activating component B, while Comparative Examples 1-3 used the same feeding ratio as Example 2.
[0063] The rebound rate was determined according to Appendix G of JGJ / T 372-2016 "Technical Specification for Application of Shotcrete". The volume of sprayed material used in each test was not less than 1 m³. 3 And a 40m² area was laid under the sprayed surface. 2 The plastic film was used for spraying. Weighing was only performed after the material output stabilized. At the end of spraying, all rebound material was collected and weighed to calculate the rebound rate as a percentage of the total mass of the rebound material. Continuous spraying lasted 30 minutes, and the number of times spraying was stopped due to blockages in the nozzle or internal flow channels was recorded. A 5x5 measuring point was divided on the vertical granite surface to be sprayed, and a total of 25 spray layer thicknesses were measured. The difference between the maximum and minimum thicknesses was taken as the spray layer thickness range. After spraying, the surface was cured under the same conditions for 7 days, and a crack observation instrument was used to inspect a 1m section of the surface. 2 The total length of cracks with a width of not less than 0.05 mm within the test area was statistically analyzed.
[0064] The 24-hour tensile bond strength was determined according to the field core-drilling pull-out method in Appendix D of JGJ / T 372-2016: three measuring points were set for each sprayed slab, the core diameter was 50 mm, the drilling depth into the granite substrate was 20 mm, and axial pull-out was performed with a loading rate of 1.3 MPa / min. A total of nine valid test results were obtained for each group. Water permeability and freeze-thaw resistance specimens were prepared as sprayed slabs and samples were taken according to Appendix B of JGJ / T 372-2016. After curing under standard conditions for 28 days, their water permeability resistance and rapid freeze-thaw resistance were determined according to GB / T 50082-2024 "Standard for Test Methods of Long-Term Performance and Durability of Concrete". The impermeability test uses 6 specimens per group; the rapid freeze-thaw test uses 3 prism specimens with dimensions of 100mm×100mm×400mm per group. The freeze resistance level is determined by the maximum number of freeze-thaw cycles that the specimens undergo before their relative dynamic elastic modulus and mass loss reach the limits specified in the standard.
[0065] Table 2. Test results of spray coating performance, interface bonding and durability.
[0066] As shown in Table 2, no clogging or spraying stoppage occurred during the continuous spraying process of Examples 1 to 3 for 30 minutes. The rebound rate was 6.8% to 10.0%, and the thickness difference of the sprayed layer was 5.0 mm to 8.2 mm. This indicates that the material can be quickly wetted and dispersed in the annular liquid curtain and form a continuous and uniform sprayed layer after reaching the sprayed surface.
[0067] Comparative Example 1 used untreated lightly calcined magnesium oxide, which had a rebound rate of 18.7%. After 30 minutes of continuous spraying, it experienced 5 instances of clogging or stopping, and the thickness variation reached 23.6 mm. This was because the untreated lightly calcined magnesium oxide reacted rapidly upon contact with phosphate, causing some material to agglomerate within the nozzle wetting area, resulting in insufficient atomization and the formation of adhering deposits in the internal flow channels. Comparative Example 2, with the addition of a magnesium silicate transition layer, showed a reduction in rebound rate, number of clogging incidents, and thickness variation, but it was still significantly worse than Example 2, further demonstrating the important role of the discontinuous island-shaped coordination layer in maintaining an effective reaction window near the nozzle.
[0068] Comparative Example 3, retaining the sequential surface-controlled lightly sintered magnesium oxide, exhibited rebound rate, clogging frequency, and thickness variation similar to Example 2, indicating that the reactive silicon source is not the sole factor improving nozzle patency. However, the total 7-day crack length in Comparative Example 3 decreased from 8 mm / m in Example 2. 2 Increased to 91mm / m 2After 24 hours, the tensile bond strength decreased to 0.86 MPa, the impermeability grade decreased from P12 to P6, and the freeze-thaw resistance grade decreased from F300 to F200. These results indicate that crystalline quartz powder only plays an inert filling role and cannot replace the magnesium silicate hydration products formed by reactive silicon sources. The gel phase formed with the participation of reactive silicon sources can fill the pores between the MgKPO4·6H2O crystal framework, improve the transition zone at the surrounding rock interface, and inhibit crack propagation.
[0069] Therefore, the technical means of this application do not merely improve construction time through retarding treatment, but rather utilize sequential surface regulation of lightly calcined magnesium oxide to control the reaction sequence near the nozzle, utilize annular liquid curtain collision and secondary atomization to improve the uniformity of dry powder wetting, and utilize the magnesium hydration products formed by reactive silicon sources to improve the density and interfacial bonding performance of the hardened layer. Examples 1-3 simultaneously achieve a rebound rate of no more than 10%, a 24-hour tensile bond strength of no less than 1.0 MPa, a permeability grade of no less than P8, and a freeze-thaw resistance grade of no less than F300, demonstrating the synergistic effect between reaction regulation, spraying process, and multiphase cementitious structure, which can provide relatively complete comparative test support for the beneficial effects and inventiveness of this application.
[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on these embodiments, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still combine, add, delete, or otherwise adjust the features of the various embodiments of the present invention according to the circumstances without conflict or creative effort, thereby obtaining different technical solutions that do not fundamentally depart from the concept of the present invention. These technical solutions also fall within the scope of protection of the present invention.
Claims
1. A rapid-release, high-strength phosphate two-component spraying material for tunnel initial support, characterized in that, Includes separately stored dry powder component A and liquid activation component B; The A dry powder component, by weight, comprises: 55-75 parts of sequentially surface-modified lightly calcined magnesium oxide, 10-22 parts of reactive silicon source, 8-18 parts of acicular silicate minerals, 15-30 parts of fine aggregate, 0.6-1.8 parts of microfiber toughening component, and 0.2-1.0 parts of rheological building block component; The liquid activation component B comprises, by weight, 20 to 32 parts of dipotassium hydrogen phosphate, 2 to 8 parts of potassium dihydrogen phosphate, 30 to 55 parts of water, and 0.05 to 0.30 parts of defoamer; The sequential surface-controlled light-burned magnesium oxide includes a light-burned magnesium oxide particle core, a magnesium silicate transition layer formed on the surface of the light-burned magnesium oxide particle core, and a carboxyl-functionalized styrene-acrylate copolymer coordination layer formed on the outside of the magnesium silicate transition layer; the carboxyl-functionalized styrene-acrylate copolymer coordination layer is distributed in a discontinuous island shape, and forms a reaction window on the particle surface of the sequential surface-controlled light-burned magnesium oxide that is not covered by the carboxyl-functionalized styrene-acrylate copolymer coordination layer.
2. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The sequentially surface-modified lightly calcined magnesium oxide was prepared using the following method: M1: Add 3 to 8 parts of water glass (based on solids) to every 100 parts of light-burned magnesia. Spray the water glass solution onto the surface of the fluidized light-burned magnesia, mix, and then dry. M2: The dried lightly calcined magnesium oxide is heat-treated at 260℃~340℃ for 30min~90min to allow the silicate components in the water glass to react with the surface of the lightly calcined magnesium oxide particles to form the magnesium silicate transition layer. M3: Add 0.5 to 2.5 parts (based on solids) of carboxyl-functionalized styrene-acrylate copolymer to 100 parts of lightly calcined magnesium oxide with the magnesium silicate transition layer. Spray the carboxyl-functionalized styrene-acrylate copolymer emulsion into the lightly calcined magnesium oxide with the magnesium silicate transition layer, and add deionized water to adjust the solid content of the resulting coating slurry to 45 wt% to 60 wt%. At 20°C to 35°C, with a stirring paddle tip linear velocity of 0.3 m / s to 1... Low-shear coating was performed at 0 m / s for 10 to 30 minutes; then the resulting coated slurry was spray-dried at an inlet air temperature of 140°C to 180°C, an outlet air temperature of 70°C to 90°C, and an atomization pressure of 0.25 MPa to 0.60 MPa to obtain sequentially surface-controlled lightly calcined magnesium oxide with a moisture content of no more than 1.5 wt%, which caused the carboxyl-functionalized styrene-acrylate copolymer to form a coordination layer with a discontinuous island distribution on the outside of the magnesium silicate transition layer.
3. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The lightly calcined magnesium oxide contains no less than 85 wt% MgO, has a median particle size D50 of 10 μm to 45 μm, and a citric acid activation time of 40 s to 120 s; the water glass modulus used to form the magnesium silicate transition layer is 2.0 to 3.2; and the acid value of the carboxyl-functionalized styrene-acrylate copolymer is 20 mg KOH / g to 80 mg KOH / g. The magnesium silicate transition layer has a coverage rate of 80% to 98% on the surface of the lightly calcined magnesium oxide particles, and the carboxyl-functionalized styrene-acrylate copolymer coordination layer has a coverage rate of 35% to 70% on the surface of the magnesium silicate transition layer.
4. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The weight ratio of dipotassium hydrogen phosphate to potassium dihydrogen phosphate is 1:(0.08-0.30); the pH value of the liquid activation component B at 20°C is 7.6-8.5; the liquid activation component B does not contain boric acid or borate; the defoamer is one or at least two of the following: polydimethylsiloxane emulsion defoamer, polyether-modified polysiloxane defoamer, polyoxypropylene glycerol ether defoamer, and mineral oil defoamer.
5. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The reactive silicon source comprises silica fume and spray-dried nano-silica, wherein the weight ratio of silica fume to spray-dried nano-silica is 1:(0.10-0.40); the median particle size D50 of the silica fume is 0.10μm-1.00μm, and the silica content is not less than 90wt%; the spray-dried nano-silica is obtained by spray drying colloidal silica with a primary particle size of 5nm-30nm.
6. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The acicular silicate mineral is wollastonite, and the aspect ratio of the wollastonite is 8 to 20; the microfiber toughening component is composed of polyvinyl alcohol fiber and basalt fiber in a weight ratio of 1:(0.2 to 0.6), the length of the polyvinyl alcohol fiber is 6 mm to 12 mm, and the length of the basalt fiber is 3 mm to 6 mm; the rheological building block is composed of starch ether and attapulgite in a weight ratio of 1:(2 to 6).
7. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The dry powder component A and the liquid activating component B are mixed at a weight ratio of 1:(0.35-0.55). After mixing, the lightly calcined magnesium oxide at the reaction window first reacts with dipotassium hydrogen phosphate and potassium dihydrogen phosphate from the liquid activating component B to form a crystal framework with MgKPO4·6H2O as the main crystal phase. The lightly calcined magnesium oxide in the region covered by the carboxyl-functionalized styrene-acrylate copolymer coordination layer participates in the reaction after the coordination layer is gradually dissociated. The magnesium silicate transition layer and the reactive silicon source jointly participate in the magnesium silicate hydration reaction, forming a hydrated magnesium silicate gel phase between the MgKPO4·6H2O crystal framework.
8. The rapid-release, high-strength phosphate two-component spraying material for tunnel initial support according to claim 1, characterized in that, The initial setting time of the mixture of dry powder component A and liquid activating component B is 6 min to 15 min, and the time interval from the initial setting state to the final setting state is no more than 5 min; the compressive strength after 1 hour of hardening is no less than 30 MPa, the compressive strength after 24 hours of hardening is no less than 45 MPa, the compressive strength after 28 days of hardening is no less than 60 MPa, the flexural strength after 28 days of hardening is no less than 6.0 MPa, the 24-hour tensile bond strength with the rock substrate is no less than 1.0 MPa, the impermeability grade is no less than P8, and the frost resistance grade is no less than F300.
9. A construction method for a rapid-acting, high-strength phosphate two-component spray material for tunnel initial support as described in any one of claims 1 to 8, characterized in that, Includes the following steps: S1: Add dry powder component A to a closed dry powder spraying equipment, and fluidize and pneumatically convey dry powder component A through a material-carrying airflow, while conveying liquid activating component B to a nozzle with an annular liquid outlet. S2: The B liquid activating component forms an annular liquid curtain from the annular liquid outlet, and the A dry powder component conveyed by pneumatic conveying passes through the annular liquid curtain. The collision between the A dry powder component and the annular liquid curtain completes the particle wetting and initial dispersion. S3: The secondary atomized airflow in the nozzle is used to shear and disperse the wetted material to form a phosphate spraying mixture; S4: The phosphate spraying mixture is sprayed onto the exposed surrounding rock surface, the surface of the reinforcing mesh, or around the steel arch frame after tunnel blasting, forming an initial support layer for the tunnel in layers.
10. The construction method according to claim 9, characterized in that, In step S1, the conveying rate of dry powder component A is 15 kg / min to 35 kg / min, the material airflow pressure is 0.35 MPa to 0.65 MPa, and the conveying pressure of liquid activating component B is 0.40 MPa to 0.80 MPa; in step S2, the width of the annular liquid outlet is 0.5 mm to 1.5 mm, and the collision angle between the movement direction of dry powder component A and the annular liquid curtain is 30° to 60°; in step S4, the distance between the nozzle and the sprayed surface is 0.8 m to 1.3 m, the spray angle is 75° to 90°, the single-layer spray thickness is 20 mm to 50 mm, and the spray rebound rate is not higher than 10%.