A polymer composite material with excellent injection molding flowability and its preparation method
By leveraging the synergistic effect of modified wollastonite whiskers and hyperbranched polyester-grafted polypropylene modifier, the problem of poor melt flow and dispersibility of polypropylene-based composites in thin-walled injection molded products was solved, achieving excellent injection flow and good filler dispersibility.
Patent Information
- Application Number
- CN202611472994.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-10
AI Technical Summary
Polypropylene-based composites exhibit poor melt flowability and dispersibility in thin-walled injection molded products, making it difficult to meet the high requirements for injection flowability. In particular, the melt viscosity increases significantly and the flowability deteriorates after the addition of wollastonite whiskers for reinforcement.
By combining modified wollastonite whisker surface treatment with hyperbranched polyester grafted polypropylene modifier, a chemical bonding interface and molecular-level lubricating layer are formed, which improves the dispersibility and melt flowability of wollastonite whiskers in polypropylene matrix.
It significantly improves the melt flow rate and injection flowability of composite materials, achieving efficient filler dispersion and improved flowability, thus meeting the injection molding requirements of thin-walled products.
Smart Images

Figure CN123062844A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a polymer composite material with excellent injection molding flowability and its preparation method. Background Technology
[0002] The application of polymer composites in thin-walled injection molded products is becoming increasingly widespread. Products such as automotive interior parts, home appliance housings, and electronic and electrical connectors are placing increasingly higher demands on the injection flowability of materials. Thin-walled products typically have a wall thickness of less than 1 mm, resulting in a long flow path and high resistance for the melt in the mold cavity. This requires materials with excellent melt flow rate and mold filling ability; otherwise, short shots, flow marks, weld lines, and other defects are likely to occur.
[0003] Polypropylene (PP) is a commonly used matrix resin for thin-walled injection molded products due to its low density, good chemical resistance, ease of processing and molding, and low cost. However, PP has relatively low melt strength. After adding inorganic fillers for reinforcement and modification, the melt viscosity increases significantly, and the flowability further decreases, making it difficult to meet the injection molding requirements of thin-walled products. Wollastonite whiskers have a high aspect ratio, high modulus, and high thermal stability, and are commonly used reinforcing fillers for PP, effectively improving the strength and rigidity of composite materials. However, Wollastonite whiskers are hydrophilic and have poor compatibility with the PP matrix. They are prone to agglomeration during melt blending. These agglomerates not only fail to provide reinforcement but also become a source of melt flow resistance, leading to a sharp increase in melt viscosity and deterioration of injection molding flowability. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a polymer composite material with excellent injection molding flowability and its preparation method. By modifying the amino groups on the surface of wollastonite whiskers and reacting them with the anhydride groups of maleic anhydride-grafted polypropylene to form a chemical bonding interface, the melt flow rate and injection molding flowability of the composite material are improved, while the dispersibility of wollastonite whiskers is also improved.
[0005] A polymer composite material with excellent injection molding flowability, comprising the following components by weight: 100 parts by weight of polypropylene matrix resin; 8-25 parts by weight of modified wollastonite whiskers; 2-8 parts by weight of hyperbranched polyester-grafted polypropylene modifier; 5-15 parts by weight of ethylene-octene copolymer toughening agent; 0.2-0.8 parts by weight of N,N'-ethylene bis-stearamide; Antioxidant 0.2-0.6 parts by weight; The modified wollastonite whiskers are aminated wollastonite whiskers that have undergone surface treatment with γ-aminopropyltriethoxysilane. The hyperbranched polyester-grafted polypropylene modifier is a graft obtained by melt esterification reaction of hydroxyl-terminated hyperbranched polyester and maleic anhydride-grafted polypropylene.
[0006] Preferably, a method for preparing a polymer composite material with excellent injection molding flowability includes the following steps: Step S1: Weigh out 100 parts by weight of polypropylene matrix resin, 8-25 parts by weight of modified wollastonite whiskers, 2-8 parts by weight of hyperbranched polyester grafted polypropylene modifier, 5-15 parts by weight of ethylene-octene copolymer toughening agent, 0.2-0.8 parts by weight of N,N'-ethylene bis-stearamide, and 0.2-0.6 parts by weight of antioxidant. Step S2: Add the weighed components to a high-speed mixer and mix at 300-800 r / min for 5-20 min at 20-40℃ to obtain a premix. Step S3: Add the premixed material to a twin-screw extruder for melt blending and extrusion. The temperatures from zone one to the die head of the extruder are 180-200℃, 190-210℃, 200-220℃, 210-230℃, 210-230℃, and 200-220℃, respectively. The screw speed is 200-500 r / min, and the melt pressure is controlled at 2-8 MPa. The extrudate is cooled with deionized water, pelletized, and dried to obtain the polymer composite material.
[0007] Preferably, the method for preparing modified wollastonite whiskers includes: Step A1: Add wollastonite whiskers to deionized water at a solid-liquid mass ratio of 1:5-1:10, stir and disperse for 10-30 minutes, add 5%-10% acetic acid aqueous solution to adjust the pH to 4.0-5.0, then add 1.0%-3.0% γ-aminopropyltriethoxysilane by mass of wollastonite whiskers, stir and react at 50-70℃ for 1-3 hours, filter to obtain wet material; Step A2: Dry the wet material at 80-110℃ for 2-6 hours, then heat it to 110-150℃ for 0.5-2 hours, cool, grind, and sieve to obtain modified wollastonite whiskers.
[0008] Preferably, the preparation method of the hyperbranched polyester-grafted polypropylene modifier includes: Step B1: By weight, add 100 parts pentaerythritol, 80-150 parts dimethylolpropionic acid, 0.5-2 parts p-toluenesulfonic acid and 150-300 parts toluene to a reaction vessel, purge with nitrogen, heat to reflux under normal pressure and react with water separation for 2-6 hours to obtain a hydroxyl-terminated hyperbranched polyester solution. Remove toluene by vacuum distillation, cool and pulverize to obtain hydroxyl-terminated hyperbranched polyester. Step B2: By weight, add 100 parts by weight of maleic anhydride-grafted polypropylene and 20-50 parts by weight of hydroxyl-terminated hyperbranched polyester to a melt mixer. Under nitrogen protection and a system pressure of 0.1-0.2 MPa, melt mix at 150-180°C for 5-20 minutes to allow the hydroxyl groups and maleic anhydride groups to undergo a ring-opening esterification reaction, thereby obtaining the melt-grafted product. Step B3: Cool the molten graft material to room temperature, crush and sieve it to obtain hyperbranched polyester-grafted polypropylene modifier.
[0009] Preferably, the grafting rate of maleic anhydride-grafted polypropylene is 0.5%-1.5%, and its melt flow rate is 20-60 g / 10 min at 230℃ / 2.16 kg.
[0010] Preferably, the polypropylene matrix resin is at least one of copolymer polypropylene or homopolymer polypropylene, and its melt flow rate is 10-60 g / 10 min at 230℃ / 2.16 kg; the wollastonite whiskers have an aspect ratio of 10-30 and an average diameter of 2-8 μm.
[0011] Preferably, the mass ratio of the modified wollastonite whiskers to the hyperbranched polyester-grafted polypropylene modifier is 3:1-12:1.
[0012] This invention introduces amino groups into wollastonite whiskers by surface treatment with γ-aminopropyltriethoxysilane. During the melt blending process, the amino groups and the anhydride groups of maleic anhydride-grafted polypropylene undergo an imidization reaction to form a chemically bonded interfacial transition layer, which effectively inhibits whisker agglomeration and improves dispersibility.
[0013] This invention produces a hyperbranched polyester-grafted polypropylene modifier by melt esterification of hydroxyl-terminated hyperbranched polyester with maleic anhydride-grafted polypropylene. Its spherical three-dimensional topological structure forms a molecular-level lubricating layer in the matrix, effectively reducing the entanglement density between polypropylene molecular chains and significantly improving melt flow rate and injection molding fluidity. This invention achieves a balance between high injection molding fluidity and uniform dispersion by utilizing the synergistic effect of modified wollastonite whiskers and the hyperbranched polyester-grafted polypropylene modifier, employing both chemical bonding interfaces and steric hindrance dispersion mechanisms to inhibit whisker agglomeration.
[0014] The preparation method of this invention is simple, and the preparation conditions of the modified wollastonite whiskers and hyperbranched polyester grafted polypropylene modifier are mild and controllable. The melt blending extrusion can be directly completed using existing twin-screw extrusion equipment without the need for additional major equipment investment, making it easy to scale up industrial production. Attached Figure Description
[0015] Figure 1 This is a flowchart of the composite material preparation process.
[0016] Figure 2These are FTIR spectra of wollastonite whiskers before and after modification.
[0017] Figure 3 These are FTIR spectra before and after the synthesis of hyperbranched polyester-grafted polypropylene modifier. Detailed Implementation
[0018] Example 1
[0019] A method for preparing a polymer composite material with excellent injection molding flowability includes the following steps: Step S1: Weigh out 100 parts by weight of polypropylene matrix resin, 8 parts by weight of modified wollastonite whiskers, 2 parts by weight of hyperbranched polyester-grafted polypropylene modifier, 15 parts by weight of ethylene-octene copolymer toughening agent, 0.8 parts by weight of N,N'-ethylene bis-stearamide, and 0.3 parts by weight of antioxidant. The polypropylene matrix resin is homopolymer polypropylene with a melt flow rate of 10 g / 10 min at 230℃ / 2.16 kg. The wollastonite whiskers have an aspect ratio of 10 and an average diameter of 2 μm. The mass ratio of the modified wollastonite whiskers to the hyperbranched polyester-grafted polypropylene modifier is 4:1. Step S2: Add the weighed components to a high-speed mixer and mix at 800 r / min for 5 min at 20°C to obtain a premix. Step S3: Add the premix to a twin-screw extruder for melt blending and extrusion. The temperatures from zone one to the die head of the extruder are 180℃, 190℃, 200℃, 210℃, 210℃, and 200℃ respectively. The screw speed is 200 r / min, and the melt pressure is controlled at 8 MPa. The extrudate is cooled with deionized water, pelletized, and dried to obtain the polymer composite material. The method for preparing the modified wollastonite whiskers includes: Step A1: Add wollastonite whiskers to deionized water at a solid-liquid mass ratio of 1:5, stir and disperse for 10 min, add 5% acetic acid aqueous solution to adjust the pH to 4.0, then add 1.0% γ-aminopropyltriethoxysilane by mass of wollastonite whiskers, stir and react at 50℃ for 1 h, filter to obtain wet material; Step A2: Dry the wet material at 80℃ for 2 hours, then heat it to 110℃ for 0.5 hours, cool, grind, and sieve to obtain modified wollastonite whiskers; The preparation method of the hyperbranched polyester-grafted polypropylene modifier includes: Step B1: By weight, add 100 parts pentaerythritol, 80 parts dimethylolpropionic acid, 0.5 parts p-toluenesulfonic acid and 150 parts toluene to a reaction vessel, purge with nitrogen, heat to reflux under normal pressure and react with water separation for 2 hours to obtain a hydroxyl-terminated hyperbranched polyester solution. Remove toluene by vacuum distillation, cool and pulverize to obtain hydroxyl-terminated hyperbranched polyester. Step B2: By weight, 100 parts by weight of maleic anhydride-grafted polypropylene and 20 parts by weight of hydroxyl-terminated hyperbranched polyester are added to a melt mixer and melt-mixed at 150°C for 5 minutes under nitrogen protection and a system pressure of 0.1 MPa, so that the hydroxyl-terminated groups and maleic anhydride groups undergo a ring-opening esterification reaction to obtain a melt-grafted product; the grafting rate of the maleic anhydride-grafted polypropylene is 0.5%, and its melt flow rate is 20 g / 10 min at 230°C / 2.16 kg. Step B3: Cool the molten graft material to room temperature, crush and sieve it to obtain hyperbranched polyester-grafted polypropylene modifier.
[0020] Example 2
[0021] A method for preparing a polymer composite material with excellent injection molding flowability includes the following steps: Step S1: Weigh out 100 parts by weight of polypropylene matrix resin, 16.5 parts by weight of modified wollastonite whiskers, 5 parts by weight of hyperbranched polyester-grafted polypropylene modifier, 10 parts by weight of ethylene-octene copolymer toughening agent, 0.5 parts by weight of N,N'-ethylene bis-stearamide, and 0.2 parts by weight of antioxidant; the polypropylene matrix resin is copolymer polypropylene, and its melt flow rate is 35 g / 10 min at 230℃ / 2.16 kg; the wollastonite whiskers have an aspect ratio of 20 and an average diameter of 5 μm; the mass ratio of modified wollastonite whiskers to hyperbranched polyester-grafted polypropylene modifier is 3.3:1; Step S2: Add the weighed components to a high-speed mixer and mix at 30°C and 550 r / min for 12.5 min to obtain a premix. Step S3: Add the premix to a twin-screw extruder for melt blending and extrusion. The temperatures from zone one to the die head of the extruder are 190℃, 200℃, 210℃, 220℃, 220℃, and 210℃ respectively. The screw speed is 350 r / min, and the melt pressure is controlled at 5 MPa. The extrudate is cooled with deionized water, pelletized, and dried to obtain the polymer composite material. The method for preparing the modified wollastonite whiskers includes: Step A1: Add wollastonite whiskers to deionized water at a solid-liquid mass ratio of 1:7.5, stir and disperse for 20 min, add 7.5% acetic acid aqueous solution to adjust the pH to 4.5, then add 2.0% γ-aminopropyltriethoxysilane by mass of wollastonite whiskers, stir and react at 60℃ for 2 h, filter to obtain wet material; Step A2: Dry the wet material at 95℃ for 4 hours, then heat it to 130℃ for 1.25 hours, cool, grind, and sieve to obtain modified wollastonite whiskers; The preparation method of the hyperbranched polyester-grafted polypropylene modifier includes: Step B1: By weight, add 100 parts pentaerythritol, 115 parts dimethylolpropionic acid, 1.25 parts p-toluenesulfonic acid and 225 parts toluene to a reaction vessel, purge with nitrogen, heat to reflux under normal pressure and react with water separation for 4 hours to obtain a hydroxyl-terminated hyperbranched polyester solution. Remove toluene by vacuum distillation, cool and pulverize to obtain hydroxyl-terminated hyperbranched polyester. Step B2: By weight, 100 parts by weight of maleic anhydride-grafted polypropylene and 35 parts by weight of hydroxyl-terminated hyperbranched polyester are added to a melt mixer and melt-mixed at 165°C for 12.5 min under nitrogen protection and a system pressure of 0.15 MPa, so that the hydroxyl groups and maleic anhydride groups undergo a ring-opening esterification reaction to obtain a melt-grafted product; the grafting rate of the maleic anhydride-grafted polypropylene is 1.0%, and its melt flow rate is 40 g / 10 min at 230°C / 2.16 kg. Step B3: Cool the molten graft material to room temperature, crush and sieve it to obtain hyperbranched polyester-grafted polypropylene modifier.
[0022] Example 3
[0023] A method for preparing a polymer composite material with excellent injection molding flowability includes the following steps: Step S1: Weigh out 100 parts by weight of polypropylene matrix resin, 25 parts by weight of modified wollastonite whiskers, 8 parts by weight of hyperbranched polyester-grafted polypropylene modifier, 5 parts by weight of ethylene-octene copolymer toughening agent, 0.2 parts by weight of N,N'-ethylene bis-stearamide, and 0.6 parts by weight of antioxidant; the polypropylene matrix resin is copolymer polypropylene, and its melt flow rate is 60 g / 10 min at 230℃ / 2.16 kg; the wollastonite whiskers have an aspect ratio of 30 and an average diameter of 8 μm; the mass ratio of modified wollastonite whiskers to hyperbranched polyester-grafted polypropylene modifier is 3.125:1; Step S2: Add the weighed components to a high-speed mixer and mix at 300 r / min for 20 min at 40°C to obtain a premix. Step S3: Add the premixed material to a twin-screw extruder for melt blending and extrusion. The temperatures from zone one to the die head of the extruder are 200℃, 210℃, 220℃, 230℃, 230℃, and 220℃ respectively. The screw speed is 500 r / min, and the melt pressure is controlled at 2 MPa. The extrudate is cooled with deionized water, pelletized, and dried to obtain the polymer composite material. The method for preparing the modified wollastonite whiskers includes: Step A1: Add wollastonite whiskers to deionized water at a solid-liquid mass ratio of 1:10, stir and disperse for 30 min, add 10% acetic acid aqueous solution to adjust the pH to 5.0, then add 3.0% γ-aminopropyltriethoxysilane by mass of wollastonite whiskers, stir and react at 70℃ for 3 h, filter to obtain wet material; Step A2: Dry the wet material at 110℃ for 6 hours, then heat it to 150℃ for 2 hours, cool, grind, and sieve to obtain modified wollastonite whiskers; The preparation method of the hyperbranched polyester-grafted polypropylene modifier includes: Step B1: By weight, add 100 parts pentaerythritol, 150 parts dimethylolpropionic acid, 2 parts p-toluenesulfonic acid and 300 parts toluene to a reaction vessel, purge with nitrogen, heat to reflux under normal pressure and react with water separation for 6 hours to obtain a hydroxyl-terminated hyperbranched polyester solution. Remove toluene by vacuum distillation, cool and pulverize to obtain hydroxyl-terminated hyperbranched polyester. Step B2: By weight, 100 parts by weight of maleic anhydride-grafted polypropylene and 50 parts by weight of hydroxyl-terminated hyperbranched polyester are added to a melt mixer and melt-mixed at 180°C for 20 minutes under nitrogen protection and a system pressure of 0.2 MPa, so that the hydroxyl groups and maleic anhydride groups undergo a ring-opening esterification reaction to obtain a melt-grafted product; the grafting rate of the maleic anhydride-grafted polypropylene is 1.5%, and its melt flow rate is 60 g / 10 min at 230°C / 2.16 kg. Step B3: Cool the molten graft material to room temperature, crush and sieve it to obtain hyperbranched polyester-grafted polypropylene modifier.
[0024] Comparative Example 1: The modified wollastonite whiskers in Example 1 were replaced with unmodified wollastonite whiskers, and the hyperbranched polyester-grafted polypropylene modifier was replaced with an equal amount of maleic anhydride-grafted polypropylene. The remaining composition and preparation process were the same as in Example 1.
[0025] Comparative Example 2: The modified wollastonite whiskers in Example 1 were replaced with unmodified wollastonite whiskers, while the rest of the composition and preparation process were the same as in Example 1.
[0026] Comparative Example 3: The hyperbranched polyester-grafted polypropylene modifier in Example 1 was replaced with an equal amount of maleic anhydride-grafted polypropylene, while the rest of the composition and preparation process were the same as in Example 1.
[0027] The samples prepared in Example 1 and Comparative Examples 1-3 were subjected to performance testing: The performance testing method is as follows: The samples of each embodiment and comparative example were conditioned for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%.
[0028] Melt flow rate: The test was conducted according to the national standard GB / T3682.1-2018 "Determination of melt mass flow rate and melt volume flow rate of thermoplastics - Part 1: Standard method". The test conditions were 230℃ / 2.16kg. The melt mass flow rate was recorded in g / 10min.
[0029] Injection Molding Flowability: The helical flow length method was used to evaluate injection molding flowability. A standard helical mold was used on an injection molding machine with a barrel temperature of 230℃, a mold temperature of 40℃, an injection pressure of 80MPa, and a holding time of 10s. The flow length of the melt in the helical channel was measured, in mm. A longer flow length indicates better injection molding flowability.
[0030] Filler dispersibility: The fracture morphology of tensile specimens was observed using a scanning electron microscope at a magnification of 5000x to evaluate the uniformity of wollastonite whiskers dispersion in the polypropylene matrix.
[0031] The test results are shown in the table below:
[0032] Results analysis: As shown in the table above, the melt flow rate of Example 1 was 28.5 g / 10 min, the spiral flow length was 186 mm, and the dispersibility evaluation was uniform dispersion with no agglomeration. Comparative Example 1 had a melt flow rate of only 16.2 g / 10 min and a spiral flow length of only 112 mm, and the dispersibility evaluation was characterized by significant agglomeration and interfacial debinding. Comparative Example 2 had a melt flow rate of 18.5 g / 10 min and a spiral flow length of 128 mm, and the dispersibility evaluation was characterized by significant agglomeration and localized debinding. Comparative Example 3 had a melt flow rate of 22.3 g / 10 min and a spiral flow length of 152 mm, and the dispersibility evaluation was characterized by moderate dispersion and a small amount of agglomeration. The melt flow rate and spiral flow length of Example 1 were significantly higher than those of Comparative Examples 1-3, and the packing dispersibility was also the best.
[0033] Comparative Example 1 uses unmodified wollastonite whiskers and maleic anhydride-grafted polypropylene to replace the hyperbranched polyester-grafted polypropylene modifier. The unmodified wollastonite whiskers have a hydrophilic surface and poor compatibility with the polypropylene matrix. During the melt blending process, a large number of agglomerates are formed. The agglomerates become the source of melt flow resistance, resulting in increased melt viscosity and a sharp decrease in fluidity. Maleic anhydride-grafted polypropylene has a linear molecular structure and does not have the spherical three-dimensional topology of hyperbranched polyester. It cannot form an effective lubricating and viscosity-reducing layer in the melt. Therefore, the melt flow rate and spiral flow length are the worst.
[0034] Comparative Example 2, which simply replaced the modified wollastonite whiskers with unmodified wollastonite whiskers, showed a melt flow rate of 18.5 g / 10 min and a spiral flow length of 128 mm, with performance between Comparative Example 1 and Comparative Example 3. This is because the presence of the hyperbranched polyester-grafted polypropylene modifier improved the matrix flowability to some extent, but the hydrophilicity and agglomeration problems of the unmodified wollastonite whisker surface were not fundamentally resolved. The whiskers, dispersed in the matrix as agglomerates, still significantly hindered melt flow.
[0035] Comparative Example 3, which replaced the hyperbranched polyester-grafted polypropylene modifier with maleic anhydride-grafted polypropylene, showed a melt flow rate of 22.3 g / 10 min and a spiral flow length of 152 mm. Its performance was superior to Comparative Examples 1 and 2 but inferior to Example 1. This is because the amination treatment on the surface of the modified wollastonite whiskers improved its interfacial compatibility with the polypropylene matrix and reduced whisker agglomeration. However, maleic anhydride-grafted polypropylene has a linear structure and lacks the spherical topology and numerous terminal functional groups of hyperbranched polyester. Therefore, it cannot form an effective lubricating and viscosity-reducing layer in the melt, resulting in limited improvement in flowability. Furthermore, the lack of hyperbranched polyester's coating and steric hindrance dispersion effect on the whiskers meant that a small amount of whisker agglomeration still occurred.
[0036] In Example 1, after surface treatment with γ-aminopropyltriethoxysilane, modified wollastonite whiskers introduce amino groups onto the whisker surface. These amino groups react with the anhydride groups of maleic anhydride-grafted polypropylene during melt blending, forming a chemically bonded interfacial transition layer. This significantly improves the interfacial bonding between the whiskers and the polypropylene matrix, reducing whisker agglomeration. Simultaneously, the hyperbranched polyester in the hyperbranched polypropylene modifier possesses a spherical three-dimensional topological structure and numerous terminal hydroxyl groups. After grafting with maleic anhydride-grafted polypropylene via melt esterification, the spherical structure of the hyperbranched polyester forms a molecular-level lubricating layer within the polypropylene matrix. Its numerous terminal functional groups extend outwards, effectively reducing the entanglement density between polypropylene molecular chains, thereby improving melt flow rate and injection molding fluidity. Furthermore, the spherical structure of the hyperbranched polyester also exerts a steric hindrance dispersion effect on the wollastonite whiskers, further inhibiting whisker agglomeration. Therefore, Example 1 achieved both excellent injection flowability and good filler dispersibility through the synergistic effect of modified wollastonite whiskers and hyperbranched polyester-grafted polypropylene modifier, while Comparative Examples 1-3 could not simultaneously meet the above performance requirements.
[0037] ·like Figure 1 As shown, line A (left) represents the amination of the whisker surface. Dispersion, pH adjustment, silane addition, drying, and heat treatment are all involved. Maintaining the pH at 4.0-5.0 is crucial; excessive acidity will damage the whisker framework, while excessive alkalinity will exacerbate silane hydrolysis and self-condensation. Line B (right) involves two steps: first, pentaerythritol and DMPA undergo condensation polymerization under p-toluenesulfonic acid catalysis to form a hydroxyl-terminated hyperbranched polyester; second, it is melt-esterified with PP-g-MAH to obtain a grafted product. The confluence section involves high-speed premixing of the products from lines A and B with PP, POE, EBS, and antioxidants before entering a twin-screw extruder. The temperature in six stages increases from 180 ℃ to 230 ℃ and then decreases back to 220 ℃.
[0038] like Figure 2 The image shows the FTIR spectra of wollastonite whiskers before and after modification. The horizontal axis represents wavenumber, and the vertical axis represents transmittance (%). The upper curve in the figure represents KH-550 amino-modified wollastonite whiskers, and the lower curve represents unmodified wollastonite whiskers. The two curves are arranged vertically in a staggered manner for comparison. Figure 2 In the infrared spectrum, unmodified wollastonite whiskers (CaSiO3) exhibit intrinsic absorption. Wollastonite is a chain-like metasilicate, and its intrinsic absorption is observed in the 1000-900 cm⁻¹ range. -1 Strong Si-O stretching absorption band and 500-450 cm -1 It is characterized by Si-O / Ca-O bending vibrations, and its surface often contains adsorbed water; its peak position and assignment are: 3400 cm⁻¹ -1 (Wide, weak) Attribution to ν(OH), representing surface physically adsorbed water; this should be weakened after modification; 1630 cm -1(Weakly) assigned to δ(HOH), representing the bending vibration of adsorbed water, 1085 / 1010 / 965 / 900 cm. -1 Belonging to vas(Si-O-Si) and v(Si-O), it represents the strongest absorption band, a wollastonite framework fingerprint; 680 / 642 cm⁻¹ -1 Belongs to (Si-O-Si), representing a symmetrical stretching of chain-like silicon-oxygen tetrahedra; 566 / 508 / 452 / 428 cm -1 Assigned to δ(Si-O) and v(Ca-O), it is a multiplet in the low wavenumber region, Ca 2+ Coordination environment leads to splitting.
[0039] The newly added characteristic peaks after modification are direct evidence of amination. In the figure, the newly added characteristic peaks after modification and their assignments are: 3372 / 3298 cm⁻¹. -1 The most crucial evidence is the attribution to vas / vs(NH); the two NH stretching vibrations of the primary amine -NH2 form a double peak, which simultaneously suppresses the original broad OH peak because the surface hydrophilic hydroxyl groups are consumed by silane condensation. (1560 cm⁻¹) -1 This peak, associated with the δ(NH) shear vibration, is another characteristic peak of primary amines; there is no amide I band (approximately 1650 cm⁻¹) here. -1 The presence of this indicates that -NH2 is still in a free state and has not yet participated in the reaction; 2932 / 2854 cm -1 The vas / vs(CH2) group, representing the methylene group of the aminopropyl chain -(CH2)3-, is evidence of the presence of an organic correlation layer; 1470 / 1332 cm⁻¹ -1 It belongs to δ(CH2) / v(CN), which is a combination of methylene scissor vibration and CN stretching. It is weak in intensity but stable in position, with a diameter of 1125 cm. -1 (Broadened) belongs to vas(Si-O-Si), which is formed by the self-condensation of silane after hydrolysis. It superimposes with the original Si-O band of the whisker, making the 1100-1000 cm^-1 region wider overall.
[0040] Therefore, compared with the unmodified sample, the modified spectrum is at 3372 / 3298 cm⁻¹. -1 A new -NH2 double peak appears at 1560 cm⁻¹. -1 An NH bending peak appears, along with a peak at 3400 cm⁻¹. -1 The adsorbed water peaks nearby narrowed significantly, supporting the conclusion that γ-aminopropyltriethoxysilane has been anchored to the whisker surface via Si-O-Si bonds and that amino groups have been exposed.
[0041] like Figure 3 The image shows the FTIR spectra of the hyperbranched polyester grafted polypropylene modifier before and after synthesis. The horizontal axis represents wavenumber, and the vertical axis represents transmittance (%). Figure 3The three curves from top to bottom are: PP-g-MAH, hydroxyl-terminated hyperbranched polyester HBPE, and grafted product HBPE-g-PP, which are arranged in a staggered vertical arrangement. Figure 3 In the study, the FTIR peak position and assignment of PP-g-MAH were: 1862 cm⁻¹. -1 The Vas (C=O) signal, representing the antisymmetric stretching of five-membered cyclic anhydrides, is weak and sharp, and is the most reliable high-wavenumber signal for identifying cyclic anhydrides. (1782 cm⁻¹) -1 Belongs to (C=O), is a cyclic acid anhydride, and is associated with 1862 cm⁻¹. -1 This constitutes a bimodal criterion; the distance between the two peaks is approximately 80 cm. -1 This is the decisive characteristic that distinguishes cyclic acid anhydrides from ordinary esters or acids, 1712 cm -1 (Weak) classification v(C=O), a partial hydrolysis product of carboxylic acid anhydrides, inevitably occurs during processing, 921 cm -1 Assigned to v(COC), representing the skeletal vibration of the cyclic anhydride ring, further confirming the relationship, 2950 / 2918 / 2848 cm. -1 Belongs to v(CH3) / vas,vs(CH2), with a PP skeleton, possessing the highest strength, 1458 / 1375 cm. -1 It belongs to δ(CH2) / δs(CH3), of which 1375 cm -1 The umbrella-shaped symmetrical curvature of PP is almost unaffected by other components and can be used as an internal standard; 1168 / 998 / 973 cm -1 The crystalline helical conformation band is a marker of the conformational regularity of the isotactic PP 31 helical chain; Figure 3 The FTIR peak position and assignment of the hydroxyl-terminated hyperbranched polyester HBP are: 3380 cm⁻¹ -1 (Broad and strong) Belonging to v(OH), with numerous terminal hydroxyl groups associating to form a broad peak; the broad peak shape and large envelope are hallmarks of this structure. 1732 cm⁻¹ Figure 3 In the middle, it belongs to the v(C=O) ester, which is the ester carbonyl group in the HBPB skeleton. The strongest peak proves that the condensation polymerization has formed an ester; 1252 / 1130 / 1042 cm -1 The peaks are attributed to vas(COC) / v(CO), representing the asymmetric stretching of the COC bond and the stretching of the CO bond in the ester bond, with multiple strong peaks. (cm⁻¹: 2972 / 2880 / 1462 / 1394 / 1372) -1 The attribute v,δ(CH) represents -CH3 and -CH2- of the DMPA unit.
[0042] Figure 3 Middle, 1738 cm -1 A new ester carbonyl group appears, positioned slightly above the 1732 cm position of the HBPE's own ester group.-1 It is classified as a monoester bond formed after the ring opening of an acid anhydride; at the same time, 3388 cm -1 The significant decrease in the intensity of the OH peak indicates that the terminal hydroxyl group was consumed but not completely reacted. The triple unidirectional changes of weakened anhydride, new ester formation, and reduced hydroxyl group constitute complete spectroscopic evidence for successful esterification grafting.
[0043] This invention achieves a melt flow rate of at least 25 g / 10 min and a spiral flow length of at least 180 mm at 230°C / 2.16 kg by synergistically combining modified wollastonite whiskers with a hyperbranched polyester-grafted polypropylene modifier, supplemented with toughening agents and processing aids. Example 1 showed a measured melt flow rate of 28.5 g / 10 min and a spiral flow length of 186 mm. In contrast, Comparative Example 1, using both unmodified wollastonite whiskers and maleic anhydride-grafted polypropylene, showed a melt flow rate of only 16.2 g / 10 min and a spiral flow length of only 112 mm. Comparative Example 2, using only unmodified wollastonite whiskers, showed a melt flow rate of 18.5 g / 10 min and a spiral flow length of 128 mm. Comparative Example 3, using only maleic anhydride-grafted polypropylene instead of the hyperbranched polyester-grafted polypropylene modifier, showed a melt flow rate of 22.3 g / 10 min and a spiral flow length of 152 mm. The above results show that neither modifying wollastonite whiskers alone nor using hyperbranched polyester-grafted polypropylene modifier alone can simultaneously achieve high injection molding flowability and good filler dispersibility. Only the synergistic effect of modified wollastonite whiskers and hyperbranched polyester-grafted polypropylene modifier can simultaneously achieve a balance between high flowability and uniform dispersion.
Claims
1. A polymer composite material with excellent injection molding flowability, characterized in that, By weight, it includes the following components: 100 parts by weight of polypropylene matrix resin; 8-25 parts by weight of modified wollastonite whiskers; 2-8 parts by weight of hyperbranched polyester-grafted polypropylene modifier; 5-15 parts by weight of ethylene-octene copolymer toughening agent; 0.2-0.8 parts by weight of N,N'-ethylene bis-stearamide; Antioxidant 0.2-0.6 parts by weight; The modified wollastonite whiskers are aminated wollastonite whiskers that have undergone surface treatment with γ-aminopropyltriethoxysilane. The hyperbranched polyester-grafted polypropylene modifier is a graft obtained by melt esterification reaction of hydroxyl-terminated hyperbranched polyester and maleic anhydride-grafted polypropylene.
2. The method for preparing the polymer composite material with excellent injection molding flowability according to claim 1, characterized in that, Includes the following steps: Step S1: Weigh out 100 parts by weight of polypropylene matrix resin, 8-25 parts by weight of modified wollastonite whiskers, 2-8 parts by weight of hyperbranched polyester grafted polypropylene modifier, 5-15 parts by weight of ethylene-octene copolymer toughening agent, 0.2-0.8 parts by weight of N,N'-ethylene bis-stearamide, and 0.2-0.6 parts by weight of antioxidant. Step S2: Add the weighed components to a high-speed mixer and mix at 300-800 r / min for 5-20 min at 20-40℃ to obtain a premix. Step S3: Add the premixed material to a twin-screw extruder for melt blending and extrusion. The temperatures from zone one to the die head of the extruder are 180-200℃, 190-210℃, 200-220℃, 210-230℃, 210-230℃, and 200-220℃, respectively. The screw speed is 200-500 r / min, and the melt pressure is controlled at 2-8 MPa. The extrudate is cooled with deionized water, pelletized, and dried to obtain the polymer composite material.
3. The polymer composite material with excellent injection molding flowability according to claim 1, characterized in that, The method for preparing the modified wollastonite whiskers includes: Step A1: Add wollastonite whiskers to deionized water at a solid-liquid mass ratio of 1:5-1:10, stir and disperse for 10-30 minutes, add 5%-10% acetic acid aqueous solution to adjust the pH to 4.0-5.0, then add 1.0%-3.0% γ-aminopropyltriethoxysilane by mass of wollastonite whiskers, stir and react at 50-70℃ for 1-3 hours, filter to obtain wet material; Step A2: Dry the wet material at 80-110℃ for 2-6 hours, then heat it to 110-150℃ for 0.5-2 hours, cool, grind, and sieve to obtain modified wollastonite whiskers.
4. The polymer composite material with excellent injection molding flowability according to claim 1, characterized in that, The preparation method of the hyperbranched polyester-grafted polypropylene modifier includes: Step B1: By weight, add 100 parts pentaerythritol, 80-150 parts dimethylolpropionic acid, 0.5-2 parts p-toluenesulfonic acid and 150-300 parts toluene to a reaction vessel, purge with nitrogen, heat to reflux under normal pressure and react with water separation for 2-6 hours to obtain a hydroxyl-terminated hyperbranched polyester solution. Remove toluene by vacuum distillation, cool and pulverize to obtain hydroxyl-terminated hyperbranched polyester. Step B2: By weight, add 100 parts by weight of maleic anhydride-grafted polypropylene and 20-50 parts by weight of hydroxyl-terminated hyperbranched polyester to a melt mixer. Under nitrogen protection and a system pressure of 0.1-0.2 MPa, melt mix at 150-180°C for 5-20 minutes to allow the hydroxyl groups and maleic anhydride groups to undergo a ring-opening esterification reaction, thereby obtaining the melt-grafted product. Step B3: Cool the molten graft material to room temperature, crush and sieve it to obtain hyperbranched polyester-grafted polypropylene modifier.
5. The polymer composite material with excellent injection molding flowability according to claim 4, characterized in that, The grafting rate of the maleic anhydride-grafted polypropylene is 0.5%-1.5%, and its melt flow rate is 20-60 g / 10 min at 230℃ / 2.16 kg.
6. The polymer composite material with excellent injection molding flowability according to claim 1, characterized in that, The polypropylene matrix resin is at least one of copolymer polypropylene or homopolymer polypropylene, and its melt flow rate is 10-60 g / 10 min at 230℃ / 2.16 kg; the wollastonite whiskers have an aspect ratio of 10-30 and an average diameter of 2-8 μm.
7. The polymer composite material with excellent injection molding flowability according to claim 1, characterized in that, The mass ratio of the modified wollastonite whiskers to the hyperbranched polyester-grafted polypropylene modifier is 3:1-12:1.