A modified basalt fiber reinforced composite material and its preparation method

By blending modified basalt fiber with modified EPDM rubber to construct a dual-network structure, the problem of poor interfacial compatibility between basalt fiber and polypropylene matrix was solved, and the impact resistance and high temperature resistance of the composite material were improved.

CN123062835APending Publication Date: 2026-11-10山东坤宇交通科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611344964.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The poor interfacial compatibility between basalt fiber and polypropylene matrix leads to insufficient impact resistance of the composite material. Existing technologies using compatibilizers have limited improvement effects and are costly, and the interface is prone to aging and debonding under long-term use.

Method used

By modifying basalt fibers with hydroxyl silicone oil and blending them with modified EPDM rubber, a dual-network structure is constructed through the formation of stable Si-O-Si and Si-OB chemical bonds, which enhances the interfacial bonding and compatibility between the fibers and the matrix.

Benefits of technology

It significantly improves the impact resistance and high temperature resistance of basalt fiber reinforced composite materials, forms uniformly dispersed reinforcing and toughening phases, and improves the overall mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a modified basalt fiber reinforced composite material and its preparation method, belonging to the field of polymer materials technology. The modified basalt fiber reinforced composite material of this invention is obtained by melt blending polypropylene as the base material, modified basalt fiber as the reinforcing filler, and modified ethylene propylene diene monomer (EPDM) rubber as the compatibilizer. The modified basalt fiber is obtained by modifying hydroxyl silicone oil; the modified EPDM rubber is obtained by grafting vinyl phenyl boric acid onto EPDM rubber. In the preparation of the modified basalt fiber reinforced composite material of this invention, the modified EPDM rubber and modified basalt fiber are first blended at high temperature, and then melt-blended with polypropylene as the base material. The modified basalt fiber reinforced composite material obtained by this invention has good mechanical properties and excellent heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, specifically to a modified basalt fiber reinforced composite material and its preparation method. Background Technology

[0002] Basalt fiber is an inorganic, non-metallic, high-performance fiber made from natural basalt ore through high-temperature melting and drawing processes. This fiber not only possesses excellent tensile strength and elastic modulus but also boasts numerous advantages such as high-temperature resistance, corrosion resistance, sound absorption and heat insulation, and good electrical insulation. Furthermore, basalt fiber raw materials are widely available, the production process is pollution-free, and it is biodegradable after disposal, making it a green and environmentally friendly reinforcing material with great development potential. In the field of composite materials, combining basalt fiber with a polymer matrix can fully leverage its reinforcing effect, leading to its widespread application in automotive lightweighting, building materials, aerospace, and environmental engineering.

[0003] Polypropylene (PP), a general-purpose thermoplastic resin, is one of the most widely used polymer matrices due to its low density, good chemical resistance, ease of processing and molding, and low cost. Theoretically, combining basalt fibers with polypropylene can produce composite materials that combine lightweight, high strength, and low cost, with broad market application prospects. However, in practical applications, significant compatibility issues exist between basalt fibers and the polypropylene matrix. The surface of basalt fibers is inert and rich in polar groups, while polypropylene is a non-polar polymer, resulting in extremely weak interfacial adhesion. This poor interfacial compatibility prevents effective stress transfer between the matrix and fibers, severely limiting the overall mechanical properties of the composite material, especially its impact resistance, which often fails to meet the requirements of actual working conditions.

[0004] To address the aforementioned issue of poor interfacial compatibility, existing technologies typically employ the addition of compatibilizers, such as maleic anhydride-grafted polypropylene (PP-g-MAH). While this method can improve interfacial bonding to some extent, it often requires a large proportion of compatibilizer to achieve the desired effect. This not only increases material costs but may also adversely affect the toughness and other physical properties of the polypropylene matrix itself. Furthermore, existing technologies have attempted to encapsulate basalt fibers with ethylene propylene diene monomer (EPDM) to improve the impact resistance of the composite material through the buffering effect of the rubber layer and interfacial compatibility. However, this encapsulation method still has several shortcomings in practical applications: firstly, the uniformity of EPDM encapsulation of fibers is poor, making it difficult to form a continuous and dense coating layer; secondly, during high-temperature melt processing, the compatibility between EPDM and the polypropylene matrix remains limited, and long-term use can easily lead to aging and debonding at the interface, resulting in insufficient long-term durability of the composite material.

[0005] Therefore, there is an urgent need to develop a modified basalt fiber reinforced composite material and its preparation method to effectively solve the above-mentioned interfacial compatibility problem and further improve the impact resistance and other mechanical properties of the composite material. Summary of the Invention

[0006] The purpose of this invention is to provide a modified basalt fiber reinforced composite material and its preparation method to solve the technical problems mentioned in the background art.

[0007] The technical solution to achieve the objective of this invention is: In a first aspect, the present invention provides a modified basalt fiber reinforced composite material, wherein the modified basalt fiber reinforced composite material is obtained by melt blending polypropylene as a base material, modified basalt fiber as a reinforcing filler, and modified EPDM rubber as a compatibilizer.

[0008] Furthermore, the amount of modified basalt fiber added is 4~8 wt%.

[0009] Furthermore, the modified basalt fiber is obtained by modifying short-cut basalt fiber with hydroxyl silicone oil. The hydroxyl silicone oil molecular chain contains active silanol groups at both ends, which can undergo condensation reaction with the silanol groups on the surface of the basalt fiber to form stable Si-O-Si chemical bonds, thereby grafting and modifying the basalt fiber.

[0010] Furthermore, the amount of modified EPDM rubber added is 1 to 2 times that of modified basalt fiber.

[0011] Furthermore, the modified EPDM rubber is obtained by grafting EPDM rubber with vinylphenylboronic acid.

[0012] In a second aspect, the present invention provides a method for preparing a modified basalt fiber reinforced composite material as described in the first aspect, comprising the following steps: (1) Weighing and mixing ingredients; (2) Under nitrogen protection, the modified basalt fiber is heated to 135~140℃, then the modified EPDM rubber is added, and the temperature is further increased to 175~180℃. The mixture is kept warm and mixed for 110~130 min to obtain the mixture. (3) The mixture obtained in step (2) is mixed with polypropylene in a mixer and 0.02~0.03wt% of polypropylene is added. The mixing temperature is controlled at 190~210℃ and the mixing time is controlled at 4~6min.

[0013] Further, the preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for at least 1 hour, then washed with deionized water 3-5 times, and dried to constant weight to obtain pretreated basalt fiber; an ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 2-4 wt% is prepared using ethanol solution as solvent, and stirred with a glass rod to fully dissolve it; the pretreated basalt fiber is placed in the ethanol solution of hydroxyl-terminated polysiloxane, soaked for at least 30 minutes, then removed and air-dried at room temperature to obtain modified basalt fiber.

[0014] Further, the preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 1-3 minutes, then 3wt%-5wt% vinylphenylboronic acid and 0.1wt%-0.15wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 120-130°C for 6-8 minutes to obtain the modified EPDM rubber.

[0015] Furthermore, the ethylene mass fraction of the EPDM rubber is 49%~55%.

[0016] Furthermore, the grafting rate of the vinylphenylboronic acid onto the EPDM rubber is 0.29%~0.56%.

[0017] By adopting the above technical solution, the present invention has the following beneficial effects: (1) The modified basalt fiber reinforced composite material of the present invention is obtained by melt blending polypropylene as base material, modified basalt fiber as reinforcing filler and modified EPDM rubber as compatibilizer. The modified basalt fiber reinforced composite material has high strength, good impact resistance and good high temperature resistance.

[0018] (2) The modified basalt fiber of the present invention is added at a rate of 4 to 8 wt%. At this rate, the strength is higher, the impact resistance is better, and the high temperature resistance is better.

[0019] (3) The modified basalt fiber of the present invention is obtained by surface modification treatment of short-cut basalt fiber with hydroxyl silicone oil. The hydroxyl silicone oil molecular chain contains active silanol groups at both ends, which can undergo condensation reaction with the silanol groups on the surface of basalt fiber to form stable Si-O-Si chemical bonds. Thus, the grafting on the fiber surface not only significantly increases the roughness of the fiber surface and enhances the mechanical interlocking effect between the fiber and the matrix material, but also effectively fills the microcrack defects on the fiber surface due to its excellent thermal stability and prevents the oxidation of ferrous ions inside the fiber at high temperature. Thus, the mechanical properties and heat resistance of basalt fiber are greatly improved.

[0020] (4) The modified EPDM rubber of the present invention is obtained by grafting vinyl phenylboronic acid onto EPDM rubber. The vinyl groups in vinyl phenylboronic acid undergo free radical grafting reaction with the unsaturated double bonds on the EPDM molecular chain under the action of an initiator, introducing phenylboronic acid groups into the side chain of EPDM. On the one hand, the phenylboronic acid groups contain a stable boron-oxygen hexacyclic structure and have a high thermal decomposition temperature, which can effectively improve the heat resistance of EPDM rubber. On the other hand, as a polar functional group, the phenylboronic acid groups can significantly increase the polarity of EPDM, thereby improving its interfacial compatibility with non-polar or weakly polar matrices. When the vinyl phenylboronic acid grafted modified EPDM rubber is blended with basalt fiber modified with hydroxyl silicone oil, the polar groups introduced on the surfaces of the two interact with each other, significantly enhancing the bonding force at the interface between the two phases, so that the modified basalt fiber is uniformly dispersed in the modified EPDM rubber matrix, avoiding fiber agglomeration, thereby giving full play to the reinforcing effect of the fiber and the toughening effect of the rubber.

[0021] (5) In the preparation of the modified basalt fiber reinforced composite material of the present invention, the modified EPDM rubber and modified basalt fiber are first blended at high temperature and then melt-blended with polypropylene as the base material; the unreacted silanol groups remaining on the surface of the modified basalt fiber undergo a condensation reaction with the phenylboronic acid groups on the side chains of the modified EPDM rubber to form stable Si-OB chemical bonds, thereby generating phenyl-containing polyborosiloxane (PBS) molecular chains in situ; these PBS molecular chains crosslink with the EPDM rubber molecular chains to construct a double network structure; this double network structure relies on the flexibility of PBS at low frequencies and its rapid hardening and energy dissipation under high-frequency impact, on the other hand... Leveraging the excellent elasticity and aging resistance of the EPDM matrix, it synergistically achieves efficient absorption and dispersion of impact energy. Simultaneously, it ensures that the modified basalt fibers are uniformly dispersed in the rubber matrix, preventing agglomeration and thus forming an effective stress transfer path. Subsequently, this pre-dispersion system is melt-blended and extruded with polypropylene (PP) matrix, resulting in a composite material with uniformly dispersed reinforcing and toughening phases in the polypropylene matrix. This not only significantly enhances the interfacial bonding strength between the basalt fibers and the matrix but also fully utilizes the impact hardening and energy dissipation characteristics of polyborosiloxane, thereby further improving the impact resistance of the modified basalt fiber reinforced composite material. Detailed Implementation

[0022] To better understand the above technical solution, the following will provide a detailed explanation of the technical solution in conjunction with specific implementation methods.

[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.

[0024] Therefore, the following detailed description of embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0025] The following embodiments are only used to illustrate the technical solutions of the present invention more clearly, and should not be used to limit the scope of protection of the present invention.

[0026] The polypropylene used is polypropylene QPB08, sourced from China Petroleum & Chemical Corporation (Sinopec).

[0027] The basalt fibers are 6 mm long and 12 μm in diameter.

[0028] The mass fraction of ethylene in EPDM rubber is 49%~55%.

[0029] Vinylphenylboronic acid includes at least one of 2-vinylphenylboronic acid, 3-vinylphenylboronic acid, and 4-vinylphenylboronic acid. The following examples use 4-vinylphenylboronic acid.

[0030] Example 1 A method for preparing a modified basalt fiber reinforced composite material, comprising the following steps: (1) Weighing and mixing: 100 parts by weight of polypropylene, 4 parts by weight of modified basalt fiber, and 4 parts by weight of modified EPDM rubber; (2) Under nitrogen protection, the modified basalt fiber was heated to 135°C, and then the modified EPDM rubber was added. The temperature was then raised to 175°C and kept warm for 130 min to obtain the mixture. (3) The mixture obtained in step (2) is mixed with polypropylene in a mixer and 0.02 wt% of polypropylene is added. The mixing temperature is controlled at 190°C and the mixing time is controlled at 6 min.

[0031] The preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for 1 hour, then washed three times with deionized water and dried to constant weight to obtain pretreated basalt fiber; an ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 2 wt% is prepared using ethanol solution as solvent, and stirred with a glass rod to fully dissolve it; the pretreated basalt fiber is placed in the ethanol solution of hydroxyl-terminated polysiloxane, soaked for 30 minutes, then removed and air-dried at room temperature to obtain modified basalt fiber.

[0032] The preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 1 min, then 3 wt% vinylphenylboronic acid and 0.1 wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 120°C for 8 min to obtain a modified EPDM rubber with a grafting rate of 0.29%.

[0033] Example 2 A method for preparing a modified basalt fiber reinforced composite material, comprising the following steps: (1) Weighing and mixing: 100 parts by weight of polypropylene, 6 parts by weight of modified basalt fiber, and 9 parts by weight of modified EPDM rubber; (2) Under nitrogen protection, the modified basalt fiber was heated to 140°C, and then the modified EPDM rubber was added. The temperature was then raised to 180°C and kept warm for 120 minutes to obtain the mixture. (3) The mixture obtained in step (2) is mixed with polypropylene in a mixer and 0.025 wt% of polypropylene is added. The mixing temperature is controlled at 200℃ and the mixing time is controlled at 5 min.

[0034] The preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for 1 hour, then washed 5 times with deionized water and dried to constant weight to obtain pretreated basalt fiber; an ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 3 wt% is prepared using ethanol solution as solvent, and stirred with a glass rod to fully dissolve it; the pretreated basalt fiber is placed in the ethanol solution of hydroxyl-terminated polysiloxane, soaked for 30 minutes, then removed and air-dried at room temperature to obtain modified basalt fiber.

[0035] The preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 2 minutes, then 4 wt% vinylphenylboronic acid and 0.15 wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 130°C for 8 minutes to obtain a modified EPDM rubber with a grafting rate of 0.56%.

[0036] Example 3 A method for preparing a modified basalt fiber reinforced composite material, comprising the following steps: (1) Weighing and mixing: 100 parts by weight of polypropylene, 8 parts by weight of modified basalt fiber, and 16 parts by weight of modified EPDM rubber; (2) Under nitrogen protection, the modified basalt fiber was heated to 140°C, and then the modified EPDM rubber was added. The temperature was then raised to 180°C and kept warm for 110 min to obtain the mixture. (3) The mixture obtained in step (2) is mixed with polypropylene in a mixer and 0.03 wt% of polypropylene is added. The mixing temperature is controlled at 190°C and the mixing time is controlled at 4 min.

[0037] The preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for 1 hour, then washed 5 times with deionized water and dried to constant weight to obtain pretreated basalt fiber; an ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 4 wt% is prepared using ethanol solution as solvent, and stirred with a glass rod to fully dissolve it; the pretreated basalt fiber is placed in the ethanol solution of hydroxyl-terminated polysiloxane, soaked for 30 minutes, then removed and air-dried at room temperature to obtain modified basalt fiber.

[0038] The preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 1 min, then 5 wt% vinylphenylboronic acid and 0.15 wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 130°C for 8 min to obtain modified EPDM rubber with a grafting rate of 0.40%.

[0039] Comparative Example 1 The only difference between Comparative Example 1 and Example 2 is that the modified basalt fiber reinforced composite material uses basalt fiber instead of modified basalt fiber.

[0040] Comparative Example 2 The only difference between Comparative Example 2 and Example 2 is that the modified basalt fiber reinforced composite material uses EPDM rubber instead of modified EPDM rubber.

[0041] Comparative Example 3 The only difference between Comparative Example 3 and Example 2 is that the modified basalt fiber reinforced composite material uses basalt fiber and EPDM rubber.

[0042] Comparative Example 4 The only difference between Comparative Example 4 and Example 2 is that the components were directly mixed and kneaded during the preparation of the modified basalt fiber reinforced composite material. Specifically: A method for preparing a modified basalt fiber reinforced composite material, comprising the following steps: (1) Weighing and mixing: 100 parts by weight of polypropylene, 6 parts by weight of modified basalt fiber, and 9 parts by weight of modified EPDM rubber; (2) The modified basalt fiber, modified EPDM rubber and polypropylene are put into a mixer and mixed for 5 minutes. Then, 0.025 wt% of dicumyl peroxide of polypropylene is added and mixed. The mixing temperature is controlled at 200℃ and the mixing time is controlled at 5 minutes.

[0043] The preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for 1 hour, then washed 5 times with deionized water and dried to constant weight to obtain pretreated basalt fiber; an ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 3 wt% is prepared using ethanol solution as solvent, and stirred with a glass rod to fully dissolve it; the pretreated basalt fiber is placed in the ethanol solution of hydroxyl-terminated polysiloxane, soaked for 30 minutes, then removed and air-dried at room temperature to obtain modified basalt fiber.

[0044] The preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 2 minutes, then 4 wt% vinylphenylboronic acid and 0.15 wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 130°C for 8 minutes to obtain a modified EPDM rubber with a grafting rate of 0.56%.

[0045] Comparative Examples 5-8 The only difference between Comparative Examples 5-8 and Example 2 is that the amount of modified basalt fiber added is 2wt%, 3wt%, 9wt%, and 10wt%, respectively.

[0046] Example of effect Table 1 below shows the performance test results of the modified basalt fiber reinforced composite materials of Examples 1-3 and Comparative Examples 1-8: Table 1

[0047] As shown in Table 1, the modified basalt fiber reinforced composite materials of Examples 1-3 have high strength and good impact resistance.

[0048] The only difference between Comparative Example 1 and Example 2 is that the modified basalt fiber reinforced composite material uses basalt fiber instead of modified basalt fiber. Compared with Example 2, the tensile strength decreased by 12.2% and the impact strength decreased by 22.3%, indicating that the surface of the unmodified fiber lacks polar groups, the interfacial bonding is weak and there is no double network structure, resulting in poor mechanical properties.

[0049] The only difference between Comparative Example 2 and Example 2 is that the modified basalt fiber reinforced composite material uses EPDM rubber instead of modified EPDM rubber. Compared with Example 2, the tensile strength decreased by 15.8% and the impact strength decreased by 28.6%.

[0050] The only difference between Comparative Example 3 and Example 2 is that the modified basalt fiber reinforced composite material uses basalt fiber and EPDM rubber. The basalt fiber is wrapped in EPDM rubber and then dispersed and compatible with polypropylene. Compared with Example 2, the performance is further reduced.

[0051] The only difference between Comparative Example 4 and Example 2 is that the components were directly mixed and kneaded during the preparation of the modified basalt fiber reinforced composite material. Compared with Example 2, the tensile strength decreased by 12.1% and the impact strength decreased by 19.0%, indicating that the premixing process is crucial for forming a uniform dispersion and a double network structure. Direct mixing can easily lead to insufficient dispersion and an incomplete double network structure.

[0052] The only difference between Comparative Examples 5-8 and Example 2 is the amount of modified basalt fiber added, which is 2, 3, 9, and 10%. As the amount of modified basalt fiber added increases, the tensile strength and impact strength of the composite material show a trend of first increasing and then decreasing: the performance improves when the amount of added basalt fiber increases from 2 wt% to 3 wt%, reaches the maximum value at 6 wt%, and the performance begins to decline when the amount of added basalt fiber continues to increase to 9 wt% and 10 wt%. This indicates that the mechanical properties are optimal when the amount of modified basalt fiber added is 4-8 wt%. When the amount of added basalt fiber is too low, the reinforcing effect is insufficient, and when the amount of added basalt fiber is too high, the fiber is prone to agglomeration and the interfacial stress is concentrated, which weakens the mechanical properties.

[0053] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A modified basalt fiber reinforced composite material, characterized in that, The modified basalt fiber reinforced composite material is obtained by melt blending polypropylene as the base material, modified basalt fiber as the reinforcing filler, and modified EPDM rubber as the compatibilizer.

2. The modified basalt fiber reinforced composite material according to claim 1, characterized in that, The amount of modified basalt fiber added is 4~8wt%.

3. The modified basalt fiber reinforced composite material according to claim 1, characterized in that, The modified basalt fiber is obtained by modifying short-cut basalt fiber with hydroxyl silicone oil.

4. The modified basalt fiber reinforced composite material according to claim 1, characterized in that, The amount of modified EPDM rubber added is 1 to 2 times that of modified basalt fiber.

5. The modified basalt fiber reinforced composite material according to claim 1, characterized in that, The modified EPDM rubber is obtained by grafting vinylphenylboronic acid onto EPDM rubber.

6. A method for preparing a modified basalt fiber reinforced composite material as described in any one of claims 1 to 5, characterized in that the steps include... include: (1) Weigh and prepare the ingredients; (2) Under nitrogen protection, the modified basalt fiber is heated to 135~140℃, then the modified EPDM rubber is added, and the temperature is further increased to 175~180℃. The mixture is kept warm and mixed for 110~130 min to obtain the mixture. (3) The mixture obtained in step (2) is mixed with polypropylene in a mixer and 0.02~0.03wt% of polypropylene is added. The mixing temperature is controlled at 190~210℃ and the mixing time is controlled at 4~6min.

7. The method for preparing the modified basalt fiber reinforced composite material according to claim 6, characterized in that, The preparation steps of the modified basalt fiber are as follows: basalt fiber is soaked in acetone and treated in an ultrasonic cleaner for at least 1 hour, then washed with deionized water 3 to 5 times, and dried to constant weight to obtain pretreated basalt fiber. An ethanol solution of hydroxyl-terminated polysiloxane with a mass fraction of 2-4 wt% was prepared using ethanol solution as solvent. The solution was stirred with a glass rod to dissolve the polysiloxane completely. The pretreated basalt fiber was then placed into the ethanol solution of hydroxyl-terminated polysiloxane and soaked for at least 30 minutes. After soaking, the fiber was removed and allowed to air dry at room temperature to obtain modified basalt fiber.

8. The method for preparing the modified basalt fiber reinforced composite material according to claim 6, characterized in that, The preparation steps of the modified EPDM rubber are as follows: EPDM rubber is added to a mixer at 120°C and mixed for 1-3 minutes, then 3wt%-5wt% vinylphenylboronic acid and 0.1wt%-0.15wt% di-tert-butyl peroxide diisopropylbenzene are added, and the mixture is mixed at 120-130°C for 6-8 minutes to obtain the modified EPDM rubber.

9. The method for preparing the modified basalt fiber reinforced composite material according to claim 8, characterized in that, The ethylene content of the EPDM rubber is 49% to 55% by mass.