Aluminum nitride powder composition, composition preparation method, aluminum nitride ceramics and ceramic preparation method
Aluminum nitride powder was treated with hydrophobic modification and composite sintering aids to generate aluminum nitride nanowires. Combined with an optimized sintering process, the strength and thermal conductivity problems of aluminum nitride ceramics under vibration, impact and alternating hot and cold conditions were solved, and high-performance aluminum nitride ceramic materials were realized.
Patent Information
- Application Number
- CN202611045408.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing aluminum nitride ceramics have limited improvement in flexural strength and fracture toughness, making them unsuitable for harsh service conditions such as long-term vibration, mechanical impact, and alternating hot and cold temperatures. Furthermore, they are prone to reacting with water vapor, leading to a decrease in thermal conductivity.
Aluminum nitride powder was hydrophobically modified, and aluminum nitride nanowires were generated by adding methyliminoaluminane solution. Combined with composite sintering aids, including metal fluorides and rare earth oxides, aluminum nitride ceramics were prepared. The sintering process was optimized by removing organic components and high-temperature heat treatment.
The flexural strength and fracture toughness of aluminum nitride ceramics are improved, ensuring their structural stability and high thermal conductivity under complex working conditions, avoiding hydrolysis reactions, and making them suitable for heat dissipation substrates in fields such as new energy vehicles.
Smart Images

Figure CN123062274A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic materials technology, and in particular to an aluminum nitride powder composition, a method for preparing the composition, aluminum nitride ceramics, and a method for preparing ceramics. Background Technology
[0002] Aluminum nitride (AlN) ceramics have become ideal heat dissipation substrates and packaging materials for high-power power electronic devices, new energy vehicle motor drives, and on-board chargers due to their excellent properties such as high theoretical thermal conductivity (≥320 W / (m·K)), good insulation performance, and thermal expansion coefficient matching with silicon. Currently, commercially available aluminum nitride ceramics have room temperature thermal conductivity of 180~220 W / (m·K), which can meet the heat dissipation requirements of high power density.
[0003] However, the flexural strength of aluminum nitride ceramics is generally below 400 MPa, and its fracture toughness is poor. Under the long-term vibration, mechanical shock, and thermal cycling conditions experienced by new energy vehicles, aluminum nitride ceramic substrates are prone to cracking and edge chipping, leading to insulation failure or interruption of heat dissipation paths. Secondly, aluminum nitride powder is highly susceptible to hydrolysis with moisture in the environment: AlN + 2H2O → AlOOH (or Al(OH)3) + NH3↑. This reaction not only generates amorphous aluminum hydroxide, blocking the heat conduction path and causing a sharp drop in the thermal conductivity of the material, but also causes the aluminum nitride ceramic surface to peel, expand in volume, and even cause the motor or metal coating to detach.
[0004] Existing technologies can improve the hydrolysis susceptibility of aluminum nitride powder by hydrophobic modification, thereby reducing the impurity phase content in aluminum nitride ceramics and improving their thermal conductivity. However, when using hydrophobically modified aluminum nitride powder as a raw material to prepare aluminum nitride ceramics, the improvement in flexural strength and fracture toughness is limited, making it unsuitable for harsh service conditions such as long-term vibration, mechanical impact, and alternating hot and cold temperatures. Summary of the Invention
[0005] In view of the shortcomings of the prior art, the present invention provides an aluminum nitride powder composition, a method for preparing the composition, an aluminum nitride ceramic, and a method for preparing the ceramic, aiming to solve the problem that when aluminum nitride ceramics are prepared by using hydrophobically modified aluminum nitride powder as raw material, the improvement in the bending strength and fracture toughness of aluminum nitride ceramics is limited, and they cannot be adapted to harsh service conditions such as long-term vibration, mechanical impact, and alternating hot and cold temperatures.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: The first aspect of this invention provides a method for preparing an aluminum nitride powder composition, comprising the following steps: S10. Disperse aluminum nitride powder in a first organic solvent to obtain aluminum nitride slurry; S20. Add organic acid to aluminum nitride slurry and mix thoroughly; S30. Add an organic encapsulation agent to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain hydrophobically modified aluminum nitride powder. S40. Disperse the hydrophobically modified aluminum nitride powder in a second organic solvent, then add a methyliminoaluminane solution to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain a filter cake. Dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
[0007] In the preparation method of the aluminum nitride powder composition, the organic acid is at least one of stearic acid, ricinoleic acid, and tartaric acid; the organic encapsulation agent is at least one of dibutyl phthalate and dimethyl phthalate.
[0008] A second aspect of the present invention provides an aluminum nitride powder composition, which is prepared by the method described above for preparing the aluminum nitride powder composition.
[0009] A third aspect of this invention provides an aluminum nitride ceramic, wherein the raw materials for preparing the aluminum nitride ceramic include the aluminum nitride powder composition described above, and the aluminum nitride ceramic has a thermal conductivity ≥210 W / (m·K), a flexural strength ≥400 MPa, and a fracture toughness ≥3.2 MPa·m. 1 / 2 .
[0010] The aluminum nitride ceramics described herein include composite sintering aids as raw materials for their preparation; the composite sintering aids include metal fluorides and rare earth oxides; the mass ratio of the rare earth oxides to the metal fluorides is (2-4):1.
[0011] In the aluminum nitride ceramic, the rare earth oxide is at least one of Y2O3, Yb2O3, Er2O3, and La2O3; and the metal fluoride is at least one of CaF2, MgF2, LiF, and YF3.
[0012] In the aluminum nitride ceramic, the mass ratio of the aluminum nitride powder composition to the composite sintering aid is (94-96):(4-6).
[0013] A fourth aspect of this invention provides a method for preparing aluminum nitride ceramics, comprising the following steps: T01. The raw materials used to prepare aluminum nitride ceramics are ball-milled and mixed to obtain composite powder; T02. The composite powder is subjected to molding treatment to obtain aluminum nitride ceramic green body; T03. The aluminum nitride ceramic green body is subjected to organic component removal treatment; T04. The aluminum nitride ceramic green body after organic component removal treatment is sintered and subjected to high-temperature heat treatment in sequence to obtain the aluminum nitride ceramic.
[0014] In the preparation method of the aluminum nitride ceramic, the sintering treatment in step T04 is carried out under a protective atmosphere, and the sintering treatment includes a low-temperature carbon removal stage, a heating stage, and a sintering densification stage; the low-temperature carbon removal stage slowly heats up to 600°C at a heating rate of 1°C / min, and then holds for 2-4 hours; the heating stage heats up from 600°C to 1200°C at a heating rate of 2°C / min, and then holds for 1 hour; the sintering densification stage heats up from 1200°C to 1800-1850°C at a heating rate of 2°C / min, and then holds for 3-4 hours.
[0015] Beneficial effects: The first aspect of this invention provides a method for preparing an aluminum nitride powder composition. By adding a methyliminoaluminane solution to an aluminum nitride mixture, the methyliminoaluminane is dispersed in the hydrophobically modified aluminum nitride powder. During the sintering process of preparing aluminum nitride ceramics, aluminum nitride nanowires are generated by the in-situ decomposition of methyliminoaluminane, thereby toughening the aluminum nitride ceramics. This reduces the brittleness of the aluminum nitride ceramics and improves their fracture toughness and bending strength, making them suitable for harsh service conditions such as long-term vibration, mechanical impact, and alternating hot and cold temperatures.
[0016] A second aspect of the present invention provides an aluminum nitride powder composition, which is prepared by a method thereof. The aluminum nitride powder composition contains dispersed methyliminoaluminane, and the aluminum nitride nanowires generated by its decomposition can achieve toughening and strengthening of aluminum nitride ceramics, thereby improving the fracture toughness and bending strength of aluminum nitride ceramics.
[0017] The third aspect of this invention provides an aluminum nitride ceramic with a room temperature thermal conductivity of over 210 W / (m·K), exhibiting excellent thermal conductivity and the ability to quickly dissipate heat generated by high-power devices, thus fully meeting the efficient heat dissipation requirements of high-power-density equipment. Simultaneously, this aluminum nitride ceramic possesses a flexural strength of not less than 400 MPa and a fracture toughness ≥3.2 MPa·m. 1 / 2 With outstanding mechanical properties, it is not prone to damage such as cracks and edge chipping under complex service environments such as long-term vibration loads, instantaneous mechanical shocks, and alternating hot and cold cycles over a wide temperature range. It can effectively prevent insulation failure and heat conduction path breakage caused by structural damage to the heat dissipation substrate, and the overall reliability is greatly improved. It is the preferred material for heat dissipation substrates for special applications such as drive motors, vehicle electronic control systems, and power battery packs in new energy vehicles.
[0018] The fourth aspect of this invention provides a method for preparing aluminum nitride ceramics. By removing organic components from the green body of aluminum nitride ceramics, molding defects such as bubbling, delamination, and cracking caused by the decomposition of organic matter during sintering can be avoided. This reduces structural defects such as internal pores and microcracks, as well as stress concentration, providing a fundamental guarantee for achieving high density, high thermal conductivity, and excellent mechanical properties in aluminum nitride ceramics. In addition, high-temperature heat treatment of aluminum nitride ceramics after sintering densification promotes the filling of residual amorphous phases at the ceramic grain boundaries, significantly reducing the phonon scattering effect caused by the amorphous phases at the grain boundaries, improving the thermal conductivity of the material under wide temperature range conditions, and effectively preventing the thermal conductivity from drifting and decaying with the operating environment. Attached Figure Description
[0019] Figure 1 This is a flowchart illustrating the preparation process of the aluminum nitride powder composition provided by the present invention.
[0020] Figure 2 This is a flowchart illustrating the preparation process of aluminum nitride ceramics provided by the present invention.
[0021] Figure 3 This is the XRD pattern of hydrophobically modified aluminum nitride powder. Detailed Implementation
[0022] This invention provides an aluminum nitride powder composition, a method for preparing the composition, an aluminum nitride ceramic, and a method for preparing the ceramic. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention.
[0023] like Figure 1 As shown, the first aspect of the present invention provides a method for preparing an aluminum nitride powder composition, comprising the following steps: S10. Disperse aluminum nitride powder in a first organic solvent to obtain aluminum nitride slurry; S20. Add organic acid to aluminum nitride slurry and mix thoroughly; S30. Add an organic encapsulation agent to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain hydrophobically modified aluminum nitride powder. S40. Disperse the hydrophobically modified aluminum nitride powder in a second organic solvent, then add a methyliminoaluminane solution to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain a filter cake. Then, dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
[0024] In the preparation method of the aluminum nitride powder composition provided by the present invention, firstly, by dispersing the aluminum nitride powder in a first organic solvent, premature hydrolysis of the aluminum nitride powder caused by the aqueous phase can be avoided, generating impurity phases such as aluminum hydroxide. This improves the purity of the aluminum nitride powder, ensuring that the thermal conductivity of the aluminum nitride ceramic does not decrease due to the presence of impurity phases. Next, after the aluminum nitride powder is dispersed in the first organic solvent, organic acid and organic encapsulation agent are sequentially added to the aluminum nitride slurry. This forms a dense, continuous hydrophobic layer on the surface of the aluminum nitride powder, preventing water vapor from reacting with the aluminum nitride surface and enhancing the hydrolysis resistance of the aluminum nitride powder. Furthermore, after achieving hydrophobic modification of aluminum nitride powder, by adding a methyliminoaluminane solution to the mixture formed by the second organic solvent and aluminum nitride powder, methyliminoaluminane can be dispersed in the hydrophobically modified aluminum nitride powder. When preparing aluminum nitride ceramics using hydrophobically modified aluminum nitride powder as raw material, methyliminoaluminane decomposes in situ to generate aluminum nitride nanowires. These aluminum nitride nanowires can interpenetrate between aluminum nitride grains to exert a fiber toughening effect, reduce the brittleness of aluminum nitride ceramics, and improve the fracture toughness and bending strength of aluminum nitride ceramics. Aluminum nitride ceramics can adapt to harsh service conditions such as long-term vibration, mechanical impact, and alternating hot and cold temperatures.
[0025] To ensure good dispersibility and prevent agglomeration of aluminum nitride powder in the first organic solvent, in a preferred embodiment, the first organic solvent used in step S10 can be anhydrous ethanol. After the aluminum nitride powder is dispersed in anhydrous ethanol, adding an organic acid to the aluminum nitride slurry allows the carboxyl groups of the organic acid molecules to chemically bond or coordinate with the active groups on the surface of the aluminum nitride powder, forming a stable chemical adsorption layer. This not only replaces and desorbs trace amounts of residual moisture on the surface of the aluminum nitride powder but also constructs a dense molecular-level hydrophobic interface, providing a solid substrate for the adhesion of organic encapsulation agents and ensuring that a dense and continuous hydrophobic layer can be formed on the surface of the aluminum nitride powder.
[0026] After a chemical adsorption layer is formed on the surface of aluminum nitride powder, an organic encapsulation agent is added to the mixed system. This allows the organic encapsulation agent to be adsorbed onto the surface of the organic acid-modified aluminum nitride powder, which can further fill the surface defects of the aluminum nitride powder and thicken the protective interface. This results in the formation of a dense and continuous hydrophobic layer, which enhances the barrier effect of the core layer structure on the surface of the aluminum nitride powder against water vapor and improves the hydrolysis resistance of the aluminum nitride powder.
[0027] To form a stable chemisorption layer on the surface of aluminum nitride powder and simultaneously impart hydrophobicity to the chemisorption layer, in a preferred embodiment, the organic acid used in step S20 can be stearic acid, ricinoleic acid, tartaric acid, etc. Stearic acid is a long-chain saturated monocarboxylic acid, and its carboxyl group can form stable chemical bonds with active groups such as Al-OH and Al-NH2 on the surface of aluminum nitride powder. Simultaneously, the long carbon chain of stearic acid extends outward to construct a hydrophobic interface, enabling the chemisorption layer to be stably adsorbed on the surface of aluminum nitride powder while also possessing hydrophobicity.
[0028] Furthermore, the long carbon chains of stearic acid can form a steric barrier between aluminum nitride powder particles. When aluminum nitride grains approach each other, the steric barrier formed by the chemisorption layer can reduce the surface energy of the aluminum nitride powder, hindering the aggregation of aluminum nitride grains. Therefore, it can reduce the degree of agglomeration of aluminum nitride powder and improve its dispersibility. Even after the hydrophobic layer is wrapped around the outside of the aluminum nitride grains, the aluminum nitride powder can still have good dispersibility, thus effectively preventing the aluminum nitride powder from agglomerating again during processing and ensuring the densest packing of aluminum nitride powder during molding. This uniform and dense packing structure can reduce the porosity of aluminum nitride ceramic products, increase the density of aluminum nitride ceramics, and at the same time eliminate agglomerates, pores, and other crack sources, avoiding stress concentration inside the aluminum nitride ceramics. This improves the mechanical properties of aluminum nitride ceramics, such as flexural strength and fracture toughness.
[0029] Furthermore, the excellent dispersibility of aluminum nitride powder enables it to form a continuous and dense thermally conductive network, reducing pores and interfacial thermal resistance, and lowering phonon scattering. Therefore, it can significantly improve the thermal conductivity of aluminum nitride ceramics, achieving synergistic optimization of high thermal conductivity, high density, and high mechanical properties of aluminum nitride ceramics.
[0030] While the hydrophobic layer enhances the barrier effect of the aluminum nitride powder's core structure against water vapor, improper selection of the organic encapsulation agent can still affect its water vapor barrier effect, allowing water vapor to still penetrate to the aluminum nitride powder surface and trigger hydrolysis. Therefore, to further improve the density and stability of the hydrophobic layer and strengthen its water vapor barrier effect, in a preferred embodiment, the organic encapsulation agent selected in step S20 is at least one of dibutyl phthalate and dimethyl phthalate.
[0031] Dibutyl phthalate (DBP) and dimethyl phthalate (DMP) contain long alkyl chains with ester groups in their molecular structure. Within these long alkyl chains, the ester groups can form intermolecular hydrogen bonds with unreacted free carboxyl and hydroxyl groups on the chemisorption layer. The long alkyl chains are hydrophobic and face outwards from the aluminum nitride powder. This gives DBP and DPP excellent film-forming properties and interfacial adhesion, enabling them to form a continuous, uniform, and pore-free dense hydrophobic film on the chemisorption layer, thus achieving a long-lasting and stable water vapor barrier effect. Furthermore, both DBP and DPP possess lubricating properties. When DBP and DPP participate in the reaction to form a hydrophobic layer, they impart a lubricating component to the surface of the modified aluminum nitride powder, significantly reducing interfacial frictional resistance between aluminum nitride powder particles, weakening the powder agglomeration tendency, and significantly improving the powder's processing flowability and feeding uniformity.
[0032] When aluminum nitride powder composition is used as raw material for injection molding aluminum nitride ceramic green body, the good powder flowability can achieve the densest packing of aluminum nitride powder inside the mold, reduce the interconnected pores and closed pores in the aluminum nitride ceramic green body, and reduce the porosity defects of the green body from the molding source. In this way, after the aluminum nitride ceramic green body is sintered, the density of aluminum nitride ceramic can be further improved, the phonon scattering caused by grain boundary pores can be reduced, and the aluminum nitride ceramic can be effectively guaranteed to have both stable high thermal conductivity and excellent mechanical properties.
[0033] When the hydrophobic layer has good density, it can enhance the water vapor barrier effect. To further enhance the density of the hydrophobic layer, when adding organic encapsulation agents to the mixture system, nano-SiO2 with a particle size range of 10-50 nm can also be added. Due to the small particle size and large specific surface area of nano-SiO2, when added to the mixture system, it can fill the gap between the chemisorption layer and the hydrophobic layer, and can further densify the hydrophobic layer, enhancing the water vapor barrier capability.
[0034] A second aspect of the present invention provides an aluminum nitride powder composition, which is prepared by a method for preparing the aluminum nitride powder composition. The aluminum nitride powder composition contains dispersed methyliminoaluminane, and the aluminum nitride nanowires generated by its decomposition can achieve toughening and strengthening of aluminum nitride ceramics, thereby improving the fracture toughness and bending strength of aluminum nitride ceramics.
[0035] A third aspect of the present invention provides an aluminum nitride ceramic, wherein the raw materials for preparing the aluminum nitride ceramic include the aluminum nitride powder composition described above, and the aluminum nitride ceramic has a thermal conductivity ≥210W / (m·K) and a flexural strength ≥400MPa.
[0036] This invention provides aluminum nitride ceramics that simultaneously possess high thermal conductivity and engineering-suitable mechanical strength. Specifically, the aluminum nitride ceramics have a thermal conductivity ≥210 W / (m·K), exhibiting excellent thermal conductivity and the ability to rapidly dissipate heat generated by high-power devices, fully meeting the efficient heat dissipation requirements of high-power-density equipment. Simultaneously, the aluminum nitride ceramics have a flexural strength ≥400 MPa and a fracture toughness ≥3.2 MPa·m. 1 / 2 The aluminum nitride ceramic exhibits outstanding mechanical properties. Under complex service environments involving long-term vibration loads, instantaneous mechanical shocks, and alternating hot and cold cycles over a wide temperature range, it is less prone to damage such as cracks and edge chipping. This effectively prevents insulation failures and thermal conductivity disruptions caused by structural damage to the ceramic material, significantly improving overall reliability. Furthermore, the aluminum nitride ceramic provided by this invention uses aluminum nitride powder with a hydrophobic protective system as a raw material, which can inhibit hydrolysis reactions from the source. This avoids the problem of a sharp decrease in thermal conductivity caused by the presence of grain boundary impurities and amorphous phases in the aluminum nitride ceramic, making the aluminum nitride ceramic provided by this invention an ideal heat dissipation material for new energy vehicle motors, electronic controls, battery packs, and other fields.
[0037] In aluminum nitride ceramics, the presence of impurity phases or amorphous phases at the aluminum nitride grain boundaries disrupts the continuity of the grain boundaries, becoming phonon scattering centers and significantly hindering phonon propagation. This results in increased thermal resistance and a significant decrease in the thermal conductivity of the aluminum nitride ceramic. The presence of these impurity phases and amorphous phases (second phases) at the grain boundaries is related not only to the degree of hydrolysis in the aluminum nitride ceramic but also to the use of sintering aids. Therefore, to further purify the grain boundaries and improve the thermal conductivity of the aluminum nitride ceramic, in a preferred embodiment, the raw materials for preparing the aluminum nitride ceramic also include a composite sintering aid; the composite sintering aid includes metal fluorides and rare earth oxides.
[0038] Specifically, among the composite sintering aids mentioned above, rare earth oxides possess excellent thermal stability and chemical inertness, effectively reducing the sintering temperature of aluminum nitride ceramics while minimizing the accumulation of grain boundary impurities. This not only improves the densification of aluminum nitride ceramics but also reduces phonon scattering and enhances their thermal conductivity. Metal fluorides, on the other hand, react with aluminum nitride and alumina to produce AlF3 and AlF4, which exhibit volatility and high-temperature sublimation properties. This further purifies the grain boundaries, reducing the damage to the thermal conductivity of the second phase in aluminum nitride ceramics, enabling them to meet the heat dissipation requirements of high power density.
[0039] For example, the rare earth oxide can be at least one of Y₂O₃, Yb₂O₃, Er₂O₃, and La₂O₃; the metal fluoride can be at least one of CaF₂, MgF₂, LiF, and YF₃. To ensure the purification effect of the composite sintering aid on the aluminum nitride grain boundaries while preserving the high thermal conductivity intrinsic structure of the aluminum nitride ceramic to the greatest extent, in a preferred embodiment, the composite sintering aid can be a Y₂O₃-CaF₂ composite sintering aid composed of Y₂O₃ and CaF₂. Specifically, during the high-temperature sintering process of aluminum nitride ceramics, CaF₂ can react with the alumina present on the surface of the aluminum nitride powder before Y₂O₃ to generate volatile substances such as AlF₃ and AlF₄, thereby achieving self-purification of the grain boundaries and purifying the direct contact surfaces between aluminum nitride grains. Subsequently, Y2O3 reacts with the alumina remaining on the surface of aluminum nitride powder to generate a yttrium aluminate liquid phase. The yttrium aluminate liquid phase can promote the reordering and migration of powder particles, causing the second phase dispersed inside the aluminum nitride grains and at the grain interfaces to migrate directionally and accumulate at the triangular grain boundaries. This achieves simultaneous purification of the grain lattice and the grain boundary interface, thereby not only reducing phonon scattering and preserving the high thermal conductivity intrinsic structure of aluminum nitride grains to the greatest extent, but also allowing the second phase, which is distributed in an island-like manner at the corners of the triangular grain boundaries, to fill the gaps between aluminum nitride powder particles, promoting the densification of aluminum nitride ceramics and enabling the density of aluminum nitride ceramics to stably reach 98.5% or higher.
[0040] Meanwhile, during the high-temperature sintering process of aluminum nitride ceramics, the Y2O3-CaF2 composite sintering aid effectively inhibits abnormal grain growth and regulates grain growth morphology, resulting in uniform aluminum nitride grain size and significantly improved grain boundary bonding strength. This achieves excellent dual effects of fine grain strengthening and grain boundary strengthening, greatly optimizing the mechanical properties and structural stability of aluminum nitride ceramics. Therefore, aluminum nitride ceramics prepared using the Y2O3-CaF2 composite sintering aid not only achieve thermal conductivity fluctuations of ≤5% within a wide automotive temperature range of -40℃ to 150℃, meeting the rapid heat dissipation requirements of high-power devices, but also possess the following excellent mechanical properties: flexural strength ≥350MPa, fracture toughness ≥3.2 MPa·m. 1 / 2 With a compressive strength of ≥1800MPa, it can stably withstand the harsh conditions such as complex vibrations, impacts and sudden temperature changes during the operation of new energy vehicles, greatly improving the long-term reliability and environmental adaptability of aluminum nitride heat dissipation substrates.
[0041] It should be noted that although the present invention prevents the aluminum nitride powder from hydrolyzing to form oxygen-containing aluminum compounds (such as aluminum hydroxide and aluminum oxide) by modifying the aluminum nitride powder, the presence of an oxide layer on the surface of the aluminum nitride powder is a normal phenomenon before the modification of the aluminum nitride powder during the preparation process.
[0042] In composite sintering aids composed of rare earth oxides and metal fluorides, if the proportion of rare earth oxides is too high, the excess rare earth oxides in the sintering system will continuously react with the residual alumina on the surface of aluminum nitride powder, generating a large amount of continuously distributed rare earth aluminate liquid phase. After cooling, this liquid phase will form a network glassy phase film at the grain boundaries, encapsulating the aluminum nitride grains, severely blocking direct contact between grains, significantly enhancing phonon scattering, and causing a significant decrease in the thermal conductivity of aluminum nitride ceramics. At the same time, excess rare earth oxides will increase the viscosity of the sintering system, hindering the reorganization and densification process of the powder, and easily causing problems such as abnormal grain coarsening and weakened grain boundary bonding strength, thereby causing a decrease in the mechanical properties of aluminum nitride ceramics such as bending strength and fracture toughness.
[0043] Excessive metal fluoride content makes it difficult for the sintering system to form a sufficient amount of rare earth aluminate liquid phase, limiting the role of sintering aids in promoting densification. Furthermore, excessive metal fluoride volatilizes excessively at high temperatures, easily causing weight loss and decreased density in the green body. At the same time, excessive metal fluoride can also erode ceramic grain boundaries, weaken the bonding strength between grains, and induce micropores and microcracks, ultimately reducing the mechanical properties of aluminum nitride ceramics.
[0044] To balance the grain boundary purification effect of metal fluorides, the liquid-phase sintering effect of rare earth oxides, and the ability of composite additives to regulate the microstructure of aluminum nitride ceramics, while also taking into account the high thermal conductivity, high density, and excellent mechanical properties of aluminum nitride ceramics, in a preferred embodiment, the mass ratio of the rare earth oxides to the metal fluorides is (2-4):1. This ratio range ensures that the rare earth oxides provide sufficient rare earth aluminate liquid phase, effectively promoting powder reorganization, densification, and grain boundary purification, and inhibiting abnormal grain growth; it also allows the metal fluorides to fully exert their grain boundary self-purification effect, avoiding excessive volatilization and grain boundary erosion, reducing phonon scattering, and ultimately achieving a synergistic improvement in the thermal conductivity, density, and mechanical properties of aluminum nitride ceramics.
[0045] In the preparation of aluminum nitride ceramics, the mass ratio of aluminum nitride powder composition to composite sintering aid directly affects the density, grain boundary phase content, thermal conductivity, and mechanical properties of aluminum nitride ceramics. If the proportion of composite sintering aid is too low, insufficient liquid phase generation in the sintering system makes it difficult to fully promote powder relocation and densification, resulting in the easy retention of interconnected or closed pores inside the aluminum nitride ceramic. At the same time, the grain boundary purification reaction is insufficient, leading to low thermal conductivity and insufficient mechanical strength of the aluminum nitride ceramic. If the proportion of aid is too high, a continuous amorphous glass phase is easily formed in the sintering system, which intensifies phonon scattering and induces abnormal grain growth, weakening the grain boundary bonding strength, resulting in a decrease in thermal conductivity and deterioration of mechanical properties of the aluminum nitride ceramic. In order to ensure that aluminum nitride ceramics simultaneously possess high thermal conductivity and high mechanical properties, in a preferred embodiment, the mass ratio of the aluminum nitride powder composition to the composite sintering aid is (94-96):(4-6). This ratio can control the total amount of composite sintering aid added to a lightweight level, ensuring the densification of aluminum nitride ceramics while minimizing grain boundary phases and avoiding phonon scattering caused by amorphous glass phases. This enables aluminum nitride ceramics to simultaneously possess both high thermal conductivity and high mechanical properties.
[0046] like Figure 2 As shown, in order to prepare the aluminum nitride ceramics described above, a fourth aspect of the present invention provides a method for preparing aluminum nitride ceramics, comprising the following steps: T01. The raw materials used to prepare aluminum nitride ceramics are ball-milled and mixed to obtain composite powder; T02. The composite powder is subjected to molding treatment to obtain aluminum nitride ceramic green body; T03. The aluminum nitride ceramic green body is subjected to organic component removal treatment; T04. The aluminum nitride ceramic green body after organic component removal treatment is sintered and subjected to high-temperature heat treatment in sequence to obtain the aluminum nitride ceramic.
[0047] In the aforementioned method for preparing aluminum nitride ceramics, the organic components in the aluminum nitride ceramic green body are removed through an organic component removal treatment. This removes organic matter from the green body, preventing bubbling, delamination, and cracking during sintering. It also avoids internal defects and stress concentration in the sintered aluminum nitride ceramic, thus ensuring its thermal conductivity and mechanical properties. After sintering, high-temperature heat treatment promotes the complete crystallization of residual amorphous phases, further reducing phonon scattering and stabilizing the thermal conductivity. This results in stable heat dissipation efficiency with minimal fluctuations over a wide temperature range, preventing localized overheating, thermal stress concentration, and performance degradation caused by thermal conductivity drift. This ensures long-term reliable operation of high-power devices and extends their lifespan.
[0048] Specifically, during the high-temperature heat treatment of aluminum nitride ceramics, the ceramics are placed in a low-pressure sintering furnace and subjected to high-temperature heat treatment under a high-purity nitrogen atmosphere (nitrogen flow rate 2-3 L / min). The high-temperature heat treatment regime is as follows: the temperature is increased to 1420-1450℃ at a heating rate of 2℃ / min, held for 4-5 hours, and then slowly cooled to room temperature at a cooling rate of 1℃ / min.
[0049] To avoid the introduction of an aqueous phase during the ball milling process, which could lead to the hydrolysis of the aluminum nitride powder, in step T01, before ball milling and mixing the raw materials, the aluminum nitride powder composition, Y2O3, CaF2, and other raw materials can be placed in a vacuum environment at 150°C (vacuum degree ≤ 10). -3 Drying at 6–8 h under high energy (Pa) removes adsorbed water and oxygen from the surface of the raw material powder, preventing moisture from causing hydrolysis of the aluminum nitride powder and the introduction of oxygen-containing components into the grain boundaries, thereby reducing grain boundary defects inside the aluminum nitride ceramic. Simultaneously, using anhydrous ethanol as the dispersion medium for high-energy ball milling of the raw material for 6–7 h further prevents the introduction of the aqueous phase.
[0050] After ball milling, the composite slurry obtained by ball milling is placed in a rotary evaporator for low-temperature de-alcoholization treatment (≤60℃) to remove anhydrous ethanol from the mixture, and then a paste-like composite powder is obtained. Then, it is passed through a 200-mesh sieve to obtain a non-agglomerated composite powder.
[0051] To obtain aluminum nitride ceramic green bodies, step T02 can be performed using molding methods such as injection molding or dry pressing. Injection molding can produce large-sized, complex-structured aluminum nitride ceramic green bodies (e.g., irregular shapes, deep cavities, positioning holes, positioning grooves, etc.), meeting the manufacturing requirements of large-sized heat dissipation substrates and significantly reducing the precision machining costs of heat dissipation substrates. For manufacturing small- to medium-sized heat dissipation substrates, injection molding can be replaced by dry pressing.
[0052] When obtaining aluminum nitride ceramic green bodies via injection molding, the composite powder and binder must first be mixed to form a uniform and stable ceramic feedstock suitable for injection molding. This feedstock then undergoes extrusion, air cooling, and pelletizing processes to obtain cylindrical injection molding granules. After obtaining the granules, they are placed in an injection molding machine to form aluminum nitride ceramic green bodies. To ensure that the molded aluminum nitride ceramic green bodies are free of cracks, delamination, and internal stress, the following injection molding process parameters can be used: material temperature 170–190℃, mold temperature 50–70℃, injection pressure 70–90 MPa, holding pressure 50–60 MPa, and holding time 5–10 seconds.
[0053] Specifically, the mixing process can adopt the following parameters: mixing temperature 150-160℃, mixing time 4-6h, and rotation speed 50-60 r / min.
[0054] For example, the adhesive can be a PEG-PMMA-paraffin ternary system adhesive, in which the mass ratio of PEG, PMMA and paraffin can be 10-15:10-15:70-80.
[0055] To ensure that the aluminum nitride ceramic green body is free from deformation, pores, and cracks after the removal of organic components, in step T03, trichloroethylene is first used to dissolve and remove the low-melting-point components in the binder, forming interconnected pore channels in the green body. This reduces the gas release pressure during subsequent organic component removal (i.e., dewaxing and degreasing), preventing the green body from bubbling, delamination, or cracking. Then, the temperature is raised to 450–500°C at a slow heating rate of 0.5–1°C / min and held for 2–3 hours for thermal dewaxing and degreasing. The remaining binder and the chemically adsorbed and hydrophobic layers coating the surface of the aluminum nitride powder are pyrolyzed and volatilized, and organic matter is gently removed to reduce stress in the green body, avoid deformation and microcracks, and finally obtain a structurally complete and defect-free ceramic green body.
[0056] In the sintering process of aluminum nitride ceramics, in order to eliminate the internal stress inside the aluminum nitride ceramic green body and prevent warping and delamination, in step T04, the sintering atmosphere can be high-purity nitrogen gas with a purity ≥99.999%, and the gas pressure is 0.1~0.4MPa. The sintering treatment includes a low-temperature carbon removal stage, a heating stage, and a sintering densification stage. Specifically, in the low-temperature carbon removal stage, the temperature is slowly increased to 600℃ at a heating rate of 1℃ / min, and then held for 2 hours. After the initial holding period, to prevent the incomplete removal of organic matter from the ceramic green body, the holding period can be extended for another 2 hours, and carbon dioxide gas is introduced for debinding. The low-temperature carbon removal stage can completely remove residual organic matter in the aluminum nitride ceramic green body. The slow heating rate and sufficient holding time ensure that the gas can escape smoothly, avoiding bubbling, cracking or formation of closed pores in the green body due to excessive internal pressure generated by the gas. This helps maintain the integrity of the green body structure, reduces internal defects and stress concentration in the ceramic, ensures uniform ceramic structure and stable performance after sintering, and reduces the risk of warping and deformation of large-size substrates, thereby improving product yield and reliability.
[0057] The heating stage involves raising the temperature from 600℃ to 1200℃ at a rate of 2℃ / min, followed by a holding time of 1 hour. During this stage, the gentle heating rhythm continuously releases the internal stress of the aluminum nitride ceramic blank, preventing stress concentration that could lead to cracking. Furthermore, during this heating stage, the composite sintering aid can selectively react with the oxides on the surface of the aluminum nitride powder, initially producing a low-melting-point aluminate liquid phase, providing diffusion channels and liquid-phase sintering driving force for subsequent ceramic densification. The sintering densification stage involves raising the temperature from 1200℃ to 1800–1850℃ at a rate of 2℃ / min, followed by a holding time of 3–4 hours. During this stage, the low-melting-point liquid phase formed enables powder repositioning and a dissolution-precipitation mechanism, promoting pore closure and shrinkage within the blank, thereby achieving densification of the aluminum nitride ceramic.
[0058] After the sintering densification stage, the temperature of the aluminum nitride ceramic is reduced to 1000℃ at a cooling rate of 1.5℃ / min, followed by natural cooling. This avoids the brittle transition range of the aluminum nitride ceramic material, reduces the thermal stress concentration caused by the internal and external temperature difference, and avoids the occurrence of microcracks or a decrease in mechanical strength of the aluminum nitride ceramic due to excessively rapid cooling.
[0059] The method for preparing aluminum nitride ceramics provided by this invention, through the removal of organic components from the aluminum nitride ceramic green body and combined with a segmented, slow-heating sintering process, can eliminate the internal stress of the aluminum nitride ceramic green body and prevent warping, deformation, and delamination. Furthermore, the gas pressure used during sintering ensures the complete decomposition of methyliminoaluminane to generate aluminum nitride nanowires, preventing impurities from remaining in the aluminum nitride ceramic. This stabilizes the high thermal conductivity of the aluminum nitride ceramic while also improving its flexural strength and fracture toughness. After precision machining, the aluminum nitride ceramic prepared by this method can stably produce aluminum nitride ceramic heat dissipation substrates with a surface roughness Ra ≤ 1.0 μm and a flatness ≤ 0.02 mm / m. Moreover, the aluminum nitride ceramic heat dissipation substrates are free from chipping and cracks, effectively ensuring the dimensional accuracy and surface quality of the heat dissipation substrates, which can meet the stringent requirements of high-power devices such as new energy vehicles and 5G base stations.
[0060] The following examples and comparative examples further illustrate the present invention. The aluminum nitride powder used in the following examples and comparative examples has an α-phase content ≥96wt%, a purity ≥99.95wt%, a powder particle size D50=1.0μm, and an oxygen content ≤0.8wt%.
[0061] Example 1 This embodiment provides a method for preparing an aluminum nitride powder composition, including the following steps: S10. Disperse aluminum nitride powder in anhydrous ethanol to obtain an aluminum nitride slurry with a solid content of 20 wt%. S20. Stearic acid is added to the aluminum nitride slurry, and the mixture is ultrasonically dispersed and stirred at 60°C for 3 hours. In this step, the amount of stearic acid added is 0.5% of the mass of the aluminum nitride powder in step S10. S30. Continue adding dibutyl phthalate to the mixture and stir for another 0.5 hours. After mixing evenly, filter the mixture. After filtration, dry and pulverize the filter cake to obtain hydrophobically modified aluminum nitride powder. In this step, the amount of dibutyl phthalate added is 0.8% of the mass of aluminum nitride powder in step S10. S40. Disperse the hydrophobically modified aluminum nitride powder in toluene, then add a 10wt% methyliminoaluminane solution to the mixture, mix evenly, filter the mixture to obtain a filter cake, and then dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
[0062] In step S30, the drying temperature of the filter cake is 40°C. In step S40, the methyliminoaluminane solution is prepared by dissolving methyliminoaluminane in toluene, and the amount of methyliminoaluminane solution added is 20% of the mass of aluminum nitride powder in step S10; the filter cake is dried in a vacuum oven at 60°C for 6 hours.
[0063] This embodiment also provides an aluminum nitride ceramic, wherein the raw materials for preparing the aluminum nitride ceramic include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid.
[0064] The aluminum nitride powder composition was prepared by the method provided in this embodiment, and the mass ratio of the aluminum nitride powder composition to the Y2O3-CaF2 composite sintering aid was 94:6. In the Y2O3-CaF2 composite sintering aid, the mass ratio of Y2O3 to CaF2 was 3:1.
[0065] This embodiment also provides a method for preparing aluminum nitride ceramics, including the following steps: T01. Place the aluminum nitride powder composition, Y2O3, and CaF2 in a vacuum environment at 150℃ (vacuum degree ≤ 10). -3 Drying at 8h under (Pa); after drying, the raw material is ball-milled for 6h using anhydrous ethanol as the dispersion medium; after ball milling, the mixture obtained by ball milling is subjected to low-temperature de-alcoholization treatment at ≤60℃, and finally passed through a 200-mesh sieve to obtain agglomerated composite powder; T02. The composite powder obtained in step T01 is mixed with the binder at a mixing temperature of 150°C for 4 hours. Then, it is processed through extrusion, air cooling, pelletizing and injection molding to obtain aluminum nitride ceramic green body. T03. The aluminum nitride ceramic green body is treated with trichloroethylene, and then the aluminum nitride ceramic green body is placed in a degreasing furnace and heated to 500°C at a slow heating rate of 1°C / min, and held at that temperature for 3 hours for hot dewaxing and degreasing. T04. The aluminum nitride ceramic green body is sintered to obtain the aluminum nitride ceramic.
[0066] In step T02, the binder is a PEG-PMMA-paraffin ternary system binder, in which the mass ratio of PEG, PMMA and paraffin is 10:10:70, and the amount of binder added is 8% of the mass of the composite powder; the injection molding process parameters are: material temperature 170℃, mold temperature 50℃, injection pressure 70MPa, holding pressure 60MPa, and holding time 10s.
[0067] In step T04, the sintering atmosphere uses high-purity nitrogen gas with a purity ≥99.999% at a pressure of 0.2 MPa. The sintering process includes a low-temperature carbon removal stage, a heating stage, and a sintering densification stage. Specifically, in the low-temperature carbon removal stage, the temperature is slowly increased to 600°C at a heating rate of 1°C / min, then held for 2 hours, followed by the introduction of carbon dioxide gas and another 2 hours of holding for debinding. In the heating stage, the temperature is increased from 600°C to 1200°C at a heating rate of 2°C / min, then held for 1 hour. In the sintering densification stage, the temperature is increased from 1200°C to 1800°C at a heating rate of 2°C / min, then held for 4 hours. After the sintering densification stage, the aluminum nitride ceramic is cooled to 1000°C at a cooling rate of 1.5°C / min, followed by natural cooling. Finally, the aluminum nitride ceramic was subjected to high-temperature heat treatment in a nitrogen atmosphere to stabilize its thermal conductivity; wherein the high-temperature heat treatment temperature was 1400℃ and the high-temperature heat treatment time was 4h.
[0068] Example 2 This embodiment provides a method for preparing an aluminum nitride powder composition, including the following steps: S10. Disperse aluminum nitride powder in anhydrous ethanol to obtain an aluminum nitride slurry with a solid content of 30wt%. S20. Stearic acid is added to the aluminum nitride slurry, and the mixture is ultrasonically dispersed and stirred at 70°C for 2 hours. In this step, the amount of stearic acid added is 1% of the mass of the aluminum nitride powder in step S10. S30. Continue adding dibutyl phthalate to the mixture and stir for another 1 hour. After mixing evenly, filter the mixture. After filtration, dry and pulverize the filter cake to obtain hydrophobically modified aluminum nitride powder. In this step, the amount of dibutyl phthalate added is 0.5% of the mass of aluminum nitride powder in step S10. S40. Disperse the hydrophobically modified aluminum nitride powder in toluene, then add a 10wt% methyliminoaluminane solution to the mixture, mix evenly, filter the mixture to obtain a filter cake, and then dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
[0069] In step S30, the drying temperature of the filter cake is 50°C. In step S40, the methyliminoaluminane solution is prepared by dissolving methyliminoaluminane in toluene, and the amount of methyliminoaluminane solution added is 10% of the mass of aluminum nitride powder in step S10; the filter cake is dried in a vacuum oven at 70°C for 5 hours.
[0070] This embodiment also provides an aluminum nitride ceramic, wherein the raw materials for preparing the aluminum nitride ceramic include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid.
[0071] The aluminum nitride powder composition was prepared by the method provided in this embodiment, and the mass ratio of the aluminum nitride powder composition to the Y2O3-CaF2 composite sintering aid was 95:5. In the Y2O3-CaF2 composite sintering aid, the mass ratio of Y2O3 to CaF2 was 2:1.
[0072] This embodiment also provides a method for preparing aluminum nitride ceramics, which is the same as the method provided in Example 1.
[0073] Example 3 This embodiment provides a method for preparing an aluminum nitride powder composition, including the following steps: S10. Disperse aluminum nitride powder in anhydrous ethanol to obtain an aluminum nitride slurry with a solid content of 40 wt%. S20. Stearic acid is added to the aluminum nitride slurry, and the mixture is ultrasonically dispersed and stirred at 80°C for 1 hour. In this step, the amount of stearic acid added is 1% of the mass of the aluminum nitride powder in step S10. S30. Continue adding dibutyl phthalate to the mixture and stir for another 1 hour. After mixing evenly, filter the mixture. After filtration, dry and pulverize the filter cake to obtain hydrophobically modified aluminum nitride powder. In this step, the amount of dimethyl phthalate added is 1% of the mass of aluminum nitride powder in step S10. S40. Disperse the hydrophobically modified aluminum nitride powder in toluene, then add a 10wt% methyliminoaluminane solution to the mixture, mix evenly, filter the mixture to obtain a filter cake, and then dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
[0074] In step S30, the filter cake is dried at 60°C. In step S40, the methyliminoaluminane solution is prepared by dissolving methyliminoaluminane in toluene, and the amount of methyliminoaluminane solution added is 25% of the mass of aluminum nitride powder in step S10; the filter cake is dried in a vacuum oven at 80°C for 4 hours.
[0075] This embodiment also provides an aluminum nitride ceramic, wherein the raw materials for preparing the aluminum nitride ceramic include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid.
[0076] The aluminum nitride powder composition was prepared by the method provided in this embodiment, and the mass ratio of the aluminum nitride powder composition to the Y2O3-CaF2 composite sintering aid was 96:4. In the Y2O3-CaF2 composite sintering aid, the mass ratio of Y2O3 to CaF2 was 4:1.
[0077] This embodiment also provides a method for preparing aluminum nitride ceramics, which is the same as the method provided in Example 1.
[0078] Comparative Example 1 This comparative example provides a method for preparing aluminum nitride powder. The only difference between this method and the method provided in Example 1 is that after the filtration process in step S30, the filter cake is dried and pulverized to directly obtain hydrophobically modified aluminum nitride powder, without step S40.
[0079] In step S30 of this comparative example, the filter cake was dried in a vacuum oven at 60°C for 6 hours.
[0080] This comparative example also provides an aluminum nitride ceramic, the raw materials for which include hydrophobically modified aluminum nitride powder and Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the hydrophobically modified aluminum nitride powder is prepared by the method provided in this comparative example.
[0081] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0082] Comparative Example 2 This comparative example provides a method for preparing an aluminum nitride powder composition. The only difference between this method and the method provided in Example 1 is that dibutyl phthalate is replaced with fatty alcohol polyoxyethylene ether, which has a molecular weight of 580.
[0083] This comparative example also provides an aluminum nitride ceramic, the raw materials for which include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the aluminum nitride powder composition is prepared by the method provided in this comparative example.
[0084] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0085] Comparative Example 3 This comparative example provides a method for preparing an aluminum nitride powder composition. The only difference between this method and the method provided in Example 1 is that in step S40, the amount of methyliminoaluminane solution added is 30% of the mass of aluminum nitride powder in step S10.
[0086] This comparative example also provides an aluminum nitride ceramic, the raw materials for which include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the aluminum nitride powder composition is prepared by the method provided in this comparative example.
[0087] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0088] Comparative Example 4 This comparative example provides a method for preparing an aluminum nitride powder composition, which is the same as the method provided in Example 1.
[0089] This comparative example also provides an aluminum nitride ceramic, the raw materials for which the aluminum nitride ceramic is prepared include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the mass ratio of Y2O3 to CaF2 in the Y2O3-CaF2 composite sintering aid is 4.5:0.5.
[0090] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0091] Comparative Example 5 This comparative example provides a method for preparing an aluminum nitride powder composition, which is the same as the method provided in Example 1.
[0092] This comparative example also provides an aluminum nitride ceramic, the raw materials for which the aluminum nitride ceramic is prepared include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the mass ratio of Y2O3 to CaF2 in the Y2O3-CaF2 composite sintering aid is 1:2.
[0093] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0094] Comparative Example 6 This comparative example provides a method for preparing an aluminum nitride powder composition, which is the same as the method provided in Example 1.
[0095] This comparative example also provides an aluminum nitride ceramic, the raw materials for which the aluminum nitride ceramic is prepared include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the mass ratio of the aluminum nitride powder composition to the Y2O3-CaF2 composite sintering aid is 90:10.
[0096] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0097] Comparative Example 7 This comparative example provides a method for preparing an aluminum nitride powder composition, which is the same as the method provided in Example 1.
[0098] This comparative example also provides an aluminum nitride ceramic, the raw materials for which the aluminum nitride ceramic is prepared include an aluminum nitride powder composition and a Y2O3-CaF2 composite sintering aid. The only difference between this and the aluminum nitride ceramic provided in Example 1 is that the mass ratio of the aluminum nitride powder composition to the Y2O3-CaF2 composite sintering aid is 98:2.
[0099] This comparative example also provides a method for preparing aluminum nitride ceramics, which is the same as the method for preparing aluminum nitride ceramics provided in Example 1.
[0100] The density, thermal conductivity, flexural strength, and fracture toughness of the aluminum nitride ceramics provided in the above embodiments and comparative examples were tested respectively. The test results are shown in the table below. The density test was conducted according to the standard GB / T 25995-2010 "Test Method for Density and Apparent Porosity of Fine Ceramics"; the flexural strength test was conducted according to the standard GB / T 4740-2024 "Test Method for Strength of Ceramic Materials"; the thermal conductivity test was conducted according to the standard GB / T 39862-2021 "Test Method for Thermal Conductivity of High Thermal Conductivity Ceramics"; and the fracture toughness test was conducted according to the standard GB / T 44547-2024 "Test Method for Fracture Toughness of Fine Ceramics - Single-Sided V-Beam (SEVNB) Method".
[0101]
[0102] The test results in the table above show that the aluminum nitride ceramics provided in Examples 1 to 3 have a density of 98.5% or higher, a thermal conductivity stable at 220~229 W / (m·K), a flexural strength of not less than 400 MPa, and a fracture toughness of not less than 3.2 (MPa·m). 1 / 2 This invention demonstrates that by dispersing methyliminoaluminane in hydrophobically modified aluminum nitride powder and using a composite sintering aid with optimized proportions, the synergistic improvement of the high thermal conductivity, high density, and high mechanical toughness of aluminum nitride ceramics can be achieved simultaneously.
[0103] Comparing the aluminum nitride ceramic provided in Comparative Example 1 with that provided in Example 1, it was found that the aluminum nitride ceramic provided in Comparative Example 1 had a lower density and lower thermal conductivity and mechanical properties (flexural strength) than the aluminum nitride ceramic provided in Example 1. This is because Comparative Example 1 did not disperse methyliminoaluminane in the hydrophobically modified aluminum nitride powder, resulting in a lack of the toughening effect of aluminum nitride nanowires in the aluminum nitride ceramic. Therefore, the ceramic was more brittle than the aluminum nitride ceramic provided in Example 1 (manifested as a decrease in fracture toughness). Furthermore, due to the lack of dense nanowire filling of grain gaps, the density of the aluminum nitride ceramic was lower than that of the aluminum nitride ceramic provided in Example 1.
[0104] Comparing the aluminum nitride ceramic provided in Comparative Example 2 with that provided in Example 1, it was found that the aluminum nitride ceramic provided in Comparative Example 2 had a lower density and lower thermal conductivity, mechanical properties, and fracture toughness than the aluminum nitride ceramic provided in Example 1. This is because in the aluminum nitride powder modification stage of Comparative Example 2, fatty alcohol polyoxyethylene ether was used as an organic encapsulating agent. Although the formation of a hydrophobic layer on the surface of the aluminum nitride powder by the fatty alcohol polyoxyethylene ether can improve the hydrolysis resistance of the powder, the processing fluidity of the powder is weaker than that of the aluminum nitride powder composition in Example 1. This will affect the injection molding effect of the aluminum nitride ceramic green body, resulting in a lower density of the sintered aluminum nitride ceramic than that provided in Example 1, which in turn affects the various properties of the aluminum nitride ceramic.
[0105] Comparing the aluminum nitride ceramic provided in Comparative Example 3 with that provided in Example 1, it was found that the aluminum nitride ceramic provided in Comparative Example 3 had a lower density and lower thermal conductivity and mechanical properties than that provided in Example 1. This is because in the powder preparation method of Comparative Example 3, the amount of methyliminoaluminane solution added was too large, which decomposed to generate excessive aluminum nitride nanowires during the sintering of the aluminum nitride ceramic, hindering powder migration and grain growth, resulting in insufficient densification of the aluminum nitride ceramic, and thus affecting the various properties of the aluminum nitride ceramic.
[0106] Comparing the aluminum nitride ceramic provided in Comparative Example 4 with the aluminum nitride ceramic provided in Example 1, it was found that all performance indicators of the aluminum nitride ceramic provided in Comparative Example 4 decreased. This is because the proportion of rare earth oxides in the composite sintering aid used in Comparative Example 4 is too high, which easily forms a continuous glass phase, exacerbates phonon scattering, and hinders the densification of aluminum nitride ceramic.
[0107] Comparing the aluminum nitride ceramic provided in Comparative Example 5 with the aluminum nitride ceramic provided in Example 1, it was found that all performance indicators of the aluminum nitride ceramic provided in Comparative Example 5 decreased. This is because the proportion of metal fluoride in the composite sintering aid used in Comparative Example 5 was too high. The metal fluoride volatilized excessively at high temperature and eroded the grain boundaries, resulting in a decrease in the bonding strength of the grain interface, an increase in micropores and microcracks inside the aluminum nitride ceramic, and a simultaneous deterioration in thermal conductivity and mechanical properties. The aluminum nitride ceramic was more brittle than the aluminum nitride ceramic provided in Example 1.
[0108] Comparing the aluminum nitride ceramic provided in Comparative Example 6 with the aluminum nitride ceramic provided in Example 1, it was found that all performance indicators of the aluminum nitride ceramic provided in Comparative Example 6 decreased. This is because the amount of composite sintering aid used in Comparative Example 6 was too large, which formed a large amount of amorphous phase, destroyed the thermal conductivity path and weakened the grain boundary bonding strength, resulting in a decrease in thermal conductivity and mechanical properties. The aluminum nitride ceramic was more brittle than the aluminum nitride ceramic provided in Example 1.
[0109] Comparing the aluminum nitride ceramic provided in Comparative Example 7 with the aluminum nitride ceramic provided in Example 1, it was found that all performance indicators of the aluminum nitride ceramic provided in Comparative Example 7 decreased. This is because the amount of composite sintering aid used in Comparative Example 7 was too small, resulting in insufficient liquid phase generation during sintering. The aluminum nitride powder could not be fully rearranged and densified, leading to a large number of residual pores inside the aluminum nitride blank. As a result, the density, thermal conductivity, flexural strength and fracture toughness of the aluminum nitride ceramic decreased.
[0110] Figure 3 The XRD pattern of the hydrophobically modified aluminum nitride powder prepared in the method of this invention is shown. The XRD pattern results show that the hydrophobically modified aluminum nitride powder has no Al(OH)3 or Al2O3 hydrolysis products or by-products. The crystal phase is mainly aluminum nitride and a small amount of yttrium oxide. This indicates that the aluminum nitride powder composition provided by this invention has excellent water resistance and ensures the high thermal conductivity of aluminum nitride ceramics.
[0111] It is understood that those skilled in the art can make equivalent substitutions or modifications to the technical solution and inventive concept of the present invention, and all such substitutions or modifications should fall within the protection scope of the appended claims.
Claims
1. A method for preparing an aluminum nitride powder composition, characterized in that, Includes the following steps: S10. Disperse aluminum nitride powder in a first organic solvent to obtain aluminum nitride slurry; S20. Add organic acid to aluminum nitride slurry and mix thoroughly; S30. Add an organic encapsulation agent to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain hydrophobically modified aluminum nitride powder. S40. Disperse the hydrophobically modified aluminum nitride powder in a second organic solvent, then add a methyliminoaluminane solution to the mixture, mix evenly, and then perform solid-liquid separation treatment on the mixture to obtain a filter cake. Dry and pulverize the filter cake to obtain an aluminum nitride powder composition.
2. The method for preparing the aluminum nitride powder composition according to claim 1, characterized in that, In step S20, the organic acid is at least one of stearic acid, ricinoleic acid, and tartaric acid.
3. The method for preparing the aluminum nitride powder composition according to claim 1, characterized in that, In step S40, the organic encapsulation agent is at least one of dibutyl phthalate and dimethyl phthalate.
4. An aluminum nitride powder composition, characterized in that, It is prepared by the method of any one of claims 1-3 for the preparation of aluminum nitride powder composition.
5. An aluminum nitride ceramic, characterized in that, The raw materials for preparing the aluminum nitride ceramic include the aluminum nitride powder composition according to claim 4, wherein the aluminum nitride ceramic has a thermal conductivity ≥210 W / (m·K), a flexural strength ≥400 MPa, and a fracture toughness ≥3.2 MPa·m. 1 / 2 .
6. The aluminum nitride ceramic according to claim 5, characterized in that, The raw materials for preparing the aluminum nitride ceramics also include composite sintering aids; the composite sintering aids include metal fluorides and rare earth oxides.
7. The aluminum nitride ceramic according to claim 6, characterized in that, The rare earth oxide is at least one of Y2O3, Yb2O3, Er2O3, and La2O3; the metal fluoride is at least one of CaF2, MgF2, LiF, and YF3.
8. The aluminum nitride ceramic according to claim 6, characterized in that, The mass ratio of the rare earth oxide to the metal fluoride is (2-4):1; the mass ratio of the aluminum nitride powder composition to the composite sintering aid is (94-96):(4-6).
9. A method for preparing aluminum nitride ceramics, characterized in that, The method for preparing the aluminum nitride ceramic according to any one of claims 5-8 is characterized by comprising the following steps: T01. The raw materials used to prepare aluminum nitride ceramics are ball-milled and mixed to obtain composite powder; T02. The composite powder is subjected to molding treatment to obtain aluminum nitride ceramic green body; T03. The aluminum nitride ceramic green body is subjected to organic component removal treatment; T04. The aluminum nitride ceramic green body after organic component removal treatment is sintered and subjected to high-temperature heat treatment in sequence to obtain the aluminum nitride ceramic.
10. The method for preparing aluminum nitride ceramic according to claim 9, characterized in that, In step T04, the sintering process is carried out under a protective atmosphere and includes a low-temperature decarburization stage, a heating stage, and a sintering densification stage. The low-temperature decarburization stage involves slowly heating to 600°C at a heating rate of 1°C / min, and then holding at that temperature for 2–4 hours. The heating stage involves heating from 600°C to 1200°C at a heating rate of 2°C / min, and then holding at that temperature for 1 hour. The sintering densification stage involves heating from 1200°C to 1800–1850°C at a heating rate of 2°C / min, and then holding at that temperature for 3–4 hours.