A fatigue-resistant polyurethane elastomer, its preparation method and application
By constructing the polyurethane main chain through a stepwise catalytic method and introducing a high-density dynamic metal coordination network, the shortcomings of traditional polyurethane materials in terms of fatigue resistance are solved, achieving high strength, high elongation and excellent elastic recovery rate, and significantly improving the fatigue resistance of the material.
Patent Information
- Application Number
- CN202611445065.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional polyurethane materials suffer from problems in fatigue resistance, such as difficulty in achieving both strength and toughness, insufficient energy dissipation under cyclic loading, and reduced lifespan due to microcrack propagation. Furthermore, existing multi-synergistic crosslinking strategies have poor control over the introduction of flexible segments and micro-phase separation structure, and uneven distribution of metal coordination sites affects material stability.
A stepwise catalytic method was used to construct the polyurethane backbone. The backbone was formed by reacting polyol with diisocyanate, followed by the introduction of bis(3-aminopropyl)-terminated polydimethylsiloxane and 2,6-diaminopyridine chain extender. Finally, a coordination reaction was carried out with zinc salt to form a high-density dynamic metal coordination network, which ensures the orderly construction of chain segments and energy dissipation.
This study achieved a polyurethane elastomer that maintains high strength and high elongation while maintaining an elastic recovery rate of ≥90% and a cycle stability of ≤5 times, significantly improving its fatigue resistance.
Smart Images

Figure CN123062671A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of polyurethane preparation methods, and in particular to a fatigue-resistant polyurethane elastomer, its preparation method, and its application. Background Technology
[0002] Polyurethane (PU) is a block copolymer formed by the reaction of diisocyanates, polyols, and chain extenders. It possesses high strength, good elasticity, and a designable molecular structure, making it widely used in tissue engineering, artificial organs, wound repair, and flexible electronics. However, in terms of fatigue resistance, traditional polyurethane materials still face challenges such as the difficulty in balancing strength and toughness, insufficient energy dissipation under cyclic loading, and reduced lifespan due to microcrack propagation. Therefore, how to prepare polyurethane elastomers with both excellent mechanical properties and superior fatigue resistance has always been one of the key technical problems urgently needing to be solved in this field.
[0003] In recent years, introducing multiple dynamic non-covalent bonds or reversible forces into polyurethane networks through molecular structure design to construct multi-synergistic crosslinking structures has proven to be an effective strategy for overcoming the aforementioned performance bottlenecks. Compared to polyurethanes constructed with a single force, these materials can simultaneously achieve high strength, high toughness, and excellent fatigue resistance. For example, Materials Horizons, 2025, 12, 599-607 reported that by introducing multiple functional groups into the main chain or side chain, multiple interactions such as hydrogen bonding, π-π interactions, and metal coordination exist simultaneously in the system, thereby forming a synergistic crosslinking network. Shen et al. (Chemical Engineering Journal, 2024, 498, 155414) further found that the synergistic effect of multi-level hydrogen bonding and metal coordination can effectively improve energy dissipation capacity, inhibit crack propagation during cyclic loading, and significantly improve the fatigue resistance of the material.
[0004] However, existing polyurethane elastomers based on multiple synergistic crosslinking strategies still have the following shortcomings: On the one hand, the introduction of flexible segments and the regulation of micro-phase separation structure still need to be optimized to more effectively alleviate stress concentration under cyclic loading; on the other hand, metal coordination sites are mostly introduced in the form of side chains or added small molecule ligands, which can easily lead to problems such as metal ion migration and uneven distribution of coordination sites, affecting the stability and fatigue resistance of the material under long-term dynamic use conditions. Summary of the Invention
[0005] The purpose of this invention is to provide a fatigue-resistant polyurethane elastomer, its preparation method, and its application. The polyurethane elastomer has excellent tensile properties, elastic recovery rate, and cycle stability, thus possessing both excellent mechanical properties and fatigue resistance.
[0006] The objective of this invention can be achieved through the following technical solutions: One objective of this invention is to provide a method for preparing a fatigue-resistant polyurethane elastomer, comprising the following steps: S1. Polyol and diisocyanate are reacted under the conditions of catalyst, inert atmosphere and heating to obtain isocyanate-terminated precursor; S2. Dissolve bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (PDMS) in a first organic solvent to obtain a polymer solution. Then add the polymer solution to the isocyanate-terminated precursor obtained in step S1 and react under an inert atmosphere and heating conditions to obtain a long-chain precursor. S3. Dissolve 2,6-diaminopyridine (DAP) and the catalyst in a second organic solvent to obtain a chain extender solution; then add the chain extender solution to the long-chain precursor obtained in step S2, and react under an inert atmosphere and heating conditions. After the reaction is completed, wash and settle to obtain a polyurethane elastomer intermediate product. S4. Dissolve the polyurethane elastomer intermediate obtained in step S3 and the zinc salt in an organic solvent, wherein the molar ratio of the zinc salt to 2,6-diaminopyridine is 3-8:1; carry out a coordination reaction under an inert atmosphere, and remove the solvent after the reaction is completed to obtain the fatigue-resistant polyurethane elastomer.
[0007] Preferably, in step S1, the polyol is either polypropylene glycol (PPG) or polycaprolactone (PCL).
[0008] More preferably, in step S1, the weight-average molecular weight of the polyol is 1500-2500.
[0009] Preferably, in step S1, the diisocyanate is any one of isophorone diisocyanate (IPDI), toluene-2,3-diisocyanate (2,3-TDI), toluene-2,4-diisocyanate (2,4-TDI), and toluene-2,5-diisocyanate (2,5-TDI).
[0010] Preferably, in step S1, the catalyst is dibutyltin dilaurate (DBTDL).
[0011] Preferably, in step S1, the molar ratio of the polyol to the diisocyanate is 1:1.8-2.5.
[0012] More preferably, in step S1, the molar ratio of the polyol to the diisocyanate is 1:1.9-2.2.
[0013] More preferably, in step S1, the molar ratio of the polyol to the diisocyanate is 1:2.
[0014] Preferably, in step S1, the amount of catalyst added is 0.01%-2% of the total mass of the polyol and diisocyanate.
[0015] More preferably, in step S1, the amount of catalyst added is 0.05%-1% of the total mass of the polyol and diisocyanate.
[0016] Preferably, in step S1, the heating temperature is 70-100℃ and the reaction time is 1-3 hours.
[0017] More preferably, in step S1, the heating temperature is 80°C and the reaction time is 1.5 hours.
[0018] Preferably, in step S2, the weight-average molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 2000-5000.
[0019] More preferably, in step S2, the weight-average molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 3000.
[0020] Preferably, in step S2, the first organic solvent is any one of dichloromethane, trichloromethane, tetrahydrofuran, or N,N-dimethylacetamide.
[0021] Preferably, in step S2, the molar ratio of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to the polyol in step S1 is 1:2-2.2.
[0022] Preferably, in step S2, the heating temperature is 70-100℃ and the reaction time is 3-5 hours.
[0023] More preferably, in step S2, the heating temperature is 70°C and the reaction time is 3 hours.
[0024] More preferably, in steps S1-S2, the polyol and the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) are both dehydrated.
[0025] Preferably, in step S3, the catalyst is dibutyltin dilaurate.
[0026] Preferably, in step S3, the second organic solvent is any one of dichloromethane, trichloromethane, tetrahydrofuran, or N,N-dimethylacetamide.
[0027] Preferably, in step S3, the molar ratio of 2,6-diaminopyridine to the polyol is 0.5-1.5:1.
[0028] More preferably, in step S3, the molar ratio of 2,6-diaminopyridine to the polyol is 0.51-1.05:1.
[0029] Preferably, in step S3, the amount of catalyst added is 0.01%-2% of the total mass of polyol, diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine.
[0030] More preferably, in step S3, the amount of catalyst added is 0.05%-1% of the total mass of polyol, diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine.
[0031] Preferably, in step S3, the heating temperature is 70-100℃ and the reaction time is 1-2 days.
[0032] More preferably, in step S3, the heating temperature is 70°C and the reaction time is 24 h.
[0033] Preferably, in step S4, the molar ratio of the zinc salt to 2,6-diaminopyridine is 6:1.
[0034] Preferably, in step S4, the zinc salt is any one of zinc chloride (ZnCl2), zinc perchlorate (Zn(ClO4)2), or zinc trifluoromethanesulfonate (Zn(CF3SO3)2).
[0035] Preferably, in step S4, the mass ratio of the polyurethane elastomer intermediate to the zinc salt is 1:0.03-0.7.
[0036] More preferably, in step S4, the mass ratio of the polyurethane elastomer intermediate to the zinc salt is 1:0.05-0.3.
[0037] Preferably, in step S4, the coordination reaction takes 1-2 days.
[0038] More preferably, in step S4, the coordination reaction takes 24 hours.
[0039] Preferably, in steps S1-S4, the inert atmosphere includes a nitrogen atmosphere.
[0040] Preferably, in step S1, the isocyanate-terminated precursor has the following structural formula: .
[0041] In step S2, the structural formula of the long-chain precursor is as follows: .
[0042] In step S3, the structural formula of the polyurethane elastomer intermediate product is as follows: .
[0043] In the above structural formula, the value of m ranges from 30 to 45, the value of n ranges from 20 to 40, and the value of a ranges from 7 to 10.
[0044] Preferably, the weight-average molecular weight of the polyurethane elastomer intermediate is 45,000-70,000, and the molecular weight distribution is 1.4-1.6.
[0045] The second objective of this invention is to provide an anti-fatigue polyurethane elastomer prepared according to the above-described preparation method. The anti-fatigue polyurethane elastomer is prepared using a stepwise construction method: first, a polyurethane backbone is formed by reacting a polyol with a diisocyanate; then, bis(3-aminopropyl)-terminated polydimethylsiloxane is covalently embedded into the polyurethane backbone by reacting its terminal amino groups with the isocyanate groups on the backbone; next, 2,6-diaminopyridine is covalently embedded into the backbone through a chain extension reaction; finally, Zn... 2+ Coordination was performed to obtain the fatigue-resistant polyurethane elastomer.
[0046] Preferably, the structure of the fatigue-resistant polyurethane elastomer is as follows: .
[0047] Preferably, the value of m ranges from 30 to 45, the value of n ranges from 20 to 40, and the value of a ranges from 7 to 10.
[0048] In this invention, Zn 2+ The coordination sites include three types: (1) the heterocyclic nitrogen atom on the pyridine ring (derived from the 2,6-diaminopyridine chain extender, this heterocyclic nitrogen atom does not participate in the isocyanate reaction, and its lone pair electrons are retained); (2) the nitrogen atom on the urea group; and (3) the carbonyl oxygen atom on the urea group. 2+ Dynamic metal coordination crosslinking nodes are constructed by forming reversible coordination bonds between the above three types of coordination sites and different polymer chains or segments. This dynamic network, together with the hydrogen bonds between polyurethane / polyurea segments and the flexible PDMS segments, forms a multi-level dynamic network, endowing the elastomer with excellent fatigue resistance.
[0049] In this invention, the intermediate polyurethane elastomer molecules are rich in hydrogen bonds, forming a reversible physical cross-linking network. Specifically, the -NH- groups in the urea and urethane groups act as hydrogen bond donors, and their carbonyl oxygen groups act as hydrogen bond acceptors, forming NH···O=C type hydrogen bonds; simultaneously, the pyridine ring nitrogen atom in the 2,6-diaminopyridine unit can also act as a hydrogen bond acceptor, forming NH···N type hydrogen bonds with the -NH- groups in adjacent segments. These multiple hydrogen bonding interactions collectively endow the polymer network with reversible physical cross-linking properties.
[0050] In this invention, PDMS forms flexible soft segments, imparting excellent flexibility and deformability to the material, while polyol segments form rigid segments (in this invention, the main chain of the polyol segments is composed of CC / CO bonds; compared to the Si-O main chain of PDMS, the segment mobility is relatively limited, resulting in greater rigidity, hence they are defined as rigid hard segments), thus imparting greater rigidity to the polymer chain. Diisocyanate and diaminopyridine serve as crosslinking sites, reacting with the soft and hard segments to generate urethane and urea groups, which, through multiple hydrogen bonds and Zn... 2+ Dynamic coordination forms a physically cross-linked network. Due to the polarity difference between soft and hard segments, a microphase separation structure is formed. The soft segments are responsible for dissipating deformation energy, while the hard segments and cross-linking sites are responsible for maintaining network stability, working together to achieve excellent fatigue resistance.
[0051] Preferably, the fatigue-resistant polyurethane elastomer has a tensile strength of 16.88-22.43 MPa, an elongation at break of 1106%-1692%, an elastic recovery rate of ≥90% under 200% strain at room temperature, and requires ≤5 cycles for cyclic stability.
[0052] The third objective of this invention is to provide an application of the aforementioned fatigue-resistant polyurethane elastomer in flexible wearable devices.
[0053] Preferably, the fatigue-resistant polyurethane elastomer can be applied to flexible wearable devices, strain sensors, electronic skin, human motion monitoring devices, or soft robots.
[0054] From the perspective of material action mechanisms, most existing technologies primarily pursue rapid self-healing performance. The core of this lies in the rapid migration of internal polymer chains after macroscopic damage to the material, and their dynamic interaction leading to the re-establishment of effective connections. A prerequisite for achieving this process is that the material network possesses high chain mobility and dynamic exchange capabilities.
[0055] However, there is an inherent contradiction between the self-healing ability and network stability of polymer materials. If the material network structure is too stable, the molecular chain segments are strongly constrained, which restricts the diffusion, migration, and rebonding processes of the chain segments at the damaged interface, leading to a decrease in self-healing efficiency. Therefore, to achieve rapid self-healing, existing technologies must endow the molecular chain segments with a high degree of freedom of movement, specifically manifested in: low crosslinking point density and low inter-segment friction. This design orientation is reflected in the macroscopic properties of the material as low tensile strength but high elongation at break; the polymer chains easily change from a coiled state to a stretched state under stress, but are difficult to resist structural damage caused by external forces.
[0056] In contrast, the fatigue resistance of materials requires the structural stability of the polymer network under long-term cyclic loading. During cyclic stretching, the material needs to dissipate stress through molecular chain segment movement, interchain friction, and dynamic bond breaking and recombination. These processes inevitably cause continuous adjustment and local evolution of the network structure, which may lead to problems such as network relaxation, reduction of effective crosslinking points, and performance degradation under long-term cyclic loading. Therefore, excellent fatigue resistance requires the network structure to have sufficient stability to resist the aforementioned structural degradation.
[0057] This invention addresses the technical challenge of fatigue failure of existing polyurethane elastomers under repeated loading. It proposes a fatigue-resistant polyurethane elastomer based on a synergistic strategy of stepwise catalytic ordered construction and high-density dynamic sacrificial bond network, starting from two aspects: the ordered arrangement of molecular chain segments and the high efficiency of energy dissipation network.
[0058] Firstly, this invention employs stepwise catalysis to achieve ordered chain segment construction, laying a structural foundation for fatigue resistance: The fatigue resistance of polyurethane elastomers essentially depends on the regularity of their molecular chain segment structure. If the main chain structure is disordered and the chain segments are randomly distributed, the stress will be unevenly transmitted along the molecular chain under repeated stress, which will easily lead to stress concentration at structural defects and accelerate crack initiation and propagation.
[0059] This invention differs from the traditional one-pot synthesis method, which involves adding a catalyst all at once. Instead, the catalyst is added independently during the prepolymerization stage of the polyol and diisocyanate and the chain extension stage of the 2,6-diaminopyridine. The essence of this stepwise catalysis lies in the fact that the functional groups of each reactant have different activities during the stepwise polymerization of polyurethane. If the catalyst is present throughout the entire process, subsequent components that have not yet participated in the prepolymerization (such as PDMS and DAP) may be non-selectively consumed during the prepolymerization stage, leading to a disordered reaction pathway and the generation of products with low molecular weight, wide molecular weight distribution, and disordered chain segment sequences. Microscopically, this manifests as a random arrangement of hard and soft segments, while macroscopically, it reflects a significant deterioration in mechanical strength and fatigue resistance.
[0060] By independently controlling the catalytic activity of each reaction step in stages, the polyol and diisocyanate can first fully react to form an isocyanate-terminated prepolymer. Then, the terminal amino groups of the bis(3-aminopropyl)-terminated PDMS react with the terminal isocyanate groups of the prepolymer, allowing the flexible PDMS segments to be covalently and orderly embedded into the polyurethane backbone. Finally, the chain is further extended by 2,6-diaminopyridine. This strategy allows the segments to be sequentially incorporated into the backbone according to the designed order, which significantly increases the probability of generating the target product compared to the one-pot method. The product has a higher molecular weight, a narrower molecular weight distribution, and a more regular segment sequence.
[0061] The polyurethane backbone constructed in this way provides a structural basis for the uniform distribution of subsequent multi-level dynamic networks: the regular backbone facilitates the formation of a stable and uniform microphase separation structure between hard and soft segments, the regular distribution of PDMS flexible segments ensures that they can fully exert their flexibility under stress, and the uniformly distributed hard segment regions provide a regular anchoring environment for coordination crosslinking sites, so that energy dissipation can be carried out uniformly and efficiently in the entire material system, avoiding local stress concentration, thus laying a molecular-level structural basis for fatigue resistance.
[0062] Secondly, this invention employs an ultra-high zinc salt ratio to construct a high-density dynamic sacrificial bond network, thereby achieving strain energy dissipation: Based on the ordered main chain structure, this invention further proposes an ultra-high zinc salt ratio design that differs from conventional coordination strategies in existing technologies. In existing technologies, the molar ratio of metal salt to chain extender is typically 1:(1-4). The underlying logic is to use a relatively low crosslinking density to allow polymer segments to maintain sufficient mobility at low temperatures, thereby endowing the material with self-healing capabilities. However, while pursuing the freedom of chain segment movement, this design sacrifices the density and uniformity of the dynamic crosslinking network, resulting in a limited number of coordinate bonds that can break and recombine per unit volume under cyclic loading, insufficient energy dissipation efficiency, and difficulty in resisting the accumulation of fatigue damage.
[0063] This invention breaks through the aforementioned technological limitations by setting the molar ratio of zinc salt to 2,6-diaminopyridine to, for example, 6:1, i.e., Zn 2+ The amount of Zn far exceeds the pyridine ring coordination sites. At this extremely high ratio, Zn... 2+ It forms abundant dynamic metal-metal coordination bonds with the nitrogen atoms of the pyridine ring on the main chain and the nitrogen and oxygen atoms on the urea group, constructing a high density of interchain crosslinking nodes. More importantly, excess Zn... 2+ It does not exist entirely in the form of fixed crosslinking points, but is partially dispersed in the polymer network in the form of free state or weak coordination. When the material is repeatedly subjected to stress, it continuously breaks and recombines as dynamic sacrificial bonds, thereby efficiently dissipating strain energy and delaying the propagation of fatigue cracks.
[0064] This invention achieves a better balance between the dynamic coordination structure and the polyurethane main chain segments by reasonably increasing the density of coordination nodes. This maintains sufficient network stability to prevent premature structural failure of the material under cyclic loading, while providing a sufficient number of dynamic bonds to improve the overall dynamic recovery capability and energy dissipation efficiency under cyclic loading. Thus, it endows the material with the ability to resist fatigue failure at the crosslinking network level.
[0065] Thirdly, this invention achieves multi-level network synergy, from molecular chain segment ordering to macroscopic fatigue resistance: In summary, this invention ensures the regularity of the hard / soft segment microphase separation structure and the uniform distribution of coordination sites through the stepwise catalytic construction of the ordered polyurethane backbone. This provides a uniform distribution environment for the dynamic crosslinking network, a structural basis for uniform energy dissipation, and avoids local stress concentration. Meanwhile, the high-density dynamic metal coordination sacrificial bond network introduced by the ultra-high zinc salt ratio continuously dissipates strain energy under stress. The synergy of these two aspects allows the material to maintain good mechanical strength while retaining the integrity of its internal structure through reversible reconstruction of dynamic bonds, even after long-term cyclic loading, ultimately achieving excellent fatigue resistance.
[0066] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention provides a fatigue-resistant polyurethane elastomer, its preparation method, and its application. The elastomer uses a polyurethane backbone composed of a polyol and a diisocyanate, with bis(3-aminopropyl)-terminated polydimethylsiloxane (PDMS) as flexible segments, and 2,6-diaminopyridine as a chain extender to introduce pyridine groups into the backbone, which are then crosslinked via zinc ion coordination. In preparation, a stepwise catalytic strategy is employed, with catalysts added independently in the prepolymerization and chain extension stages to achieve ordered chain segment construction. Simultaneously, a high-density dynamic metal coordination network is constructed using an ultra-high molar ratio of zinc salt to 2,6-diaminopyridine of 6:1. This design enables the elastomer to maintain high strength and high elongation while exhibiting an elastic recovery rate ≥90% and a cycle stability of ≤5 cycles, demonstrating excellent fatigue resistance.
[0067] (2) This invention achieves the ordered construction of the polyurethane backbone through a stepwise catalytic strategy. Unlike the traditional one-pot method where the catalyst is present throughout the entire process, leading to disordered reaction pathways and disorganized chain segments, this invention independently controls catalytic activity in the prepolymerization and chain extension stages. This allows the PDMS flexible segments and the 2,6-diaminopyridine chain extender to be sequentially integrated into the backbone in the designed order, significantly increasing the probability of generating the target product and resulting in a higher molecular weight (weight-average molecular weight as high as 5.3 × 10⁻⁶). 4 The molecular weight distribution is narrower (g / mol), and the molecular weight distribution is 1.5, with a more regular chain segment sequence. The resulting regular main chain provides a structural basis for the uniform distribution of the subsequent dynamic network, avoids local stress concentration, and ensures fatigue resistance at the molecular level.
[0068] (3) This invention uses an ultra-high zinc salt ratio (Zn 2+ A high-density dynamic metal coordination network is constructed using a 6:1 ratio of Zn (metal salt:chain extender = 1:1-4). Unlike existing technologies that employ low crosslinking density (metal salt:chain extender = 1:1-4) to achieve self-healing, this invention significantly increases the Zn content. 2+ The content of Zn allows for a better balance between the dynamic coordination structure and the polyurethane main chain segments, maintaining sufficient network stability to prevent structural damage under cyclic loading, while also achieving this balance through excessive Zn content. 2+ The formed dynamic sacrificial bonds continuously dissipate strain energy, thereby significantly improving the material's ability to resist fatigue failure.
[0069] (4) In this invention, the PDMS flexible chain segments are embedded in the polyurethane main chain in an orderly manner through a step-by-step construction method. Their regular distribution ensures that they can effectively absorb some deformation energy through changes in chain segment conformation when under stress, thereby alleviating stress concentration. At the same time, due to the polarity difference between the soft and hard segments of PDMS, a micro-phase separation structure is formed inside the elastomer. Under the action of external force, the interface between the soft and hard phases can slip and generate interface energy dissipation, further dissipating strain energy and effectively delaying the initiation and propagation of fatigue cracks.
[0070] (5) In this invention, 2,6-diaminopyridine is introduced into the main chain as a chain extender. The pyridine group is introduced without disrupting the original hydrogen bond interactions of the polyurethane elastomer main chain, thereby increasing the metal coordination ability of the elastomer. Furthermore, the direct introduction of pyridine into the polyurethane main chain structure avoids the metal ion migration problems present in traditional side-chain coordination or external ligand systems, making it easier for the elastomer to interact with Zn. 2+ Coordination crosslinking occurs, increasing strength.
[0071] (6) The preparation method of the fatigue-resistant polyurethane elastomer in this invention is simple, and the controllability of each reaction stage is high, which is conducive to large-scale production and application. Attached Figure Description
[0072] Figure 1 The results are obtained by gel permeation chromatography (GPC) of the fatigue-resistant polyurethane elastomer intermediate product with synergistic coordination between PDMS flexible segments and main chain obtained in Example 1.
[0073] Figure 2 The stress-strain curves of the fatigue-resistant polyurethane elastomers obtained in Examples 1-7 show the synergistic effect of the coordination between the PDMS flexible segments and the main chain.
[0074] Figure 3 The data are from a cyclic tensile test at a strain of 200% for the fatigue-resistant polyurethane elastomer with synergistic coordination between the PDMS flexible segments and the main chain obtained in Example 1.
[0075] Figure 4 The data are from a cyclic tensile test at a strain of 200% for the fatigue-resistant polyurethane elastomer with synergistic coordination between the PDMS flexible segments and the main chain obtained in Example 2.
[0076] Figure 5 This is a reaction route diagram for the fatigue-resistant polyurethane elastomer of the present invention. Detailed Implementation
[0077] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.
[0078] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.
[0079] This invention provides a method for preparing an anti-fatigue polyurethane elastomer, which is prepared using a stepwise construction method: first, a polyurethane backbone is formed by reacting a polyol with a diisocyanate; then, bis(3-aminopropyl)-terminated polydimethylsiloxane is covalently embedded into the polyurethane backbone by reacting its terminal amino groups with the isocyanate groups on the backbone; next, 2,6-diaminopyridine is covalently embedded into the backbone through a chain extension reaction; finally, Zn... 2+ Coordination was performed to obtain the fatigue-resistant polyurethane elastomer.
[0080] Its preparation method specifically includes the following steps: S1. A polyol and a diisocyanate are reacted under the conditions of a catalyst, an inert atmosphere, and heating to obtain an isocyanate-terminated precursor; the polyol is any one of polypropylene glycol or polycaprolactone, with a weight-average molecular weight of 1500-2500; the diisocyanate is any one of isophorone diisocyanate, toluene-2,3-diisocyanate, toluene-2,4-diisocyanate, and toluene-2,5-diisocyanate; the catalyst is dibutyltin dilaurate; the molar ratio of the polyol to the diisocyanate is 1:1.8-2.5; the amount of catalyst added is 0.01%-2% of the total mass of the polyol and the diisocyanate; the heating temperature is 70-100℃, and the reaction time is 1-3 hours.
[0081] S2. Dissolve bis(3-aminopropyl)-terminated poly(dimethylsiloxane) in a first organic solvent to obtain a polymer solution. Then, add the polymer solution to the isocyanate-terminated precursor obtained in step S1 and react under an inert atmosphere and heating conditions to obtain a long-chain precursor. The weight-average molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 2000-5000. The first organic solvent is any one of dichloromethane, trichloromethane, tetrahydrofuran, or N,N-dimethylacetamide. The molar ratio of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to the polyol in step S1 is 1:2-2.2. The heating temperature is 70-100℃, and the reaction time is 3-5 hours.
[0082] S3. Dissolve 2,6-diaminopyridine and the catalyst in a second organic solvent to obtain a chain extender solution; then add the chain extender solution to the long-chain precursor obtained in step S2, and react under an inert atmosphere and heating conditions. After the reaction is completed, wash and settle to obtain a polyurethane elastomer intermediate product. In step S3, the catalyst is dibutyltin dilaurate; the second organic solvent is any one of dichloromethane, trichloromethane, tetrahydrofuran, or N,N-dimethylacetamide; the molar ratio of 2,6-diaminopyridine to the polyol is 0.5-1.5:1; the amount of catalyst added is 0.01%-2% of the total mass of the polyol, diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine; the heating temperature is 70-100℃, and the reaction time is 1-2 days.
[0083] S4. Dissolve the polyurethane elastomer intermediate obtained in step S3 and the zinc salt in an organic solvent, wherein the molar ratio of the zinc salt to 2,6-diaminopyridine is 3-8:1; carry out a coordination reaction under an inert atmosphere, and remove the solvent after the reaction is completed to obtain the fatigue-resistant polyurethane elastomer; wherein the zinc salt is any one of zinc chloride, zinc perchlorate, or zinc trifluoromethanesulfonate; wherein the mass ratio of the polyurethane elastomer intermediate to the zinc salt is 1:0.03-0.7, and the coordination reaction takes 1-2 days.
[0084] The structural formula of the fatigue-resistant polyurethane elastomer prepared is as follows: .
[0085] Wherein, m ranges from 30 to 45, n ranges from 20 to 40, and a ranges from 7 to 10; the weight-average molecular weight of the polyurethane elastomer intermediate is 45,000 to 70,000, and the molecular weight distribution is 1.4 to 1.6.
[0086] Furthermore, the reaction pathway of the fatigue-resistant polyurethane elastomer is as follows: Figure 5As shown.
[0087] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0088] Example 1 Example 1 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which includes the following steps: Step S1: Weigh 1 g of polypropylene glycol (0.5 mmol) with a weight-average molecular weight of 2000 and heat it under vacuum at 100 °C. Stir for 30 min to remove residual moisture. Cool to 80 °C and use a microsyringe to extract 240 μL of isophorone diisocyanate (IPDI, with a density of 1.058 g / mL and a molecular weight of 222.29, equivalent to 254 mg and 1.14 mmol) and add it dropwise to the reaction vessel. Use a microsyringe to extract 15 μL of dibutyltin dilaurate (DBTDL, with a density of 1.066 g / mL and a molecular weight of 631.56, equivalent to 16 mg and 0.0253 mmol) and add it dropwise to the reaction vessel. Stir at 80 °C under a nitrogen atmosphere for 1.5 h to obtain the isocyanate-terminated polypropylene glycol precursor.
[0089] In step 1, the molar ratio of polypropylene glycol to isophorone diisocyanate is 1:2.28, and the amount of dibutyltin dilaurate added is 1.27% of the total mass of polypropylene glycol and isophorone diisocyanate.
[0090] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture. Then, 0.75 g (equivalent to 0.25 mmol) of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide to obtain a polymer solution. The polymer solution was added dropwise to the isocyanate-terminated polypropylene glycol precursor obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h to obtain a long-chain precursor.
[0091] In step S2, the molar ratio of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to polypropylene glycol in step S1 is 1:2.
[0092] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine (molecular weight 109, equivalent to 0.255 mmol) and 10 μL of DBTDL (equivalent to 10.66 mg, 0.017 mmol) in 1 mL of N,N-dimethylacetamide. After complete dissolution, add the solution dropwise to the long-chain precursor obtained in step S2. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer intermediate.
[0093] In step S3, the molar ratio of 2,6-diaminopyridine to polypropylene glycol in step S1 is 0.51:1; the amount of catalyst DBTDL added is 0.52% of the total mass of polypropylene glycol, isophorone diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine.
[0094] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer intermediate in tetrahydrofuran, and then dissolve 0.2g of ZnCl2 in methanol. The mass ratio of the hydrogen-bonded polyurethane elastomer intermediate to the zinc salt is 1:0.13, and the molar ratio of the zinc salt to 2,6-diaminopyridine is approximately 6:1. Under nitrogen protection, carry out the coordination reaction for 24h. Then, spread the reaction solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain.
[0095] Figure 1 The GPC test results of the polyurethane elastomer intermediate prepared in Example 1 are shown. It exhibits a single chromatographic peak within a retention time of 20-28 min, and its weight-average molecular weight is as high as 5.3 × 10⁻⁶. 4 The molecular weight distribution is 1.5 g / mol, exhibiting a relatively narrow molecular weight distribution characteristic. The above results indicate that the stepwise catalytic synthesis strategy adopted in this invention can effectively achieve the ordered construction of chain segments and successfully obtain the target polymer with high molecular weight and uniform distribution.
[0096] like Figure 2 As shown, the elastomer has a strength of 16.88 MPa and an elongation at break of 1692%. Figure 3 As shown, the elastic recovery rate is ≥90%, the number of cycles required for cyclic stability is ≤5, and it has good fatigue resistance.
[0097] Example 2 Example 2 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1g of polycaprolactone with a weight average molecular weight of 2000 and heat it under vacuum at 100℃. Stir for 30min to remove residual moisture. Cool to 80℃ and use a microsyringe to extract 240µL of isophorone diisocyanate (IPDI) and add it dropwise to the reaction vessel. Also use a microsyringe to extract 15µL of dibutyltin dilaurate (DBTDL) and add it dropwise to the reaction vessel. Stir at 80℃ under a nitrogen atmosphere for 1.5h to obtain the isocyanate-terminated polycaprolactone precursor.
[0098] In step 1, the molar ratio of polycaprolactone to isophorone diisocyanate is 1:2.28, and the amount of dibutyltin dilaurate added is 1.27% of the total mass of polycaprolactone and isophorone diisocyanate.
[0099] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture; 0.75 g of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide to obtain a polymer solution; the polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h to obtain a long-chain precursor.
[0100] In step S2, the molar ratio of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to polycaprolactone in step S1 is 1:2.
[0101] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine and 10 μL of DBTDL in 1 mL of N,N-dimethylacetamide until fully dissolved. Then add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0102] In step S3, the molar ratio of 2,6-diaminopyridine to polycaprolactone in step S1 is 0.51:1; the amount of catalyst DBTDL added is 0.52% of the total mass of polycaprolactone, isophorone diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine.
[0103] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 0.2g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 6:1. Under nitrogen protection, the coordination reaction is carried out for 24 hours. The resulting solution is then poured into a polytetrafluoroethylene mold and evaporated to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between the flexible segments and the main chain of PDMS. The elastomer has a strength of 22.43 MPa and an elongation at break of 1106%. Figure 4 As shown, the elastic recovery rate is ≥90%, the number of cycles required for cyclic stability is ≤5, and it has good fatigue resistance.
[0104] Example 3 Example 3 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1 g of polypropylene glycol (0.5 mmol) with a weight average molecular weight of 2000 and heat it under vacuum at 100 °C. Stir for 30 min to remove residual moisture. Cool to 80 °C and use a microsyringe to extract 150 μL of toluene-2,4-diisocyanate (2,4-TDI, with a density of 1.220 g / mL and a molecular weight of 174.16, equivalent to 183 mg and 1.05 mmol) and add it dropwise to the reaction vessel. Then, use a microsyringe to extract 15 μL of dibutyltin dilaurate (DBTDL, 16 mg and 0.0253 mmol) and add it dropwise to the reaction vessel. Stir at 80 °C under a nitrogen atmosphere for 1.5 h to obtain the isocyanate-terminated polycaprolactone precursor.
[0105] In step 1, the molar ratio of polycaprolactone to toluene-2,4-diisocyanate is 1:2.1, and the amount of dibutyltin dilaurate added is 1.35% of the total mass of polypropylene glycol and isophorone diisocyanate.
[0106] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture; 0.75 g (equivalent to 0.25 mmol) of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide to obtain a polymer solution; the polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h to obtain a long-chain precursor.
[0107] In step S2, the molar ratio of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to polycaprolactone in step S1 is 1:2.
[0108] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine (0.255 mmol) and 10 μL of DBTDL (10.66 mg, 0.017 mmol) in 1 mL of N,N-dimethylacetamide. After complete dissolution, add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0109] In step S3, the molar ratio of 2,6-diaminopyridine to polycaprolactone in step S1 is 0.51:1; the amount of catalyst DBTDL added is 0.54% of the total mass of polycaprolactone, toluene-2,4-diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine.
[0110] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 0.2g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 6:1. Under nitrogen protection, react for 24 hours. Then, spread the reacted solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain. The elastomer has a strength of 20.96 MPa and an elongation at break of 1215%.
[0111] Comparative Example 1 Comparative Example 1 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1g of polypropylene glycol with a weight average molecular weight of 2000 and heat it under vacuum at 100℃. Stir for 30min to remove residual moisture. Cool to 80℃ and use a microsyringe to extract 240µL of isophorone diisocyanate (IPDI) and add it dropwise to the reaction vessel. Also use a microsyringe to extract 15µL of dibutyltin dilaurate (DBTDL) and add it dropwise to the reaction vessel. Stir at 80℃ under a nitrogen atmosphere for 1.5h to obtain the isocyanate-terminated polycaprolactone precursor.
[0112] Step S2: 0.75 g of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight average molecular weight of 3000 was heated under vacuum at 120 °C and stirred for 30 min to remove residual moisture. The dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide until fully dissolved to obtain a polymer solution. The polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70 °C under a nitrogen atmosphere for 3 h to obtain a long-chain precursor.
[0113] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine and 10 μL of DBTDL in 1 mL of N,N-dimethylacetamide until fully dissolved. Then add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0114] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 0.05g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 1.44:1. Under nitrogen protection, react for 24 hours. Then, spread the reacted solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain. The elastomer has a strength of 14.1 MPa and an elongation at break of 1721%.
[0115] Comparative Example 2 Comparative Example 2 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1g of polypropylene glycol with a weight average molecular weight of 2000 and heat it under vacuum at 100℃. Stir for 30min to remove residual moisture. Cool to 80℃ and use a microsyringe to extract 240µL of isophorone diisocyanate (IPDI) and add it dropwise to the reaction vessel. Also use a microsyringe to extract 15µL of dibutyltin dilaurate (DBTDL) and add it dropwise to the reaction vessel. Stir at 80℃ under a nitrogen atmosphere for 1.5h to obtain the isocyanate-terminated polycaprolactone precursor.
[0116] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight-average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture. 0.75 g of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide until fully dissolved to obtain a polymer solution. The polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h.
[0117] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine and 10 μL of DBTDL in 1 mL of N,N-dimethylacetamide until fully dissolved. Then add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0118] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 1g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 28.8:1. Under nitrogen protection, react for 24 hours. Then, spread the reacted solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain. The elastomer has a strength of 20.88 MPa and an elongation at break of 1164%.
[0119] Comparative Example 3 Comparative Example 3 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1g of polypropylene glycol with a weight average molecular weight of 2000 and heat it under vacuum at 100℃. Stir for 30min to remove residual moisture. Cool to 80℃ and use a microsyringe to extract 240µL of isophorone diisocyanate (IPDI) and add it dropwise to the reaction vessel. Also use a microsyringe to extract 15µL of dibutyltin dilaurate (DBTDL) and add it dropwise to the reaction vessel. Stir at 80℃ under a nitrogen atmosphere for 1.5h to obtain the isocyanate-terminated polycaprolactone precursor.
[0120] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight-average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture. 0.83 g (equivalent to 0.28 mmol) of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide until fully dissolved to obtain a polymer solution. The polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h.
[0121] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine and 10 μL of DBTDL in 1 mL of N,N-dimethylacetamide until fully dissolved. Then add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0122] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 0.2g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 6:1. Under nitrogen protection, react for 24 hours. Then, spread the reacted solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain. The elastomer has a strength of 8.88 MPa and an elongation at break of 1867%.
[0123] Comparative Example 4 Comparative Example 4 provides a fatigue-resistant polyurethane elastomer, the specific preparation method of which is as follows: Step S1: Weigh 1g of polypropylene glycol with a weight average molecular weight of 2000 and heat it under vacuum at 100℃. Stir for 30min to remove residual moisture. Cool to 80℃ and use a microsyringe to extract 240µL of isophorone diisocyanate (IPDI) and add it dropwise to the reaction vessel. Also use a microsyringe to extract 15µL of dibutyltin dilaurate (DBTDL) and add it dropwise to the reaction vessel. Stir at 80℃ under a nitrogen atmosphere for 1.5h to obtain the isocyanate-terminated polycaprolactone precursor.
[0124] Step S2: Bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a weight-average molecular weight of 3000 was heated under vacuum at 120°C and stirred for 30 min to remove residual moisture. 0.68 g (equivalent to 0.227 mmol) of the dehydrated bis(3-aminopropyl)-terminated poly(dimethylsiloxane) was dissolved in 0.5 mL of N,N-dimethylacetamide until fully dissolved to obtain a polymer solution. The polymer solution was added dropwise to the product obtained in step S1, and the reaction was carried out at 70°C under a nitrogen atmosphere for 3 h.
[0125] Step S3: Dissolve 0.0278 g of 2,6-diaminopyridine and 10 μL of DBTDL in 1 mL of N,N-dimethylacetamide until fully dissolved. Then add the long-chain precursor obtained in step S2 dropwise. React at 70 °C under a nitrogen atmosphere for 24 h to obtain a viscous liquid. Wash and precipitate the liquid with methanol to obtain a hydrogen-bonded polyurethane elastomer.
[0126] Step S4: Dissolve 1.5g of hydrogen-bonded polyurethane elastomer in tetrahydrofuran, and then dissolve 0.2g of ZnCl2 in methanol. The molar ratio of zinc salt to 2,6-diaminopyridine is approximately 6:1. Under nitrogen protection, react for 24 hours. Then, spread the reacted solution into a polytetrafluoroethylene mold and evaporate the solution to obtain a fatigue-resistant polyurethane elastomer with synergistic coordination between PDMS flexible segments and the main chain. The elastomer has a strength of 13.56 MPa and an elongation at break of 1480%.
[0127] The raw material composition of Examples 1-Comparative Examples 4 is shown in Table 1. Tensile properties, cyclic tensile tests and elastic recovery rate tests were performed on each example to examine its fatigue resistance. The performance of each example is shown in Table 2.
[0128] Tensile property testing: An Instron 5943 universal testing machine was used. The elastomer samples obtained in the examples and preparation examples were cut into dumbbell-shaped specimens (50 mm in length, 4 mm in width of the narrow section, and 0.3 ± 0.02 mm in thickness). The tensile rate was set to 20 mm / min. At least five parallel specimens were tested for each group of samples, and the average value was taken. The stress-strain curves were recorded to obtain the tensile strength (MPa) and elongation at break (%). The stress-strain curves for each example are shown below. Figure 2 As shown.
[0129] Cyclic tensile and elastic recovery rate test: Using the same equipment as described above, a cyclic tensile test was conducted at 200% strain. The specimen size was the same as above, and the tensile rate was 20 mm / min. After stretching the specimen from 0% to 200% strain, it was unloaded at the same rate until the stress returned to zero, completing one cycle.
[0130] Table 1 Table 2 This invention achieves precise control over the micro-crosslinking network and macroscopic mechanical properties of polyurethane elastomers by adjusting the type of soft segment matrix, the rigid structure of diisocyanate, the density of metal coordination crosslinking, and the content of flexible organosilicon segments. The specific analysis of the performance differences among the various embodiments is as follows: (1) The effect of soft segment matrix type on performance (Example 1, Example 2) Data from cyclic tensile tests at 200% strain in Examples 1 and 2 are as follows: Figure 3 and Figure 4 As shown. Example 1 uses polypropylene glycol (PPG) polyether soft segments. The main molecular chain is dominated by flexible ether bonds, resulting in low steric hindrance and excellent flexibility. Under external force, it can achieve a wide range of slippage and relaxation, thus achieving an elongation at break of up to 1692%, an elastic recovery rate of over 90%, and cyclic stability of ≤5 cycles, exhibiting excellent fatigue resistance. However, the intermolecular forces of the polyether structure are relatively weak, limiting physical aggregation and rigid support capabilities, with a tensile strength of 16.88 MPa. Example 2 uses polycaprolactone (PCL) polyester soft segments. The molecular chain contains polar ester groups, significantly enhancing intermolecular forces and improving chain segment rigidity. The hard segment phase has a higher degree of aggregation, effectively improving the material's load-bearing capacity, with a tensile strength increased to 22.43 MPa. However, the polar ester groups restrict chain segment movement, limiting the stretching and slippage of the polymer chain, thus reducing the elongation at break to 1106%. Both matrix formulations possess high elastic recovery and rapid cyclic stability.
[0131] (2) The effect of the rigid structure of diisocyanate on performance (Example 1, Example 3) Compared to alicyclic IPDI, aromatic toluene diisocyanate contains a rigid benzene ring conjugated structure, resulting in a more densely packed polyurethane hard segment structure with higher structural stiffness. In Example 3, 2,4-TDI was used instead of IPDI, which significantly improved the rigidity of the hard segments, with a tensile strength reaching 20.96 MPa. However, the benzene ring structure restricted the compliant movement of the chain segments, leading to a decrease in material toughness and a reduction in elongation at break to 1215%. At the same time, the rigid hard segments resulted in a slight decrease in dynamic recovery capability, with an elastic recovery rate ≥88% and a cycle stability of ≤7 cycles.
[0132] (3) Regulation of performance by zinc ion coordination crosslinking density (Example 1, Comparative Example 1, Comparative Example 2) Zn 2+ It can form dynamic metal coordination bonds with nitrogen atoms of 2,6-diaminopyridine heterocyclic rings, and synergistically form a reversible cross-linking network with inter-chain hydrogen bonds. The cross-linking density directly determines the material's stiffness, toughness, and fatigue resistance. Compared to Example 1, Comparative Example 1 is a low-zinc salt doped system. The system has fewer metal coordination cross-linking sites, weaker cross-linking network binding effect, and higher degree of freedom of polymer chain movement. During stretching, the chain segments can fully slide and relax, dissipating stress, thus increasing the elongation at break to 1721%. However, insufficient cross-linking density leads to decreased structural stability, with tensile strength decreasing to 14.10 MPa. At the same time, the compactness of the dynamic reversible network deteriorates, the elastic recovery rate decreases to ≥85%, and the number of cycles increases to ≤10.
[0133] Compared to Example 1, Comparative Example 2 is a high-zinc salt doped system with a significant increase in coordination crosslinking sites and a marked improvement in the density of the crosslinking network. This effectively constrains molecular chain deformation and enhances the structural load-bearing capacity, achieving a tensile strength of up to 20.88 MPa. However, the excessively high crosslinking density severely restricts the relaxation and slippage capabilities of the polymer chains, making the material prone to stress concentration under stress. The chain segments break before they are fully extended, resulting in a decrease in the elongation at break to 1164%. At the same time, excessive metal coordination crosslinking reduces the dynamic reversibility of the network, decreasing the elastic recovery rate to ≥80%, increasing the number of cycles to ≤15, and significantly deteriorating fatigue stability.
[0134] (4) Effect of PDMS flexible siloxane segment content on performance (Example 1, Comparative Example 3, Comparative Example 4) PDMS, an ultra-low modulus flexible segment, can significantly improve the chain flexibility of polyurethane systems and is a core soft segment component for controlling the toughness and elasticity of materials. Compared with Example 1, Comparative Example 3 has a higher PDMS content, significantly increasing the proportion of flexible soft segments in the system and significantly enhancing the overall relaxation ability of the polymer chain. During stretching, external forces can be continuously dissipated through chain segment friction and slippage, resulting in the highest elongation at break of 1867% among all groups. However, the intermolecular forces of the flexible siloxane segments are weak, and the rigid support is poor, reducing the proportion of the effective load-bearing structure in the system and causing the tensile strength to drop significantly to 8.88 MPa.
[0135] Compared to Example 1, the PDMS content in Comparative Example 4 was too low, resulting in insufficient supply of flexible soft segments and an excessively high proportion of rigid hard segments. This led to decreased flexibility and insufficient toughness of the polymer chains, making it impossible to adequately buffer stress through the slippage of flexible chain segments. Consequently, the elongation at break dropped to 1480%, and the rigid network was prone to local stress defects. The tensile strength also decreased to 13.56 MPa, resulting in a deterioration in the overall mechanical properties of the material. This demonstrates the crucial role of appropriate PDMS content in balancing strength and toughness.
[0136] The test results above show that the polyurethane elastomer obtained in this invention has a high cycle stability and elastic recovery rate, indicating that it can maintain a relatively stable network structure under repeated loading and is not prone to significant structural relaxation or irreversible damage due to repeated deformation. This is because the flexible PDMS segments can buffer local stress through segment extension and retraction during the stress process, reducing the continuous damage of stress concentration to the polymer network. Simultaneously, due to the long polymer chains generated in the reaction and their microscopic phase separation, when subjected to external force, energy can be dissipated not only through rapid bond breakage and recombination but also through friction between chains and between phases. These multiple dissipation channels make the polymer network skeleton less susceptible to damage. Furthermore, Zn... 2+The dynamic coordination interactions formed with the coordinating groups can stabilize the polymer network as much as possible after it is disturbed, protecting the network. Even if the coordination bonds are broken, they can quickly re-establish connections because they are non-covalent, thus stabilizing and restoring the network structure. Multiple synergistic interactions enable the formation of a network within the material that combines flexible adjustment capabilities with structural stability. During repeated loading-unloading cycles, this network better maintains its integrity, reducing the gradual accumulation of residual deformation and damage, thereby delaying fatigue damage and the initiation and propagation of microcracks. Consequently, the material's cyclic stability and elastic recovery rate are improved, ultimately resulting in better fatigue resistance.
[0137] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a fatigue-resistant polyurethane elastomer, characterized in that, Includes the following steps: S1. Polyol and diisocyanate are reacted under the conditions of catalyst, inert atmosphere and heating to obtain isocyanate-terminated precursor; S2. Dissolve bis(3-aminopropyl)-terminated poly(dimethylsiloxane) in a first organic solvent to obtain a polymer solution. Then add the polymer solution to the isocyanate-terminated precursor obtained in step S1 and react under an inert atmosphere and heating conditions to obtain a long-chain precursor. S3. Dissolve 2,6-diaminopyridine and the catalyst in a second organic solvent to obtain a chain extender solution; then add the chain extender solution to the long-chain precursor obtained in step S2, and react under an inert atmosphere and heating conditions. After the reaction is completed, wash and settle to obtain a polyurethane elastomer intermediate product. S4. Dissolve the polyurethane elastomer intermediate obtained in step S3 and the zinc salt in an organic solvent, wherein the molar ratio of the zinc salt to 2,6-diaminopyridine is 3 to 8:1; carry out a coordination reaction under an inert atmosphere, and remove the solvent after the reaction is completed to obtain the fatigue-resistant polyurethane elastomer.
2. The method for preparing an anti-fatigue polyurethane elastomer according to claim 1, characterized in that, In step S1, the polyol is any one of polypropylene glycol or polycaprolactone, and the weight-average molecular weight of the polyol is 1500-2500; the diisocyanate is any one of isophorone diisocyanate, toluene-2,3-diisocyanate, toluene-2,4-diisocyanate, and toluene-2,5-diisocyanate; and the catalyst is dibutyltin dilaurate.
3. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S1, the molar ratio of the polyol to the diisocyanate is 1:1.8 to 2.5; the amount of catalyst added is 0.01% to 2% of the total mass of the polyol and diisocyanate; the heating temperature is 70-100℃, and the reaction time is 1-3 hours.
4. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S2, the weight-average molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 2000-5000, and the first organic solvent is any one of dichloromethane, trichloromethane, tetrahydrofuran, or N,N-dimethylacetamide; the molar ratio of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to the polyol in step S1 is 1:2-2.2; the heating temperature is 70-100℃, and the reaction time is 3-5 hours.
5. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S3, the catalyst is dibutyltin dilaurate; the second organic solvent is any one of dichloromethane, chloroform, tetrahydrofuran, or N,N-dimethylacetamide.
6. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S3, the molar ratio of 2,6-diaminopyridine to the polyol is 0.5-1.5:1; the amount of catalyst added is 0.01%-2% of the total mass of the polyol, diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and 2,6-diaminopyridine; the heating temperature is 70-100℃, and the reaction time is 1-2 days.
7. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S4, the zinc salt is any one of zinc chloride, zinc perchlorate, or zinc trifluoromethanesulfonate; the mass ratio of the polyurethane elastomer intermediate to the zinc salt is 1:0.03-0.7, and the coordination reaction takes 1-2 days.
8. The method for preparing a fatigue-resistant polyurethane elastomer according to claim 1, characterized in that, In step S1, the structural formula of the isocyanate-terminated precursor is as follows: ; In step S2, the structural formula of the long-chain precursor is as follows: ; In step S3, the structural formula of the polyurethane elastomer intermediate product is as follows: ; In the above structural formula, the value of m ranges from 30 to 45, the value of n ranges from 20 to 40, and the value of a ranges from 7 to 10; the weight-average molecular weight of the polyurethane elastomer intermediate product is 45,000-70,000, and the molecular weight distribution is 1.4-1.
6.
9. A fatigue-resistant polyurethane elastomer prepared by the method according to any one of claims 1-8, characterized in that, The fatigue-resistant polyurethane elastomer is prepared using a stepwise construction method: first, a polyurethane backbone is formed by reacting a polyol with a diisocyanate; then, bis(3-aminopropyl)-terminated polydimethylsiloxane is covalently embedded into the polyurethane backbone by reacting its terminal amino groups with the isocyanate groups on the backbone; next, 2,6-diaminopyridine is covalently embedded into the backbone through a chain extension reaction; finally, Zn... 2+ Coordination was performed to obtain the fatigue-resistant polyurethane elastomer; The structural formula of the fatigue-resistant polyurethane elastomer is as follows: ; Where m ranges from 30 to 45, n ranges from 20 to 40, and a ranges from 7 to 10.
10. The application of the fatigue-resistant polyurethane elastomer according to claim 9 in flexible wearable devices.