A copolymer of glycolide and lactide, its preparation method and application
By adjusting the polymerization rates of glycolide and lactide, a uniform distribution of lactide units within glycolide units was achieved, solving the problem of inconsistent degradation rates of PGLA and expanding its application in the pharmaceutical field.
Patent Information
- Application Number
- CN202510596185.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-10
AI Technical Summary
In existing PGLA block polymers, lactide and glycolide units are mostly present in the form of small blocks, resulting in poor consistency in degradation rate and limiting their application in the pharmaceutical field.
By adjusting the polymerization rate of glycolide and lactide through compound catalysts, a uniform distribution of lactide units in glycolide units can be achieved, and the polymer sequence structure can be adjusted to change its degradation time.
The prepared glycolide-lactide copolymer has a longer degradation time, expanding its application range in the pharmaceutical field.
Smart Images

Figure BDA0005394650220000071
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyester, and more specifically, to a glycolide-lactide copolymer, its preparation method, and its application. Background Technology
[0002] Poly(glycolic acid-co-lactic) (PGLA) combines the advantages of both PGA and PLA polyester materials. It is a semi-crystalline / amorphous biodegradable functional polymer that has been certified by the U.S. Food and Drug Administration (FDA) and officially included in the United States Pharmacopeia as a pharmaceutical excipient. PGLA exhibits good biocompatibility, is non-toxic, and possesses excellent encapsulation and film-forming properties, making it widely used in pharmaceuticals, medical engineering materials, and modern industrial fields.
[0003] Currently, PGLA is mostly prepared using ring-opening polymerization, which involves dehydrating and cyclizing glycolic acid and lactic acid separately to synthesize glycolide (GA) and lactide (LA) monomers, and then using LA and GA for ring-opening polymerization to prepare PGLA. Compared with polycondensation, this method has milder reaction conditions, no by-product small molecules are generated, the obtained polymer product has high purity, and the molecular weight is controllable. It is more suitable for controlling the monomer sequence in copolymers and regulating polymer chain ends.
[0004] Currently, commonly used polymerization processes include one-pot polymerization (e.g., patent CN219400134U) and batch feeding polymerization (e.g., patent US11058792B2). The resulting PGLA block or multiblock copolymers have a limited degradation rate due to the fact that the lactide and glycolide units are mostly in the form of small blocks, thus restricting their application in the pharmaceutical field.
[0005] Therefore, it is necessary to develop a special structure of PGLA with different degradation rates, so that the block units in PGLA are more dispersed and the lactide units can be more uniformly distributed in the glycolide units, thereby improving its degradation rate. Summary of the Invention
[0006] To address the technical problems existing in the prior art, the present invention provides a glycolide-lactide copolymer, its preparation method, and its application.
[0007] Through in-depth research, the inventors discovered that in the aforementioned PGLA block polymers, both lactide and glycolide units exist primarily in small block form, and the differences in this polymer sequence structure significantly influence the degradation rate. In the pharmaceutical field, different treatment regimens require PGLA with varying degradation rates. The aforementioned block polymers limit the application range of PGLA, necessitating the development of a glycolide-lactide copolymer with a special structure, in which lactide units can be more uniformly distributed within the glycolide units, thereby resulting in a longer degradation time.
[0008] Through further research, the inventors discovered that the aforementioned technical problem may be due to the uneven distribution of lactide units within glycolide units. This problem can be effectively solved by using a special glycolide-lactide polymer where lactide structural units are uniformly distributed within glycolide units. This invention provides a method for preparing this special glycolide-lactide polymer with uniformly distributed lactide structural units within glycolide units. Specifically, it involves adjusting the polymerization reactivity ratios of glycolide and lactide to obtain the special glycolide-lactide polymer. Since the polymerization rates of lactide and glycolide differ significantly, it is difficult to achieve a near-alternating copolymerization effect. This invention adjusts the polymerization rates of glycolide and lactide by using a compound catalyst, thereby accelerating the polymerization rate of lactide and slowing down the polymerization rate of glycolide, achieving regulation and preventing localized block homopolymerization of lactide. This adjusts the polymer sequence structure, thereby altering its degradation time and other properties, expanding the application areas of PGLA materials.
[0009] One objective of this invention is to provide a glycolide-lactide copolymer comprising glycolide units and lactide units, wherein the number of lactide units connected to the glycolide units accounts for 50% to 100% of the total number of lactide units. For example, the ratio can be 50%, 60%, 70%, 80%, 90%, 100%, or any two of the above ratios, such as 70% to 100%.
[0010] In a preferred embodiment of the present invention,
[0011] The intrinsic viscosity of the glycolide-lactide copolymer is 0.2–3.0 dL / g; and / or,
[0012] The weight-average molecular weight of the glycolide-lactide copolymer is 5w to 40w, preferably 10w to 35w; and / or,
[0013] The yellowness value of the glycolide-lactide copolymer is 30-60, preferably 30-45; and / or,
[0014] The residual monomers in the glycolide-lactide copolymer are less than 5 wt%, preferably less than 2 wt%, and more preferably less than 1.7 wt%; the residual monomers are glycolide monomers and lactide monomers.
[0015] A second objective of this invention is to provide a method for preparing a glycolide-lactide copolymer, comprising the following steps:
[0016] (1) The monomer, initiator and catalyst are mixed and reacted in a first reactor to obtain mixture A; the monomer is glycolide monomer and lactide monomer;
[0017] (2) The mixture A obtained in step (1) is continuously fed into the second reactor to react and obtain mixture B;
[0018] (3) The mixture B obtained in step (2) is continuously transferred to a plug flow reactor for reaction to obtain mixture C. After removing the residual monomer, the glycolide-lactide copolymer is obtained.
[0019] Preferably,
[0020] The lactide monomer is L-lactide monomer; and / or,
[0021] The method for preparing the glycolide-lactide copolymer is used to prepare the above-mentioned glycolide-lactide copolymer; and / or,
[0022] The first reactor and the second reactor are each independently selected from at least one of a batch reactor, a continuous stirred tank reactor, and an SCP self-cleaning reactor.
[0023] In a preferred embodiment of the present invention,
[0024] Step (1),
[0025] The water content of the glycolide monomer is 50–1000 ppm, and the acid value is 1–100 mol / t; the water content of the glycolide monomer can be 50 ppm, 100 ppm, 300 ppm, 500 ppm, 800 ppm, 1000 ppm, or any two of the above values, such as 50–300 ppm; the acid value of the glycolide monomer can be 1 mol / t, 3 mol / t, 5 mol / t, 10 mol / t, 30 mol / t, 50 mol / t, 80 mol / t, 100 mol / t, or any two of the above values, such as 1–3 mol / t; and / or,
[0026] The lactide monomer has a water content of 50–1000 ppm and an acid value of 1–100 mol / t; the water content of the lactide monomer can be 50 ppm, 100 ppm, 300 ppm, 500 ppm, 800 ppm, 1000 ppm, or any two of the above values, such as 50–300 ppm; the acid value of the lactide monomer can be 1 mol / t, 3 mol / t, 5 mol / t, 10 mol / t, 30 mol / t, 50 mol / t, 80 mol / t, 100 mol / t, or any two of the above values, such as 1–3 mol / t; and / or,
[0027] The initiator is at least one of an alkyl alcohol and water; the alkyl alcohol is preferably at least one of decanol, decanediol, lauryl alcohol, and tetradecyl alcohol; and / or,
[0028] The catalyst is a composite catalyst of catalyst D and catalyst E, wherein catalyst D is a metal catalyst, preferably at least one of stannous chloride, stannous octoate, and stannous chloride; and / or, catalyst E is a pyridine catalyst, preferably at least one of 4-dimethylaminopyridine (DMAP) and 4-pyrrolidinylpyridine (4-PPY).
[0029] In a preferred embodiment of the present invention,
[0030] Step (1),
[0031] The glycolide monomer accounts for 5-95% of the total molar percentage of the monomers, preferably 20-95%; and / or,
[0032] The lactide monomer accounts for 5-95% of the total molar percentage of the monomers, preferably 5-80%; and / or,
[0033] The molar ratio of the initiator to the total monomer is 1:(10-5000), preferably 1:(300-2000), more preferably 1:(500-2000); and / or,
[0034] The catalyst has a mass of 0–5000 ppm of the total monomer mass, preferably 30–1000 ppm, more preferably 50–600 ppm; and / or,
[0035] The catalyst D accounts for 5-95% of the total mass of the catalyst, preferably 30-70%.
[0036] In a preferred embodiment of the present invention,
[0037] Step (1),
[0038] The first reactor comprises at least two reactors connected in parallel, which can be used alternately to continuously feed the second reactor; and / or,
[0039] The mixing is carried out under a protective gas atmosphere, wherein the protective gas is at least one selected from nitrogen and an inert gas; and / or,
[0040] The mixing temperature in the first reactor is 125–150°C, preferably 125–140°C; and / or,
[0041] The reaction time in the first reactor is 5 to 30 minutes, preferably 10 to 30 minutes.
[0042] In a preferred embodiment of the present invention,
[0043] The monomer conversion rate of glycolide in mixture A is greater than or equal to 40%;
[0044] The monomer conversion rate of lactide in mixture A is greater than or equal to 10%.
[0045] In a preferred embodiment of the present invention,
[0046] Step (2),
[0047] The reaction temperature of mixture A in the second reactor is 185–210°C, preferably 185–200°C; and / or,
[0048] The reaction time of mixture A in the second reactor is 10 to 60 minutes, preferably 15 to 50 minutes.
[0049] In a preferred embodiment of the present invention,
[0050] The monomer conversion rate of glycolide in mixture B is greater than or equal to 70%;
[0051] The monomer conversion rate of lactide in mixture B is greater than or equal to 50%.
[0052] In a preferred embodiment of the present invention,
[0053] Step (3),
[0054] The reaction temperature of mixture B in the plug flow reactor is 190–210°C, preferably 200–210°C; and / or,
[0055] The reaction time of mixture B in the plug flow reactor is 20–60 min, preferably 30–50 min; and / or,
[0056] The plug flow reactor is a screw extruder or a tubular reactor; and / or
[0057] The method for removing residual monomers is melt devolatilization; the melt devolatilization preferably uses a devolatilization screw, and the devolatilization temperature is more preferably 200-230°C, and most preferably 210-220°C.
[0058] In a preferred embodiment of the present invention,
[0059] The monomer conversion rate of glycolide in mixture C is greater than or equal to 90%;
[0060] The monomer conversion rate of lactide in mixture C is greater than or equal to 60%.
[0061] The third objective of this invention is to provide a glycolide-lactide copolymer obtained by the above preparation method; preferably,
[0062] In the aforementioned glycolide-lactide copolymer, the proportion of lactide units linked to glycolide units to all lactide units is 50%–100%, for example, the proportion can be 50%, 60%, 70%, 80%, 90%, 100%, or any two of the above proportions, such as 70%–100%; and / or,
[0063] The intrinsic viscosity of the glycolide-lactide copolymer is 0.2–3.0 dl / g; and / or,
[0064] The weight-average molecular weight of the glycolide-lactide copolymer is 5w to 40w, preferably 10w to 35w; and / or,
[0065] The yellowness value of the glycolide-lactide copolymer is 30-60, preferably 30-45; and / or,
[0066] The residual monomers in the glycolide-lactide copolymer are less than 5 wt%, preferably less than 2 wt%, and more preferably less than 1.7 wt%; the residual monomers are glycolide monomers and lactide monomers.
[0067] The fourth objective of this invention is to provide an application of glycolide-lactide copolymer in the pharmaceutical field, preferably in drug-loaded microspheres.
[0068] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0069] This invention develops a special glycolide-lactide copolymer, which can adjust the polymerization rate of glycolide and lactide by compounding catalysts, avoid local block homopolymerization of lactide, adjust the polymer sequence structure, and thus change its degradation time and other properties, thereby expanding the application fields of PGLA materials.
[0070] The aliphatic polyester prepared by this invention has an intrinsic viscosity of 0.2-3.0 dl / g, a weight-average molecular weight of 5w-40w, a yellowness value of 30-60, a residual monomer content of less than 5wt%, and a ratio of lactide units connected to glycolide units to all lactide units of 50-100%. Detailed Implementation
[0071] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0072] All raw materials used in the examples are commercially available.
[0073] Test method:
[0074] Determination of molecular weight and its distribution:
[0075] An Agilent PL50 gel permeation chromatography (GPC) system was used. PGLA samples were dissolved in a hexafluoroisopropanol solution containing 5 mM sodium trifluoroacetate. The column temperature was set at 40 °C; the eluent was hexafluoroisopropanol solution containing 5 mM sodium trifluoroacetate; the flow rate was set at 1 mL / min; and relative molecular mass correction was performed using five different standard polymethyl methacrylates to obtain the weight-average molecular weight (Mw).
[0076] Determination of intrinsic viscosity ([η]):
[0077] Using hexafluoroisopropanol as solvent, the outflow time t of the pure solvent and the sample solution was measured using an Ubbelohde viscometer in a constant temperature water bath at 25°C. o t and t are obtained using the "one-point method" formula.
[0078]
[0079] Analysis of residual monomers:
[0080] An Agilent 7890B gas chromatograph with a DB-FFAP column was used. The initial column temperature was 160℃, with a programmed temperature increase, a column flow rate of 1 mL / min, a split ratio of 20:1, and an injection port temperature of 300℃. An FID detector with a detector temperature of 300℃ was used. The PGLA sample was mixed with dimethyl sulfoxide and heated to 140℃ to dissolve. After cooling to room temperature, the supernatant was collected by centrifugation and placed in a sample vial for testing of residual monomers.
[0081] Measurement of yellowness value:
[0082] The yellowness index was measured using a Hunter Lab Scan XE yellowness index instrument from the United States. Polyglycolic acid particles were poured into a cylindrical container made of quartz glass and the yellowness value was measured by reflection method.
[0083] NMR 13C carbon spectroscopy determination:
[0084] Nuclear magnetic resonance (NMR) experiments were performed at JEOL 500 MHz with a magnetic field strength of 11.74 T. The 90° pulse width was 11.88 μs, the waiting time was 2 s, and the number of scans was 5100. 35 mg of sample was added to 0.6 mL of deuterated DMSO, and the temperature was gradually increased to 140 h. After stirring for 4–5 h until completely dissolved, carbon NMR was obtained at 120 °C for 4 h. Two characteristic peaks of lactide were observed between 169 ppm and 170 ppm: the characteristic peak of the lactide unit connected to the lactide unit was at 169.33 ppm, and the characteristic peak of the lactide unit connected to the glycolide unit was at 169.50 ppm.
[0085] In vitro degradation experiment:
[0086] The sample was prepared into particles with a diameter between 2 and 4 micrometers using the standard emulsion method. The sample was then immersed in a phosphate buffer solution with a pH of 7.4 at 37°C for 14 days, and the change in molecular weight was measured.
[0087] Example 1
[0088] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 50 ppm water content, 1 mol / t acid value), 1.21 kg (8.4 mol) of lactide (10% molar percentage, 50 ppm water content, 1 mol / t acid value), 31.3 g (0.168 mol) of lauryl alcohol (molar ratio to monomer 1:500), 0.5 g of stannous octoate (50 ppm), and 0.5 g of DMAP (50 ppm) were added to the first reaction vessel under a dry nitrogen atmosphere. The first reaction vessel was a batch reactor with a temperature of 130°C, containing two reactors connected in parallel, which could be used alternately to continuously feed the second reactor. After reacting in the first reactor for 15 minutes, the material was transferred to the second reactor, a batch reactor, at 190℃ for 30 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200℃ for 30 minutes. After polymerization, the material was transferred to a devolatilization screw at 210℃ for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 1.53 dl / g, a weight-average molecular weight of 18.74 w, a yellowness value of 40, and 1.52 wt% residual monomer. The polymer contained 74% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 40%.
[0089] Example 2
[0090] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 50 ppm water content, 1 mol / t acid value), 1.21 kg (8.4 mol) of lactide (10% molar percentage, 50 ppm water content, 1 mol / t acid value), 18.0 g (0.084 mol) of tetradecanol (molar ratio to monomer 1:1000), 0.5 g of stannous octoate (50 ppm), and 0.5 g of DMAP (50 ppm) were added to the first reaction vessel under a dry nitrogen atmosphere. The first reaction vessel was a batch reactor with a temperature of 130°C, containing two reactors connected in parallel, which could be used alternately to continuously feed the second reactor. After reacting in the first reactor for 15 minutes, the material was transferred to the second reactor, a batch reactor, at 190℃ for 30 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200℃ for 30 minutes. After polymerization, the material was transferred to a devolatilization screw at 210℃ for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 1.90 dl / g, a weight-average molecular weight of 25.73 w, a yellowness value of 40, and 1.47 wt% residual monomer. The polymer contained 72% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 37%.
[0091] Example 3
[0092] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 50 ppm water content, 1 mol / t acid value) and 1.21 kg (8.4 mol) of lactide (10% molar percentage, 50 ppm water content, 1 mol / t acid value), 6.7 g (0.042 mol) of decanol (molar ratio to monomer 1:2000), 0.5 g of stannous octoate (50 ppm), 0.5 g DMAP (50 ppm) was introduced into the first reactor (a batch reactor) under a dry nitrogen atmosphere at 130°C. The first reactor consisted of two parallel reactors that could be used alternately to continuously feed the second reactor. After reacting in the first reactor for 15 minutes, the material was transferred to the second reactor (a batch reactor) at 190°C for 30 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200°C for 30 minutes. After polymerization, the material was transferred to a devolatilization screw at 210°C for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 2.8 dl / g, a weight-average molecular weight of 32.12 w, a yellowness value of 43, and 1.58 wt% residual monomer. The polymer contained 72% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 31%.
[0093] Example 4
[0094] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 50 ppm water content, 1 mol / t acid value), 1.21 kg (8.4 mol) of lactide (10% molar percentage, 50 ppm water content, 1 mol / t acid value), 31.3 g (0.168 mol) of lauryl alcohol (molar ratio to monomer 1:500), 2.1 g of stannous chloride (210 ppm), and 0.9 g of DMAP (90 ppm) were added to the first reaction vessel under a dry nitrogen atmosphere. The first reaction vessel was a batch reactor with a temperature of 130°C, containing two reactors connected in parallel, which could be used alternately to continuously feed the second reactor. After reacting in the first reactor for 15 minutes, the material was transferred to the second reactor, a batch reactor, at 190℃ for 30 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200℃ for 30 minutes. After polymerization, the material was transferred to a devolatilization screw at 210℃ for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 1.57 dl / g, a weight-average molecular weight of 19.71 w, a yellowness value of 42, and 1.61 wt% residual monomer. The polymer contained 71% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 39%.
[0095] Example 5
[0096] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 50 ppm water content, 1 mol / t acid value), 1.21 kg (8.4 mol) of lactide (10% molar percentage, 50 ppm water content, 1 mol / t acid value), 31.3 g (0.168 mol) of lauryl alcohol (molar ratio to monomer 1:500), 3.0 g of stannous octoate (300 ppm), and 3.0 g of 4-PPY (300 ppm) were added to the first reaction vessel under a dry nitrogen atmosphere. The first reaction vessel was a batch reactor with a temperature of 130°C, containing two parallel reactors that could be used alternately to continuously feed the second reaction vessel. After reacting in the first reactor for 15 minutes, the material was transferred to the second reactor, a batch reactor, at 190°C for 10 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200°C for 50 minutes. After polymerization, the material was transferred to a devolatilization screw at 210°C for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 1.55 dl / g, a weight-average molecular weight of 18.86 w, a yellowness value of 43, and 1.48 wt% residual monomer. The polymer contained 73% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 42%.
[0097] Example 6
[0098] 8.79 kg (75.7 mol) of glycolide (90% molar percentage, 300 ppm water content, 3 mol / t acid value), 1.21 kg (8.4 mol) of lactide (10% molar percentage, 300 ppm water content, 3 mol / t acid value), 31.3 g (0.168 mol) of lauryl alcohol (molar ratio to monomer 1:500), 0.5 g of stannous octoate (50 ppm), and 0.5 g of DMAP (50 ppm) were added to the first reaction vessel under a dry nitrogen atmosphere. The first reaction vessel was a batch reactor, with a temperature of 130°C, containing two reactors connected in parallel, which could be used alternately to continuously feed the second reaction vessel. In the first reactor, after reacting for 15 minutes, the material was transferred to a second reactor (a batch reactor) at 190°C for 30 minutes. Subsequently, the material was continuously transferred to a screw extruder at 200°C for 30 minutes. After polymerization, the material was transferred to a devolatilization screw at 210°C for extrusion and pelletizing. The resulting product had an intrinsic viscosity of 0.87 dl / g, a weight-average molecular weight of 10.25 w, a yellowness value of 41, and 1.52 wt% residual monomer. The polymer contained 75% lactide units linked to glycolide units. After 14 days of in vitro degradation, the molecular weight decreased by 54%.
[0099] Comparative Example 1
[0100] The difference from Example 1 is that DMAP was not added to the catalyst, but 1.0 g of stannous octoate (100 ppm) was added instead;
[0101] Except for the differences mentioned above, all other conditions in Comparative Example 1 were the same as in Example 1, resulting in a glycolide-lactide copolymer.
[0102] The obtained glycolide-lactide copolymer had an intrinsic viscosity of 1.51 dl / g, a weight-average molecular weight of 18.52 w, a yellowness value of 41, and 1.48 wt% residual monomer. The number of lactide units linked to glycolide units accounted for 50% of all lactide units in the obtained polymer, and the molecular weight decreased by 60% after 14 days of in vitro degradation.
[0103] Compared to Example 1, in the glycolide-lactide copolymer prepared in Comparative Example 1, the proportion of lactide units connected to glycolide units accounted for 50% of the total number of lactide units, while in Example 1 it was 74%. After 14 days of in vitro degradation, the molecular weight reduction was 1.5 times that of Example 1. This demonstrates that Example 1, by adjusting the polymerization rate of glycolide and lactide through a compound catalyst, avoided local block homopolymerization of lactide, thus resulting in a longer degradation time.
[0104] The glycolide-lactide copolymers prepared in Examples 1-6, by adjusting the polymerization rates of glycolide and lactide using a compound catalyst, avoided local block homopolymerization of lactide, and ensured that the number of lactide units connected to glycolide units accounted for more than 70% of the total number of lactide units. After 14 days of in vitro degradation, the molecular weight decreased to 31-54%, indicating a relatively long degradation time.
Claims
1. A glycolide-lactide copolymer, comprising glycolide units and lactide units, wherein the number of lactide units connected to the glycolide units accounts for 50-100% of the total number of lactide units.
2. The glycolide-lactide copolymer as described in claim 1, characterized in that: The intrinsic viscosity of the glycolide-lactide copolymer is 0.2–3.0 dL / g; and / or, The weight-average molecular weight of the glycolide-lactide copolymer is 5w to 40w, preferably 10w to 35w; and / or, The yellowness value of the glycolide-lactide copolymer is 30-60, preferably 30-45; and / or, The residual monomers in the glycolide-lactide copolymer are less than 5 wt%, preferably less than 2 wt%, and more preferably less than 1.7 wt%; the residual monomers are glycolide monomers and lactide monomers.
3. A method for preparing a glycolide-lactide copolymer, comprising the following steps: (1) The monomer, initiator and catalyst are mixed and reacted in a first reactor to obtain mixture A; the monomer is glycolide monomer and lactide monomer; (2) The mixture A obtained in step (1) is continuously fed into the second reactor to react and obtain mixture B; (3) The mixture B obtained in step (2) is continuously transferred to a plug flow reactor for reaction to obtain mixture C. After removing the residual monomer, the glycolide-lactide copolymer is obtained. Preferably, The method for preparing the glycolide-lactide copolymer is used to prepare the glycolide-lactide copolymer according to claim 1 or 2; and / or, The first reactor and the second reactor are each independently selected from at least one of a batch reactor, a continuous stirred tank reactor, and an SCP self-cleaning reactor.
4. The method for preparing the glycolide-lactide copolymer as described in claim 3, characterized in that: Step (1), The glycolide monomer has a water content of 50–1000 ppm and an acid value of 1–100 mol / t; and / or, The lactide monomer has a water content of 50–1000 ppm and an acid value of 1–100 mol / t; and / or, The initiator is at least one of an alkyl alcohol and water; the alkyl alcohol is preferably at least one of decanol, decanediol, lauryl alcohol, and tetradecane alcohol; and / or, The catalyst is a composite catalyst of catalyst D and catalyst E, wherein catalyst D is a metal catalyst, preferably at least one of stannous chloride, stannous octoate, and stannous chloride; and / or, catalyst E is a pyridine catalyst, preferably at least one of 4-dimethylaminopyridine and 4-pyrrolidinylpyridine.
5. The method for preparing the glycolide-lactide copolymer as described in claim 3, characterized in that: Step (1), The glycolide monomer accounts for 5-95% of the total molar percentage of the monomers, preferably 20-95%; and / or, The lactide monomer accounts for 5-95% of the total molar percentage of the monomers, preferably 5-80%; and / or, The molar ratio of the initiator to the total monomer is 1:(10-5000), preferably 1:(300-2000), more preferably 1:(500-2000); and / or, The catalyst has a mass of 0–5000 ppm of the total monomer mass, preferably 30–1000 ppm, more preferably 50–600 ppm; and / or, The catalyst D accounts for 5-95% of the total mass of the catalyst, preferably 30-70%.
6. The method for preparing the glycolide-lactide copolymer as described in claim 3, characterized in that: Step (1), The first reactor comprises at least two reactors connected in parallel; and / or, The mixing is carried out under a protective gas atmosphere, wherein the protective gas is at least one selected from nitrogen and an inert gas; and / or, The mixing temperature in the first reactor is 125–150°C, preferably 125–140°C; and / or, The reaction time in the first reactor is 5 to 30 minutes, preferably 10 to 30 minutes.
7. The method for preparing the glycolide-lactide copolymer as described in claim 3, characterized in that: Step (2), The reaction temperature of mixture A in the second reactor is 185–210°C, preferably 185–200°C; and / or, The reaction time of mixture A in the second reactor is 10 to 60 minutes, preferably 15 to 50 minutes.
8. The method for preparing the glycolide-lactide copolymer as described in claim 3, characterized in that: Step (3), The reaction temperature of mixture B in the plug flow reactor is 190–210°C, preferably 200–210°C; and / or, The reaction time of mixture B in the plug flow reactor is 20–60 min, preferably 30–50 min; and / or, The plug flow reactor is a screw extruder or a tubular reactor; and / or The method for removing residual monomers is melt devolatilization; the melt devolatilization preferably uses a devolatilization screw, and the devolatilization temperature is more preferably 200-230°C, and most preferably 210-220°C.
9. A glycolide-lactide copolymer obtained by the preparation method according to any one of claims 3 to 8; preferably, In the glycolide-lactide copolymer, the number of lactide units linked together by glycolide units accounts for 50% to 100% of the total number of lactide units; and / or, The intrinsic viscosity of the glycolide-lactide copolymer is 0.2–3.0 dl / g; and / or, The weight-average molecular weight of the glycolide-lactide copolymer is 5w to 40w, preferably 10w to 35w; and / or, The yellowness value of the glycolide-lactide copolymer is 30-60, preferably 30-45; and / or, The residual monomers in the glycolide-lactide copolymer are less than 5 wt%, preferably less than 2 wt%, and more preferably less than 1.7 wt%; the residual monomers are glycolide monomers and lactide monomers.
10. The application of the glycolide-lactide copolymer as described in claim 1, 2 or 9 in the pharmaceutical field, preferably in the application of drug-loaded microspheres.
Citation Information
Patent Citations
Readily absorbable copolymer compositions for high strength sutures having enhanced strength retention post-implantation
US11058792B2