An electrolyte solvent, an electrolyte, and a sodium-ion battery

By introducing halogen atoms, amide groups, and silicon-oxygen functional groups into the electrolyte, a stable inorganic interface film is formed, which solves the problem of easy decomposition of ether electrolytes under high voltage and achieves high cycle stability and safety of negative electrode-free sodium batteries.

CN123062479APending Publication Date: 2026-11-10HUNAN LIFANG NEW ENERGY SCI & TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610938846.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-26
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing ether-based electrolytes are prone to oxidation and decomposition under high voltage, making it difficult to meet the application requirements of voltage windows of 4V and above, resulting in insufficient cycle performance of sodium batteries without negative electrodes.

Method used

Using electrolyte solvent of structure I, an inorganic interface film rich in sodium halide and Na3N is formed by introducing halogen atoms, amide groups and silicon-oxygen functional groups in synergy with sodium salt electrolyte, thereby improving the high voltage resistance and interface stability of the battery.

Benefits of technology

It significantly improves battery cycle performance, extends battery high-voltage cycle life, enhances battery safety and fast-charging capability, and improves overall battery electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_9
    Figure SMS_9
Patent Text Reader

Abstract

This invention belongs to the field of sodium-ion battery technology, and specifically relates to an electrolyte solvent, an electrolyte, and a sodium-ion battery. The electrolyte solvent provided by this invention comprises a compound shown in structural formula I, wherein R1, R2, R3, R4, R5, R6, and R7 are independently selected from one of the following: hydrogen atom, halogen atom, alkane group with 1 to 10 carbon atoms, unsaturated hydrocarbon group with 2 to 10 carbon atoms, alkoxy group with 1 to 10 carbon atoms, and alkanoyl group with 2 to 10 carbon atoms; and at least one of R1, R2, R3, R4, R5, R6, and R7 contains a halogen atom. The halogen atom, amide group, and silicon-oxygen functional group in the electrolyte solvent provided by this invention can synergistically interact with the sodium salt electrolyte, giving the electrolyte excellent high-voltage stability, interfacial stability, and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of sodium-ion battery technology, and in particular relates to an electrolyte solvent, an electrolyte, and a sodium-ion battery. Background Technology

[0002] Electrodeless sodium batteries, because their negative electrode only uses a current collector and does not contain active materials, have their "actual negative electrode" formed in situ by electrochemical deposition on the current collector surface during the first charge. This significantly improves the overall energy density of the battery and represents a crucial development direction in the sodium battery field. Ether solvents have attracted widespread attention due to their good compatibility with sodium metal negative electrodes. However, conventional ether solvents lack the conjugated structure to stabilize the lone pairs of electrons in oxygen atoms, resulting in poor oxidation resistance and easy oxidative decomposition at high voltages, typically making them unsuitable for applications requiring voltage windows of 4V and above.

[0003] Patent CN119852527A discloses an electrolyte and a sodium battery containing it. It uses a specific structure of ether-based organic solvent, siloxane-based organic solvent, or a fluorinated product of both as a solvent, which is mixed with a sodium salt to form a weakly solvated electrolyte. This approach weakens the interaction between the solvent and sodium by increasing steric hindrance, introducing higher-energy Si 3d orbitals for conjugation, or utilizing the electron-withdrawing effect of fluorine atoms. + The solvation between the electrodes promotes the entry of anions into the solvation structure and the formation of contact ion pairs and aggregates, thereby constructing an interface film rich in inorganic matter at the electrode / electrolyte interface, achieving 100 stable cycles of the negative electrode-free sodium battery.

[0004] In summary, how to fully leverage the excellent compatibility between ether-based electrolytes and sodium metal anodes while effectively improving the oxidation stability and interfacial stability of the electrolyte at higher voltages, thereby enhancing battery cycle performance, has become a pressing technical challenge in the field of anode-free sodium batteries. Summary of the Invention

[0005] The purpose of this invention is to provide an electrolyte solvent, an electrolyte, and a negative electrode-free sodium-ion battery. By modifying an ether solvent of formula I, the synergistic effect of its halogen atoms, amide groups, and silicon-oxygen functional groups with the sodium salt electrolyte is utilized to achieve excellent high-voltage stability and interfacial stability, thereby further improving the cycle performance of the battery.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: In a first aspect, the present invention provides an electrolyte solvent, characterized in that: the electrolyte solvent comprises a compound represented by structural formula I;

[0007] R1, R2, R3, R4, R5, R6, and R7 are each independently selected from one of the following: hydrogen atom, halogen atom, alkane group with 1 to 10 carbon atoms, unsaturated hydrocarbon group with 2 to 10 carbon atoms, alkoxy group with 1 to 10 carbon atoms, and alkanoyl group with 2 to 10 carbon atoms; and at least one of R1, R2, R3, R4, R5, R6, and R7 contains a halogen atom.

[0008] Preferably, the H in the alkane group, unsaturated hydrocarbon group, alkoxy group and alkanoyl group may be partially or completely replaced by one or more of the halogen atom, cyano group, carboxyl group and sulfonic acid group.

[0009] Preferably, at least one of R1, R2, R3, R4, R5, R6, and R7 contains an F atom.

[0010] Preferably, the electrolyte solvent includes at least one of structural formula I-1, structural formula I-2, and structural formula I-3; ; ; .

[0011] Preferably, the electrolyte solvent includes at least two of structural formulas I-1, I-2, and I-3; and the mass ratio of any two of them is 1:1; the mass ratio of all three of them is 1:1:1.

[0012] In a second aspect, the present invention provides an electrolyte comprising a sodium salt electrolyte and any of the above-described electrolyte solvents.

[0013] Preferably, the mass ratio of the sodium salt to the electrolyte solvent is (10~20):(80~90).

[0014] Preferably, the sodium salt electrolyte of the electrolyte includes at least one of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium bis(oxalate)borate, and sodium bis(oxalate)borate.

[0015] Thirdly, the present invention provides a negative electrode-free sodium-ion battery, comprising a positive electrode, a negative electrode, a separator, a casing, and any of the above-described electrolytes.

[0016] Preferably, the positive electrode active material of the positive electrode sheet includes at least one of layered oxide and polyanionic material; the layered oxide includes at least one of sodium nickel iron manganese oxide and sodium copper iron manganese oxide; the polyanionic material includes at least one of sodium iron pyrophosphate, sodium vanadium phosphate and sodium iron pyrophosphate.

[0017] The beneficial effects of this invention are: 1) The electrolyte solvent of structural formula I provided by this invention simultaneously introduces halogen atoms, amide groups, and silicon-oxygen functional groups into the polyether molecular skeleton. The halogen atoms participate in the formation of the positive and negative electrode interface film with a sodium halide-rich inorganic layer, which has stronger mechanical properties and improves the high-voltage resistance of the battery. The amide group is composed of a polar carbonyl group (C=O) and an imino group (-NH-), which forms a large π-conjugated system, giving it a high antioxidant potential and generating a Na3N-rich inorganic interface film, thus improving the high-voltage resistance of the electrolyte. The introduction of silicon-oxygen functional groups can remove acid and water, participate in the formation of a more high-voltage-resistant positive and negative electrode interface film, and complex the positive electrode to inhibit the dissolution of the positive electrode metal, improving the high-voltage resistance of the solvent and further improving the stability of the electrolyte. The introduction of the three active functional groups makes up for the shortcomings of ether electrolytes in high-voltage stability and interface stability, thereby improving the high-voltage cycle life of the battery cell.

[0018] 2) The novel weakly coordinated solvent of this invention weakens the binding between sodium ions and the solvent, lowers the desolvation energy barrier, and achieves faster interfacial charge transfer. At the same time, the anions in the sodium salt are preferentially decomposed to generate an interfacial film rich in inorganic substances such as sodium halides, thereby improving the high-voltage resistance of the electrolyte. Detailed Implementation

[0019] To make the objectives, technical solutions, and technical effects of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely. The embodiments described below are some embodiments of the present invention, but not all embodiments. All other embodiments obtained by those skilled in the art in conjunction with the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed; where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0020] In the description of this invention, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0021] It should be understood that the weights of the relevant components mentioned in the embodiments of this invention can refer not only to the specific content of each component, but also to the proportional relationship between the weights of the components. Therefore, any scaling up or down of the content of the relevant components according to the embodiments of this invention is within the scope of this invention. Specifically, the weights mentioned in the embodiments of this invention can be well-known mass units in the chemical industry, such as ug, mg, g, and kg.

[0022] Furthermore, unless the context explicitly uses it otherwise, the singular form of a word should be understood as including the plural form of that word. The terms "comprising" or "having" are intended to specify the presence of a feature, quantity, step, operation, element, part, or combination thereof, but are not intended to exclude the presence or possible addition of one or more other features, quantities, steps, operations, elements, parts, or combinations thereof.

[0023] According to a first aspect of the present invention, an electrolyte solvent is provided, the electrolyte solvent comprising a compound represented by structural formula I;

[0024] R1, R2, R3, R4, R5, R6, and R7 are each independently selected from one of the following: hydrogen atom, halogen atom, alkane group with 1 to 10 carbon atoms, unsaturated hydrocarbon group with 2 to 10 carbon atoms, alkoxy group with 1 to 10 carbon atoms, and alkanoyl group with 2 to 10 carbon atoms; and at least one of R1, R2, R3, R4, R5, R6, and R7 contains a halogen atom.

[0025] In this invention, the halogen atoms in the electrolyte solvent of formula I participate in the formation of a sodium halide-rich inorganic layer at the positive and negative electrode interface, which is a core strategy for improving the overall performance of sodium-ion batteries. Its advantages are mainly reflected in three aspects: interface stability, safety and reliability, and kinetic optimization. First, this interface layer, thanks to the excellent chemical inertness and high mechanical strength of sodium halide, constructs a robust physical barrier between the electrode and the electrolyte. This effectively suppresses side reactions and the continuous decomposition of the electrolyte, and buffers the volume changes of the electrode material during charging and discharging, thereby significantly extending the battery's cycle life. Second, this high-modulus interface guides sodium ions to achieve uniform deposition on the electrode surface and effectively suppresses the growth of sodium dendrites through physical barriers and chemical induction, avoiding the risk of internal short circuits and greatly improving battery safety. Finally, the NaF-rich interface layer exhibits excellent ion conduction characteristics. It effectively reduces the desolvation barrier of sodium ions and provides a fast transport channel at the interface formed by sodium ions and other components, thereby significantly improving the battery's rate performance and power density. The synergistic effect of these three levels ultimately enabled sodium-ion batteries to achieve a breakthrough in comprehensive electrochemical performance, combining long cycle stability, high safety, and excellent fast charging capability.

[0026] In solvent I, the polar carbonyl group (C=O) and imino group (-NH-) form a large π-conjugated system, giving it a high antioxidant potential and generating a Na3N-rich inorganic interface film. In sodium-ion batteries, amide groups and their derived nitrogen-rich inorganic interface films are another effective strategy to improve battery performance, with advantages mainly reflected in three aspects: enhanced sodium-ion storage, stable electrode structure, and optimized interface kinetics. First, the introduction of amide groups can effectively improve the sodium storage capacity and structural stability of electrode materials. Through amidation structure design, the interlayer distance of carbon materials can be significantly increased, providing a wider insertion / extraction channel for larger sodium ions. At the same time, this process can also introduce abundant active sites, providing additional adsorption sites for sodium ions, thereby increasing capacity. Second, nitrogen-rich inorganic interface films (mainly composed of Na3N, etc.) play a key role in stabilizing the interface and suppressing dendrite growth. These interface films have high ionic conductivity and excellent mechanical strength, which can effectively promote the rapid transport of sodium ions at the interface, while providing robust physical protection for the electrode and inhibiting the growth of sodium dendrites. This sodium-loving interface can also create a uniform electric field and sodium ion concentration, guiding sodium ions to achieve uniform, dendrite-free deposition, which significantly improves the cycle life and safety of the battery.

[0027] The core advantage of silicon-oxygen functional groups as solvent molecules lies in their unique weak solvation properties and high stability, which systematically optimize the interfacial dynamics and operating temperature range of batteries at the molecular level. Specifically, silicon-oxygen solvents, due to their weak binding energy with sodium ions, can effectively reduce the sodium ion desolvation energy barrier, promoting rapid ion transport at the electrode interface. Simultaneously, their weak coordination environment facilitates the formation of a thin and stable interfacial film on the negative electrode surface, thereby suppressing side reactions and improving cycle stability. Furthermore, these solvents generally possess low melting points and excellent thermal stability, ensuring good electrolyte flow at low temperatures and effectively suppressing the hydrolysis of hexafluorophosphate and side reactions at the electrode interface at high temperatures. Some fluorinated siloxane solvents can even maintain an average coulombic efficiency of over 98% at 90°C, significantly widening the safe operating temperature range of the battery. At the same time, the low density of siloxanes can effectively reduce the overall mass of the electrolyte, directly contributing to increasing the battery's energy density.

[0028] The introduction of three active functional groups compensates for the shortcomings of ether electrolytes in high-voltage stability and interfacial stability, thereby improving the high-voltage cycle life of the battery cell.

[0029] Preferably, the hydrogen atoms in the alkane group, the unsaturated hydrocarbon group, the alkoxy group, and the alkanoyl group are partially or completely substituted by one or more of the halogen group, cyano group, carboxyl group, and sulfonic acid group.

[0030] Preferably, at least one of R1, R2, R3, R4, R5, R6, and R7 contains an F atom.

[0031] Preferably, solvent formula I includes one or more of formula I-1, formula I-2, and formula I-3; ; ; .

[0032] The substances in Formula I-1, Formula I-2, and Formula I-3 all contain fluorine atoms, amide groups, and silicon-oxygen functional groups. They participate in the formation of NaF-rich inorganic layer positive and negative electrode interface films and Na3N-rich inorganic interface films. They can remove acid and water, and also form high-voltage resistant positive and negative electrode interface films, improving the high-voltage resistance of the solvent and further improving the stability of the electrolyte, thereby enhancing the high-voltage cycle life of the battery.

[0033] Preferably, the electrolyte solvent includes at least two of structural formulas I-1, I-2, and I-3; and the mass ratio of any two of them is 1:1; the mass ratio of all three of them is 1:1:1.

[0034] According to a second aspect of the present invention, an electrolyte is provided, comprising a sodium salt electrolyte and any of the above-described electrolyte solvents, wherein the electrolyte has high voltage and high temperature resistance, and can effectively improve battery cycle performance and high temperature storage performance.

[0035] The mass ratio of the sodium salt to the electrolyte solvent is (10~20):(80~90).

[0036] The electrolyte sodium salt includes at least one of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium dioxolane-borate, and sodium dioxolane-borate.

[0037] The aforementioned sodium salts each possess different dissociation capabilities, providing ample sodium ions in organic solvents to enhance the ionic conductivity of the electrolyte. Sodium hexafluorophosphate exhibits high solubility in organic solvents, resulting in electrolytes with high ionic conductivity and good chemical and electrochemical stability. Sodium perchlorate demonstrates excellent thermal and chemical stability, rapid ion migration, and low cost. Sodium tetrafluoroborate can be used to formulate electrolytes operating over a wide temperature range (e.g., -40°C to 60°C), exhibiting high conductivity and low viscosity. Sodium difluorooxalate borate exhibits extremely high thermal stability and intrinsic flame retardancy. Sodium difluorooxalate borate effectively improves the conductivity, stability, and antioxidant decomposition voltage of the electrolyte.

[0038] In summary, selecting at least one of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium dioxolane-borate, and sodium dioxolane-borate as the sodium salt electrolyte can significantly optimize the performance of the electrolyte, improve the energy density, power density, cycle life, and safety of the battery, and meet the needs of different application scenarios.

[0039] According to a third aspect of the present invention, the present invention provides a negative electrode-free sodium-ion battery, comprising a positive electrode, a negative electrode, a separator, a casing, and any of the above-described electrolytes, which has good high-voltage stability and cycle performance.

[0040] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a positive active material, which includes at least one of layered oxides and polyanionic materials. The layered oxide includes at least one of sodium nickel iron manganese oxide and sodium copper iron manganese oxide. The polyanionic material includes at least one of sodium iron pyrophosphate, sodium vanadium phosphate, and sodium iron pyrophosphate.

[0041] The positive electrode active material can also be modified. The methods for modifying the positive electrode active material are known to those skilled in the art. For example, the positive electrode active material can be modified by coating, doping and other methods. The materials used for modification can be one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce and W.

[0042] A positive current collector is typically a structure or component that collects current. Positive current collectors can be any material suitable for use as a positive current collector in a sodium-ion battery without a negative electrode.

[0043] The negative electrode is made by die-cutting carbon-coated aluminum foil.

[0044] The separator can be any material suitable for lithium-ion battery separators in the art, such as one or more of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, and natural fibers.

[0045] The casing is made of either stainless steel or aluminum-plastic film.

[0046] To enable those skilled in the art to clearly understand the above-described implementation details and operations of the present invention, and to demonstrate the significant advancements in the performance of the embodiments of the present invention, the following examples illustrate the above technical solutions.

[0047] Example 1

[0048] Battery manufacturing 1) Preparation of the positive electrode sheet: The positive electrode active material sodium iron pyrophosphate (Na4Fe3(PO4)2P2O7), binder polyvinylidene fluoride (PVDF), conductive agent, and dispersant were dispersed in NMP (N-methylpyrrolidone) organic solvent at a mass ratio of 94.5:2:3:0.5. The mixture was stirred under vacuum until stable and homogeneous, and then uniformly coated onto an aluminum foil with a thickness of 12μm. After drying the aluminum foil at room temperature, it was transferred to a 120℃ forced-air oven for 1 hour to dry. Then, it was cold-pressed and die-cut to form the positive electrode sheet. 2) Preparation of negative electrode sheet: The negative electrode sheet is prepared by die-cutting carbon-coated aluminum foil; 3) Electrolyte preparation: The electrolyte was prepared in a nitrogen-filled glove box (O2 < 2 ppm, H2O < 3 ppm). The sodium salt and electrolyte solvent were mixed evenly by magnetic stirring. The sodium salt was NaPF6, and the electrolyte solvent was a compound with structural formula I-1 (a nine-carbon perfluoropolyether siloxane), which was purchased commercially from Guangdong Wengjiang Chemical Reagent Co., Ltd. The weight ratio of NaPF6 to compound with structural formula I-1 was 14:86; the structure of compound with structural formula I-1 is shown below:

[0049] Sodium-ion battery preparation: The positive electrode, separator, and negative electrode are stacked in sequence to obtain a bare cell. The cell is then packaged with an aluminum-plastic film, baked, injected with electrolyte, left to stand, formed, shaped with a fixture, resealed, and its capacity is tested to complete the preparation of the sodium-ion battery.

[0050] Example 2

[0051] The only difference from Example 1 is that the weight ratio of NaPF6 to compound I-1 in the electrolyte preparation step is 12:88.

[0052] The other steps are the same as in Example 1.

[0053] Example 3

[0054] The only difference from Example 1 is that the weight ratio of NaPF6 to compound I-1 in the electrolyte preparation step is 10:90.

[0055] The other steps are the same as in Example 1.

[0056] Example 4

[0057] The only difference from Example 1 is that the weight ratio of NaPF6 to compound I-1 in the electrolyte preparation step is 16:84.

[0058] The other steps are the same as in Example 1.

[0059] Example 5

[0060] The only difference from Example 1 is that the weight ratio of NaPF6 to compound I-1 in the electrolyte preparation step is 20:80.

[0061] Example 6

[0062] The only difference from Example 1 is that the sodium salt electrolyte used in the electrolyte preparation step is NaFSI.

[0063] The other steps are the same as in Example 1.

[0064] Example 7

[0065] The only difference from Example 1 is that the sodium salt electrolyte in the electrolyte preparation step is NaBF4.

[0066] The other steps are the same as in Example 1.

[0067] Example 8

[0068] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a compound with structural formula I-2 (hexacarbon perfluoropolyether siloxane), which was purchased commercially from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0069]

[0070] The other steps are the same as in Example 1.

[0071] Example 9

[0072] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a compound with structural formula I-3 (hexacarbon perfluoropolyether triethoxysilane), which was purchased commercially from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0073]

[0074] The other steps are the same as in Example 1.

[0075] Example 10

[0076] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a mixture of Formula I-1 and Formula I-2, and the weight ratio is 1:1.

[0077] The other steps are the same as in Example 1.

[0078] Example 11

[0079] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a mixture of Formula I-1 and Formula I-3, and the weight ratio is 1:1.

[0080] The other steps are the same as in Example 1.

[0081] Example 12

[0082] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a mixture of Formula I-2 and Formula I-3, and the weight ratio is 1:1.

[0083] The other steps are the same as in Example 1.

[0084] Example 13

[0085] The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a mixture of Formula I-1, Formula I-2 and Formula I-3, and the weight ratio is 1:1:1.

[0086] The other steps are the same as in Example 1.

[0087] Example 14

[0088] The only difference from Example 1 is that the positive electrode active material is sodium nickel iron manganese oxide, and the other steps are the same as in Example 1.

[0089] Example 15

[0090] The only difference from Example 1 is that the positive electrode active material is sodium vanadium phosphate, and the other steps are the same as in Example 1.

[0091] Comparative Example 1 The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is DOL (1,3-dioxolane).

[0092] The other steps are the same as in Example 1.

[0093] Comparative Example 2 The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is DME (1,2-dimethoxyethane).

[0094] The other steps are the same as in Example 1.

[0095] Comparative Example 3 The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a compound of structural formula II (right panthenol), which was purchased commercially from Changzhou Huixin Biotechnology Co., Ltd.

[0096]

[0097] The other steps are the same as in Example 1.

[0098] Comparative Example 4 The only difference from Example 1 is that the electrolyte solvent in the electrolyte preparation step is a compound of structural formula III (polyether modified heptamethyltrisiloxane), which was purchased commercially from Hubei Qifei Pharmaceutical Chemical Co., Ltd.

[0099]

[0100] The other steps are the same as in Example 1.

[0101] Table 1. Composition ratio of electrolytes prepared in the examples and comparative examples

[0102] The sodium-ion batteries prepared in the above embodiments and comparative examples were subjected to the following performance tests, and the test results are shown in Table 2.

[0103] 1) Room temperature cycle test: Place the battery in an oven at a constant temperature of 25℃ for 4 hours, then charge it at a constant current of 1C to 3.8V, then charge it at a constant voltage until the current drops to 0.05C, then discharge it at a constant current of 1C to 1.5V. Repeat this cycle and record the initial capacity and the discharge capacity of the last cycle (1000th cycle); Capacity retention rate = discharge capacity of the last cycle (1000th cycle) / initial capacity × 100%.

[0104] 2) 45℃ Cyclic Test: The battery was placed in a constant temperature 45℃ oven for 4 hours, then charged at a constant current of 1C to 3.8V, then charged at a constant voltage until the current dropped to 0.05C, and then discharged at a constant current of 1C to 1.5V. This cycle was repeated, and the initial capacity and the discharge capacity of the battery in the last cycle (500th cycle) were recorded. Capacity retention rate = discharge capacity in the last cycle (500th cycle) / initial capacity × 100%. Table 2 shows the experimental battery performance test results provided in the examples and comparative examples.

[0105]

[0106] As can be seen from the test results in Table 2, the electrolyte additive of the present invention can significantly improve the cycle performance of the battery.

[0107] 1) A comparison of the experimental results in Examples 1-5 shows that the mass fraction of solvent in the electrolyte has a significant impact on battery cycle performance. When the solvent content is controlled within the range of 82% to 88% of the total electrolyte mass, the cycle stability of the battery can be effectively improved and its service life extended. In particular, when the solvent accounts for 86% of the electrolyte mass fraction, the battery exhibits optimal cycle performance, and the capacity retention rate reaches its highest value after 500 cycles.

[0108] 2) The comparison of the test results of Examples 1 and 6-7 shows that, in different sodium salt systems, the electrolyte with sodium hexafluorophosphate (NaPF6) as the sodium salt has a significantly better capacity retention rate after 500 cycles than the system with sodium difluorosulfonamide (NaFSI) and sodium tetrafluoroborate (NaBF4) as the sodium salt, indicating that NaPF6 has the best compatibility in the electrolyte system of the present invention.

[0109] 3) A comparison of the experimental results of Examples 1 and 8-13 shows that, in the selected solvent systems, when the compound shown in Formula I-1 is used as a single solvent, the 500-cycle capacity retention rate of the battery is higher than that of systems using single solvents of Formula I-2 and Formula I-3 or any combination thereof (with the same weight ratio). This result proves that the structure shown in Formula I-1 is the optimal choice for the electrolyte solvent of this invention.

[0110] 4) A comparison of the experimental results of Examples 1 and 14-15 shows that, among the selected positive electrode active materials, the battery's 500-cycle capacity retention rate is higher when sodium iron pyrophosphate is used as the positive electrode active material than the system using sodium nickel iron manganese oxide and sodium vanadium phosphate. This result proves that the structure shown in Formula I-1 is the optimal choice for the electrolyte solvent of this invention.

[0111] 5) A comparison of the experimental results of Example 1 and Comparative Examples 1-4 shows that the electrolyte solvent of Formula I-1 used in this invention (which simultaneously introduces amide groups, silicon-oxygen functional groups, and fluorine atoms into its molecular structure) achieves a significantly higher 500-cycle capacity retention rate than systems using conventional ether solvents (DOL, DME). More importantly, compared to ether solvents that only introduce amide groups (Formula II) or only introduce silicon-oxygen functional groups (Formula III), this invention significantly improves the long-term cycle stability of the battery through the synergistic effect of the above three types of functional groups, thereby verifying the advanced nature and effectiveness of the electrolyte solvent design of this invention.

[0112] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.

Claims

1. An electrolyte solvent, characterized in that: The electrolyte solvent includes the compound shown in structural formula I; R1, R2, R3, R4, R5, R6, and R7 are each independently selected from one of the following: hydrogen atom, halogen atom, alkane group with 1 to 10 carbon atoms, unsaturated hydrocarbon group with 2 to 10 carbon atoms, alkoxy group with 1 to 10 carbon atoms, and alkanoyl group with 2 to 10 carbon atoms; and at least one of R1, R2, R3, R4, R5, R6, and R7 contains a halogen atom.

2. The electrolyte solvent according to claim 1, characterized in that, The hydrogen atoms in the alkane group, the unsaturated hydrocarbon group, the alkoxy group, and the alkanoyl group are partially or completely substituted by one or more of the halogen group, cyano group, carboxyl group, and sulfonic acid group.

3. The electrolyte solvent according to claim 1, characterized in that, At least one of R1, R2, R3, R4, R5, R6, and R7 contains an F atom.

4. The electrolyte solvent according to claim 1 or 3, characterized in that, The electrolyte solvent includes at least one of structural formulas I-1, I-2, and I-3. ; ; 。 5. The electrolyte solvent according to claim 4, characterized in that: The electrolyte solvent includes at least two of structural formulas I-1, I-2, and I-3; and the mass ratio of any two of them is 1:1; the mass ratio of all three of them is 1:1:

1.

6. An electrolyte, characterized in that, Includes sodium salts and the electrolyte solvents according to any one of claims 1-5.

7. The electrolyte according to claim 6, characterized in that, The mass ratio of the sodium salt to the electrolyte solvent is (10~20):(80~90).

8. The electrolyte according to claim 6, characterized in that, The sodium salt includes at least one of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium dioxaborate, and sodium dioxaborate.

9. A sodium-ion battery, characterized in that, It includes a positive electrode, a negative electrode, a separator, and the electrolyte as described in any one of claims 6 to 8.

10. The sodium-ion battery according to claim 9, characterized in that, The positive electrode active material of the positive electrode sheet includes at least one of layered oxide and polyanionic material; the layered oxide includes at least one of sodium nickel iron manganese oxide and sodium copper iron manganese oxide; the polyanionic material includes at least one of sodium iron pyrophosphate, sodium vanadium phosphate and sodium iron pyrophosphate.

Citation Information

Patent Citations

  • Electrolyte and sodium battery containing same

    CN119852527A