A fire-retardant and heat-resistant coating and its application

By using a specific ratio of epoxy-modified acrylic emulsion, modified shell powder, and hydrotalcite, a dense, expanded carbon layer is formed, which solves the problem of traditional coatings being prone to carbonization and peeling at high temperatures, and achieves excellent fire resistance, heat resistance, and heat insulation effects in a thin-layer state.

CN123063017APending Publication Date: 2026-11-10GUANGZHOU JOINTAS CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611295902.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional fire-retardant coatings are prone to carbonization and peeling at high temperatures, making it difficult to provide effective fire resistance, heat resistance, and insulation performance in thin layers. Traditional insulation materials also have poor insulation effects in confined spaces.

Method used

A dense expanded carbon layer is formed by using a specific ratio of epoxy-modified acrylic emulsion, modified shell powder, hydrotalcite, and mullite fiber. The dispersion stability is improved through hydrogen bonds and chemical bonds. Combined with the porous structure of modified shell powder and the layered structure of hydrotalcite, the fire resistance, heat resistance, and thermal insulation properties of the coating are enhanced.

Benefits of technology

In a thin layer of 0.8-1.2mm, it provides excellent fire resistance, heat resistance and thermal insulation properties, effectively blocking heat transfer and preventing the coating from cracking or peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a fire-retardant and heat-resistant coating and its application, belonging to the field of coating technology. The fire-retardant and heat-resistant coating provided by this invention, through the selection and compounding of appropriate mass parts of components, forms a coating that, even at a relatively thin thickness (0.8-1.2 mm), still exhibits excellent fire resistance and heat resistance, as well as excellent thermal insulation properties. It can be widely applied in the preparation of fire-retardant and heat-resistant coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology, and particularly relates to a fire-retardant and heat-resistant coating and its application. Background Technology

[0002] The explosive growth of the battery coating market is directly driven by the ongoing escalation of battery safety issues and the comprehensive tightening of regulatory policies. Experimental data from the China Automotive Engineering Research Institute shows that the peak heat release rate of new energy vehicles can reach 11.6MW, and the interval between a battery emitting a large amount of black smoke and bursting into flames is only 1 second, posing extremely stringent challenges to the fire-retardant performance required for coatings and packaging materials.

[0003] Policy support has been fully implemented. In April 2025, the mandatory national standard GB 38031-2025 "Safety Requirements for Power Batteries for Electric Vehicles" was officially released. The new standard upgraded the thermal runaway test requirements for the first time from "an alarm 5 minutes before ignition or explosion" to "no fire, no explosion, and smoke does not cause harm to occupants." Therefore, there is an urgent need to develop a heat-insulating and fire-retardant coating system as a key "passive fire protection measure" that can be triggered when thermal runaway occurs, quickly forming a highly efficient heat insulation barrier on the substrate surface to block the spread of heat to adjacent cells and the entire battery pack.

[0004] Traditional organic fire-retardant and heat-insulating coatings cannot withstand the extremely high temperatures experienced during thermal runaway. For example, ordinary epoxy fire-retardant coatings only withstand temperatures up to about 200°C, and will carbonize and peel off in 15 seconds in a flame exceeding 1000°C. At the same time, traditional insulation materials also struggle to achieve efficient heat insulation within confined spaces. For instance, traditional aerogel insulation sheets used between battery cells, even with thicknesses generally exceeding 1.5mm, still cannot provide an effective temperature difference exceeding 500°C. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a fire-resistant and heat-resistant coating and its application that has excellent fire resistance, heat resistance and heat insulation properties when prepared into a thin coating (0.8-1.2 mm).

[0006] To achieve the above objectives, in a first aspect, the present invention provides a fire-retardant and heat-resistant coating, the fire-retardant and heat-resistant coating comprising the following components in parts by weight: 40-60 parts epoxy-modified acrylic emulsion, 5-15 parts ammonium polyphosphate, 5-15 parts melamine, 5-15 parts dipentaerythritol, 5-15 parts hydrotalcite, 5-30 parts modified shell powder, 1-10 parts mullite fiber, 0.5-1 part dispersant, 0.5-3 parts coupling agent, 1-3 parts film-forming agent, 0.5-1 part defoamer, 0.5-1 part mildew inhibitor; The epoxy-modified acrylic emulsion has an acid value of 10-25 mg / KOH and an average particle size of 100-300 nm. The modified shell powder is a trialkoxysilane modified shell powder.

[0007] The fire-retardant and heat-resistant coating provided by this invention, by selecting appropriate mass proportions of components and compounding them, forms a coating that, even in a relatively thin state (0.8-1.2 mm), still possesses excellent fire-retardant and heat-resistant properties, as well as excellent heat insulation performance.

[0008] Specifically, in the first aspect, this invention selects an epoxy-modified acrylic emulsion with an acid value within a certain range. This emulsion effectively provides carboxyl groups to form hydrogen bonds or other chemical bonds with the surfaces of hydrotalcite, modified shell powder, and mullite fibers, effectively improving the dispersion stability and uniformity of hydrotalcite, modified shell powder, and mullite fibers in the emulsion; it also enhances the stability and water resistance of the epoxy-modified acrylic emulsion itself. In the second aspect, selecting an epoxy-modified acrylic emulsion with an average particle size within a certain range enhances the emulsion's permeability and compatibility with hydrotalcite, modified shell powder, and mullite fibers, and also improves the stability of the emulsion itself. Furthermore, by selecting an epoxy-modified acrylic emulsion, the epoxy groups can participate in cross-linking reactions at high temperatures, forming a denser and stronger expanded carbon layer with hydrotalcite, modified shell powder, and mullite fibers, effectively improving fire resistance, heat resistance, and the ability to block heat and mass transfer.

[0009] Secondly, this invention selects trialkoxysilane-modified shell powder as the modified shell powder. The shell powder has abundant surface pores, and its porous structure gives it a unique water-breathing function. In high-humidity environments, coatings with added shell powder can effectively absorb condensed water droplets, and when the environment is dry, the coating can release the stored moisture promptly. This effectively reduces blistering and chalking of the coating, mitigating the negative impact of environmental humidity on the fire resistance and heat resistance of the coating. In particular, modification with the specific modifying groups of this invention results in better compatibility with epoxy-modified acrylic emulsions and better interaction with mullite fibers and epoxy-modified acrylic emulsions, acting as a rigid skeleton to improve the density and strength of the expanded carbon layer, thereby effectively blocking heat and mass transfer. Furthermore, the modified shell powder added in this invention can react with ammonium polyphosphate at high temperatures to generate highly stable Ca3(PO4)2, thus reducing the content of ammonium polyphosphate that can react with dipentaerythritol, thereby improving the excellent carbonization and heat insulation effects of the coating.

[0010] Thirdly, hydrotalcite (LDH), as a layered two-dimensional material, possesses excellent barrier properties, thermal stability, and flame retardant properties. The interlayer spaces of LDH allow for the intercalation of anti-corrosion anions, thus providing continuous anti-corrosion protection for the coating. LDH's strong ion exchange capacity enables it to combine with other functional substances, enhancing its anti-corrosion performance. Furthermore, LDH releases CO2 and water vapor upon heating, inhibiting flame propagation and lowering the temperature. Moreover, the layered structure of LDH expands to form a denser thermal barrier, improving the coating's high-temperature resistance. These characteristics allow LDH to not only improve the coating's anti-corrosion ability but also provide reliable fire resistance, meeting the multi-performance requirements of ultra-thin intumescent fire-retardant and anti-corrosion coatings. Especially in this invention, it can be better dispersed in epoxy-modified acrylic emulsions and further compounded with modified shell powder and mullite fibers, releasing water vapor and carbon dioxide at high temperatures and generating mixed metal oxides with high specific surface area, promoting the formation of a dense, high-strength carbon layer.

[0011] Fourthly, the mullite fiber added in this invention can achieve a ternary compound with hydrotalcite and modified shell powder, which can significantly improve the fireproof and heat insulation performance of the coating. The core of its synergistic effect lies in constructing a three-dimensional protective network that combines rigidity and flexibility, and integrates air and solid elements: hydrotalcite and modified shell powder react at high temperatures to generate metal oxides (MgO, Al2O3, CaO) and ceramic products, forming the "cement and sand" matrix of the carbon layer. Mullite fiber itself has extremely high temperature resistance (>1700℃), acting as "reinforcing steel" to significantly improve the mechanical strength and thermal shock resistance of the carbon layer, preventing the coating from cracking or peeling after high-temperature combustion. The coating with added mullite fiber forms a denser and more uniform "honeycomb" structure after combustion. This structure effectively traps air, significantly reduces thermal conductivity, and improves the heat insulation effect. The low thermal conductivity and unique structure of mullite fiber effectively extend the heat conduction path in the coating, hindering heat transfer to the substrate.

[0012] For example, the acid value of the epoxy-modified acrylic emulsion can be any point value or a range between any two points between 10-25 mg / KOH, such as 10 mg / KOH, 12 mg / KOH, 15 mg / KOH, 18 mg / KOH, 20 mg / KOH, 23 mg / KOH, 25 mg / KOH, etc.

[0013] For example, the average particle size of the epoxy-modified acrylic emulsion can be any point value between 100-300 nm or a range between any two points, such as 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, etc.

[0014] It should be noted that the test method for the acid value of the epoxy-modified acrylic emulsion is as follows: the sample is dissolved or dispersed in a solvent (a mixed solution of ethanol and deionized water in a volume ratio of 2:1), and the free acid is titrated with potassium hydroxide-ethanol standard solution using thymol blue as an indicator. The titration ends when the solution turns blue and does not fade within 30 seconds. The acid value is calculated based on the amount of alkali consumed.

[0015] It should be noted that the test method for the average particle size of the epoxy-modified acrylic emulsion is as follows: Refer to standard GB / T 29022-2021 (ISO 22412) "Particle size analysis - Dynamic light scattering method". During the test, take an appropriate amount of emulsion and gradually dilute it with a dilute alkaline solution with a pH of 8-9 and a composition similar to the continuous phase of the emulsion, until the photon count rate detected by the instrument is within the manufacturer's recommended range (usually 100-500 kcps). The volume concentration is generally between 0.001% and 0.1%. Next, use low-speed centrifugation (2000 rpm, 5 min) to remove air bubbles and occasional large particles. The sample needs to be equilibrated at the instrument's set temperature (usually 25℃) for 2-5 minutes. Then, the particle size is measured using a dynamic light scattering instrument.

[0016] It should be noted that this invention does not have any particular requirements for the solid content of the epoxy-modified acrylic emulsion; any content within the conventional range in the art is acceptable. For example, the solid content of the epoxy-modified acrylic emulsion is 50-55%.

[0017] As a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the fire-retardant and heat-resistant coating comprises the following components in parts by weight: 48-52 parts epoxy-modified acrylic emulsion, 8-10 parts ammonium polyphosphate, 9-12 parts melamine, 9-12 parts dipentaerythritol, 8-12 parts hydrotalcite, 15-20 parts modified shell powder, 4-8 parts mullite fiber, 0.5-1 part dispersant, 1-2 parts coupling agent, 1.5-2 parts film-forming agent, 0.5-1 part defoamer, and 0.5-1 part mildew inhibitor.

[0018] This invention has found that the mass fraction of a component affects the overall performance of the product, and when the mass fraction of the component is further selected within the above-mentioned range, the overall performance of the obtained product is even better.

[0019] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the ratio of the sum of the mass parts of hydrotalcite and modified shell powder to the mass parts of mullite fiber is 2-35.

[0020] For example, the ratio of the sum of the mass fractions of the hydrotalcite and modified shell powder to the mass fraction of the mullite fiber can be any point value between 2 and 35 or a range between any two points, such as 2, 5, 8, 10, 12, 15, 18, 20, 22, 25, 28, 30, 32, 35, etc.

[0021] Preferably, the ratio of the sum of the mass parts of the hydrotalcite and modified shell powder to the mass part of the mullite fiber is 2.9-5.6. For example, it can be 2.9, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5, 5.2, 5.5, 5.6, etc.

[0022] The present invention has found that by further selecting the ratio of the sum of the mass fractions of hydrotalcite and modified shell powder to the mass fraction of mullite fiber within the above-mentioned range, the resulting coating exhibits superior fire resistance, heat resistance, and heat insulation capabilities.

[0023] As a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the glass transition temperature of the epoxy-modified acrylic emulsion is 15-35°C.

[0024] For example, the glass transition temperature of the epoxy-modified acrylic emulsion can be any point value between 15-35°C or a range between any two points, such as 15°C, 20°C, 25°C, 30°C, 35°C, etc.

[0025] It should be noted that the test method for the glass transition temperature of the epoxy-modified acrylic emulsion is as follows: referring to standard ISO 16805:2003 "Determination of glass transition temperature of paint bases for paints and varnishes" (specifically for coating resins and emulsions); specifically including the following steps: Film formation: Pour an appropriate amount of emulsion into a polytetrafluoroethylene (PTFE) or silicone mold and dry it slowly at a temperature at least 20°C below the estimated Tg to avoid partial cross-linking or structural changes caused by high temperature. If necessary, air dry at room temperature until a transparent film is formed before placing it in a vacuum oven.

[0026] Drying: Typically, vacuum drying at 40-60°C for more than 24 hours is used, or vacuum drying at room temperature until constant weight is achieved. Ensure that water, residual monomers, and film-forming aids completely evaporate, as they will significantly reduce the measured Tg.

[0027] Sampling: Weigh 5-15 mg of dry film sample and place it in a standard aluminum crucible. Seal the crucible (a perforated cap can be used to allow volatiles to escape, but it is usually sealed). The sample should have good thermal contact with the bottom of the crucible.

[0028] Finally, the Tg of the sample was tested using a DSC analyzer under nitrogen protection.

[0029] This invention has found that the glass transition temperature of epoxy-modified acrylic emulsion affects the film-forming properties and hardness of fire-retardant and heat-resistant coatings. At high temperatures, a suitable glass transition temperature affects the coating's ability to soften without flowing, providing a suitable platform for the formation of an expanded carbon layer. Further selecting the glass transition temperature of the epoxy-modified acrylic emulsion within the above-mentioned range can effectively improve the fire-retardant, heat-resistant, and heat-insulating properties of the fire-retardant and heat-resistant coating.

[0030] As a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the epoxy value of the epoxy-modified acrylic emulsion is 0.03-0.08 eq / 100g.

[0031] For example, the epoxy value of the epoxy-modified acrylic emulsion can be any point value or a range between any two points between 0.03 and 0.08 eq / 100g, such as 0.03 eq / 100g, 0.04 eq / 100g, 0.05 eq / 100g, 0.06 eq / 100g, 0.07 eq / 100g, 0.08 eq / 100g, etc.

[0032] It should be noted that the test method for the epoxy value of the epoxy-modified acrylic emulsion is as follows: refer to GB / T41929-2022 "Test Methods for Epoxy Resins in Plastics". Weigh a sample containing 0.6 mmol to 0.9 mmol of epoxy groups into an Erlenmeyer flask, accurate to 0.1 mg. Add 10 mL of chloroform, then dissolve the sample with a magnetic stirrer, and heat slightly if necessary. Cool to room temperature, add 20 mL of glacial acetic acid, then add 30 mL of tetraethylammonium bromide solution using a pipette; dissolve 100 mg of crystal violet in 100 mL of glacial acetic acid. Add 4 to 6 drops of crystal violet solution, and titrate with a standard perchloric acid solution (0.1 mol / L). Stir with a magnetic stirrer simultaneously, and titrate until a stable green color is obtained.

[0033] This invention has found that the epoxy value of epoxy-modified acrylic emulsion affects the number of reactive groups, thereby affecting the cross-linking of the surface groups of hydrotalcite, modified shell powder, and mullite fibers at film formation or high temperature, forming a dense network structure, and further affecting the strength of the carbon layer; when the epoxy value of epoxy-modified acrylic emulsion is further selected within the above range, the overall performance of the obtained fire-retardant and heat-resistant coating is better.

[0034] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the trialkoxysilane accounts for 2-6% of the mass of the modified shell powder.

[0035] For example, the mass percentage of the trialkoxysilane in the modified shell powder can be any point value or any range between two points between 2% and 6%, such as 2%, 3%, 4%, 5%, 6%, etc.

[0036] The present invention has found that selecting a percentage of trialkoxysilane in the modified shell powder within the above-mentioned range can better improve the compatibility and dispersibility between components, ensure the performance of shell powder, and thus improve the overall performance of the coating.

[0037] As a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the trialkoxysilane includes at least one of γ-aminopropyltriethoxysilane (KH-550) and γ-methacryloyloxypropyltrimethoxysilane (KH-570).

[0038] It should be noted that the modified seashell powder can be commercially available or homemade. If homemade, it is a conventional preparation method in this field.

[0039] For example, the preparation method of the modified seashell powder includes the following steps: S1. Add shell powder to anhydrous ethanol to form a slurry; S2. Add a trialkoxysilane hydrolysis solution to the slurry and react. After the reaction is complete, filter, collect the filter residue, wash and dry it to obtain modified shell powder.

[0040] In one embodiment, the trialkoxysilane hydrolysis solution comprises trialkoxysilane, anhydrous ethanol, and water.

[0041] In one embodiment, the volume ratio of trialkoxysilane, anhydrous ethanol, and water in the trialkoxysilane hydrolysis solution is 200:(700-740):(75-85).

[0042] In one embodiment, the preparation method of the trialkoxysilane hydrolysis solution is as follows: trialkoxysilane, anhydrous ethanol and water are mixed and stirred for 20-40 min to obtain the trialkoxysilane hydrolysis solution.

[0043] In one embodiment, the solid content of the shell powder in the slurry is 15-20%.

[0044] In one embodiment, the mass percentage of trialkoxysilane is 1-7% based on the mass of the shell powder.

[0045] In one embodiment, the reaction temperature is 60-80°C and the reaction time is 1-3 hours.

[0046] In one embodiment, the drying temperature is 60-80°C and the time is 1-3 hours.

[0047] In a preferred embodiment of the fireproof and heat-resistant coating of the present invention, the hydrotalcite includes magnesium and aluminum elements, and the molar ratio of magnesium to aluminum is (2-4):3.

[0048] It should be noted that the molar ratio of magnesium to aluminum is tested using inductively coupled plasma atomic emission spectrometry.

[0049] It should be noted that the hydrotalcite can be commercially available or homemade. If homemade, it is a conventional preparation method in this field.

[0050] For example, the method for preparing the hydrotalcite includes the following steps: S1. Mix magnesium solution, aluminum solution and urea salt solution and sonicate, then carry out hydrothermal reaction; S2. After the hydrothermal reaction is completed, the crystals are aged, then cooled to separate the solid and liquid. The solid is collected, washed, dried, and ground to obtain hydrotalcite.

[0051] In one embodiment, the magnesium solution includes magnesium nitrate hexahydrate with a molar concentration of 0.2-0.3 mol / L; the aluminum solution includes aluminum nitrate nonahydrate with a molar concentration of 0.7-0.8 mol / L.

[0052] In one embodiment, the urea salt solution is prepared by adding uric acid and hydrochloric acid to water in a stoichiometric ratio of 1:1 to obtain the urea salt solution.

[0053] In one embodiment, the mass-to-volume ratio of urea to water is 1 g: (45-55) mL.

[0054] When urea and hydrochloric acid are added to water, they react to form urea hydrochloride crystals.

[0055] In one embodiment, the frequency of the ultrasound is 55-65 kHz and the duration is 30-60 min.

[0056] In one embodiment, the hydrothermal reaction is carried out at a temperature of 100-200°C for 1-3 hours.

[0057] In one embodiment, the crystallization aging temperature is 80-120°C and the time is 15-18 hours.

[0058] In one embodiment, the drying is vacuum drying at a temperature of 60-80°C for 15-18 hours.

[0059] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the aspect ratio of the mullite fiber is 31-100.

[0060] For example, the aspect ratio of the mullite fiber can be any point value between 31 and 100 or a range between any two points, such as 31, 40, 50, 60, 70, 80, 90, 100, etc.

[0061] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the mullite fibers have an average diameter of 2-7 μm.

[0062] For example, the average diameter of the mullite fiber can be any point value or a range between any two points between 2 and 7 μm, such as 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, etc.

[0063] It should be noted that the aspect ratio of mullite fibers is tested using an electron microscope.

[0064] The present invention has found that the aspect ratio and length of mullite fibers affect the strength of the carbon layer formed by the coating at high temperature, as well as its dispersion effect in the matrix. When the aspect ratio and length are further selected within the above range, the overall performance of the fireproof and heat-resistant coating is better.

[0065] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the dispersant includes at least one of polyester dispersant, polyacrylate dispersant, polyurethane dispersant, polyolefin dispersant or polyether dispersant.

[0066] For example, the dispersant may be at least one of SN-1729 and 4790.

[0067] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the coupling agent includes a silane coupling agent.

[0068] For example, the coupling agent may be at least one of KH550 and KH570.

[0069] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the film-forming agent includes at least one of propylene glycol ethyl ether and propylene glycol butyl ether.

[0070] In a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the defoamer includes silicone-based defoamers.

[0071] For example, the defoamer may be at least one of DT-155 and DT-80.

[0072] As a preferred embodiment of the fire-retardant and heat-resistant coating of the present invention, the anti-mildew agent includes at least one of nano zinc oxide, nano titanium dioxide, and isothiazolinone derivatives.

[0073] For example, the antifungal agent may be at least one of LV5020 and LV660.

[0074] A second aspect of the present invention provides a method for preparing the fire-retardant and heat-resistant coating, the method comprising the following steps: First, epoxy-modified acrylic emulsion and dispersant are added to a disperser. Then, coupling agent and film-forming aid are added and stirred for the first time. Then, while stirring, ammonium polyphosphate, melamine, dipentaerythritol, hydrotalcite, modified shell powder and mullite fiber are added in sequence and stirred for the second time. Finally, defoamer and mildew inhibitor are added and stirred for the third time to obtain fire-retardant and heat-resistant coating.

[0075] In a preferred embodiment of the preparation method described in this invention, the first stirring speed is 400-600 rpm, the time is 10-20 min, and the temperature is 20-30℃.

[0076] As a preferred embodiment of the preparation method described in this invention, the second stirring speed is 1000-1200 rpm, the time is 30-60 min, and the temperature is 20-30℃.

[0077] As a preferred embodiment of the preparation method described in this invention, the third stirring speed is 600-800 rpm, the time is 15-30 min, and the temperature is 20-30℃.

[0078] A third aspect of the present invention provides the application of the fire-retardant and heat-resistant coating described herein in the preparation of fire-retardant coatings.

[0079] In a preferred embodiment of the application described in this invention, the fire-retardant coating is a fire-retardant coating in a battery.

[0080] Preferably, the fire-retardant coating is applied to the inside of the battery pack cover.

[0081] In a fourth aspect, the present invention provides a fire-retardant coating comprising a fire-retardant and heat-resistant coating, wherein the fire-retardant and heat-resistant coating is prepared from the fire-retardant and heat-resistant coating of the present invention.

[0082] In a preferred embodiment of the fire-retardant coating of the present invention, the fire-retardant coating is disposed on the inner side of the battery pack cover.

[0083] As a preferred embodiment of the fire-retardant coating of the present invention, the thickness of the fire-retardant and heat-resistant coating is 0.8-1.2 mm.

[0084] As a preferred embodiment of the fire-retardant coating of the present invention, the fire-retardant coating further includes a thermal insulation coating, which comprises the following components in parts by weight: 40-70 parts of water-based acrylic emulsion, 15-20 parts of aerogel powder, 10-20 parts of hollow glass microspheres, 10-20 parts of mica powder, 5-10 parts of nano-calcium carbonate, 10-20 parts of flame retardant, 0.5-1 part of dispersant, 0.1-1 part of film-forming aid, 0.1-1 part of defoamer, 0.1-1 part of rheology modifier, and 10-20 parts of water.

[0085] As a preferred embodiment of the fire-retardant coating of the present invention, the viscosity of the water-based acrylic emulsion at 25°C is 3000-6000 cps.

[0086] In a preferred embodiment of the fire-retardant coating of the present invention, the aerogel powder has a specific surface area of ​​400-800 m². 2 / g.

[0087] For example, the aerogel powder may be silica aerogel.

[0088] In a preferred embodiment of the fire-retardant coating of the present invention, the hollow glass microspheres have an average particle size of 20-50 μm.

[0089] In a preferred embodiment of the fire-retardant coating of the present invention, the mica powder has an average particle size of 800-1200 mesh.

[0090] In a preferred embodiment of the fire-retardant coating of the present invention, the average particle size of the nano-calcium carbonate is 60-100 nm.

[0091] As a preferred embodiment of the fire-retardant coating of the present invention, the flame retardant includes at least one of ammonium polyphosphate, melamine, and pentaerythritol.

[0092] In a preferred embodiment of the fire-retardant coating of the present invention, the dispersant includes polyester dispersant, polyacrylate dispersant, polyurethane dispersant, polyolefin dispersant or polyether dispersant.

[0093] In a preferred embodiment of the fire-retardant coating of the present invention, the film-forming aid includes at least one of propylene glycol ethyl ether and propylene glycol butyl ether.

[0094] In a preferred embodiment of the fire-retardant coating of the present invention, the defoamer includes at least one of silicone defoamers and polyether defoamers.

[0095] In a preferred embodiment of the fire-retardant coating of the present invention, the rheology modifier includes at least one of polyurethane rheology modifier and acrylic rheology modifier.

[0096] In a preferred embodiment of the fireproof coating of the present invention, the thickness of the thermal insulation coating is 0.8-1.2 mm.

[0097] In a preferred embodiment of the fireproof coating of the present invention, the heat-insulating coating is applied to the inside of the battery pack cover, and a fireproof and heat-resistant coating is then applied on the heat-insulating coating.

[0098] Compared with the prior art, the beneficial effects of the present invention are as follows: The fire-retardant and heat-resistant coating provided by this invention, through the selection and compounding of appropriate mass proportions of components, forms a coating that, even in a relatively thin state (0.8-1.2 mm), still exhibits excellent fire resistance and heat resistance, as well as excellent thermal insulation performance. It can be widely applied in the preparation of fire-retardant and heat-resistant coatings. Detailed Implementation

[0099] To better illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0100] Unless otherwise specified, the reagents, methods and equipment used in this invention are all conventional reagents, methods and equipment in the field.

[0101] The raw materials for fire-retardant and heat-resistant coatings come from the following sources: Epoxy-modified acrylic emulsion 1: acid value of 18 mg / KOH, average particle size of 200 nm, epoxy value of 0.05 eq / 100g, glass transition temperature of 25℃, purchased from Jining Fangyu Chemical Co., Ltd. WR-888W; Epoxy-modified acrylic emulsion 2: acid value 24 mg / KOH, average particle size 200 nm, epoxy value 0.05 eq / 100g, glass transition temperature 25℃, purchased from TY of Greenlink (Jining) Chemical Technology Co., Ltd. Epoxy-modified acrylic emulsion 3: acid value 12 mg / KOH, average particle size 200 nm, epoxy value 0.06 eq / 100g, glass transition temperature 25℃, purchased from Xiamen Kangdilong Trading Co., Ltd. (WL-103A); Epoxy-modified acrylic emulsion 4: acid value 13 mg / KOH, average particle size 280 nm, epoxy value 0.05 eq / 100g, glass transition temperature 25℃, purchased from Wanhua's WH-3260; Epoxy-modified acrylic emulsion 5: acid value 13 mg / KOH, average particle size 120 nm, epoxy value 0.06 eq / 100g, glass transition temperature 38℃, purchased from Huangshan Aoshengyuan New Material Technology Co., Ltd. as EPOXYOCR345; Epoxy-modified acrylic emulsion 6: acid value of 8 mg / KOH, average particle size of 200 nm, epoxy value of 0.05 eq / 100g, glass transition temperature of 30℃, purchased from Wanhua WR-155; Epoxy-modified acrylic emulsion 7: acid value 28 mg / KOH, average particle size 200 nm, epoxy value 0.06 eq / 100g, glass transition temperature 30℃, purchased from Wanhua's W-1000; Epoxy-modified acrylic emulsion 8: acid value 15 mg / KOH, average particle size 80 nm, epoxy value 0.05 eq / 100g, glass transition temperature 30℃, purchased from Tuosheng New Materials 6215; Epoxy-modified acrylic emulsion 9: acid value 13 mg / KOH, average particle size 400 nm, epoxy value 0.06 eq / 100g, glass transition temperature 30℃, purchased from Guangdong Hongke WR-773C.

[0102] Hydrotalcite 1: The molar ratio of magnesium to aluminum is 4:3. It was purchased from Kaisma (Dandong) High-Tech Materials Technology Co., Ltd. as 1-C hydrotalcite. Hydrotalcite 2: The molar ratio of magnesium to aluminum is 2:3. It was purchased from Hubei Xinfu Biotechnology Co., Ltd. as THP-24.

[0103] Modified shell powder 1: γ-aminopropyltriethoxysilane modified shell powder, wherein γ-aminopropyltriethoxysilane accounts for 2% of the mass of the modified shell powder, and is prepared in-house. The preparation method is as follows: S1. Weigh 500g of shell powder and add 720 mL of anhydrous ethanol, stir well to prepare 1000mL of shell powder slurry. S2. Prepare 1000 mL of trialkoxysilane hydrolysis solution according to the volume ratio (γ-aminopropyltriethoxysilane KH-550: ethanol: deionized water = 200 mL: 720 mL: 80 mL), and stir for 30 min to ensure complete hydrolysis of γ-aminopropyltriethoxysilane. S3. Slowly add 60 mL of trialkoxysilane hydrolysis solution to 1000 mL of shell powder slurry. Stir for 2 h under 70 °C water bath heating to fully react. Wash once with anhydrous ethanol and deionized water in sequence. Place in a drying oven and dry at 120 °C for 6 h to obtain modified shell powder 1. Modified shell powder 2: γ-aminopropyltriethoxysilane modified shell powder, γ-aminopropyltriethoxysilane accounts for 6% of the mass of modified shell powder, self-made, the preparation method is different from modified shell powder 1 in that the amount of trialkoxysilane hydrolysis solution is increased. Modified shell powder 3: γ-methacryloxypropyltrimethoxysilane modified shell powder, γ-methacryloxypropyltrimethoxysilane accounts for 2% of the mass of modified shell powder, self-made, the preparation method is different from modified shell powder 1 in that γ-methacryloxypropyltrimethoxysilane is used instead of γ-aminopropyltriethoxysilane. Modified shell powder 4: N-aminoethyl-3-aminopropylmethyldimethoxysilane modified shell powder, N-aminoethyl-3-aminopropylmethyldimethoxysilane accounts for 2% of the mass of modified shell powder, self-made, the preparation method is different from modified shell powder 1 in that N-aminoethyl-3-aminopropylmethyldimethoxysilane is used instead of γ-aminopropyltriethoxysilane.

[0104] Mullite fiber 1: with an aspect ratio of 50 and an average diameter of 4μm, it is a polycrystalline mullite fiber purchased from Zhejiang Jinglu Refractory Materials Co., Ltd. Mullite fiber 2: aspect ratio 31, average diameter 2μm, purchased from Jiahe Fiber Co., Ltd. Mullite fiber 3: with an aspect ratio of 100 and an average diameter of 7μm, purchased from Ouyihui Refractory Materials Co., Ltd.

[0105] Dispersant: 2774, purchased from Qingdao Gudao Technology Co., Ltd.

[0106] Coupling agent: KH550, purchased from Shandong Ruifeng New Materials Co., Ltd.

[0107] Film-forming agent: HLT-12, purchased from Guangdong Hualitai Chemical Co., Ltd.

[0108] Defoamer: DP-243, purchased from Guangdong Tianfeng Defoamer Co., Ltd.

[0109] Mildew inhibitor: GY-511, purchased from Changzhou Runyang Chemical Co., Ltd.

[0110] The raw materials for the thermal insulation coating are sourced as follows: Aqueous acrylic emulsion: 6968, purchased from Qingdao Enze Chemical Co., Ltd.

[0111] Aerogel powder: W20, purchased from Anhui Keang Nanomaterials Co., Ltd.

[0112] Hollow glass microspheres: HL25, purchased from Zhengzhou Shenglait Hollow Microsphere New Material Co., Ltd.

[0113] Mica powder: GB-2, purchased from Chuzhou Gree Mining Co., Ltd.

[0114] Nano calcium carbonate: Nano calcium carbonate, purchased from Guangdong Bangyou New Materials Co., Ltd.

[0115] Flame retardant: 8100, purchased from Guangdong Yinyuan New Materials Co., Ltd.

[0116] Dispersant: 2774, purchased from Qingdao Gudao Technology Co., Ltd.

[0117] Film-forming aid: CF-12, purchased from Guangdong Mairui New Materials Co., Ltd.

[0118] Defoamer: DP-215, purchased from Guangdong Tianfeng Defoamer Co., Ltd.

[0119] Rheology modifier: AKN-099, purchased from Foshan Qianyou Chemical Co., Ltd.

[0120] Examples 1-13 and Comparative Examples 1-10 The present invention provides a fire-retardant and heat-resistant coating in embodiments and comparative examples, the components (parts by mass) of the fire-retardant and heat-resistant coating being shown in Tables 1-3; Table 1 Table 2 Table 3 The method for preparing the fire-retardant and heat-resistant coating provided in Example 1 includes the following steps: First, add the epoxy-modified acrylic emulsion and dispersant to the disperser. Then, add the coupling agent and film-forming aid and stir at 500 rpm for 15 minutes. Next, while stirring, add ammonium polyphosphate, melamine, dipentaerythritol, hydrotalcite, modified shell powder, and mullite fiber in sequence and stir at 1100 rpm for 45 minutes. Finally, add the defoamer and mildew inhibitor and stir at 700 rpm for 25 minutes.

[0121] The preparation methods of Examples 2-13 and Comparative Examples 1-10 are consistent with those of Example 1.

[0122] Example 1 The performance of the fire-retardant and heat-resistant coatings prepared in the embodiments and comparative examples of this invention are verified by the following aspects: The prepared fire-resistant and heat-resistant coating was sprayed onto an electrophoretic steel plate and cured to form a 1 mm thick coating. The coating was baked at 80°C for 30 min and then cured. A fire test was then conducted on the coating using a 1300°C butane spray gun (in the tests of the examples and comparative examples, the distance and angle between the spray gun and the coating were kept the same, the nozzle of the flame spray gun was 10 cm away from the coating, and the angle was 90 degrees perpendicular to the coating). The test measured the time it took for the coating to burn through and expose the substrate to the naked eye, as well as the temperature of the back of the substrate facing the flame spray gun when it burned through. The test results are shown in Table 4. Table 4 As can be seen from Table 4, when the technical solution provided by the present invention is adopted, the obtained product has excellent fire resistance, heat resistance and heat insulation performance; specifically, when the obtained product is tested with a butane spray gun at 1300℃, the temperature of the back side of the substrate is below 339℃ when it is observed by the naked eye that the substrate has been burned through and exposed, and the time for the substrate to be burned through and exposed is more than 7 minutes and 21 seconds.

[0123] As can be seen from Example 1 and Comparative Examples 1-5, the hydrotalcite, modified shell powder and mullite fiber added in this invention are indispensable. When the above three are not included in Comparative Examples 1-5, the fire resistance and temperature resistance of the obtained products are poor.

[0124] As can be seen from Examples 1, 5-8 and Comparative Examples 6-9, the parameters of the epoxy-modified acrylic emulsion also affect the overall performance of the product. When the acid value of the epoxy-modified acrylic emulsion in Comparative Examples 6-7 is outside the range, the fire resistance and temperature resistance of the obtained product deteriorates. When the particle size of the epoxy-modified acrylic emulsion in Comparative Examples 8-9 is outside the range, the fire resistance and temperature resistance of the obtained product deteriorates.

[0125] As can be seen from Example 1 and Comparative Example 10, when the modifier of the modified shell powder is not the one in this invention, the fire resistance and temperature resistance of the obtained product are worse.

[0126] Example 2 Example 2 of the present invention tests the effect of simultaneously introducing a thermal insulation coating and a fire-resistant and heat-resistant coating, including the following steps: The preparation method of the thermal insulation coating is as follows: 55 parts of water-based acrylic emulsion and 15 parts of water are added to a dispersion tank, followed by the sequential addition of 0.8 parts of dispersant, 0.5 parts of film-forming aid and 0.5 parts of defoamer. The mixture is stirred at a stirring speed of 400-600 rpm for 25 min. Then, 18 parts of aerogel powder, 15 parts of hollow glass microspheres, 15 parts of mica powder, 8 parts of nano calcium carbonate and 15 parts of flame retardant are added sequentially and dispersed at a stirring speed of 1000 rpm for 45 min. Finally, 0.5 parts of rheology modifier are added to adjust the viscosity to 8000 cps at 25℃ to obtain the thermal insulation coating.

[0127] First, a 0.5mm heat-insulating coating is sprayed onto the electrophoretic aluminum plate. After curing, a 0.5mm fire-retardant and heat-resistant coating is sprayed on. The plate is baked at 80℃ for 50 minutes. After curing, a 1300℃ flame torch is used to conduct a fire test on the coating (the nozzle of the flame torch is 10cm away from the coating and the angle is 90 degrees, burning the coating perpendicularly). The coating burns through and the substrate is visible to the naked eye in 12 minutes. The corresponding temperature of the flame directly facing the back of the substrate is 180℃.

[0128] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of the present invention and not to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A fire-retardant and heat-resistant coating, characterized in that, The fire-retardant and heat-resistant coating comprises the following components in parts by weight: 40-60 parts epoxy-modified acrylic emulsion, 5-15 parts ammonium polyphosphate, 5-15 parts melamine, 5-15 parts dipentaerythritol, 5-15 parts hydrotalcite, 5-30 parts modified shell powder, 1-10 parts mullite fiber, 0.5-1 part dispersant, 0.5-3 parts coupling agent, 1-3 parts film-forming agent, 0.5-1 part defoamer, 0.5-1 part mildew inhibitor; The epoxy-modified acrylic emulsion has an acid value of 10-25 mg / KOH and an average particle size of 100-300 nm. The modified shell powder is a trialkoxysilane modified shell powder.

2. The fire-retardant and heat-resistant coating according to claim 1, characterized in that, The fire-retardant and heat-resistant coating comprises the following components in parts by weight: 48-52 parts epoxy-modified acrylic emulsion, 8-10 parts ammonium polyphosphate, 9-12 parts melamine, 9-12 parts dipentaerythritol, 8-12 parts hydrotalcite, 15-20 parts modified shell powder, 4-8 parts mullite fiber, 0.5-1 part dispersant, 1-2 parts coupling agent, 1.5-2 parts film-forming agent, 0.5-1 part defoamer, and 0.5-1 part mildew inhibitor.

3. The fire-retardant and heat-resistant coating according to claim 1, characterized in that, The ratio of the total mass fraction of the hydrotalcite and modified shell powder to the mass fraction of the mullite fiber is 2-35.

4. The fire-retardant and heat-resistant coating according to claim 1, characterized in that, Satisfy at least one of the following: (1) The glass transition temperature of the epoxy-modified acrylic emulsion is 15-35℃; (2) The epoxy value of the epoxy-modified acrylic emulsion is 0.03-0.08 eq / 100g; (3) The trialkoxysilane accounts for 2-6% of the mass of the modified seashell powder; (4) The trialkoxysilane includes at least one of γ-aminopropyltriethoxysilane and γ-methacryloyloxypropyltrimethoxysilane; (5) The hydrotalcite includes magnesium and aluminum, and the molar ratio of magnesium to aluminum is (2-4):

3.

5. The fire-retardant and heat-resistant coating according to claim 1, characterized in that, The aspect ratio of the mullite fiber is 31-100; And / or, the average diameter of the mullite fibers is 2-7 μm.

6. The fire-retardant and heat-resistant coating according to claim 1, characterized in that, Satisfy at least one of the following: (1) The dispersant includes at least one of polyester dispersant, polyacrylate dispersant, polyurethane dispersant, polyolefin dispersant, and polyether dispersant; (2) The coupling agent includes a silane coupling agent; (3) The film-forming agent includes at least one of propylene glycol ethyl ether and propylene glycol butyl ether; (4) The defoamer includes silicone-based defoamers; (5) The antifungal agent includes at least one of nano zinc oxide, nano titanium dioxide, and isothiazolinone derivatives.

7. The use of the fire-retardant and heat-resistant coating as described in any one of claims 1-6 in the preparation of fire-retardant coatings.

8. A fire-retardant coating, characterized in that, The fire-retardant coating includes a fire-retardant and heat-resistant coating, which is prepared from the fire-retardant and heat-resistant coating as described in any one of claims 1-6.

9. The fire-retardant coating according to claim 8, characterized in that, The thickness of the fireproof and heat-resistant coating is 0.8-1.2 mm.

10. The fire-retardant coating according to claim 8, characterized in that, The fireproof coating also includes a thermal insulation coating, which comprises the following components in parts by weight: 40-70 parts of water-based acrylic emulsion, 15-20 parts of aerogel powder, 10-20 parts of hollow glass microspheres, 10-20 parts of mica powder, 5-10 parts of nano-calcium carbonate, 10-20 parts of flame retardant, 0.5-1 part of dispersant, 0.1-1 part of film-forming aid, 0.1-1 part of defoamer, 0.1-1 part of rheology modifier, and 10-20 parts of water.