A high-gloss, wear-resistant PMMA material and its preparation method
By using ternary copolymerization of zinc ionomer resin and PMMA matrix and the use of compatibilizers, a synergistic effect of high gloss, high transparency and wear resistance of PMMA material is achieved, solving the problem of insufficient wear resistance in existing technologies.
Patent Information
- Application Number
- CN202611076694.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
AI Technical Summary
Existing PMMA materials have insufficient wear resistance, and existing modification schemes cannot achieve both high transparency and high wear resistance.
The material achieves physical compatibility by using zinc ionomer resin and PMMA matrix through a ternary copolymer structure, and imparts excellent wear resistance through zinc ion crosslinking network. Combined with methyl methacrylate-glycidyl methacrylate copolymer as a compatibilizer, it achieves nanoscale uniform dispersion.
While maintaining high gloss and high transparency, it significantly improves the abrasion resistance of PMMA, avoiding problems such as increased haze and insufficient abrasion resistance caused by insufficient compatibility or excessive neutralization.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically relating to a high-gloss, wear-resistant PMMA material and its preparation method. Background Technology
[0002] Polymethyl methacrylate (PMMA) possesses excellent optical transparency, surface gloss, and weather resistance, making it widely used in optical lenses, display light guides, automotive taillight covers, and decorative panels. However, PMMA has relatively low surface hardness (typically only HB-H pencil hardness), resulting in insufficient abrasion and scratch resistance. It is prone to scratches during daily use and cleaning, affecting its transparency and lifespan.
[0003] To improve the wear resistance of PMMA, existing technologies mainly focus on the following directions: (1) Surface coating treatment, such as hard coating technology, which can effectively improve surface hardness, but the process is complicated, costly and the coating durability is limited; (2) Blending with high-hardness inorganic fillers, which can improve wear resistance, but the fillers can easily lead to a significant increase in haze, which seriously damages optical transparency; (3) Blending with polymers with excellent wear resistance, such as CN119175925A which discloses a weather-resistant, wear-resistant and anti-friction white PMMA transparent film, by adding polyurethane acrylate as a toughening material and introducing epoxy resin to improve surface hardness, and using a multi-layer co-extrusion process to achieve wear resistance modification; CN104086969A discloses a transparent and scratch-resistant PC / PMMA alloy material, by introducing high-pressure inert gas into the PMMA melt, so that the PC phase and PMMA phase can be well dispersed and blended, thereby preparing an alloy material with both transparency and scratch resistance. However, existing polymer blending modification schemes still have problems such as poor compatibility, increased haze due to phase separation, and decreased light transmittance, making it difficult to simultaneously meet the dual requirements of high transparency and high wear resistance for optical applications.
[0004] Therefore, there is an urgent need to develop a technical solution that can significantly improve the wear resistance of PMMA while maintaining its high gloss and high transparency. Summary of the Invention
[0005] The purpose of this invention is to provide a high-gloss, wear-resistant PMMA material and its preparation method, so as to solve the technical problems of insufficient wear resistance of existing PMMA materials and the inability of existing modification schemes to simultaneously achieve high transparency and high wear resistance.
[0006] The technical solution for achieving the objective of this invention is as follows.
[0007] In a first aspect, the present invention provides a high-gloss, wear-resistant PMMA material, which, by weight, comprises the following components: 100 parts PMMA resin; 3-8 parts zinc ionomer resin; 1-3 parts compatibilizer; 0.1-0.5 parts lubricant; and 0.1-0.5 parts antioxidant. The compatibilizer is a methyl methacrylate-glycidyl methacrylate copolymer. The zinc ionomer resin is a zinc ion neutralizer of an ethylene-methyl methacrylate-methyl methacrylate terpolymer, wherein the content of methacrylic acid units is 8-12 mol% (based on the total structural units of the ionomer resin), the content of methyl methacrylate units is 5-20 mol%, and the degree of neutralization of methacrylic acid units is 50-60 mol%.
[0008] The ternary copolymer structure of the zinc ionomer resin contains the same MMA segments as PMMA in its main chain, which can form good physical compatibility with the PMMA matrix. At the same time, the zinc ion crosslinking network endows the material with excellent wear resistance.
[0009] The content of methacrylic acid units and methyl methacrylate units in the zinc ionomer resin can be determined by nuclear magnetic resonance spectroscopy. 1 ¹H-NMR determination: The ionomer resin was dissolved in deuterated o-dichlorobenzene and measured at 120℃. The content of each unit was calculated based on the integral area ratio of the methyl proton peak (δ≈1.2-1.5ppm) in the methacrylic acid unit, the methoxy proton peak (δ≈3.5-3.7ppm) in the MMA unit, and the methylene proton peak (δ≈1.0-1.8ppm) in the ethylene unit. The degree of neutralization can be obtained by converting the zinc content determined by inductively coupled plasma optical emission spectrometry (ICP-OES): Based on the zinc elemental content determined by ICP-OES, the molar percentage of carboxyl groups neutralized by zinc ions to the total carboxyl groups is calculated in combination with the MAA content.
[0010] The number average molecular weight of the zinc ionomer resin is 10,000-80,000 g / mol.
[0011] The content of glycidyl methacrylate units in the methyl methacrylate-glycidyl methacrylate copolymer is 5-15 mol.
[0012] Furthermore, the PMMA resin is injection molding grade or extrusion grade polymethyl methacrylate with a melt index between 5 and 20 g / 10 min (test conditions: 230℃, 3.8 kg).
[0013] Furthermore, the lubricant is pentaerythritol stearate (PETS) or stearamide.
[0014] Furthermore, the antioxidant is a compound system of hindered phenolic antioxidants and phosphite antioxidants, preferably antioxidant 1010 and antioxidant 168 are compounded in a 1:1 mass ratio.
[0015] In this invention, zinc ionomer resin and PMMA matrix achieve nanoscale uniform dispersion (dispersed phase size <100nm) through the natural compatibility of MMA segments in the ternary copolymer structure and the bridging effect of methyl methacrylate-glycidyl methacrylate copolymer, resulting in an unexpected synergistic effect of high gloss, high transparency and wear resistance.
[0016] The mechanism of action may be as follows: First, the ternary copolymer backbone of the zinc ionomer resin contains 5-20 mol% MMA segments. These MMA segments have the same chemical structure as the PMMA matrix, enabling them to form a tight physical entanglement with the PMMA molecular chains. This provides a natural compatibility basis for the ionomer within the PMMA matrix, facilitating initial uniform dispersion. Second, the zinc ion crosslinking network endows the material with excellent scratch resistance and abrasion resistance. Compared to alkali metal ions such as sodium and potassium, or alkaline earth metal ions such as calcium and magnesium, the d-orbital electronic structure of zinc ions results in smaller and more uniformly distributed ion clusters, with extremely weak scattering of visible light, thus maximizing the preservation of PMMA's optical transparency. When the neutralization degree of the zinc ionomer is below 50 mol%, the ion crosslinking density is insufficient, limiting the improvement in abrasion resistance; when the neutralization degree is above 60 mol%, excessive zinc ions lead to excessive aggregation of ion clusters, increasing haze.
[0017] The amount of zinc ionomer added needs to be strictly controlled: if the amount is too small (<3 parts), the improvement in abrasion resistance is not significant; if the amount is too large (>8 parts), although the abrasion resistance is further improved, the volume fraction of the dispersed phase is too high, which will still have an adverse effect on haze. The MMA segment content also needs to be controlled within the range of 5-20 mol%: if the content is too low, the natural compatibility between the ionomer and PMMA is not improved enough; if the content is too high, the ethylene segment characteristics of the ionomer are diluted, which may affect its flexibility and abrasion resistance.
[0018] Secondly, the present invention provides a method for preparing the high-gloss, wear-resistant PMMA material as described above, comprising the following steps: (1) Place PMMA resin and zinc ionomer resin in an oven at 80-100℃ and dry for 4-6 hours to remove moisture from the resin; (2) By weight, add the dried PMMA resin, zinc ionomer resin, methyl methacrylate-glycidyl methacrylate copolymer, lubricant and antioxidant into a high-speed mixer and stir to mix evenly to obtain a premix. (3) Add the premixed material to a twin-screw extruder and melt extrude and granulate it at a temperature of 220-250℃. The screw speed is 200-400 rpm to obtain PMMA composite material granules. The obtained granules are injection molded or extruded to make PMMA products.
[0019] Furthermore, the screw length-to-diameter ratio of the twin-screw extruder described in step (3) is 40:1-52:1 to ensure sufficient dispersion and reaction of each component.
[0020] Thirdly, the present invention provides the application of the high-gloss, wear-resistant PMMA material as described above in optical lenses, display screen light guide plates, automotive taillight covers, and decorative panels.
[0021] By adopting the above technical solution, the present invention has the following beneficial effects: (1) This invention, by adding ethylene-methyl methacrylate-methacrylic acid ternary copolymer zinc ionomer resin, utilizes the natural compatibility between the MMA segments in the ionomer backbone and the PMMA matrix, as well as the zinc ion crosslinking network, to endow PMMA materials with excellent scratch resistance and wear resistance. The introduction of MMA segments gives the ionomer better initial compatibility with PMMA, which is beneficial to achieving uniform dispersion at the nanoscale.
[0022] (2) By limiting the methacrylic acid content of the zinc ionomer to 8-12 mol%, the MMA content to 5-20 mol%, and the degree of neutralization to 50-60 mol%, the present invention ensures the best balance between the compatibility of the ionomer and PMMA, the density of ionic crosslinking and the optical transparency, and avoids the increase of haze due to insufficient compatibility, the insufficient wear resistance due to too low neutralization and the aggregation of ion clusters due to too high neutralization.
[0023] (3) In this invention, methyl methacrylate-glycidyl methacrylate copolymer is used as a compatibilizer in the PMMA / zinc ionomer system to form a synergistic compatibilizing effect with the MMA segments of the ionomer itself. The MMA segments of the ionomer provide a "pre-compatibility" basis, and the epoxy groups of the compatibilizer GMA provide chemical bonding anchoring. The two work together to construct a dual compatibilizing mechanism of "physical entanglement + chemical bonding", so that the zinc ionomer is uniformly dispersed in the PMMA matrix at the nanoscale (TEM observation dispersed phase size <100nm), ensuring the high transparency and high gloss of the material. Detailed Implementation
[0024] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0025] In the following examples, PMMA resin (injection molding grade, MFR=10 g / 10min, 230℃ / 3.8kg) was purchased from Zhenjiang Chimei; zinc ionomer resin (ethylene-methyl methacrylate-methacrylic acid terpolymer zinc salt, MAA content 8-12 mol%, MMA content 5-20 mol%, neutralization degree 50-60 mol%) was prepared in-house; methyl methacrylate-glycidyl methacrylate copolymer (GMA content 5-15 mol%) was prepared in-house; PETS lubricant and antioxidant 1010 / 168 were purchased commercially available.
[0026] Preparation Example 1: Preparation of Zinc Ionomer Resin Ethylene, methyl methacrylate, and methacrylic acid were solution polymerized in a target composition ratio to obtain an ethylene-methyl methacrylate-methacrylic acid terpolymer (10 mol% methacrylic acid unit content, 10 mol% methyl methacrylate unit content). This terpolymer was then mixed with zinc acetate in a stoichiometric ratio (target neutralization degree 55 mol%) and subjected to a melt neutralization reaction using a twin-screw extruder at an extrusion temperature of 180-200℃ and a screw speed of 200 rpm to obtain a zinc ionomer resin.
[0027] Preparation Example 2: Preparation of methyl methacrylate-glycidyl methacrylate copolymer By weight, 90 parts of methyl methacrylate, 10 parts of glycidyl methacrylate and 0.2 parts of azobisisobutyronitrile were mixed and subjected to solution polymerization at 70°C for 6 hours. After methanol precipitation, washing and drying, methyl methacrylate-glycidyl methacrylate copolymer (GMA content 10 mol%, number average molecular weight about 30,000 g / mol) was obtained.
[0028] Example 1
[0029] (a) Raw material ratio 100 parts PMMA resin; 5 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 2 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168.
[0030] (II) Preparation process (1) Drying treatment: Place PMMA resin and zinc ionomer resin in an oven at 90°C and dry for 4 hours respectively; (2) Mixing and batching: Add the dried components to a high-speed mixer and mix at 600 rpm for 15 minutes to obtain a premix; (3) Melt extrusion: The premixed material is added to a twin-screw extruder (length-to-diameter ratio 44:1) and melt extruded and granulated at a temperature of 240°C with a screw speed of 300 rpm to obtain PMMA composite material granules; the obtained granules are injection molded to make standard test strips.
[0031] Example 2
[0032] Raw material ratio: 100 parts PMMA resin; 3 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 1.5 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The remaining preparation steps are the same as in Example 1.
[0033] Example 3
[0034] Raw material ratio: 100 parts PMMA resin; 8 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 3 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The remaining preparation steps are the same as in Example 1.
[0035] Example 4
[0036] The difference between this embodiment and Example 1 is that the MMA content of the zinc ionomer resin is different (5 mol%), while the rest of the formulation and preparation steps are the same as in Example 1.
[0037] Example 5
[0038] The difference between this embodiment and Example 1 is that the MMA content of the zinc ionomer resin is different (20 mol%), while the rest of the formulation and preparation steps are the same as in Example 1.
[0039] Example 6
[0040] The difference between this embodiment and Example 1 is that the MAA content of the zinc ionomer resin is different (8 mol%), while the rest of the formulation and preparation steps are the same as in Example 1.
[0041] Example 7
[0042] The difference between this embodiment and Example 1 is that the MAA content of the zinc ionomer resin is different (12 mol%), while the rest of the formulation and preparation steps are the same as in Example 1.
[0043] Comparative Example 1 The difference from Example 1 is that zinc ionomer resin and methyl methacrylate-glycidyl methacrylate copolymer are not added; only PMMA resin is used. Raw material ratio: 100 parts PMMA resin; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0044] Comparative Example 2 The difference from Example 1 is that methyl methacrylate-glycidyl methacrylate copolymer is not added. Raw material ratio: 100 parts PMMA resin; 5 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0045] Comparative Example 3 The difference from Example 1 is that the amount of zinc ionomer resin added is 12 parts. Raw material ratio: 100 parts PMMA resin; 12 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 4 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0046] Comparative Example 4 The difference from Example 1 is that the degree of neutralization of the zinc ionomer resin is 40 mol%. Raw material ratio: 100 parts PMMA resin; 5 parts zinc ionomer resin (MAA content 10 mol%, MMA content 10 mol%, degree of neutralization 40 mol%); 2 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0047] Comparative Example 5 The difference from Example 1 is that a conventional zinc ionomer resin (ethylene-methacrylate copolymer zinc salt) without MMA segments is used instead of the standard zinc ionomer resin. Raw material ratio: 100 parts PMMA resin; 5 parts conventional zinc ionomer resin (ethylene-methacrylate copolymer zinc salt, MAA content 10 mol%, neutralization degree 55 mol%); 2 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0048] Comparative Example 6 The difference from Example 1 is that zinc ionomer resin is not added; only methyl methacrylate-glycidyl methacrylate copolymer is added. Raw material ratio: 100 parts PMMA resin; 2 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0049] Comparative Example 7 The difference from Example 1 is that sodium ionomer resin (sodium salt of ethylene-methyl methacrylate-methacrylic acid terpolymer) is used instead of zinc ionomer resin. Raw material ratio: 100 parts PMMA resin; 5 parts sodium ionomer resin (MAA content 10 mol%, MMA content 10 mol%, neutralization degree 55 mol%); 2 parts methyl methacrylate-glycidyl methacrylate copolymer; 0.3 parts PETS lubricant; 0.15 parts antioxidant 1010; 0.15 parts antioxidant 168. The preparation steps are the same as in Example 1.
[0050] Performance testing The PMMA materials prepared in Examples 1-7 and Comparative Examples 1-7 were subjected to the following performance tests: (1) Transmittance and haze test According to GB / T 2410-2008, the transmittance and haze of a 2mm thick sample were tested using a transmittance / haze meter.
[0051] (2) Gloss test According to the current valid standard GB / T 8807-2019, the surface gloss of the sample at an incident angle of 60° was tested using a gloss meter.
[0052] (3) Abrasion resistance test According to GB / T 2411-2008, the abrasion resistance of the specimens was tested using a Taber abrasion tester (CS-17 grinding wheel, 500g load, 500 rpm), and the abrasion loss was evaluated in mg.
[0053] (4) Pencil hardness test According to GB / T 6739-2006, the pencil hardness of the sample was tested.
[0054] (5) Microscopic morphological observation The microstructure of the blends was observed using transmission electron microscopy (TEM). Specifically, the samples were ultra-thinly sectioned (approximately 70 nm thick) at -120°C, stained with ruthenium tetroxide for 5 minutes, and then observed under a JEM-2100 TEM with an accelerating voltage of 200 kV to observe the dispersion state and dispersed phase size of the zinc ionomers.
[0055] The test results are shown in Tables 1 and 2.
[0056] Table 1 Performance test results of Examples 1-7
[0057] Table 2 Performance test results of Comparative Examples 1-7
[0058] As can be seen from the test results in Tables 1 and 2, the PMMA materials prepared in Examples 1-7 of this invention have excellent comprehensive performance: light transmittance ≥91%, haze ≤1.5%, gloss ≥92, abrasion loss (30-42mg) is much lower than that of pure PMMA (72mg) and the system containing only compatibilizer (68mg), pencil hardness increased from H to 2H, TEM confirmed that zinc ionomers are uniformly dispersed at a size of <80nm, verifying the synergistic compatibilization effectiveness of "pre-compatibility" of ionomer MMA segments and "chemical bonding anchoring" of compatibilizer.
[0059] Comparative Example 2 (without compatibilizer): Haze increased to 3.5%, and dispersed phase size reached 300-800 nm, demonstrating that the MMA segments of the ionomer alone are insufficient to achieve optimal dispersion; the chemical bonding and anchoring of the compatibilizer is key to achieving nanoscale dispersion. Comparative Example 5 (conventional zinc ionomer without introduced MMA segments): Haze 3.2%, dispersed phase size 150-500 nm, confirming that MMA segments provide a natural compatibility basis for the ionomer with PMMA. Comparative Example 7 (sodium ionomer): Haze 3.0%, indicating that zinc ionomers are irreplaceable in maintaining optical transparency. Comparative Example 3 (12 parts ionomer): Haze increased to 5.0%, indicating that 3-8 parts is the optimal range for achieving a balance between abrasion resistance and transparency. Comparative Example 4 (40% neutralization): Abrasion loss increased to 50 mg, and pencil hardness decreased to H, demonstrating that a neutralization degree of 50-60% is the critical condition for ensuring sufficient ionic crosslinking density.
[0060] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A high-gloss, wear-resistant PMMA material, characterized in that, By weight, it consists of the following components: 100 parts of PMMA resin; 3-8 parts zinc ionomer resin; 1-3 parts compatibilizer; Lubricant 0.1-0.5 parts; Antioxidant 0.1-0.5 parts; The zinc ionomer resin is a zinc ion neutralized product of ethylene-methyl methacrylate-methacrylic acid terpolymer, wherein the content of methacrylic acid units is 8-12 mol%, the content of methyl methacrylate units is 5-20 mol%, and the degree of neutralization of methacrylic acid units is 50-60 mol%.
2. The high-gloss, wear-resistant PMMA material according to claim 1, characterized in that, The compatibilizer is a methyl methacrylate-glycidyl methacrylate copolymer.
3. The high-gloss, wear-resistant PMMA material according to claim 2, characterized in that, The content of glycidyl methacrylate units in the methyl methacrylate-glycidyl methacrylate copolymer is 5-15 mol.
4. The high-gloss, wear-resistant PMMA material according to claim 1, characterized in that, The number average molecular weight of the zinc ionomer resin is 10,000-80,000 g / mol.
5. The high-gloss, wear-resistant PMMA material according to claim 1, characterized in that, The PMMA resin is injection molding grade or extrusion grade polymethyl methacrylate with a melt index between 5 and 20 g / 10 min, and the test conditions are 230℃ and 3.8 kg.
6. The high-gloss, wear-resistant PMMA material according to claim 1, characterized in that, The lubricant is pentaerythritol stearate or stearamide.
7. The high-gloss, wear-resistant PMMA material according to claim 1, characterized in that, The antioxidant is a compound system of hindered phenolic antioxidants and phosphite antioxidants.
8. A method for preparing a high-gloss, wear-resistant PMMA material as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) Drying treatment: Place PMMA resin and zinc ionomer resin in an oven at 80-100℃ and dry for 4-6 hours respectively; (2) Mixing ingredients: By weight, add the dried PMMA resin, zinc ionomer resin, methyl methacrylate-glycidyl methacrylate copolymer, lubricant and antioxidant into a high-speed mixer and stir to mix evenly to obtain a premix; (3) Melt extrusion: The premixed material is added to a twin-screw extruder and melt extruded and granulated at a temperature of 220-250℃ to obtain PMMA composite material granules. The obtained granules are then injection molded or extruded to produce PMMA products.
9. The preparation method according to claim 8, characterized in that, The twin-screw extruder described in step (3) has a screw length-to-diameter ratio of 40:1-52:1 and a screw speed of 200-400 rpm.
Citation Information
Patent Citations
Transparent scratch-resistant PC / PMMA (Poly Carbonate / Polymethyl Methacrylate) alloy material and preparation method thereof
CN104086969A
Weather-resistant wear-resistant fracture-resistant white PMMA transparent film and preparation method thereof
CN119175925A