Halogen-free flame retardants for polycarbonate, pc flame retardant composites
By forming chemical bonds through the hydrolysis-cocondensation reaction of BTMSPA-ED, OPZ and PHS, a three-dimensional network skeleton is constructed, which solves the problems of sulfonate damaging the impact strength of polycarbonate and low organosilicon efficiency in the prior art. This results in a polycarbonate composite material that is highly flame-retardant, maintains high transparency and high impact strength.
Patent Information
- Application Number
- CN202611431523.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
AI Technical Summary
In the prior art, sulfonate flame retardants severely impair the impact strength of polycarbonate, while silicone flame retardants have low efficiency. Furthermore, the physical mixing and synergistic effect of sulfonates and silicones is unstable, and sulfonates are prone to migration and precipitation, making it difficult to simultaneously achieve efficient flame retardancy while maintaining the impact strength and transparency of polycarbonate.
By forming chemical bonds through the hydrolysis-cocondensation reaction of BTMSPA-ED, organopolysilazane (OPZ), and potassium p-hydroxybenzenesulfonate (PHS), a three-dimensional network framework is constructed to achieve synergistic flame retardancy between sulfonate and organosilicon. The Si-N backbone of OPZ absorbs impact energy and forms a dense SiO2 protective layer, while PHS is introduced into the cross-linked network to form an organic-inorganic hybrid structure.
It achieves UL-94 V-0 flame retardant rating for polycarbonate with low addition amount (5-8 parts), notched impact strength is increased by 300%, light transmittance is maintained above 83%, and the overall performance is excellent, meeting the high performance requirements of the electronics and electrical appliance fields.
Smart Images

Figure CN123062718A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flame retardant modification technology of polymer materials, and in particular to a halogen-free flame retardant for polycarbonate, a PC flame retardant composite material based on the flame retardant, the preparation method thereon, and its application. Background Technology
[0002] Polycarbonate (PC) is a high-performance engineering plastic with high transparency, high impact resistance, and good heat resistance, and is widely used in electronic and electrical housings, automotive parts, lighting equipment, and other fields. However, pure PC has a low limiting oxygen index (LOI), making it difficult to meet the UL-94 V-0 flame retardant requirement for thin-walled parts, necessitating the addition of flame retardants for modification.
[0003] Currently, the main flame retardants used in PC are phosphate esters, sulfonates, and silicones. Phosphate ester flame retardants, when added in large quantities, severely impair the mechanical properties of PC. Sulfonate flame retardants have extremely high flame retardant efficiency, but when used alone, they are insufficient to achieve a V-0 rating for thin-walled PC and significantly reduce the impact strength of the PC. Silicone flame retardants form a dense silicon-based carbon layer during combustion, having a relatively small impact on the mechanical properties of PC, but their flame retardant efficiency is lower.
[0004] In existing technologies, the compounding of sulfonates and organosilicones is mostly a simple physical mixing, with both existing independently in the PC matrix. The synergistic effect is unstable, and small-molecule sulfonates are prone to migration and precipitation, failing to effectively address the damage to the impact strength of PC. Polysilazanes are a class of element-organic polymers with Si-N backbones, possessing both silicon-based and nitrogen-based flame-retardant properties. Their flexible Si-N backbones have the potential to improve mechanical properties. BTMSPA-ED is a silane coupling agent containing two trimethoxysilyl groups, and its secondary amine can provide a weakly basic catalytic environment. However, there are currently no reports on using BTMSPA-ED, polysilazanes, and sulfonates through chemical bonding for PC flame-retardant modification. If the catalytic and cross-linking effects of BTMSPA-ED can be utilized to construct polysilazanes and sulfonates within the same network, it is expected to simultaneously achieve high-efficiency flame retardancy, high impact strength, and high transparency retention.
[0005] Therefore, developing a flame retardant that can synergistically combine sulfonates and organosilicon to maintain the impact strength of PC while achieving high flame retardancy is of significant industrial value. Summary of the Invention
[0006] The purpose of this invention is to overcome the above-mentioned technical deficiencies and propose a halogen-free flame retardant for polycarbonate, its preparation method and application, thereby solving the technical problems in the prior art where sulfonate flame retardants seriously damage the impact strength of PC, organosilicon flame retardants have low efficiency and poor physical mixing synergistic effect.
[0007] In a first aspect, the present invention provides a halogen-free flame retardant for polycarbonate, which is prepared by a hydrolysis-co-condensation reaction of three raw materials: BTMSPA-ED, organopolysilazane (OPZ), and potassium p-hydroxybenzenesulfonate (PHS).
[0008] In this invention, the BTMSPA-ED (N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine) molecule contains two trimethoxysilyl groups and one secondary amine group. The trimethoxysilyl groups hydrolyze in the presence of moisture to generate silanols (Si-OH), and the secondary amine provides a weakly alkaline environment, catalyzing the hydrolysis of Si-NH-Si and Si-H bonds in OPZ. The silanols generated from the hydrolysis of BTMSPA-ED undergo a co-condensation reaction with the silanols generated from the hydrolysis of OPZ, forming Si-O-Si crosslinks and constructing a three-dimensional network framework.
[0009] In this invention, organopolysilazane (OPZ) is a polymethylhydrosilazane with a Si-N-Si main chain containing Si-H and Si-NH-Si bonds. The Si-N main chain of OPZ exhibits high flexibility (bond energy approximately 435 kJ / mol), enabling it to absorb and disperse impact energy within a PC matrix, thus improving mechanical properties. Simultaneously, OPZ undergoes ceramization at high temperatures to form a dense SiO2 protective layer, providing flame retardancy.
[0010] In this invention, the potassium p-hydroxybenzenesulfonate (PHS) molecule contains phenolic hydroxyl groups and potassium sulfonate groups. The phenolic hydroxyl groups undergo a condensation reaction with the residual silanol or silazane group in the system, introducing the flame-retardant functional group of potassium sulfonate into the cross-linked network structure, forming an organic-inorganic hybrid structural unit of silicon-oxygen-phenyl-sulfonate.
[0011] In this invention, the weight ratio of BTMSPA-ED, OPZ, and PHS is: 5-40 parts BTMSPA-ED, 30-80 parts OPZ, and 1-20 parts PHS. A preferred ratio is: 20 parts BTMSPA-ED, 70 parts OPZ, and 10 parts PHS.
[0012] Secondly, the present invention provides a method for preparing the above-mentioned flame retardant, comprising the following steps: Weigh out BTMSPA-ED, OPZ (polymethylhydrosilazane), and potassium p-hydroxybenzenesulfonate (PHS). Dissolve BTMSPA-ED and OPZ in n-butyl ether and stir to form a clear solution. Dissolve PHS in a mixture of deionized water and methanol (2-3:1 volume ratio) and slowly add it dropwise to the above solution while stirring at room temperature. After the addition is complete, raise the temperature to 60-80℃ and continue stirring for 3-4 hours. After the reaction is complete, remove the solvent by vacuum distillation and dry under vacuum at 60-80℃ for 10-12 hours to obtain a white to pale yellow solid powder, named flame retardant R.
[0013] Thirdly, the present invention provides a method for preparing PC flame-retardant composite materials, comprising the following steps: S1. Mix the PC matrix components and flame retardant R evenly to obtain the mixture; S2. The mixture is then subjected to intensive kneading to obtain the intensively kneaded material; S3. The intensively mixed material is subjected to hot pressing and cold pressing in sequence to obtain flame-retardant PC composite material.
[0014] In this invention, the process of uniformly mixing the PC matrix component and the flame retardant R includes: placing the PC matrix component and the flame retardant R in a high-speed mixer with a rotation speed of 1000-2000 rpm at room temperature and mixing for 5-10 minutes. By weight, the components are 85-99 parts of PC resin and 1-15 parts of flame retardant, preferably 85-95 parts of PC resin and 5-15 parts of flame retardant.
[0015] In this invention, the mixing process includes: placing the mixture in a rotational rheometer and mixing it for 5-8 minutes at 220-240°C and 40-60 rpm.
[0016] In this invention, the process of sequentially hot-pressing and cold-pressing the refractory material includes: placing the refractory material in a flat vulcanizing machine and sequentially performing hot-pressing and cold-pressing treatments.
[0017] In this invention, the hot pressing process is carried out at a temperature of 220-240℃, a pressure of 8-12MPa, and a time of 4-12 minutes.
[0018] In this invention, the cold pressing process is carried out at room temperature, with a pressure of 3-10 MPa and a time of 10-15 minutes.
[0019] In this invention, it should be noted that the temperature range corresponding to room temperature and normal temperature is 15-40℃.
[0020] Compared with the prior art, the beneficial effects of the present invention include: This invention is the first to propose a chemical bonding process involving N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine (BTMSPA-ED), organopolysilazane (OPZ), and potassium p-hydroxybenzenesulfonate (PHS) to prepare a halogen-free flame retardant. Unlike existing technologies that involve simple physical mixing of sulfonates and organosilicones, this invention utilizes the secondary amine functional groups in BTMSPA-ED to provide a weakly alkaline autocatalytic environment. This allows OPZ to hydrolyze and co-condense with BTMSPA-ED to form a three-dimensional cross-linked network without the need for an external catalyst. Simultaneously, the phenolic hydroxyl groups in PHS condense with residual silanols in the network, firmly introducing the flame-retardant functional groups of potassium sulfonate into the network structure, achieving synergistic effects of the three components at the molecular level. When applied to polycarbonate, this flame retardant exhibits a synergistic flame-retardant effect through silicon-based char formation and sulfonate-catalyzed char formation. Only 5-8 parts are needed to achieve a UL-94 V-0 rating and a limiting oxygen index exceeding 35% for 1.6mm thick PC. Furthermore, OPZ's flexible Si-N backbone effectively absorbs impact energy, significantly increasing notched impact strength to 50-80 kJ / m² while providing flame retardancy. 2 This invention overcomes the technical challenge of traditional sulfonate flame retardants severely degrading the impact strength of PC. Simultaneously, the flame retardant is uniformly dispersed at the nanoscale, maintaining a light transmittance of over 83%, exhibiting excellent overall performance. It breaks through the bottleneck of existing technologies that struggle to simultaneously achieve high-efficiency flame retardancy, high mechanical properties, and high transparency, meeting the urgent needs of the electronics and electrical appliance industries for high-performance flame-retardant PC. This invention achieves simultaneous improvement in flame retardant efficiency, mechanical properties, and optical transparency, with mild, halogen-free, and environmentally friendly processing conditions, demonstrating significant substantial progress and industrial application value. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the preparation reaction mechanism of the halogen-free flame retardant provided by the present invention.
[0022] Figure 2 This is the Fourier Transform Infrared (FT-IR) spectrum of the halogen-free flame retardant R prepared in this invention.
[0023] Figure 3 This is the thermogravimetric (TGA) curve of the halogen-free flame retardant R prepared in this invention.
[0024] Figure 4 These are transparency photographs of the PC composite material obtained in Example 2-2 of this invention. Detailed Implementation
[0025] To more clearly illustrate the technical solution of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that these embodiments are merely for explaining the present invention and are not intended to limit the scope of protection of the present invention.
[0026] Example 1 Weigh out 20 g of BTMSPA-ED, 70 g of OPZ (polymethylhydrosilazane), and 10 g of potassium p-hydroxybenzenesulfonate (PHS). Dissolve BTMSPA-ED and OPZ in 200 g of n-butyl ether and stir to form a clear solution. Dissolve PHS in 30 g of a 2:1 volume ratio of deionized water / methanol mixture and slowly add it dropwise to the above solution while stirring at room temperature. After the addition is complete, raise the temperature to 60 °C and continue stirring for 4 hours. After the reaction is complete, remove the solvent by vacuum distillation and dry under vacuum at 60 °C for 12 hours to obtain a white to pale yellow solid powder, named flame retardant R.
[0027] The flame retardant R prepared in this embodiment was subjected to Fourier transform infrared spectroscopy using the potassium bromide (KBr) pellet method, with a scanning range of 4000-400 cm⁻¹. -1 The infrared spectrum obtained is as follows Figure 2 As shown. 3200-3450cm -1 This is attributed to the residual NH stretching vibration of the system; 2160 cm. -1 Characteristic absorption peaks of residual Si-H from OPZ raw materials are visible nearby; 904-1120 cm⁻¹ -1 A strong and broad absorption band appears, which is a characteristic stretching vibration peak for the formation of the Si-O-Si three-dimensional cross-linked network through co-condensation; 1030 cm⁻¹ -1 The presence of a characteristic absorption peak for the sulfonate-SO3K group at 1590-1490 cm⁻¹ confirms that the potassium sulfonate functional group of PHS has been successfully integrated into the hybrid network; -1 The presence of benzene ring skeletal vibrational absorption corresponds to the aromatic ring of the PHS structural unit; the methoxy-OCH3 in the raw material BTMSPA-E exhibits absorption at 2840 cm⁻¹. -1 The characteristic peaks weakened significantly, indicating that the trimethoxysilyl group underwent complete hydrolysis; the free phenolic hydroxyl group in the PHS raw material reached 3600 cm⁻¹. -1 The sharp absorption peaks were significantly reduced, proving that the phenolic hydroxyl group participated in the condensation reaction with the silanol, rather than a simple physical blending. This verifies the successful synthesis of the integrated hybrid flame retardant at the molecular level.
[0028] Thermogravimetric analysis (TGA) was performed on flame retardant R using a thermogravimetric analyzer. Figure 3The test was conducted under a nitrogen atmosphere, with a heating rate of 10℃ / min, a test range of 40-800℃, and a sample mass of 3-8mg. The 5% thermogravimetric temperature (T5wt%) of flame retardant R was 412℃, which is higher than the melt processing temperature of PC composites by 220-240℃, indicating that the flame retardant does not undergo significant thermal decomposition under PC processing conditions and has good processing stability. The thermal decomposition was divided into two stages: the first stage, at 410-520℃, mainly involved the decomposition of a small amount of residual organic side chains and incompletely cross-linked small molecule fragments in the network; simultaneously, the potassium sulfonate groups chemically anchored on the three-dimensional network framework were thermally activated, playing a solid-phase catalytic role, inducing cross-linking and aromatization reactions in the hybrid network, and initially constructing an organic carbon framework. In the second stage (520-650℃), the silazane (Si-N) main chain undergoes large-scale pyrolysis and rearrangement, resulting in the removal of a large amount of organic components and the gradual transformation into the SiO2 inorganic ceramic phase. Under 800℃ conditions, the residual char rate of flame retardant R in a nitrogen atmosphere can reach 70-75wt%. The high residual char rate is due to the synergistic effect of the high-temperature transformation of silazane into the SiO2 ceramic phase and the catalytic cross-linking of sulfonates. The formation of a dense barrier char layer at high temperatures is an important basis for the flame retardant to exert its flame retardant effect.
[0029] Example 2 The preparation method of PC flame-retardant composite material includes the following steps: S1. Mix the PC matrix components and flame retardant R evenly to obtain the mixture; S2. The mixture is then subjected to intensive kneading to obtain the intensively kneaded material; S3. The intensively mixed material is subjected to hot pressing and cold pressing in sequence to obtain flame-retardant PC composite material.
[0030] In this invention, the process of uniformly mixing the PC matrix component and the flame retardant R includes: placing the PC matrix component and the flame retardant R in a high-speed mixer with a rotation speed of 2000 rpm at room temperature and mixing for 10 minutes.
[0031] In this invention, the mixing process includes placing the mixture in a rotational rheometer and mixing it for 5-8 minutes at 220-240°C and 60 rpm.
[0032] In this invention, the process of sequentially hot-pressing and cold-pressing the refractory material includes: placing the refractory material in a flat vulcanizing machine and sequentially performing hot-pressing and cold-pressing treatments.
[0033] In this invention, the hot pressing process is carried out at a temperature of 220-240℃, a pressure of 8-12MPa, and a time of 8-12 minutes.
[0034] In this invention, the cold pressing process is carried out at room temperature, with a pressure of 3-10 MPa and a time of 10-15 minutes.
[0035] In this invention, it should be noted that the temperature range corresponding to room temperature and normal temperature is 15-40℃.
[0036] To investigate the effect of flame retardant addition on the performance of PC composite materials, this invention set up examples with addition amounts of 3 parts, 5 parts, 8 parts and 10 parts, respectively, and the specific formulations are shown in Table 1.
[0037] Table 1. Formulations for Examples (Unit: Parts by Weight)
[0038] Blank control group Pure PC was used as a blank control group. The only difference between the two cases was that no flame retardant was added. Otherwise, they were the same as the cases.
[0039] Comparative Example 1 20g of BTMSPA-ED, 70g of OPZ, and 10g of PHS are directly mixed in dry powder (without hydrolysis and condensation reaction), and then melt-blended with 95 parts of PC at a ratio of 5 parts. This is recorded as PC-physical blending.
[0040] Comparative Example 2 0.5 parts of potassium p-hydroxybenzenesulfonate (PHS) were directly added and melt-blended with 99.5 parts of PC, and this mixture was designated as PC-PHS.
[0041] Comparative Example 3 3.5 parts of polysilazane (OPZ) were directly added and melt-blended with 96.5 parts of PC, and this mixture was designated as PC-OPZ.
[0042] Comparative Example 4 Weigh 20 g of BTMSPA-ED and 70 g of OPZ (polymethylhydrosilazane). Dissolve BTMSPA-ED and OPZ in a mixed solvent of 200 g of n-butyl ether and 20 g of deionized water, and stir to form a transparent solution. Heat to 60°C and continue stirring for 4 hours. After the reaction is complete, remove the solvent by vacuum distillation, and dry under vacuum at 60°C for 12 hours to obtain the reaction product of BTMSPA-ED and OPZ (without adding PHS), named flame retardant BTO. Melt blend this reaction product with 95 parts of PC at an addition rate of 5 parts, in the same way as the preparation method of the PC flame retardant composite material provided in the example, and denote it as PC-BTO.
[0043] Performance testing methods The performance of the PC composite materials prepared in the blank control group, Examples 1-4, and Comparative Examples 1-4 was tested, and the test results are shown in Table 2. The test methods are as follows: Limiting Oxygen Index (LOI) Test: Performed according to ASTM D2863-24 standard. The sample size is 130 mm × 6.5 mm × 3.2 mm. The minimum oxygen volume concentration required for the sample to burn continuously in a nitrogen-oxygen mixture for 3 minutes and reach a burning length of 50 mm is determined on an oxygen index tester and expressed as a percentage.
[0044] Vertical flammability rating (UL-94) test: Performed according to GB / T 2408-2021 standard, with a sample size of 130 mm × 13 mm × 1.6 mm. Measure and record the vertical flammability rating of the sample (V-0, V-1, V-2 or no rating).
[0045] Notched impact strength test: Performed according to GB / T 1843-2008 standard, using a cantilever beam impact testing machine. The pendulum energy was selected as 5.5 J based on the expected toughness of the specimen. The specimen size was 80 mm × 10 mm × 4 mm, with a V-notch depth of 2.0 mm and a notch bottom curvature radius of 0.25 mm. The notch was prepared by machining. The specimen was conditioned for at least 48 hours at 23±2℃ and 50±5% relative humidity before testing. The specimen was fixed on the fixture with the notch facing the direction of the pendulum impact. The pendulum was released to impact the specimen, and the impact absorbed energy was read. Five parallel samples were tested for each specimen. The results are expressed as notched impact strength (kJ / m²). 2 () indicates that the arithmetic mean is taken and rounded to two decimal places.
[0046] Transmittance test: Performed according to GB / T 2410-2008 standard, using a transmittance / haze meter with a D65 standard light source and measurement geometry of 0 / d. The sample size is 50 mm × 50 mm, and the thickness is 2 mm. The sample surface should be flat, clean, free of scratches and bubbles. Place the sample into the measuring hole of the instrument at room temperature and measure the transmittance. Test five different locations for each sample, and take the arithmetic mean. The result is expressed as a percentage, rounded to one decimal place.
[0047] Table 2 Performance Test Results
[0048] Results Analysis 1. Performance Analysis of the Example As shown in Table 2, as the amount of flame retardant R added in this invention increases from 3 parts to 10 parts, the limiting oxygen index of the PC composite material gradually increases from 34.2% to 38.9%, and the UL-94 flame retardant rating (1.6 mm thickness) increases from V-2 to V-0 (reaching V-0 when the amount added is ≥5 parts). The notched impact strength first increases and then decreases with the amount added: 48.21 kJ / m when 3 parts are added. 2 At 5 minutes, it rose to 66.32 kJ / m³. 2The value reached its highest level of 75.45 kJ / m³ at 8 minutes. 2 At 10 minutes, it slightly decreased to 73.26 kJ / m³. 2 This indicates that there is an optimal addition amount (approximately 8 parts). The light transmittance decreased slightly from 87.2% to 83.8%, remaining good.
[0049] 2. Comparative Analysis Comparing Comparative Example 1 (physical mixture) with Example 2: At the same addition amount (5 parts), the flame retardant R of the present invention (prepared via hydrolysis-cocondensation reaction) increased the LOI from 29.7% to 36.8% compared to the simple physical mixture, the UL-94 rating increased from V-2 to V-0, and the impact strength increased from 13.27 kJ / m. 2 Increased to 66.32 kJ / m 2 The light transmittance increased from 81.1% to 86.3%. This indicates that combining the three raw materials into one through hydrolysis-co-condensation reaction is fundamentally different from simple physical mixing and can produce a significant synergistic effect.
[0050] Comparing Comparative Example 2 (PHS only) with Example 2: Under similar flame retardant efficiencies, the flame retardant R of the present invention exhibits an impact strength as high as 66.32 kJ / m. 2 The impact strength is only 9.87 kJ / m when PHS is used alone. 2 The decrease was as high as 85%. This shows that the introduction of OPZ effectively overcomes the defect of PC embrittlement caused by sulfonates.
[0051] Comparing Comparative Example 3 (OPZ only) with Example 2: When OPZ is used alone, the LOI is only 27.7%, and the UL-94 rating is V-2, which cannot meet the V-0 flame retardant requirement; the impact strength is 49.33 kJ / m. 2 It is lower than 66.32 kJ / m³ in Example 2. 2 This indicates that OPZ alone is insufficient in flame retardant efficiency and lacks the synergistic effect of PHS, and its impact strength is also inferior to that of the present invention.
[0052] Comparing Comparative Example 4 (BTMSPA-ED reacting with OPZ to produce BTO, without PHS) with Example 2: In Comparative Example 4, BTMSPA-ED and OPZ reacted first and then were added to PC, resulting in an LOI of only 29.9% and a UL-94 rating of V-2, significantly lower than the 36.8% and V-0 rating of Example 2; the impact strength was 59.69 kJ / m. 2 It is lower than 66.32 kJ / m³ in Example 2. 2This indicates that without PHS, the flame retardant lacks a sulfonate component that efficiently catalyzes char formation, resulting in a significant decrease in flame retardant efficiency and an inability to achieve a V-0 rating. Simultaneously, due to the absence of chemical bonding with PHS, residual silanol groups in the network structure may affect compatibility with PC, and the impact strength is also slightly reduced.
[0053] Further comparison of Comparative Example 1 and Comparative Example 2: The theoretical amount of PHS added in both groups was 0.5 parts, but the LOI of Comparative Example 1 (simple dry powder physical blend of BTMSPA-ED, OPZ, and PHS) was only 29.7%, significantly lower than the 34.1% of Comparative Example 2 with PHS added alone. This result indicates that simple physical blending of BTMSPA-ED, OPZ, and PHS not only fails to produce a synergistic flame retardant effect, but also exhibits an antagonistic phenomenon of decreased flame retardant performance. The reason for this is that the components did not undergo hydrolysis-co-condensation reaction, and were independently dispersed in the PC matrix, failing to effectively cooperate in the processing and combustion processes.
[0054] The above comparison shows that the flame retardant prepared by the present invention by integrating BTMSPA-ED, OPZ and PHS through hydrolysis-co-condensation reaction achieves synergistic improvement in flame retardant performance, impact strength and light transmittance in PC. All three components are indispensable, and the chemical bonding between the three is the key to exerting the synergistic effect.
[0055] This invention has the following advantages: (1) Highly efficient synergistic flame retardancy: A three-dimensional network is constructed by co-condensation of BTMSPA-ED and OPZ, and potassium sulfonate groups are introduced into it to achieve the synergistic effect of silicon-based char formation and sulfonate catalytic char formation. Only 5-8 parts are needed to increase the LOI of 1.6mm thick PC from 24.0% to 36.0%-39.0%, achieving UL-94 V-0 rating.
[0056] (2) Ultra-high impact strength: This is the most prominent advantage of this invention. Traditional sulfonate flame retardants severely impair the impact strength of PC. This invention utilizes the compliant Si-N backbone of OPZ to significantly improve the impact resistance of PC while achieving flame retardancy. While maintaining a V-0 rating, the notched impact strength is increased from 14.62 kJ / m². 2 Increased to 66-76 kJ / m 2 The increase exceeded 300%.
[0057] (3) High transparency is maintained: The flame retardant of the present invention has good compatibility with PC and is uniformly dispersed at the nanoscale. The light transmittance is maintained at 83%-88%, which is very little lower than that of pure PC (89.7%), meeting the needs of optically transparent application scenarios.
[0058] (4) Halogen-free and environmentally friendly: The flame retardant of the present invention does not contain halogen elements such as bromine and chlorine, and will not produce toxic and corrosive hydrogen halide gas when burning, which complies with the requirements of RoHS and other environmental protection directives.
[0059] (5) The preparation process is simple and the conditions are mild: the entire preparation process only requires stirring and reaction in an aqueous solution at 20-80℃. It does not require expensive catalysts, high temperature and high pressure, and is easy to operate and can be mass-produced in industrial applications.
[0060] (6) Adjustable addition amount to flexibly adapt to different needs: The amount of flame retardant added can be adjusted between 3 and 10 parts. If only V-2 rating is required and high light transmittance is desired, only 3 parts can be added; if V-0 rating is required and high toughness is required, 5-8 parts can be added; if the flame retardancy requirements are extremely stringent, 10 parts can still maintain 73.26 kJ / m 2 It boasts high impact strength and 83.8% light transmittance. This flexibility allows it to meet a wide range of needs, from ordinary household appliances to high-end electronic products.
[0061] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A halogen-free flame retardant for polycarbonate, characterized in that, The flame retardant is prepared from the following three raw materials via hydrolysis-co-condensation reaction: N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine (BTMSPA-ED), organopolysilazane (OPZ), and potassium p-hydroxybenzenesulfonate (PHS). The flame retardant contains BTMSPA-ED, OPZ and PHS in the following weight ratios: BTMSPA-ED 5-40 parts, OPZ 30-80 parts, and PHS 1-20 parts.
2. The halogen-free flame retardant according to claim 1, characterized in that, The organopolysilazane (OPZ) is a polymethylhydrosilazane with a main chain of Si-N-Si structure containing Si-H and Si-NH-Si bonds.
3. The halogen-free flame retardant according to claim 1, characterized in that, The molecular formula of BTMSPA-ED is C14H36N2O6Si2, and the CAS number is 68845-16-9; the molecular formula of potassium p-hydroxybenzenesulfonate is C6H5KO4S.
4. The method for preparing the halogen-free flame retardant according to any one of claims 1 to 3, characterized in that, The process includes the following steps: mixing BTMSPA-ED and OPZ according to the specified ratio, dissolving them in an aprotic organic solvent, and stirring until homogeneous to obtain a premixed solution; dissolving potassium p-hydroxybenzenesulfonate in a polar solvent and adding it to the premixed solution under stirring, and reacting at 20-80°C for 1-8 hours; after the reaction is complete, removing the solvent by vacuum distillation, drying, and obtaining a solid halogen-free flame retardant.
5. The preparation method according to claim 4, characterized in that, The aprotic organic solvent is selected from one or more of n-butyl ether, toluene, xylene, and butyl acetate; the polar solvent is a mixture of deionized water and alcohol.
6. A PC flame-retardant composite material, characterized in that, It comprises the flame retardant and PC resin as described in any one of claims 1 to 3.
7. The PC flame-retardant composite material according to claim 6, characterized in that, By weight, 85-99 parts PC resin and 1-15 parts flame retardant, preferably 85-95 parts PC resin and 5-15 parts flame retardant; The PC flame-retardant composite material has a limiting oxygen index ≥34%, achieves UL-94 V-0 rating in vertical burning tests at a thickness of 1.6 mm, and has a notched impact strength ≥45 kJ / m². 2 Light transmittance ≥83%.
8. The PC flame-retardant composite material according to claim 7, characterized in that, The preparation method of PC flame-retardant composite material includes the following steps: after drying PC resin, it is mixed evenly with the flame retardant in a high-speed mixer, and then the mixture is added to a rotational rheometer for melt blending at a melting temperature of 220-240℃. After melt blending, it is hot-pressed in a flat vulcanizing apparatus at a hot-pressing temperature of 220-240℃, and then cold-pressed at room temperature for 10-15 minutes to obtain PCH flame-retardant composite material.
9. The PC flame-retardant composite material according to claim 8, characterized in that, When the amount of the flame retardant added is 5-10 parts, the limiting oxygen index is 34%-39% and the notched impact strength is 50-80 kJ / m. 2 The light transmittance is 83%-87%.
10. The flame retardant application of any one of claims 1 to 3 or the PC flame retardant composite material of claim 7 in the fields of electronic and electrical housings, automotive parts, lighting equipment, and building materials.