A surface-dense gradient-reinforced phenolic aerogel thermal protection material and a preparation method and application thereof

By using phenolic aerogel materials with gradient design and nanoporous structure, the problem of balancing thermal insulation performance and structural strength of phenolic resin-based thermal protection materials in hypersonic flight environments has been solved, achieving improved high-efficiency thermal insulation and high-temperature oxidation resistance, and preventing interface peeling.

CN123062779APending Publication Date: 2026-11-10BEIJING HANGTIAN XINFENG MECHANICAL EQUIP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611504764.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing phenolic resin-based thermal protection materials cannot balance thermal insulation performance and structural strength in hypersonic flight environments. The surface of the material has insufficient resistance to aerodynamic shearing and cannot meet the requirements of high airflow erosion and high temperature oxidation.

Method used

A three-dimensional quartz fiber braided preform with a gradient design is combined with an organic-inorganic hybrid phenolic sol and a carborane cage-like structure modified silicone resin. A densified layer is formed through sol-gel treatment, which constructs a continuous thermal resistance gradient and a nanoporous structure to realize the functional division and interface connection within the material.

Benefits of technology

While ensuring lightweight properties, the material achieves high-efficiency thermal insulation, significantly improves high-temperature oxidation resistance and mechanical properties, solves the technical contradiction of difficulty in balancing thermal insulation and load-bearing function in traditional materials, and prevents the interface structure from peeling off under high-temperature thermal shock conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062779A_ABST
    Figure CN123062779A_ABST
Patent Text Reader

Abstract

This invention relates to the field of high-temperature thermal protection materials. The invention discloses a method for preparing a surface-dense gradient-reinforced phenolic aerogel thermal protection material, comprising: preparing a hybrid phenolic sol containing silicon and boron sources; preparing a gradient three-dimensional quartz fiber braided preform; performing sol-gel treatment to obtain a hybrid phenolic aerogel block; infiltrating with carborane-modified silicone resin and curing; and the application of this protective material in high-speed aircraft materials. This invention combines a resin with a fixed silicon / boron in-situ grafted hybridization rate with a density gradient preform. The low-density portion of the density gradient preform provides nanopore formation conditions for the resin, while its high-density portion combines with the carborane-modified silicone resin to form a dense layer. This dense layer undergoes eutectic bonding at high temperatures to eliminate interfaces and further provides support, enabling the material to possess high-efficiency thermal insulation, excellent high-temperature oxidation resistance, and superior thermal shock resistance while remaining lightweight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature thermal protection materials technology, specifically to a surface-dense gradient-reinforced phenolic aerogel thermal protection material, its preparation method, and its application. Background Technology

[0002] As aircraft continue to develop, they will experience extreme aerodynamic heating environments during high-speed flight. In order to meet development needs, the thermal protection system of aircraft is constantly improving in terms of lightweight, efficient heat insulation, high strength, and long-term ablation resistance.

[0003] For example, under prolonged high-speed flight conditions in near space, the local temperature of the thermal protection structure can reach over 2000℃. Simultaneously, it must withstand high pressure, high-speed airflow erosion, and intense aerodynamic shearing, placing higher demands on thermal protection materials. Fiber-reinforced phenolic resin matrix composites, due to their high ablation resistance, low density, and good processability, are currently important candidate materials for thermal protection systems of hypersonic vehicles.

[0004] In the prior art, various phenolic resin-based thermal protection materials are disclosed in relevant Chinese patents and published documents. For example, phenolic resin reinforced with quartz fiber, carbon fiber and other materials is used to form fiber-reinforced ablation materials. A carbon layer is formed by high-temperature pyrolysis of the resin to achieve heat insulation and ablation resistance.

[0005] Traditional phenolic ablation materials rely on high char residue to achieve heat protection, but high char residue results in high material density, making it difficult to achieve lightweight properties. Furthermore, material density increases thermal conductivity to some extent, limiting further improvements in thermal insulation performance.

[0006] Meanwhile, in hypersonic flight environments, the material surface is not only subjected to high-temperature oxidation, but also to mechanical scouring by high-speed airflow. If the material is lightweighted by increasing its porosity, it may result in insufficient aerodynamic shear resistance on the material surface, which will not meet the requirements for aerodynamic shear resistance and aerodynamic shape maintenance in high airflow scouring environments. Summary of the Invention

[0007] The purpose of this invention is to provide a surface-dense gradient-reinforced phenolic aerogel thermal protection material, its preparation method and application, in order to solve the technical problems in the prior art where it is difficult to balance the thermal insulation performance and structural strength of the material, and the surface has insufficient resistance to aerodynamic shear.

[0008] To solve the above-mentioned technical problems, the present invention specifically provides the following technical solution:

[0009] A method for preparing a surface-dense gradient-reinforced phenolic aerogel thermal protection material includes the following steps:

[0010] S100. Prepare an organic-inorganic hybrid phenolic sol, wherein the organic-inorganic phenolic sol is formed from a phenolic sol containing a silicon source and a boron source.

[0011] S200. Prepare a gradient three-dimensional quartz fiber braided preform, wherein the preform is configured to form a low-density braided region, a medium-density braided region, and a high-density braided region sequentially from the inside to the outside along the thickness direction.

[0012] S300. The phenolic sol is injected into the preform for impregnation, and then a sol-gel treatment is performed. Inorganic elements are introduced in situ and uniformly dispersed during the formation of the phenolic resin molecular network to construct a hybrid cross-linked structure in which the organic polymer network and the inorganic oxide network interpenetrate each other. At the same time, as the solvent evaporates, a uniform nanoporous structure is formed in the phenolic sol to obtain a hybrid phenolic aerogel block. The pore size of the nanopore is 20-50 nm.

[0013] S400. A carborane cage-like modified silicone resin is infiltrated into the phenolic aerogel block. The silicone resin is capillarily attached to the inside of the phenolic aerogel block along the nanopores. After curing, the silicone resin forms a densified layer on the surface of the phenolic aerogel block. Organic compounds containing silicon and boron elements in the phenolic sol are grafted in situ onto the side chains of the phenolic resin in the phenolic sol.

[0014] In particular, at 1900-2100℃, the densification layer undergoes in-situ ceramization to form a dense ceramization network. The ceramization network is fused with the quartz fibers in the phenolic aerogel block, and the in-situ grafted organic matter generates a borosilicate glass phase at high temperature.

[0015] Furthermore, the fiber density of the high-density braided region of the gradient three-dimensional quartz fiber braided preform is 0.8-1.2 g / cm³, the fiber density of the medium-density braided region is 0.6-0.8 g / cm³, and the fiber density of the low-density braided region is 0.3-0.6 g / cm³.

[0016] Further, in step S100, the phenolic sol is prepared as follows:

[0017] Boron-modified components, silicon-modified components, curing agents, and organic solvents are added to phenolic resin and stirred to dissolve them to obtain the phenolic sol. The phenolic sol is then sealed and placed in an 80°C water bath.

[0018] The stirring speed was 500 r / min to 2000 r / min, the dissolution time was 4 h to 12 h, and the temperature was room temperature.

[0019] Furthermore, the phenolic resin is any one or more of barium phenolic resin or aminophenolic resin;

[0020] The silicon-modifying component is one or more of tetraethyl orthosilicate and methoxysilane, and the amount of silicon-modifying component added is 3-10 wt% based on the solid mass of phenolic resin.

[0021] The boron-modifying component is one or more of tributylboronic acid ester and triacetylazaborane, and the amount of the boron-modifying component added is 1-5 wt% based on the solid mass of the phenolic resin.

[0022] The curing agent is hexamethylenetetramine.

[0023] Furthermore, the hybridization rate of the organic-inorganic hybrid components in the phenolic sol is 3.85-13.04%, preferably 6.54-10.71%;

[0024] The organic-inorganic hybridization rate of the organic-inorganic hybrid component is calculated according to Equation I:

[0025] .............Formula I;

[0026] Where H is the organic-inorganic hybridization rate, ms is the solid mass of the silicon-modified component, mb is the solid mass of the boron-modified component, and mp is the solid mass of the phenolic resin.

[0027] Further, in step S300, the sol-gel treatment includes the following steps:

[0028] The impregnated preform was aged for 3 days, then air-dried at room temperature for 1 day, and then air-dried at 50°C and 80°C for 1 day respectively to obtain hybrid phenolic aerogel blocks.

[0029] Furthermore, in step S400, the curing temperature is 140℃~150℃.

[0030] The structural formula of the organosilicon resin is shown in Formula II:

[0031] ...Form II.

[0032] The present invention further provides a surface-dense gradient-reinforced phenolic aerogel thermal protection material, comprising:

[0033] A gradient three-dimensional quartz fiber braided preform, wherein the preform consists of a low-density braided region, a medium-density braided region, and a high-density braided region from the inside to the outside along the thickness direction, so that a continuous thermal resistance gradient is formed inside the material.

[0034] The phenolic aerogel matrix is ​​composed of phenolic resin and organic compounds containing silicon and boron elements grafted in situ onto its side chains, and is filled in the preform. The phenolic aerogel matrix has a uniform nanoporous structure.

[0035] A densification layer is filled along the nanopores on the preform. The densification layer is composed of an organosilicon resin modified with a carborane cage structure and is bonded to the quartz fiber.

[0036] Specifically, at 1900-2100℃, the densification layer generates a ceramicized network in situ within the preform, and the ceramicized network is fused with the quartz fiber; simultaneously, the B and Si elements in the phenolic aerogel matrix generate a borosilicate glass phase in situ.

[0037] This invention provides the above-mentioned preparation method and the application of the surface-dense gradient-reinforced phenolic aerogel thermal protection material obtained by the preparation method in the field of aircraft. At 1900-2100℃, the densification layer on the surface of the surface-dense gradient-reinforced phenolic aerogel thermal protection material undergoes in-situ ceramization to form a dense ceramization network. The ceramization network is fused with the quartz fibers in the phenolic aerogel block, and the organic matter containing silicon and boron elements grafted in-situ onto the side chains of the phenolic sol generates a borosilicate glass phase at high temperature.

[0038] Compared with the prior art, the present invention has the following advantages:

[0039] This invention features a series of woven regions along the thickness direction, from the inside out: a low-density woven region (fiber density 0.3-0.6 g / cm³), a medium-density woven region (fiber density 0.6-0.8 g / cm³), and a high-density woven region (fiber density 0.8-1.2 g / cm³). This creates a continuous thermal resistance gradient within the material. Simultaneously, the phenolic aerogel matrix possesses a uniform nanoporous structure of 20-50 nm. This size range of nanopores effectively suppresses convective heat transfer from gas molecules. The synergistic effect of these two factors results in a room temperature thermal conductivity ≤0.08 W / (m·K). This achieves high-efficiency thermal insulation while maintaining lightweight properties (density 0.30-0.80 g / cm³). Furthermore, the silicon and boron hybrids on the phenolic resin side chains form a high-temperature borosilicate glass phase, significantly improving the material's high-temperature oxidation resistance and high-temperature mechanical properties.

[0040] This invention utilizes the capillary effect of nanopores to allow the carborane cage-like modified silicone resin to penetrate into the interior of a continuous thermal resistance gradient structure. During subsequent high-temperature service, the carborane cage-like modified silicone resin on the material surface is in-situ ceramicized and integrally fused with quartz fibers. The reaction process is endothermic, which can further improve the thermal insulation effect and the material's support performance. This solves the technical contradiction of the difficulty in balancing thermal insulation and load-bearing functions in traditional homogeneous materials and prevents the interface structure from peeling off under high-temperature thermal shock conditions. Attached Figure Description

[0041] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0042] Figure 1 The material preparation flowchart provided in the embodiments of this application.

[0043] Figure 2 This is a schematic diagram of the overall gradient structure of the material provided in Embodiment 1 of this application.

[0044] Figure 3 This is a physical image of the three-dimensional quartz fiber gradient braided structure provided in Embodiment 1 of this application.

[0045] Figure 4 The images show the surface of the hybrid phenolic aerogel block provided in Example 1 of this application and an electron microscope image of the nanoporous structure of the phenolic aerogel.

[0046] Figure 5 The images shown are of the physical objects before and after the 850℃ heating treatment (left) and electron microscope images after the treatment (middle and right) provided in Example 1 of this application.

[0047] Figure 6 A surface morphology image of a test specimen after wind tunnel testing is provided for Embodiment 1 of this application.

[0048] Figure 7 This application provides an SEM image of the surface of the test piece after a wind tunnel test for Embodiment 1. Detailed Implementation

[0049] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0050] like Figure 1 As shown, the present invention provides a method for preparing a surface-dense gradient-reinforced phenolic aerogel thermal protection material, comprising the following steps:

[0051] S100. First, silicon and boron elements are uniformly dispersed at the molecular scale in the phenolic resin precursor to prepare an organic-inorganic hybrid phenolic sol, wherein the organic-inorganic phenolic sol is formed from phenolic sol containing silicon and boron sources.

[0052] S200. Prepare a gradient three-dimensional quartz fiber braided preform. The preform forms a low-density braided region, a medium-density braided region, and a high-density braided region from the inside to the outside along the thickness direction to construct a continuous thermal resistance gradient. The lower the density, the higher the porosity and the better the thermal insulation performance; the higher the density, the higher the fiber content and the better the mechanical properties.

[0053] S300. The phenolic sol is injected into the preform for impregnation, and then a sol-gel treatment is performed. Inorganic elements are introduced in situ and uniformly dispersed during the formation of the phenolic resin molecular network to construct a hybrid cross-linked structure in which the organic polymer network and the inorganic oxide network interpenetrate each other. At the same time, as the solvent evaporates, a uniform nanoporous structure is formed in the phenolic sol to obtain a hybrid phenolic aerogel block.

[0054] S400. A carborane cage-like modified silicone resin is infiltrated into the phenolic aerogel block. The silicone resin is capillarily attached to the inside of the phenolic aerogel block along the nanopores. After curing, the silicone resin forms a densified layer on the surface of the phenolic aerogel block. Organic compounds containing silicon and boron elements in the phenolic sol are grafted in situ onto the side chains of the phenolic resin in the phenolic sol.

[0055] In particular, at 1900-2100℃, the densification layer undergoes in-situ ceramization to form a dense ceramization network. The ceramization network is fused with the quartz fibers in the phenolic aerogel block, and the in-situ grafted organic matter generates a borosilicate glass phase at high temperature.

[0056] This invention essentially provides a thermal insulation material with a continuous thermal resistance gradient, placing the low-density region on the inner side and the high-density region on the outer side, achieving a spatial division of functions. The inner side primarily undertakes the thermal insulation function, while the outer side primarily undertakes the load-bearing function. This allows a single material to simultaneously possess both thermal insulation and load-bearing functions, resolving the contradiction that these two functions cannot be simultaneously achieved.

[0057] The thermal insulation effect of gradient design stems from the cascading superposition of multiple thermal resistance layers. When heat is introduced from the inner low-density region, the high porosity of the low-density region (due to the low fiber volume fraction) provides an efficient thermal barrier. As heat continues to transfer outward to the medium-density region, the porosity decreases, the solid heat transfer path increases, and the thermal resistance changes. Upon reaching the high-density region, the high fiber content provides better mechanical support and further thermal resistance. The cascading of the three density regions forms a continuously varying thermal resistance gradient, resulting in a more gradual temperature distribution along the thickness direction of the material, avoiding the temperature abrupt changes and thermal stress concentrations that may occur in materials with a single density.

[0058] Furthermore, the present invention also designs a nanoporous structure. Specifically, during the sol-gel process, the phenolic resin precursor undergoes a cross-linking condensation reaction to form an organic polymer network. Then, during the drying process, as the solvent evaporates, a uniform nanoporous structure is formed within the phenolic sol.

[0059] Specifically, during the gelation process, the solvent is encapsulated within the gel network; during the subsequent drying process, the solvent gradually evaporates, leaving behind nanoscale pores. The pore size of the nanopores is 20-50 nm. Experiments show that when the pore size is smaller than the mean free path of gas molecules (approximately 70 nm), the collision frequency between gas molecules and the pore walls is much higher than the collision frequency between molecules, thus significantly suppressing convective heat transfer.

[0060] In traditional composite materials, a clear interface exists between the fiber and the matrix. This interface is a weak point in mechanical properties and is prone to debonding and peeling under high-temperature thermal shock conditions. To address this issue, after designing standard-sized nanopores, in step S400 of this invention, a carborane cage-like modified silicone resin is infiltrated into the phenolic aerogel block. The key to this is the traction effect of the nanopores; the phenolic aerogel block containing nanopores acts like a sponge, enabling efficient infiltration of the silicone resin. After curing, the silicone resin forms a dense layer on the block surface, while the silicon and boron sources undergo hydrolysis and condensation reactions to form an inorganic oxide network, thereby improving the resin's oxidizing properties.

[0061] The effect of this densification layer is as follows: under high-temperature service conditions of 1900-2100℃, the silicone resin on the surface undergoes in-situ ceramization, forming a dense ceramization network. This ceramization network undergoes "eutectic bonding" with the quartz fiber.

[0062] Carboranes are cage-like cluster compounds composed of boron, carbon, and hydrogen. Their introduction into the molecular structure of organosilicon resins primarily yields the following effects: the cage-like structure of carboranes provides excellent thermal stability, significantly improving the polymer's thermo-oxidative stability and high-temperature char yield; the boron in carboranes participates in the formation of a borosilicate glass phase at high temperatures, contributing to the densification of the ceramic network; and the introduction of the carborane structure results in higher yields and a more compact structure in the pyrolysis ceramic products.

[0063] Specifically, at ultra-high temperatures of 1900-2100℃, the ceramic phase formed by the ceramicization of organosilicon resin and the quartz fiber (mainly composed of SiO2) undergo fusion at the interface. The borosilicate glass phase acts as a medium, fusing the ceramicized matrix and the quartz fiber together. Furthermore, at high temperatures, the silicon, boron, and oxygen elements in the ceramicized product interdiffusion with the silicon and oxygen elements on the surface of the quartz fiber, resulting in a gradual rather than abrupt elemental distribution at the interface.

[0064] In addition, the ceramization reaction itself is an endothermic reaction, which absorbs heat during high-temperature service, further reducing the temperature rise on the back of the material and improving the thermal insulation effect.

[0065] Meanwhile, the introduction of silicon and boron sources into the phenolic resin phase forms a SiO2 network at high temperature, while boron forms a B2O3 glass phase. Together, they generate a borosilicate glass phase, which exhibits better high-temperature stability and oxygen barrier capability than single silicon modification.

[0066] This invention features a series of woven regions—low-density, medium-density, and high-density—that sequentially extend from the inside to the outside along the thickness direction, creating a continuous thermal resistance gradient within the material. Simultaneously, the phenolic aerogel matrix possesses a uniform nanoporous structure of 20-50 nm. This size range of nanopores effectively suppresses convective heat transfer from gas molecules, enabling the material to achieve highly efficient thermal insulation while maintaining its lightweight nature.

[0067] The gradient and porosity settings affect the strength of materials. To reduce this impact and even further improve material strength, this invention utilizes a nanoporous structure to successfully impregnate a carborane cage-like modified silicone resin into a continuous thermal resistance gradient structure, forming a dense layer. During subsequent high-temperature service (1900-2100℃), the carborane cage-like modified silicone resin on the material surface undergoes in-situ ceramization, and the resulting ceramized network fuses with the quartz fibers in the phenolic aerogel block. This structure fundamentally eliminates the weak interfacial links between fibers and the matrix in traditional composite materials, resolving the technical contradiction of balancing thermal insulation and load-bearing functions in traditional homogeneous materials, and effectively preventing peeling and debonding of the interfacial structure under high-temperature thermal shock conditions. Furthermore, during high-temperature service, silicon and boron elements in the phenolic resin form a uniform borosilicate glass phase in situ, creating a continuous and dense oxygen diffusion barrier inside and on the surface of the material, significantly improving the material's high-temperature oxidation resistance and overcoming the problems of uneven inorganic particle dispersion and poor interfacial compatibility in traditional physical blending methods.

[0068] The optimal temperature range for the ceramization reaction of this material is 1900-2100℃, within which a dense ceramization network can be formed; below this temperature, the degree of ceramization is insufficient, but the material still has basic heat insulation function.

[0069] like Figure 2 As shown, the density gradient scheme defined in this invention is as follows: 0.3-0.6 g / cm³ for low-density knitting area, 0.6-0.8 g / cm³ for medium-density knitting area, and 0.8-1.2 g / cm³ for high-density knitting area.

[0070] The low-density region (0.3-0.6 g / cm³) serves as the inner layer, which has a lower fiber volume fraction and provides a larger filling space for the phenolic aerogel matrix. This allows the region to accommodate more aerogel insulation components, thereby achieving optimal insulation performance and reducing overall thermal conductivity.

[0071] The medium-density region (0.6-0.8 g / cm³) serves as a transition layer, acting as a bridge and buffer between thermal insulation and mechanical properties. This region maintains a certain porosity to ensure the continuity of thermal insulation performance, while increasing the fiber content to improve structural integrity and prevent performance mismatch and thermal stress concentration caused by abrupt density changes between the low-density and high-density regions.

[0072] The high-density region (0.8-1.2 g / cm³) serves as the outer layer. Its high fiber volume fraction provides excellent mechanical strength and load-bearing capacity. At the same time, as a densification substrate on the surface, it provides a good adhesion basis for the infiltration of silicone resin and the formation of the ceramic layer.

[0073] In low-density regions, if the fiber density is below 0.3 g / cm³, there are insufficient contact and entanglement points between fibers, making it difficult for the preform to maintain the integrity of its three-dimensional structure. Subsequent sol-gel injection may lead to deformation or collapse of the fiber network. If the density is too high, the lightweight advantage will be lost, and excessively high fiber content will significantly reduce the filling space of the aerogel matrix, weakening the thermal insulation performance.

[0074] In the actual manufacturing process, the density difference between the medium-density region and the preceding and following layers is 0.2-0.3 g / cm³ to ensure density continuity between adjacent regions. This avoids thermal expansion coefficient mismatch and interfacial stress concentration caused by excessive density abrupt changes, while also ensuring functional differentiation between regions, allowing for a smooth transition between thermal insulation and load-bearing functions along the same thickness direction.

[0075] Regarding the realization of the gradient three-dimensional quartz fiber woven preform, a three-dimensional weaving process can be used. The surface high-density layer can be made of 2.5D quartz fiber fabric, while the middle and bottom layers can be made of satin-textured quartz fabric and fiber web needle-punched structures, layered one by one through a fiber needle-punching process. The surface 2.5D fabric is a monolithic structure, while the needle-punched structures of the middle and bottom layers achieve differentiated weaving densities by adjusting the needle-punching density. The surface 2.5D fabric and the middle and bottom needle-punched structures are integrated into the preform through a through-stitching process, achieving a differentiated density gradient from the outside to the inside.

[0076] By adjusting the weaving process parameters (such as weaving density, needle punching density, etc.) to control the fiber density of each layer, a gradient three-dimensional quartz fiber woven preform with continuously varying density along the thickness direction can be obtained.

[0077] In step S100, the phenolic sol preparation method essentially achieves the integrated composite of phenolic resin and silicon and boron modified components at the molecular scale through liquid phase mixing.

[0078] Specifically, the preparation method of the phenolic sol is as follows:

[0079] Boron-modified components, silicon-modified components, curing agents, and organic solvents are added to phenolic resin and stirred to dissolve, thereby obtaining the phenolic sol. The phenolic sol is then sealed and placed in an 80°C water bath, so that the silicon and boron sources are fully mixed with the phenolic resin molecules and undergo preliminary chemical bonding during the sol stage.

[0080] The stirring speed was 500 r / min to 2000 r / min, the dissolution time was 4 h to 12 h, and the temperature was room temperature.

[0081] The phenolic resin is any one or more of barium phenolic resin or acetaminophenic resin. Barium phenolic resin is a modified product obtained by introducing barium (usually prepared using barium hydroxide as a catalyst) into ordinary phenolic resin, and it has a higher char residue rate compared to ordinary phenolic resin. Acetaminophenic resin is a phenolic resin synthesized under ammonia catalysis, characterized by the introduction of nitrogen into its molecular chain. The introduction of nitrogen improves the resin's flowability, facilitating uniform mixing with the modified components; furthermore, nitrogen atoms can form heat-resistant structural units such as C3N4 with carbon at high temperatures, which positively contributes to improving high-temperature structural stability.

[0082] The silicon-modifying component is tetraethyl orthosilicate or methoxysilane. Tetraethyl orthosilicate is the most classic silicon precursor in the sol-gel method, and the reaction conditions are easy to control. Methoxysilanes (such as methyltrimethoxysilane MTMS, dimethyldimethoxysilane DMDMS, etc.) contain organic groups in their molecules, which can maintain a certain degree of organic compatibility while introducing silicon, and are beneficial for forming a more stable hybrid structure with phenolic resin.

[0083] The silicon-modified component content is 3-10 wt% of the phenolic resin mass. When the silicon content is less than 3 wt%, the SiO2 network generated at high temperature is insufficient to form a continuous protective barrier, and its effect on improving the high-temperature oxidation resistance of the material is limited. When the silicon content is greater than 10 wt%, excessive silicon sources may agglomerate during the sol-gel process, forming independent SiO2 particle phases rather than a hybrid structure interpenetrating with the phenolic network, which may instead damage the mechanical properties of the material.

[0084] The boron-modifying component is any one or more of tributylboronic acid ester or triacetylazaborane. Tributylboronic acid ester (B(Obu)3) is a commonly used borate ester compound. The B-C bond in its molecule can be hydrolyzed to generate boric acid, which then forms a B2O3 network, exhibiting good kinetic matching with the hydrolytic condensation reaction of silicon sources. Triacetylazaborane is a boron compound containing BN bonds. Its molecular structure contains both boron and nitrogen elements, providing an additional nitrogen source while introducing boron.

[0085] The boron-modified component content is 1-5 wt% of the phenolic resin mass. When the boron content is below 1 wt%, the amount of B2O3 glass phase formed at high temperatures is insufficient to effectively fill the voids in the SiO2 network, resulting in insufficient density of the borosilicate glass phase. When the boron content is above 5 wt%, excessive boron oxides exhibit high volatility at high temperatures (B2O3 begins to volatilize significantly at approximately 1500℃), which is detrimental to long-term stability at high temperatures.

[0086] This invention limits the content range of silicon source to 3-10wt% and boron source to 1-5wt%, and limits the silicon-boron mass ratio to (3:1) to (10:1). An appropriate amount of B2O3 can reduce the high-temperature viscosity of the SiO2 network, promote the flow and spread of the glass phase, and facilitate the formation of a dense oxygen diffusion barrier.

[0087] The curing agent is hexamethylenetetramine. At room temperature, hexamethylenetetramine exhibits good compatibility with phenolic resin and can be uniformly dispersed in the sol system. At a water bath temperature of 80°C, hexamethylenetetramine slowly decomposes, and the released formaldehyde promotes the pre-crosslinking of the phenolic resin.

[0088] In the phenolic sol, the proportion of silicon is 15%-30% and the proportion of boron is 5%-15%.

[0089] The hybridization rate of the organic-inorganic hybrid components in the phenolic sol is 3.85-13.04%, preferably 6.54-10.71%.

[0090] The organic-inorganic hybridization rate of the organic-inorganic hybrid component is calculated according to Equation I:

[0091] .............Formula I;

[0092] Where H is the organic-inorganic hybridization rate, and m s m is the solid mass of the silicon-modified component. b m is the solid mass of the boron-modified component. p This refers to the solid mass of phenolic resin.

[0093] Solid mass is based on the effective solid component after removing solvent and volatile small molecules from the reaction system.

[0094] During the sol-gel reaction, the silicon-containing precursor first undergoes hydrolysis to generate silanol groups, which then undergo condensation reactions to form a continuous silicon-oxygen network structure. Simultaneously, the silanol groups can condense with the hydroxyl groups in the phenolic resin or form stable interfacial bonds, allowing the silicon-oxygen inorganic network to be uniformly embedded in the phenolic organic cross-linked network, thus forming an organic-inorganic hybrid network. A boron-containing component is also introduced into the phenolic resin precursor solution; this boron-containing component can be selected from boric acid, borate esters, organoboron compounds, or other boron-containing precursors. During the sol-gel and curing processes, boron can coordinate and condense with the phenolic hydroxyl groups, resulting in a uniform distribution of boron within the phenolic molecular network. Due to boron's high-temperature glass transition properties, during high-temperature service, the boron-containing structure can further transform into a B₂O₃ glass phase, which, together with the silicon-oxygen structure, forms a Si / B ceramic protective layer. This protective layer effectively hinders oxygen diffusion into the interior, improving the material's high-temperature oxidation resistance and ablation resistance.

[0095] This invention points out that the formation process of the sol-gel network can be controlled by adjusting the concentration of the phenolic resin precursor and the solvent ratio. When the resin mass fraction is low, the intermolecular crosslinking density decreases, forming a looser gel network structure, and the pore size of the resulting aerogel increases; when the resin mass fraction increases, the degree of condensation reaction increases, the network structure becomes denser, and the pore size decreases.

[0096] Therefore, this invention achieves precise control over the nanoporous structure of aerogels by adjusting the resin-solvent ratio and controlling the degree of silicon-boron hybridization. When the hybridization degree reaches approximately 80%, a uniform and stable nanoporous structure can be formed, with the average pore size controllable within the range of approximately 20 nm. This nanoporous structure can effectively reduce solid-state heat conduction, gas-gas heat convection, and high-temperature radiative heat transfer within the material, thereby endowing the material with excellent thermal insulation properties.

[0097] The average pore size of the nanopore is 20 nm.

[0098] In step S300, the sol-gel treatment includes the following steps: aging the impregnated preform for 3 days, then ventilating and drying it at room temperature for 1 day, and then drying it in a forced-air environment at 50°C and 80°C for 1 day respectively, to obtain a hybrid phenolic aerogel block.

[0099] In the initial stage after injection into the preform, the cross-linking and polycondensation of the phenolic resin and the hydrolytic polycondensation of the silicon / boron source are not yet complete, and the network structure is not yet incomplete. During aging, the movement of molecular chain segments continues, and unreacted active groups (phenolic hydroxyl, hydroxymethyl, silanol) continue to undergo condensation reactions, further increasing the degree of cross-linking and molecular weight of both the organic and inorganic networks. The increased degree of cross-linking during aging significantly enhances the mechanical strength of the gel network, enabling the gel to resist shrinkage and collapse caused by capillary forces during subsequent drying.

[0100] After aging, the gel is first dried under ventilation at room temperature. The aged gel contains free solvent filling the pores of the gel network, as well as bound solvent that is physically adsorbed or hydrogen-bonded to the surface of the gel network. Under ventilation at room temperature, the free solvent initially evaporates at a slower rate, resulting in a relatively uniform evaporation rate across the entire bulk surface, effectively preventing the formation of a skin effect.

[0101] After ventilation at room temperature, the subsequent gentle heating to 50°C allows the binding solvent, which is difficult to completely evaporate at room temperature, to evaporate further. As the binding solvent is removed, the gel network shrinks further, the pore walls gradually thicken, and the size of the nanopores becomes more uniform.

[0102] At 80°C, the evaporation rate of common solvents such as water and ethanol increases significantly, and the trace amounts of solvent remaining in the nanopores are completely removed at this stage, reaching the final dry state of the aerogel product. Complete curing of phenolic resin typically requires a temperature range of 80-150°C. Drying at 80°C for one day allows for a more thorough cross-linking reaction of the phenolic resin, forming an organic network framework with sufficient mechanical strength.

[0103] The temperature gradient, from room temperature (approximately 20-30°C) to 50°C and then to 80°C, creates a smooth temperature change. This gradual heating method avoids thermal shock and thermal stress concentration caused by abrupt temperature changes.

[0104] In step S400, when silicone resin is infiltrated into the phenolic aerogel block, the block contains ① an organic polymer network (phenolic resin cross-linking structure) and ② carborane-modified silicone resin.

[0105] To ensure the curing of the carborane-modified silicone resin, the curing temperature in step S400 is 140℃~150℃.

[0106] The secondary heating at 140-150℃ provides further crosslinking reaction conditions for the residual active hydroxymethyl groups in the phenolic resin, which supplements and strengthens the structural integrity of the phenolic network, makes the inorganic network in the organic-inorganic hybrid crosslinking structure more compact, and further increases the number of Si-B bonds.

[0107] Simultaneously, sufficient curing at 140-150℃ allows the carborane-modified silicone resin to form a continuous, dense layer with good adhesion to the substrate on the surface of the phenolic aerogel block. If curing is insufficient, the continuity of the dense layer will be poor, and the bonding force with the substrate will be weak, which may lead to peeling during subsequent high-temperature service.

[0108] The structural formula of the organosilicon resin is shown in Formula I:

[0109] ...Form II.

[0110] The structural formula of carborane is shown in Formula II:

[0111] ...Form III.

[0112] The reaction formula for carborane is shown in Formula III:

[0113] ...Form IV.

[0114] Carborane-modified silicone resins introduce flexible siloxane linkages into their molecular structure, giving them a certain degree of flexibility. This improves the low-temperature resistance of the modified silicone resin adhesives and ensures the compatibility of the high-temperature rigid structure and the low-temperature flexible structure of the carborane-modified polymer matrix within the polymer molecular chain structure.

[0115] After introducing carborane as a modifier and combining it with organosilicon resin, the high-temperature resistance of the resulting modified resin matrix is ​​significantly improved. Whether in a nitrogen atmosphere or an air atmosphere, the carbon residue of the resin matrix is ​​as high as 60% or more at a high temperature of 600℃.

[0116] The silicone resin is selected from one or more of methylphenyl polysiloxane resin, hydrogen-containing polysiloxane, or polysilazane; the carborane is selected from one or more of o-carborane (1,2-dicarborane), meta-carborane, or para-carborane.

[0117] Specifically, the organosilicon resin is: methylphenyl polysiloxane resin, whose molecular structure contains Si element - Si silicon-oxygen backbone, and contains methyl and phenyl side groups.

[0118] The present invention further provides a surface-dense gradient-reinforced phenolic aerogel thermal protection material, characterized in that it comprises:

[0119] A gradient three-dimensional quartz fiber braided preform, wherein the preform consists of a low-density braided region, a medium-density braided region, and a high-density braided region from the inside to the outside along the thickness direction, so that a continuous thermal resistance gradient is formed inside the material.

[0120] A phenolic aerogel matrix is ​​filled within the preform, and the phenolic aerogel matrix has a uniform nanoporous structure.

[0121] The phenolic aerogel matrix is ​​composed of phenolic resin and organic compounds containing silicon and boron elements grafted in situ onto its side chains, and is filled in the preform. The phenolic aerogel matrix has a uniform nanoporous structure.

[0122] Specifically, at 1900-2100℃, the densification layer generates a ceramicized network in situ within the preform, and the ceramicized network is fused with the quartz fiber to form an integral fiber; simultaneously, the boron and silicon elements in the phenolic aerogel matrix generate a borosilicate glass phase in situ, and organic matter containing silicon and boron elements is grafted in situ onto the side chains of the phenolic resin within the phenolic aerogel matrix.

[0123] In this invention, there are no artificial interfaces formed by adhesives, stitching, or other methods between the three weaving regions of low density, medium density, and high density. Instead, they are formed in one step through a three-dimensional weaving process, allowing the fibers to continuously penetrate in the thickness direction and exhibiting a gradual change in density. A phenolic aerogel matrix is ​​filled within the preform and possesses a uniform nanoporous structure. Furthermore, the surface of the material contains a densification layer. This densification layer is not simply coated on the material surface but rather penetrates into the internal pores of the block through capillary action of the nanopores, forming a thin layer covering the pore walls.

[0124] Under high-temperature service conditions of 1900-2100℃, the ceramicized network generated in situ in the densification layer is fused with the quartz fiber to form an integrated fiber. There is no longer a distinguishable interface between the ceramicized product and the quartz fiber. The fiber is "wrapped" by the ceramicized layer and integrated with its appearance, forming a composite structure with a gradual change in composition.

[0125] This composite structure results in a much higher degree of densification on the surface than on the interior, achieving a dense surface and a porous interior, thus ensuring a synergistic improvement in material strength and thermal insulation performance; at the same time, it eliminates interlayer interfaces, further improving the interfacial bonding strength.

[0126] Organic compounds containing silicon and boron are grafted in situ onto the side chains of phenolic resin, rather than being dispersed in the matrix as independent particles or phases. At high temperatures, the boron element (from the boron source) and the silicon element (from the silicon source) undergo further condensation and rearrangement to form a SiO2-B2O3 composite glass phase, thus solving the defect of uneven glass phase distribution caused by the agglomeration of inorganic particles.

[0127] This product exhibits different structural forms at different temperature levels:

[0128] Initial stage: The material comprises a gradient preform, a nanoporous phenolic aerogel matrix (containing in-situ grafted silicon and boron elements), and a carborane-modified silicone resin densification layer distributed along the nanopores and adhered to the fiber surface. In this stage, the densification layer mainly serves as a sealant and surface reinforcement layer, with silicon and boron elements existing in the form of chemical grafts on the phenolic side chains.

[0129] High-temperature evolution stage: During service at 1900-2100℃, the organic network of phenolic resin undergoes pyrolysis and carbonization, but the inorganic oxide network, as the structural framework, supports the nanopores and does not completely collapse; the silicon and boron elements grafted on the side chains detach from the phenolic framework and uniformly generate a borosilicate glass phase through the condensation rearrangement of Si and B elements; the carborane-modified organosilicon resin undergoes a ceramic transformation, and the generated ceramic products are fused together with quartz fibers.

[0130] The present invention further provides the application of the above preparation method or the above surface dense gradient enhanced phenolic aerogel thermal protection material in the field of aircraft. The technical essence is that the product (or the product itself) obtained by the above preparation method is applied to the field of aircraft, and thermal protection function is achieved by utilizing the multi-mechanism synergistic response of the material itself under ultra-high temperature service conditions of 1900-2100℃.

[0131] At 1900-2100℃ (the aerodynamic thermal environment temperature experienced by the corresponding part of the aircraft during service), that is, when the actual temperature of the material surface or near the surface reaches this range, the densification layer on the surface of the surface-densified gradient-enhanced phenolic aerogel thermal protection material undergoes in-situ ceramization, forming a dense ceramization network. The ceramization network is fused and connected with the quartz fibers in the phenolic aerogel block, and the organic matter containing silicon and boron elements grafted in-situ onto the side chains of the phenolic sol generates a borosilicate glass phase at high temperature.

[0132] This temperature is not a constant temperature maintained by the material throughout its service life, but rather the peak temperature range reached on the material surface during specific flight phases (such as the peak heating period of reentry into the atmosphere).

[0133] It is worth noting that the ceramization of carborane-modified organosilicon resin is a temperature-dependent gradual process, and preliminary pyrolysis and structural transformation may have already begun at lower temperatures (such as 1000-1500℃).

[0134] Both the ceramization reaction and the formation of the borosilicate glass phase are endothermic processes, absorbing a large amount of heat in an ultra-high temperature environment, which reduces the rate of temperature rise on the back side of the material and has a supplementary effect on improving the thermal insulation effect.

[0135] Application sites may include the leading edge / nose cone, wing leading edge, combustion chamber wall, and heat shield of hypersonic aircraft. Application methods include at least: installing the prepared material product on a specific part of the aircraft, designing and selecting the material as a component of the aircraft's thermal protection system, or including the material in the aircraft design scheme.

[0136] The following specific examples are provided for illustration:

[0137] Example 1

[0138] A three-dimensional quartz fiber gradient braid is used as the reinforcing skeleton. The surface layer (high-density anti-oxidation and ablation layer) has a fiber density of 1.0 g / cm³; the middle layer (medium-density insulation layer) has a fiber density of 0.7 g / cm³; and the bottom layer (low-density insulation layer) has a fiber density of 0.4 g / cm³.

[0139] Boric acid, tetraethyl orthosilicate, and n-butanol were added to acetaminophen-formaldehyde resin and stirred at 1500 r / min for 8 h to obtain a silicon- and boron-containing phenolic sol. In this system, the amount of silicon added was 5 wt%, the amount of boron added was 2 wt%, and the resin hybridization rate was 6.54%.

[0140] The phenolic aerogel block was obtained by impregnation using an atmospheric pressure RTM impregnation molding process with an injection pressure of 0.1 MPa, followed by gelation, aging, and drying.

[0141] The process employs a low-pressure melting and infiltration technique, with the surface treated with a carborane cage-like modified silicone resin. The melting and infiltration pressure is 0.05 MPa, and the resin is cured at 150°C for 3 hours.

[0142] A physical image of a three-dimensional quartz fiber gradient braid is shown below. Figure 3 As shown; physical images and electron microscope images of the phenolic aerogel block are as follows. Figure 4 As shown, from Figure 4 As can be seen from this, the pore size of the nanopores is 20-50 nm, and the average pore size is 30 nm.

[0143] The resulting material has a density of 0.52 g / cm³, a thermal conductivity of 0.072 W / (m·K), a flexural strength of 112 MPa, and a flexural strength of 86 MPa at 500℃. Under conditions of 2000℃ thermal environment, a maximum pressure of 200 kPa, a time of 650 s, and a material thickness of 8 mm, the back temperature is 278℃.

[0144] Among them, the material density was tested according to GB / T34336-2017 "Nanoporous Aerogel Composite Thermal Insulation Products"; the thermal conductivity was tested using the heat flow meter method, specifically GB / T10295-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Thermal Insulation Materials - Heat Flow Meter Method"; the bending strength was tested using the three-point bending method, specifically GB / T1449-2005 "Test Method for Bending Properties of Fiber Reinforced Plastics"; the 500℃ bending strength was tested according to GB / T1449-2005 as the test method standard, and was tested in conjunction with a high-temperature environmental chamber at 500℃, and the bending strength value at this temperature was recorded.

[0145] The high-temperature thermal insulation performance / back temperature test is based on aerospace industry standards or national military standards, and is conducted using QJ20276-2014 "Test Method for Ablation Heat Transfer of Aircraft Thermal Protection Flat Plate Model" and GJB7347-2011 "Test Method for Blunt Wedge of Thermal Protection Materials of Spacecraft in Electric Arc Wind Tunnel". This test simulates a high heat flux environment in an electric arc wind tunnel, and thermocouples are placed on the back (cold side) of the specimen to measure the back temperature in order to evaluate the thermal insulation performance of the material.

[0146] Example 2

[0147] It adopts a three-dimensional quartz fiber gradient braid. The surface fiber density is 0.9 g / cm³, the middle fiber density is 0.65 g / cm³, and the bottom fiber density is 0.35 g / cm³.

[0148] Boric acid, tetraethyl orthosilicate, and n-butanol were added to acetaminophen-formaldehyde resin and stirred at 1500 r / min for 8 h to obtain a silicon- and boron-containing phenolic sol. In this system, the amount of silicon added was 6 wt%, the amount of boron added was 2.5 wt%, and the resin hybridization rate was 7.83%.

[0149] Molding is performed by RTM impregnation under normal pressure, with an injection pressure of 0.08 MPa. The gel is then aged and dried.

[0150] The process employs a low-pressure melting and infiltration technique, with the surface treated with a carborane cage-like modified silicone resin. The melting and infiltration pressure is 0.03 MPa, and the resin is cured at 140°C for 4 hours.

[0151] The resulting material has a density of 0.48 g / cm³, a thermal conductivity of 0.068 W / (m·K), a flexural strength of 105 MPa, and a flexural strength of 82 MPa at 500℃. Under conditions of 2000℃ thermal environment, a maximum pressure of 200 kPa, a time of 600 s, and a material thickness of 8 mm, the back temperature is 285℃.

[0152] Example 3

[0153] It adopts a three-dimensional quartz fiber gradient braid. The surface fiber density is 1.1 g / cm³, the middle fiber density is 0.75 g / cm³, and the bottom fiber density is 0.5 g / cm³.

[0154] Boric acid, tetraethyl orthosilicate, and n-butanol were added to acetaminophen-formaldehyde resin and stirred at 1500 r / min for 8 h to obtain a silicon- and boron-containing phenolic sol. In this system, the amount of silicon added was 8 wt%, the amount of boron added was 3.5 wt%, and the resin hybridization rate was 10.31%.

[0155] The gel is formed by RTM impregnation under normal pressure, with an injection pressure of 0.15 MPa. It is then gelled, aged, and dried.

[0156] The process employs a low-pressure melting and infiltration technique, with the surface treated with a carborane cage-like modified silicone resin. The melting and infiltration pressure is 0.1 MPa, and the curing time is 150℃ for 3 hours.

[0157] The resulting material has a density of 0.58 g / cm³, a thermal conductivity of 0.076 W / (m·K), a flexural strength of 118 MPa, and a flexural strength of 90 MPa at 500℃. Under conditions of 2000℃ thermal environment, a maximum pressure of 200 kPa, a time of 700 s, and a material thickness of 8 mm, the back temperature is 270℃.

[0158] Performance Testing and Results Analysis

[0159] The preparation process parameters for Examples 1-3 are shown in Table 1:

[0160] Table 1

[0161]

[0162] The material property test results of Examples 1-3 are shown in Table 2:

[0163] Table 2

[0164]

[0165] The test results in Tables 1 and 2 show that:

[0166] In the three embodiments, the fiber densities of the high-density layers were 1.0 g / cm³, 0.9 g / cm³, and 1.1 g / cm³, respectively; the medium-density layers were 0.7 g / cm³, 0.65 g / cm³, and 0.75 g / cm³, respectively; and the low-density layers were 0.4 g / cm³, 0.35 g / cm³, and 0.5 g / cm³, respectively. Although the three embodiments differed in the magnitude of the gradient density change, they all maintained good mechanical properties and back-temperature control, and did not experience sudden performance changes or interface defects due to differences in the gradient change rate.

[0167] The thermal conductivity of the three embodiments remained stable between 0.068 and 0.076 W / (m·K), all meeting the design requirement of ≤0.08 W / (m·K). This indicates that within this hybridization range, the phenolic aerogel can form a uniform nanoporous structure with a pore size of 20-50 nm, and the pore structure will not collapse or the thermal conductivity will increase significantly due to slight deviations in the hybridization ratio, verifying that the hybrid resin has good process tolerance.

[0168] Furthermore, the room temperature flexural strengths of the three embodiments were 112 MPa, 105 MPa, and 118 MPa, respectively, and the flexural strengths at 500°C were 86 MPa, 82 MPa, and 90 MPa, respectively, all significantly higher than those of traditional aerogel materials. In Example 3, the fiber density of each layer was higher than that of Example 2, resulting in correspondingly higher room temperature and 500°C flexural strengths (118 MPa vs. 105 MPa, 90 MPa vs. 82 MPa), while the material density only increased from 0.48 g / cm³ to 0.58 g / cm³, and the thermal conductivity only increased from 0.068 W / (m·K) to 0.076 W / (m·K). This demonstrates that the increased density of the gradient fiber structure can simultaneously meet the dual functional requirements of thermal insulation and load-bearing capacity. Because the increase in density of the gradient fiber structure is gradual, heat undergoes a continuous thermal resistance gradient as it is conducted from the high-density layer to the medium- and low-density layers. The thermal conductivity does not increase sharply due to the increase in surface layer density, thus ensuring the synergy between thermal insulation and load-bearing capacity.

[0169] The flexural strength retention rates of the three embodiments at 500℃ were 76.8% (86 / 112), 78.1% (82 / 105), and 76.3% (90 / 118), respectively, all remaining above 75%. The silicon- and boron-modified phenolic sol and the ceramicized protective layer of the surface carborane cage-like structure modified organosilicon resin have a combined effect. Despite differences in fiber density, hybridization rate, and curing temperature, the high-temperature strength retention rates of the three embodiments were highly consistent, concentrated in the range of 76-78%. The main reason is that silicon forms a Si-Si network structure at high temperatures, and boron promotes the high-temperature ceramicization of the resin and improves residual strength; both synergistically enhance the structural stability of the material at high temperatures. Simultaneously, the ceramicized network formed in situ by the dense surface layer at high temperatures forms a fusion bond with the high-density quartz fiber layer. This fusion bond is essentially a chemical bond and mechanical interlocking structure formed by the interfacial chemical reaction between the ceramicized products and the SiO2 on the quartz fiber surface, thus avoiding thermal stress concentration and interfacial debonding.

[0170] Under a thermal environment of 2000℃ and a pressure of 200kPa, the back temperatures of the three embodiments were 278℃, 285℃, and 270℃, respectively, all ≤300℃. Although Embodiment 2 had the lowest density and the most gradual gradient span in the thickness direction, its back temperature of 285℃ still met the design requirement of ≤300℃; while Embodiment 3 had the highest density and the strongest surface erosion resistance, with a back temperature of 270℃ or even lower. This phenomenon indicates that the thermal insulation effect of the present invention is not simply achieved by low density, but by the synergistic effect of the continuous thermal resistance gradient structure and the low thermal conductivity nanoporous aerogel matrix. At the same time, the fusion connection between the dense surface layer and the high-density layer ensures that there are no air gaps or defect layers with abrupt changes in thermal conductivity at the interface under high temperature and high pressure conditions, avoiding the uncertainty of additional thermal resistance at the interface, and allowing heat flow to attenuate in an orderly manner according to the design gradient when passing through each layer. This integrated structure makes the thermal insulation effect predictable and repeatable, and does not deviate significantly from the expectation due to differences in density or gradient change rate.

[0171] The present invention further provides a detection example: high-temperature heating treatment at 850°C.

[0172] Samples were cut from the surface-dense gradient-reinforced phenolic aerogel thermal protection material sheet or block prepared in Example 1 using a diamond wire cutter or a low-speed precision cutter. The sample size was 10mm × 10mm × 5mm (length × width × thickness).

[0173] Before heat treatment, the macroscopic morphology of the sample should be photographed and recorded. The photographing conditions (light source, angle, background, camera model and parameters) should be consistent with the photographing conditions after treatment.

[0174] Heating was performed using a box-type high-temperature resistance furnace (muffle furnace). The sample was placed in a high-temperature crucible made of alumina (Al2O3) or quartz and then placed inside the high-temperature resistance furnace. The maximum operating temperature was 1000℃. The heating process was as follows: the temperature was increased from room temperature to 850℃ at a rate of 5-10℃ / min; and then held at 850℃±5℃ for 2 hours. After the holding period, the heating power was turned off, and the sample was allowed to cool naturally to room temperature with the furnace.

[0175] The heating process is carried out in an air atmosphere. The air contains approximately 21% oxygen.

[0176] The sample was removed after cooling to room temperature. Images of the sample before and after treatment are shown below. Figure 5 As shown on the left, the electron microscope image of the product treated at 850℃ for 2 hours is as follows. Figure 5 As shown on the right.

[0177] The images show that the nanoporous structure remains intact, the pore size has not changed significantly, and a borosilicate glass phase has been formed.

[0178] This invention further provides wind tunnel testing, in which the heat flux reaches a maximum of 1300 KW / m in a typical wind tunnel test. 2 The maximum pressure was 120 kPa, the test time was 200 s, the surface temperature of the test piece was 2000 ℃, and the maximum back temperature of the test piece was 187 ℃. The test piece consisted of 7.5 mm dense gradient reinforced phenolic aerogel and a 2.5 mm metal backing plate.

[0179] The surface morphology of the specimen after wind tunnel testing was captured using a high-resolution digital camera, as shown in the image below. Figure 6 As shown.

[0180] A small piece measuring 10×10×5mm was cut from the central ablation zone of the sample. The sample surface was cleaned with organic solvents such as acetone to remove contaminants, and then thoroughly dried. The sample was firmly attached to the metal sample stage with conductive adhesive to ensure good conductivity. A 5-10nm gold (Au) or platinum (Pt) thin film was deposited on the surface using an ion sputtering instrument to eliminate charge accumulation under electron beam irradiation and obtain a clear image. The prepared sample was placed in a SEM and observed and photographed under an accelerating voltage of 5-15kV to capture the microstructure of the surface.

[0181] SEM image of the surface as follows Figure 7 As shown.

[0182] from Figure 3 It can be seen that the surface of the test piece exhibits a complete, continuous morphological feature without obvious macroscopic defects. The material surface shows the unique color of the ceramic products, and the color is uniform, indicating that the surface temperature field is uniformly distributed and the ceramic reaction is sufficient and consistent in the in-plane direction.

[0183] from Figure 4 It can be seen that the blurred fiber edges and the continuous morphological gradient characteristics with the surrounding ceramization products indicate that the two materials underwent mutual diffusion and melting connection at ultra-high temperature. Moreover, the ceramization products fill the pores between the fibers, forming a three-dimensional interconnected integrated network, rather than isolated and dispersed granular ceramic products. This shows that the ceramization products of carborane-modified organosilicon resin form a continuous and dense network structure.

[0184] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. All such modifications or substitutions should be covered within the protection scope of this application, and should not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application. Therefore, the protection scope of this application should be determined by the protection scope of the claims.

Claims

1. A method for preparing a surface-dense gradient-reinforced phenolic aerogel thermal protection material, characterized in that, Includes the following steps: S100. Prepare an organic-inorganic hybrid phenolic sol, wherein the organic-inorganic phenolic sol is formed from a phenolic sol containing a silicon source and a boron source; S200. Prepare a gradient three-dimensional quartz fiber braided preform, wherein the preform is configured to form a low-density braided region, a medium-density braided region, and a high-density braided region sequentially from the inside to the outside along the thickness direction. S300. The phenolic sol is injected into the preform for impregnation, and then a sol-gel treatment is performed. Inorganic elements are introduced in situ and uniformly dispersed during the formation of the phenolic resin molecular network to construct a hybrid cross-linked structure in which the organic polymer network and the inorganic oxide network interpenetrate each other. At the same time, as the solvent evaporates, a uniform nanoporous structure is formed in the phenolic sol to obtain a hybrid phenolic aerogel block. The pore size of the nanopore is 20-50 nm. S400. A carborane cage-like modified silicone resin is infiltrated into the phenolic aerogel block. The silicone resin is capillarily attached to the inside of the phenolic aerogel block along the nanopores. After curing, the silicone resin forms a densified layer on the surface of the phenolic aerogel block. Organic compounds containing silicon and boron elements in the phenolic sol are grafted in situ onto the side chains of the phenolic resin in the phenolic sol.

2. The preparation method according to claim 1, characterized in that, At 1900-2100℃, the densification layer undergoes in-situ ceramization to form a dense ceramization network. The ceramization network is fused with the quartz fibers in the phenolic aerogel block, and the in-situ grafted organic matter generates a borosilicate glass phase at high temperature.

3. The preparation method according to claim 1, characterized in that, In step S100, the phenolic sol is prepared as follows: Boron-modified components, silicon-modified components, curing agents, and organic solvents are added to phenolic resin and stirred to dissolve them to obtain the phenolic sol. The phenolic sol is then sealed and placed in an 80°C water bath. The stirring speed was 500 r / min to 2000 r / min, the dissolution time was 4 h to 12 h, and the temperature was room temperature.

4. The preparation method according to claim 3, characterized in that, The phenolic resin is any one or more of barium phenolic resin or aminophenolic resin; The silicon-modifying component is one or more of tetraethyl orthosilicate and methoxysilane, and the amount of silicon-modifying component added is 3-10 wt% based on the solid mass of phenolic resin. The boron-modifying component is one or more of tributylboronic acid ester and triacetylazaborane, and the amount of the boron-modifying component added is 1-5 wt% based on the solid mass of the phenolic resin. The curing agent is hexamethylenetetramine.

5. The preparation method according to claim 4, characterized in that, The hybridization rate of the organic-inorganic hybrid components in the phenolic sol is 3.85-13.04%, preferably 6.54-10.71%. The organic-inorganic hybridization rate of the organic-inorganic hybrid component is calculated according to Equation I: ...............Formula I; Wherein, H is the organic-inorganic hybridization rate, ms is the solid mass of the silicon-modified component, mb is the solid mass of the boron-modified component, and mp is the solid mass of the phenolic resin.

6. The preparation method according to claim 5, characterized in that, In step S300, the sol-gel treatment includes the following steps: The impregnated preform was aged for 3 days, then air-dried at room temperature for 1 day, and then blow-dried at 50°C and 80°C for 1 day respectively to obtain hybrid phenolic aerogel blocks.

7. The preparation method according to claim 1, characterized in that, In step S400, the curing temperature is 140℃~150℃.

8. The preparation method according to claim 7, characterized in that, The structural formula of the organosilicon resin is shown in Formula II: ...Form II.

9. A surface-dense gradient-reinforced phenolic aerogel thermal protection material prepared by the preparation method according to any one of claims 1-8, characterized in that, include: A gradient three-dimensional quartz fiber braided preform, wherein the preform consists of a low-density braided region, a medium-density braided region, and a high-density braided region from the inside to the outside along the thickness direction, so that a continuous thermal resistance gradient is formed inside the material. The phenolic aerogel matrix is ​​composed of phenolic resin and organic compounds containing silicon and boron elements grafted in situ onto its side chains, and is filled in the preform. The phenolic aerogel matrix has a uniform nanoporous structure. A densification layer is filled along the nanopores on the preform. The densification layer is composed of an organosilicon resin modified with a carborane cage structure and is bonded to the quartz fiber. The fiber density of the high-density braided region of the gradient three-dimensional quartz fiber braided preform is 0.8-1.2 g / cm³, the fiber density of the medium-density braided region is 0.6-0.8 g / cm³, and the fiber density of the low-density braided region is 0.3-0.6 g / cm³.

10. The preparation method according to any one of claims 1-8 or the application of the material according to claim 9 in the field of aircraft, characterized in that, At 1900-2100℃, the densification layer on the surface of the surface-densified gradient-reinforced phenolic aerogel thermal protection material undergoes in-situ ceramization, forming a dense ceramization network. The ceramization network is fused with the quartz fibers in the phenolic aerogel block, and the organic matter containing silicon and boron elements grafted in-situ onto the side chains of the phenolic sol generates a borosilicate glass phase at high temperature.