A high dielectric constant C0G dielectric ceramic material and its preparation method
By combining the main phase with a uranium-type structure and the regulating phase with a perovskite structure, and by manganese-zinc doping, the problems of second-phase precipitation and lattice mismatch in COG dielectric ceramic materials when improving the dielectric constant are solved, achieving a balance between high dielectric constant and temperature stability, which is suitable for aerospace, medical electronics and other fields.
Patent Information
- Application Number
- CN202611247027.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing COG dielectric ceramic materials are prone to second-phase precipitation and lattice mismatch when the dielectric constant is increased, resulting in a sharp increase in temperature coefficient. This makes it difficult to maintain COG characteristics over a wide temperature range and fails to meet the application requirements of high-reliability electronic components.
A method for preparing high dielectric constant C0G dielectric ceramic materials was adopted. By combining the main phase with the ochre-type structure with the perovskite structure regulating phase and adding manganese and zinc sources, a local structure was formed, which achieved both improved dielectric constant and temperature stability.
The dielectric constant is increased to over 140, and the temperature coefficient of capacitance is controlled within the range of -28ppm/℃ to +19ppm/℃, meeting the requirements for high reliability over a wide temperature range and reducing the difficulty and cost of process control in industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic ceramic materials technology, and in particular to a high dielectric constant COG dielectric ceramic material and its preparation method. Background Technology
[0002] COG dielectric ceramic materials possess advantages such as near-zero temperature coefficient of dielectric constant, low dielectric loss, and high stability, making them widely used in aerospace, medical electronics, industrial automation, and other applications with stringent power density and reliability requirements. As electronic systems continue to evolve towards higher frequencies, higher voltages, and higher power densities, and as entire devices continue to miniaturize, the market is placing higher demands on the dielectric constant of COG dielectric ceramic materials. The goal is to maximize the dielectric constant while maintaining near-zero temperature drift and low loss, thereby achieving miniaturization and high capacity in components.
[0003] Currently, commercially available COG dielectric ceramic materials are mainly based on composite perovskite, pyrochlore, and tungsten bronze-type structural systems. The intrinsic dielectric constant of these material systems generally does not exceed 130. When researchers attempt to increase the dielectric constant to above 130 through doping, solid solution, or the introduction of a high-dielectric second phase, the material system is highly susceptible to the precipitation of non-target impurity phases within the grains, leading to severe lattice mismatch. These microstructural changes not only limit further effective increases in dielectric constant but also cause a sharp deterioration in the dielectric constant temperature coefficient, deviating from the near-zero range. This makes it impossible for the material to maintain COG characteristics within a wider temperature range of -55℃ to 125℃, making it difficult to meet the application requirements of high-reliability electronic components. Summary of the Invention
[0004] (a) Technical problems to be solved In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a high dielectric constant COG dielectric ceramic material and its preparation method, which solves the technical problem that when the dielectric constant of the existing COG dielectric ceramic material is increased, a second phase and lattice mismatch appear in the ceramic material grains, resulting in a sharp increase in the temperature coefficient, and thus making it difficult to meet the requirements of wide temperature range operation.
[0005] (II) Technical Solution To achieve the above objectives, the main technical solutions adopted by the present invention include: In a first aspect, embodiments of the present invention provide a high dielectric constant COG dielectric ceramic material, the dielectric ceramic material comprising a main crystalline phase, a regulating phase, and a dopant; the chemical formula of the main crystalline phase is BaNd2Bi. 0.6 Sm 0.8 Ti6O 18 The chemical formula of the regulating phase is Bi(Mg) 2 / 3 Nb 1 / 3 O3; Based on a total mass of 1 part for the main crystalline phase and the regulating phase, the mass fraction of the main crystalline phase is 91.33wt%-98.08wt%, and the mass fraction of the regulating phase is 1.92wt%-8.67wt%. Based on a total mass of 100 parts for the main crystalline phase and the regulating phase, the dopant comprises 0.23-2.30 parts by mass of manganese source and 0.16-1.63 parts by mass of zinc source.
[0006] Wherein, the manganese source is calculated as MnCO3, and the zinc source is calculated as ZnO.
[0007] Alternatively, the dielectric constant of the dielectric ceramic material is not less than 140.
[0008] In a further technical solution, the dielectric constant of the dielectric ceramic material varies in the range of 140-152.
[0009] In a further technical solution, the temperature coefficient of capacitance of the dielectric ceramic material fluctuates within a range of -28ppm / ℃ to +19ppm / ℃.
[0010] In a further technical solution, the sintering temperature of the dielectric ceramic material is 1150℃-1300℃.
[0011] Secondly, embodiments of the present invention provide a method for preparing a high dielectric constant C0G dielectric ceramic material, comprising the following steps: S1. Weigh and prepare the raw materials Ba source, Nd source, Bi source, Ti source, Sm source, Mg source and Nb source according to the chemical formulas of the main crystalline phase and the regulating phase respectively; S2. Place the two powders prepared in step S1 into two ball mill jars, add zirconia balls and solvent, and ball mill; place the ball-milled raw materials in a drying oven to dry, and sieve the dried materials to obtain the first mixture and the second mixture; S3. Pre-calcine the first mixture at 1000℃-1150℃ for 2h-4h to synthesize the main crystalline phase powder; pre-calcine the second mixture at 900℃-1000℃ for 2h-4h to synthesize the regulating phase powder; S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 according to the ratio, add the manganese source and the zinc source, put them into a ball mill jar, add zirconia balls and solvent, and ball mill; dry the ball-milled slurry, and sieve the dried material to obtain a mixture; S5. The mixture is mixed with the binder, granulated, and then pressed and debonded to obtain a ceramic green body; S6. The ceramic green body is sintered to obtain a high dielectric constant COG dielectric ceramic material.
[0012] Alternatively, in step S1, the Ba source is BaCO3 powder, the Nd source is Nd2O3 powder, the Bi source is Bi2O3 powder, the Ti source is TiO2 powder, the Sm source is Sm2O3 powder, the Mg source is MgCO3 powder, and the Nb source is Nb2O5 powder.
[0013] Alternatively, in step S4, the Mn source is MnCO3 powder and the Zn source is ZnO powder.
[0014] Alternatively, in steps S2 and S4, the mesh size of the sieve is 60 mesh.
[0015] Alternatively, in steps S2 and S4, the mass ratio of powder, zirconia balls, and solvent is 1:2:0.8.
[0016] In a further technical solution, in step S2, the ball milling parameters are: rotation speed 300r / min-400r / min, ball milling time 3h-5h; in step S4, the ball milling parameters are: rotation speed 400r / min-500r / min, ball milling time 3h-6h.
[0017] Alternatively, in step S5, the adhesive is PVB, and the mass concentration of the adhesive is 5%-10%.
[0018] Alternatively, in step S6, the sintering temperature is 1150℃-1300℃ and the time is 2h-4h.
[0019] (III) Beneficial Effects The beneficial effects of this invention are as follows: This invention provides a high-dielectric-constant COG dielectric ceramic material and its preparation method. It combines a high-dielectric-constant tungsten bronze-type main phase with a perovskite-type regulating phase possessing stable temperature characteristics. Through precise chemical proportioning and process control, the two structures achieve atomic-scale mutual doping and mutual restraint during sintering, forming a localized structure between complete order and disorder. This composite phase antagonistic mechanism allows the tungsten bronze main phase to perform the function of high dielectric constant while the perovskite regulating phase effectively relaxes the lattice stress caused by temperature changes, thus overcoming the bottleneck of the prior art where high dielectric constant and near-zero temperature drift are difficult to achieve simultaneously.
[0020] The dielectric ceramic material of this invention maintains the characteristics of COG while increasing the dielectric constant to over 140, exhibiting both high dielectric constant and high temperature stability. Its capacitance temperature coefficient fluctuation range is firmly controlled within -28ppm / ℃ to +19ppm / ℃, meeting the industrial requirements for COG materials in wide temperature range and high reliability scenarios.
[0021] The preparation method of this invention ensures the purity and homogeneity of the target phase under complex chemical composition through a stepwise synthesis of the main crystalline phase and the regulating phase, followed by recombination. This process requires minimal equipment, and the addition of elements such as Mn and Zn effectively broadens the sintering temperature window of the material. More importantly, Mn and Zn ions enter the interstitial spaces or replace specific lattice sites during sintering, effectively pinning ion displacements that easily induce temperature drift and fundamentally suppressing temperature coefficient drift. This mechanism enables the material to achieve sintering densification within a wide temperature range of 1180℃-1290℃, significantly reducing the difficulty and cost of process control in industrial-scale production, and possessing high practical value. Detailed Implementation
[0022] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below through specific embodiments.
[0023] To better understand the above technical solutions, exemplary embodiments of the present invention will be described in more detail below. While exemplary embodiments of the present invention have been shown, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the present invention can be understood more clearly and thoroughly, and that the scope of the present invention can be fully conveyed to those skilled in the art.
[0024] Example 1: This embodiment provides a high dielectric constant C0G dielectric ceramic material, including a main crystalline phase, a regulating phase, and a dopant; the chemical formula of the main crystalline phase is BaNd2Bi. 0.6 Sm 0.8 Ti6O 18 The chemical formula of the regulating phase is Bi(Mg) 2 / 3 Nb 1 / 3 O3; based on a total mass of 1 part of the main crystalline phase and the regulating phase, with a mass fraction of 95.78 wt% for the main crystalline phase and 4.22 wt% for the regulating phase; based on a total mass of 100 parts of the main crystalline phase and the regulating phase, the dopants are 0.72 parts by mass of manganese source (calculated as MnCO3) and 1.22 parts by mass of zinc source (calculated as ZnO). The preparation method includes the following steps: S1. Weigh and mix the raw materials BaCO3 powder, Nd2O3 powder, Bi2O3 powder, TiO2 powder, Sm2O3 powder, MgCO3 powder and Nb2O5 powder according to the chemical formulas of the main crystalline phase and the regulating phase.
[0025] S2. Place the two powders prepared in step S1 into two ball mill jars respectively. Add zirconia balls and deionized water at a mass ratio of powder, zirconia balls, and deionized water of 1:2:0.8, and ball mill at 350 r / min for 4 hours. Place the two slurries after ball milling into drying ovens and dry them. Pass the dried materials through a 60-mesh sieve to obtain the first mixture and the second mixture.
[0026] S3. The first mixture is pre-calcined at 1100℃ for 2 hours to synthesize the main crystalline phase powder; the second mixture is pre-calcined at 920℃ for 3 hours to synthesize the regulating phase powder.
[0027] S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 at a mass ratio of 95.78:4.22, and add 0.72 parts by mass of MnCO3 powder and 1.22 parts by mass of ZnO powder. Place the mixture into a ball mill jar, and simultaneously add zirconia balls and deionized water at a mass ratio of 1:2:0.8. Ball mill at 450 r / min for 6 hours. Dry the ball-milled slurry and pass the dried material through a 60-mesh sieve to obtain a mixture.
[0028] S5. The mixture is mixed with a polyvinyl butyral (PVB) binder with a mass concentration of 8%, granulated, and then pressed and debonded to obtain a ceramic green body.
[0029] S6. The ceramic green body was sintered at 1250℃ for 4 hours to obtain a high dielectric constant C0G dielectric ceramic material.
[0030] Example 2: This embodiment provides a high dielectric constant C0G dielectric ceramic material, which differs from Embodiment 1 in that the total mass of the main crystalline phase and the regulating phase is 1 part, the mass fraction of the main crystalline phase is 98.08 wt%, and the mass fraction of the regulating phase is 1.92 wt%; the total mass of the main crystalline phase and the regulating phase is 100 parts, and the dopants are 1.15 parts by mass of MnCO3 and 0.41 parts by mass of ZnO.
[0031] The preparation method differs from that in Example 1 in that: S2, the ball mill speed is 400 r / min, and the ball milling time is 5 h.
[0032] S3. Pre-calcine the first mixture at 1120℃ for 3 hours to synthesize the main crystalline phase powder. Pre-calcine the second mixture at 980℃ for 2 hours to synthesize the regulating phase powder.
[0033] S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 at a mass ratio of 98.08:1.92, and add 1.15 parts by mass of MnCO3 powder and 0.41 parts by mass of ZnO powder. Place the mixture into a ball mill jar, and simultaneously add zirconia balls and deionized water at a mass ratio of 1:2:0.8. Ball mill at 500 r / min for 6 hours. Dry the ball-milled slurry and pass the dried material through a 60-mesh sieve to obtain a mixture.
[0034] The mass concentration of S5 and PVB is 5%.
[0035] S6. The ceramic green body was sintered at 1290℃ for 2 hours to obtain a high dielectric constant C0G dielectric ceramic material.
[0036] The remaining steps are the same as in Example 1.
[0037] Example 3 This embodiment provides a high dielectric constant C0G dielectric ceramic material, which differs from Embodiment 1 in that the total mass of the main crystalline phase and the regulating phase is 1 part, the mass fraction of the main crystalline phase is 93.88 wt%, and the mass fraction of the regulating phase is 6.12 wt%; the total mass of the main crystalline phase and the regulating phase is 100 parts, and the dopants are 2.30 parts by mass of MnCO3 and 1.22 parts by mass of ZnO.
[0038] The preparation method differs from that in Example 1 in that: S3. The first mixture is pre-calcined at 1150℃ for 2 hours to synthesize the main crystalline phase powder. The second mixture is pre-calcined at 970℃ for 3 hours to synthesize the conditioning phase powder.
[0039] S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 at a mass ratio of 93.88:6.12, and add 2.30 parts by mass of MnCO3 powder and 1.22 parts by mass of ZnO powder. Place the mixture into a ball mill jar, and simultaneously add zirconia balls and deionized water at a mass ratio of powder:zirconia balls:deionized water of 1:2:0.8. Ball mill at 500 r / min for 6 hours. Dry the ball-milled slurry and pass the dried material through a 60-mesh sieve to obtain a mixture.
[0040] S6. The ceramic green body was sintered at 1210℃ for 2 hours to obtain a high dielectric constant COG dielectric ceramic material.
[0041] The remaining steps are the same as in Example 1.
[0042] Example 4: This embodiment provides a high dielectric constant C0G dielectric ceramic material, which differs from Embodiment 1 in that the total mass of the main crystalline phase and the regulating phase is 1 part, the mass fraction of the main crystalline phase is 92.98 wt%, and the mass fraction of the regulating phase is 7.02 wt%; the total mass of the main crystalline phase and the regulating phase is 100 parts, and the dopants are 2.30 parts by mass of MnCO3 and 0.81 parts by mass of ZnO.
[0043] The preparation method differs from that in Example 1 in that: S2, the ball mill speed is 400 r / min, and the ball milling time is 5 h.
[0044] S3. The first mixture is pre-calcined at 1160℃ for 3 hours to synthesize the main crystalline phase powder. The second mixture is pre-calcined at 940℃ for 3 hours to synthesize the conditioning phase powder.
[0045] S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 at a mass ratio of 92.98:7.02, and add 2.30 parts by mass of MnCO3 powder and 0.81 parts by mass of ZnO powder. Place the mixture into a ball mill jar, and simultaneously add zirconia balls and deionized water at a mass ratio of 1:2:0.8. Ball mill at 400 r / min for 4 hours. Dry the ball-milled slurry and pass the dried material through a 60-mesh sieve to obtain a mixture.
[0046] The mass concentration of S5 and PVB is 10%.
[0047] S6. The ceramic green body was sintered at 1180℃ for 4 hours to obtain a high dielectric constant C0G dielectric ceramic material.
[0048] The remaining steps are the same as in Example 1.
[0049] Comparative Example 1: This comparative example provides a dielectric ceramic material, including a main crystalline phase, a moderating phase, and a dopant; the chemical formula of the main crystalline phase is BaNd2Bi. 0.6 Sm 0.8 Ti6O 18 The chemical formula of the regulating phase is Bi(Mg) 2 / 3 Nb 1 / 3 O3; based on a total mass of 1 part of the main crystal phase and the regulating phase, the mass fraction of the main crystal phase is 89.48 wt% and the mass fraction of the regulating phase is 10.52 wt%; based on a total mass of 100 parts of the main crystal phase and the regulating phase, the dopants are 0.57 parts by mass of MnCO3 and 0.41 parts by mass of ZnO.
[0050] The preparation method differs from Example 1 in the following steps: S4, the main crystalline phase powder and the conditioning phase powder obtained in step S3 are weighed at a mass ratio of 89.48:10.52, and 0.57 parts by mass of MnCO3 powder and 0.41 parts by mass of ZnO powder are added. The mixture is placed in a ball mill jar, and simultaneously, zirconia balls and deionized water are added at a mass ratio of powder, zirconia balls, and deionized water of 1:2:0.8. The mixture is ball-milled at 450 r / min for 6 hours. The ball-milled slurry is dried, and the dried material is passed through a 60-mesh sieve to obtain a mixture. The remaining steps are the same as in Example 1.
[0051] Comparative Example 2: This comparative example provides a dielectric ceramic material comprising a main crystalline phase and a modifier phase, free of dopants (i.e., without trace amounts of Mn / Zn composite doping). The chemical formula of the main crystalline phase is BaNd₂Bi. 0.6 Sm 0.8 Ti6O 18 The chemical formula of the regulating phase is Bi(Mg) 2 / 3 Nb 1 / 3 O3; the total mass of the main crystalline phase and the regulating phase is 1 part, the mass fraction of the main crystalline phase is 95.78 wt%, and the mass fraction of the regulating phase is 4.22 wt%. The preparation method is the same as in Example 1.
[0052] Dielectric properties were tested on Examples 1-4 and Comparative Examples 1-2, and the test results are shown in Table 1.
[0053] Table 1 Dielectric properties of dielectric ceramic materials
[0054] The following conclusions can be drawn from Table 1: (1) In Examples 1-4, the mass fraction of the main crystalline phase was in the range of 91.33wt%-98.08wt%, the mass fraction of the regulating phase was in the range of 1.92wt%-8.67wt%, and the mass fraction of the dopant was in the ranges of 0.23-2.30 and 0.16-1.6%, respectively. The dielectric constant of the resulting materials was above 140, and the temperature coefficient of capacitance was within ±30ppm / ℃, meeting the COG specification requirements. Furthermore, comparing the sintering temperatures of Examples 1-4, it can be seen that the sintering temperature of the material can be controlled within the range of 1180℃-1290℃ as the content of the regulating phase and the amount of manganese and zinc sources added change. This indicates that the material system of the present invention has a wide sintering process window, which is beneficial for process control and cost optimization in industrial production.
[0055] (2) The mass fraction of the main crystal phase in Comparative Example 1 was 89.48 wt% (lower than the lower limit of 91.33 wt%). The dielectric constant of the material dropped sharply to 123 and the temperature coefficient deteriorated severely, indicating that the high dielectric constant and temperature stability could not be maintained when the content of the main phase of the Wuqing bronze type was too low.
[0056] (3) The ratio of the main crystalline phase and the regulating phase in Comparative Example 2 was exactly the same as that in Example 1 (95.78 wt% main crystalline phase and 4.22 wt% regulating phase), the only difference being that no manganese or zinc source was added in Comparative Example 2. The test results showed that the dielectric constant of Comparative Example 2 was 142, which was still at a high level, but its capacitance temperature coefficient was -45 ppm / ℃, which no longer met the COG specification requirements. In contrast, Example 1, by adding 0.72 parts by mass of manganese source and 1.22 parts by mass of zinc source, maintained a high dielectric constant while achieving a temperature coefficient of -25 ppm / ℃. It can be seen that manganese and zinc in the system of this invention are not merely traditional cooling sintering aids, but directly participate in the pinning effect of the microstructure. Mn and Zn ions enter the interstitial space of the lattice or replace certain lattice sites during sintering, forming an effective pinning effect on the displacement of ions in the lattice that are prone to temperature drift, fundamentally suppressing the temperature coefficient drift and controlling it within ±30 ppm / ℃.
[0057] Further analysis from a materials design perspective reveals that this invention employs a composite antagonistic mechanism to achieve a balance between dielectric constant and temperature coefficient. Existing technologies typically rely on a single-phase structure to increase the dielectric constant, but single-phase structures at high dielectric constants often suffer from severe temperature coefficient collapse. This invention constructs a composite system of tungsten bronze-type and perovskite structures: with a tungsten bronze-type main phase (BaNd2Bi)... 0.6 Sm 0.8 Ti6O 18 ) undertakes the function of supporting the high dielectric constant, and uses the perovskite structure to regulate the phase (Bi(Mg)). 2 / 3 Nb 1 / 3 O3 provides structural buffering and temperature stability regulation. More importantly, during sintering, Mn and Zn dopants promote atomic-level local interdiffusion and doping at the interface between the two structural phases, forming a local structure between complete order and complete disorder. This local structure effectively relaxes the lattice stress of the high dielectric constant phase under temperature changes, achieving precise antagonism and balance of the temperature coefficient. Thus, while obtaining a high dielectric constant of over 140, the capacitance temperature coefficient is stably controlled within ±30 ppm / ℃ as required by the COG specification.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
[0059] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0060] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0061] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0062] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, for example, sequentially. For instance, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For instance, the method may also include step (c), indicating that step (c) can be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0063] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0064] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
Claims
1. A high dielectric constant C0G dielectric ceramic material, characterized in that, The dielectric ceramic material comprises a main crystalline phase, a regulating phase, and a dopant; the chemical formula of the main crystalline phase is BaNd2Bi. 0.6 Sm 0.8 Ti6O 18 The chemical formula of the regulating phase is Bi(Mg) 2 / 3 Nb 1 / 3 O3; Based on a total mass of 1 part for the main crystalline phase and the regulating phase, the mass fraction of the main crystalline phase is 91.33wt%-98.08wt%, and the mass fraction of the regulating phase is 1.92wt%-8.67wt%. Based on a total mass of 100 parts for the main crystalline phase and the regulating phase, the dopant comprises 0.23-2.30 parts by mass of manganese source and 0.16-1.63 parts by mass of zinc source.
2. The high dielectric constant COG dielectric ceramic material as described in claim 1, characterized in that, The dielectric constant of the dielectric ceramic material is not less than 140.
3. The high dielectric constant COG dielectric ceramic material as described in claim 1, characterized in that, The capacitance temperature coefficient of the dielectric ceramic material fluctuates from -28 ppm / ℃ to +19 ppm / ℃.
4. A method for preparing a high dielectric constant COG dielectric ceramic material as described in any one of claims 1-3, comprising the following steps: S1. Weigh and prepare the raw materials Ba source, Nd source, Bi source, Ti source, Sm source, Mg source and Nb source according to the chemical formulas of the main crystalline phase and the regulating phase respectively; S2. Place the two powders prepared in step S1 into two ball mill jars, add zirconia balls and solvent, and ball mill; place the ball-milled raw materials in a drying oven to dry, and sieve the dried materials to obtain the first mixture and the second mixture; S3. Pre-calcine the first mixture at 1000℃-1150℃ for 2h-4h to synthesize the main crystalline phase powder; pre-calcine the second mixture at 900℃-1000℃ for 2h-4h to synthesize the regulating phase powder; S4. Weigh the main crystalline phase powder and conditioning phase powder obtained in step S3 according to the ratio, add the manganese source and the zinc source, put them into a ball mill jar, add zirconia balls and solvent, and ball mill; dry the ball-milled slurry, and sieve the dried material to obtain a mixture; S5. The mixture is mixed with the binder, granulated, and then pressed and debonded to obtain a ceramic green body; S6. The ceramic green body is sintered to obtain a high dielectric constant COG dielectric ceramic material.
5. The preparation method according to claim 4, characterized in that, In step S1, the Ba source is BaCO3 powder, the Nd source is Nd2O3 powder, the Bi source is Bi2O3 powder, the Ti source is TiO2 powder, the Sm source is Sm2O3 powder, the Mg source is MgCO3 powder, and the Nb source is Nb2O5 powder.
6. The preparation method according to claim 4, characterized in that, In step S4, the Mn source is MnCO3 powder and the Zn source is ZnO powder.
7. The preparation method according to claim 4, characterized in that, In steps S2 and S4, the mass ratio of powder, zirconia balls, and solvent is 1:2:0.
8.
8. The preparation method according to claim 4, characterized in that, In step S2, the ball milling parameters are: rotation speed 300 r / min-400 r / min, ball milling time 3h-5h; In step S4, the ball milling parameters are: rotation speed 400r / min-500r / min, ball milling time 3h-6h.
9. The preparation method according to claim 5, characterized in that, In step S5, the adhesive is PVB, and the mass concentration of the adhesive is 5%-10%.
10. The preparation method according to claim 5, characterized in that, In step S6, the sintering temperature is 1150℃-1300℃ and the time is 2h-4h.