A low-gloss powder coating and its preparation method

By measuring the changes in the main resin composition of the pre-pulverized flakes, graded fine powder, and finished powder, and combining this with a calibration model for the amount of compatibilizer added, the problem of finished product composition shift caused by the selective distribution of resin in low-gloss powder coatings was solved, achieving a balanced resin composition and a low-gloss effect.

CN123063045APending Publication Date: 2026-11-10LIAONING TUOTIAN ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611506914.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the crushing and grading process of low-gloss powder coatings made from a blend of polyester and acrylic resins, the selective distribution of the main resins leads to a shift in the composition of the finished product. Existing methods cannot simultaneously guarantee the main resin composition and low-gloss performance of the finished powder.

Method used

By measuring the changes in the main resin composition of the pre-pulverized flakes, the fine powder discharged after grading, and the finished powder, and combining this with the amount of compatibilizer added, a calibration model and verification method were used to determine the appropriate amount of compatibilizer to maintain resin composition balance and achieve a low-gloss effect.

Benefits of technology

It effectively maintains the balance of the main resin composition during the crushing and grading process, and ensures the low-gloss performance of the coating, avoiding the low-gloss degradation caused by excessive compatibilizer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063045A_ABST
    Figure CN123063045A_ABST
Patent Text Reader

Abstract

This invention discloses a low-gloss powder coating and its preparation method, relating to the field of thermosetting powder coating technology. For a powder coating system comprising polyester resin P and acrylic resin A, a zero-feed control and multiple positive-feed candidates are set up for the same compatibilizer candidate K. Premixing, melt extrusion, cooling, pulverizing, and grading are performed sequentially to obtain flakes S, graded fine powder F, and finished powder T, respectively. The composition of the main resin in the three streams is measured. When the zero-feed control shows acrylic resin enrichment into fine powder, resulting in a decrease in the finished product composition, the degree of fine powder enrichment, finished product composition shift, and low-gloss performance of the positive-feed candidates are jointly evaluated. From the actual tested candidates, a compatibilizer feed amount that simultaneously satisfies the requirements of reduced fine powder enrichment, reduced finished product composition shift, and a 60° gloss rating value not exceeding 30 GU is determined. The low-gloss powder coating is then prepared according to the determined feed amount and corresponding preparation conditions, thus balancing powder composition maintenance and low-gloss performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermosetting powder coating technology, specifically to a low-gloss powder coating and its preparation method. Background Technology

[0002] Polyester resins and acrylic resins can be blended to prepare low-gloss powder coatings. The low-gloss performance of this type of system is not only related to the feeding ratio of the two main resins and the curing reaction, but also affected by the compatibility of the two resins, the pulverization behavior, and the powder classification process.

[0003] Powder coatings are typically produced through batching, melt extrusion, cooling, pulverization, and grading to obtain the finished powder. For systems containing two main resins, the distribution behavior of the different main resins during pulverization and grading may differ, resulting in the fine powder discharged from grading having a different main resin composition than the unpulverized flakes. This causes the main resin composition of the finished powder to deviate from the original feeding relationship.

[0004] When acrylic resin is enriched in the fine powder discharged from the classification process, the proportion of acrylic resin in the total amount of the two main resins in the finished powder will decrease. Evaluating the formulation solely based on the raw material feeding ratio cannot reflect the above compositional changes; evaluating the formulation solely based on the final coating gloss makes it difficult to identify whether the compatibilizer has improved the compositional retention during the grinding and classification process with a lower feeding amount.

[0005] On the other hand, increasing the amount of compatibilizer added can alter the interphase interaction, melt flow, and curing film state between the two main resins. The amount of compatibilizer required to reduce the compositional shift in the finished product may not be the same as the amount allowed to maintain low-gloss performance. Therefore, it is necessary to establish a method for determining the amount of compatibilizer that simultaneously considers both the preservation of the fragmented composition and the low-gloss performance of the coating. Summary of the Invention

[0006] The technical problem to be solved by this invention is to provide a method for preparing low-gloss powder coatings, which may have selective distribution of the main resin and deviation of the finished product composition during the crushing and grading process of polyester resin and acrylic resin compound low-gloss powder coatings. This method can determine the appropriate amount of compatibilizer to be added based on the changes in the main resin composition of the three material streams (sheet material, fine powder and finished powder) and the low-gloss performance of the coating, taking into account the specific main resin, compatibilizer candidate and powdering conditions.

[0007] To solve the above-mentioned technical problems, the present invention selects polyester resin P, acrylic resin A and the same compatibilizer candidate K, mixes P and A according to a preset feeding ratio, and sets up a zero feeding control of K and multiple different positive feeding candidates.

[0008] In the same formulation determination process, all formulations adopt other formulation components of the same type and feeding amount, and keep the melt extrusion, cooling, pulverization, classification and feeding conditions consistent, so as to respectively obtain the pre-pulverization sheet material S, the fine powder F discharged from classification, and the retained finished powder T.

[0009] The mass percentage of the main acrylic resin A in the sum of the mass of the main polyester resin P and the main acrylic resin A is measured for S, F and T respectively, and recorded as xS,i, xF,i and xT,i respectively, where i=0 represents the zero-feed control, i=1, 2, ..., n represent different positive feed candidates respectively, and n is a positive integer not less than 2. The detection signals of the compatibilizer candidate K and other components that are the same as or similar to the main resin shall be distinguished by a calibration model or other verified methods.

[0010] When the zero-feed control satisfies xF,0>xS,0 and xT,0<xS,0, it indicates that under the current material and powder preparation conditions, there exists a phenomenon that the main acrylic resin A is enriched in the fine powder discharged by classification, resulting in a decrease in the proportion of the main acrylic resin A in the finished powder. At this time, the fine powder enrichment, finished product composition deviation and low-gloss combined evaluation are continuously carried out for each positive feed candidate.

[0011] The decrease in the composition of the finished powder of the zero-feed control is defined as D0=xS,0-xT,0, and the fine powder enrichment amount of the zero-feed control is defined as E0=xF,0-xS,0; for each positive feed candidate, the decrease in the composition of its finished powder is defined as Di=xS,i-xT,i, and its fine powder enrichment amount is defined as Ei=xF,i-xS,i. Taking 0≤Di<D0 and 0≤Ei<E0 as the judgment conditions for the reduction of both the selective enrichment of fine powder and the composition deviation of the finished product relative to the zero-feed control.

[0012] For the positive feed candidates that meet the composition migration improvement condition, their finished powders are made into test panels under the same predetermined curing conditions, and measured using the same 60° gloss measurement and sampling rules, the 60° gloss evaluation value corresponding to the i-th positive feed candidate is recorded as Gi, and Gi≤30GU is taken as the low-gloss judgment condition.

[0013] The feeding amount of the compatibilizer candidate K that simultaneously satisfies the reduction of fine powder enrichment, the reduction of finished product composition deviation and Gi≤30GU is determined from the actually tested positive feed candidates, and the determined feeding amount, as well as the same materials, other formulation components and main preparation conditions as the corresponding candidate formulation are used to prepare the low-gloss powder coating.

[0014] In a preferred embodiment, when there are multiple positive feed candidates that simultaneously meet the above conditions, the feed amount corresponding to the positive feed candidate with the smallest feed amount of compatibilizer candidate K is selected to avoid further increasing the amount of compatibilizer when the powder composition and low light requirements have been met, thereby reducing the possibility of further increasing the compatibility and causing the low light performance to deteriorate, and reducing unnecessary compatibilizer addition.

[0015] In a preferred embodiment, the mass ratio of polyester resin P to acrylic resin A is 70:30, and at least three different positive feed candidates are set; further, 0≤Di≤0.8 percentage points is used as the preferred quantitative condition for the finished product composition offset, and Gi≤15GU is used as the preferred low-light screening condition.

[0016] Preferably, to eliminate false improvements caused by detection fluctuations, the compositional improvement of the i-th positive feed candidate relative to the zero feed control is defined as Ii = D0 - Di, and Ii is further required to be greater than the corresponding expanded uncertainty U(Ii).

[0017] Preferably, three test plates are prepared for each candidate material being fed. Each test plate undergoes a 60° gloss measurement at five different locations, and the maximum value among the fifteen measurements is taken as the gloss evaluation value Gi. The 60° gloss measurement is performed according to the 60° measurement method specified in GB / T9754—2025. Preferably, the test plates are cured at 200°C for 15 minutes, resulting in a coating thickness of 60–80 μm. After curing, the test plates are placed at 23±2°C and 50±5% relative humidity for 24 hours before measurement.

[0018] If the zero-feed control does not show the aforementioned fine powder enrichment and product composition decrease phenomenon, or if there is no feed amount that simultaneously satisfies the reduction in fine powder enrichment, reduction in product composition shift, and Gi≤30GU among the positive feed candidates in this round of actual testing, then terminate the formulation determination of the current compatibilizer candidate K; and repeat the above steps after changing the main polyester resin P, main acrylic resin A, compatibilizer candidate K, or main preparation conditions.

[0019] This invention incorporates the changes in the main resin composition in the three streams of pre-pulverized flakes, graded and discharged fine powder, and finished powder into the process of determining the amount of compatibilizer added. It evaluates both the enrichment degree of the main acrylic resin in the graded and discharged fine powder and the compositional shift of the finished powder relative to the flakes, thereby identifying and quantifying the selective distribution of the main resin caused by pulverization and grading.

[0020] This invention uses the reduction of fine powder enrichment, the reduction of finished product composition shift, and low gloss performance as screening conditions for candidate feed amounts, so that the determination of compatibilizer feed amount no longer depends solely on the final gloss or a single compatibility index.

[0021] This invention determines the amount of compatibilizer to be added based on specific materials and powdering conditions, and repeats the determination steps after changing materials or main preparation conditions, thereby avoiding directly extrapolating the empirical dosage window of a certain compatibilizer to other compatibilizers or other powdering conditions.

[0022] By using calibrated and validated quantitative methods for the main resin and standardized rules for gloss evaluation, repeatable criteria for formulation can be established without requiring specific phase region structures that have not been confirmed by morphological characterization as necessary criteria. Attached Figure Description

[0023] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute an undue limitation of this application.

[0024] Figure 1 The graph shows the relationship between the amount of compatibilizer C1 added and the mass percentage of the main acrylic resin in the graded fine powder and finished powder.

[0025] Figure 2 The graph shows the relationship between the amount of compatibilizer C1 added and the representative value of the 60° gloss of the resulting coating. Detailed Implementation

[0026] The present invention will be further described below with reference to specific embodiments and experimental data. The following content is used to illustrate the technical solution of the present invention, and is not intended to limit the scope of protection of the present invention.

[0027] It should be noted that P and A represent the main polyester resin and main acrylic resin in the formulation, respectively, and K represents the selected compatibilizer candidate. Polyester or acrylic structures in K and other components such as pigments, fillers, leveling agents, and benzoin are not directly included in the main resin P or A.

[0028] For any sample of raw material, fine powder, or finished powder, the mass percentage x of the main acrylic resin A is calculated as x = 100mA / (mP + mA), where mP and mA represent the mass of the main polyester resin and the main acrylic resin in the sample, respectively.

[0029] The pre-crushed flakes, the graded and discharged fine powder, and the finished powder are denoted as S, F, and T, respectively; the subscript for zero-feed control is 0, and the subscript for positive-feed candidate is i, where i = 1, 2, ..., n, and n is a positive integer not less than 2.

[0030] The decrease in finished powder composition in the zero-feed control is defined as D0 = xS,0 - xT,0; the enrichment of fine powder in the zero-feed control is defined as E0 = xF,0 - xS,0. For the i-th positive-feed candidate, the decrease in finished powder composition is defined as Di = xS,i - xT,i, and the enrichment of fine powder is defined as Ei = xF,i - xS,i, all in percentage points. The measured xS,i of the flake material of each positive-feed candidate is used as the composition baseline.

[0031] The composition improvement relative to the zero-feed control is Ii = D0 - Di. When uncertainty enhancement judgment is required, the combined standard uncertainty u(Ii) of Ii is calculated based on the standard uncertainty and covariance of the measurement vector (xS,0, xT,0, xS,i, xT,i), and the expanded uncertainty U(Ii) = 2u(Ii) is obtained with a coverage factor k = 2. The correlation introduced by the common calibration model is included in the covariance.

[0032] The term "limited compatibility" as used in this specification refers to a state in which, for a given P, A, K and powder preparation conditions, the amount of K added is controlled to reduce the offset of the main resin composition of the finished powder relative to the flake material, while the resulting coating has a 60° gloss rating value Gi that is not higher than 30 GU.

[0033] Furthermore, the preparation and screening process is as follows:

[0034] Generally, P and A are mixed according to a preset feeding ratio, and a zero-feed control of K and several different positive feeding candidates are set. As a preferred embodiment, the P / A feeding mass ratio is 70:30, with the total feeding mass of P and A being 100 parts by mass, and at least three different positive feeding candidates are set. The positive feeding candidates are preferably arranged from low to high and adjacent feeding amounts are different.

[0035] All formulations use the same other formulation components. These other formulation components may include one or more of pigments, fillers, leveling agents, wetting agents, benzoin, wax powder, and curing accelerators.

[0036] Each formulation was premixed, melt-extruded, and cooled to form sheets, using the same equipment, melt mixing temperature, extrusion operation settings, and cooling method.

[0037] The flakes were crushed and graded separately. Each formula used the same crushing operation settings, grading method and feeding conditions. The flakes S were collected separately, the fine powder F was discharged after grading and the finished powder T was retained.

[0038] Representative samples were taken from S, F, and T, and the composition of the main resin was determined. Sampling boundaries, sample pretreatment, and quantitative analysis methods remained consistent throughout the same round of screening.

[0039] Preferably, samples of equal mass increment are respectively taken from the front section, middle section and rear section of the entire batch of materials for each material stream, so as to form at least three independent composite samples covering the entire batch of materials; then the independent composite samples are divided in equal mass and physically combined to form a combined sample M for judgment, the combined sample M is reloaded for measurement at least three times, and the average value of the measurement results is taken as the composition value of the material stream. This sampling method is used to reduce the influence of in-batch inhomogeneity and single-point sampling on the judgment result.

[0040] When the zero-feed control satisfies xF,0>xS,0 and xT,0<xS,0, the positive feed candidates are continuously evaluated; otherwise, the current screening of K is terminated.

[0041] Calculate Di and Ei for the positive feed candidate; when 0≤Di<D0 and 0≤Ei<E0, it is considered that the candidate simultaneously reduces the finished product composition deviation and the fine powder enrichment degree relative to the zero-feed control, and enters the low-gloss evaluation. In a preferred embodiment, it is further required that 0≤Di≤0.8 percentage points. For the embodiment using uncertainty enhanced judgment, it is also required that Ii>U(Ii).

[0042] The finished powder that has entered the low-gloss evaluation is made into test panels under the same substrate and spraying conditions, and Gi is obtained using the same predetermined curing conditions as well as the same 60° gloss measurement and sampling rules; candidates satisfying Gi≤30GU enter the feed amount determination. In a preferred embodiment, it is further required that Gi≤15GU.

[0043] The applicable feed amount of K is determined from the tested candidates that simultaneously satisfy the reduction of fine powder enrichment, the reduction of finished product composition deviation and Gi≤30GU, and the low-gloss powder coating is prepared according to P, A, K, other formula components and main preparation conditions corresponding to the determined feed amount. In a preferred embodiment, when a plurality of candidates all meet the above conditions, the group with the smallest K feed amount is selected.

[0044] In a preferred embodiment, after the feed amount of K is determined, a new zero-feed control and a verification formula prepared according to the determined feed amount are re-weighed and prepared, and pre-mixing, melt extrusion, cooling, pulverization, classification, sampling and testing are independently completed respectively; in the verification stage, new zero-feed control is used to re-determine D0 and E0, and the measurement results of the zero-feed control in the screening stage are not used. When the verification formula again meets the same conditions of fine powder enrichment, finished product composition deviation and Gi≤30GU, the feed amount is verified.

[0045] Further, the composition of the main resin can adopt a quantitative analysis method that can distinguish the signal contributions of P, A and K, and has been verified to meet the judgment accuracy. A multivariate quantitative infrared method is preferably used.

[0046] When using the multivariate quantitative infrared method, a known composition calibration sample is prepared by weighing using the actually selected P, A, K and other formulation components. The calibration sample covers the range of variation of the main resin ratio, K content and pigment and filler content in the test flakes, fine powder and finished powder.

[0047] After the calibration model is established, it is independently verified using known composition samples that are not involved in the modeling. When the sample to be tested exceeds the calibration range, the calibration range is expanded and the measurement is repeated, without using the extrapolation results of the calibration range.

[0048] Independent validation samples are preferably used to cover the decision range of the main resin composition involved in low-light screening. At the same time, the content of compatibilizer candidate K and the content of non-main components are changed to evaluate the model's average bias, root mean square prediction error and maximum absolute error. When the independent validation results are insufficient to support the set composition determination threshold, the model is not used to make the formulation selection in this round.

[0049] To avoid the structural signals of K and other additives being incorrectly included in the main resin P or A, the calibration model should include variations in K and major organic additives; if the model cannot reliably distinguish between P, A and K, it should not be used for this round of formulation selection.

[0050] In one optional infrared acquisition method, the ATR-FTIR scanning range is 4000–650 cm⁻¹, the resolution is 4 cm⁻¹, and each sample is scanned a total of 32 times and re-measured three times. The same sample preparation method and spectral acquisition parameters are used in the same round of screening.

[0051] The finished powder of each candidate formulation was electrostatically sprayed onto a flat, opaque test plate of the same batch and with the same surface treatment. Each group used the same spraying parameters and controlled similar coating thicknesses.

[0052] In a preferred embodiment, the coating thickness is controlled to be 60–80 μm, and the test panel is cured for 15 min after reaching 200°C. After curing, the test panel is placed at 23±2°C and 50±5% relative humidity for 24 h before a 60° gloss measurement is performed. For base resin systems suitable for other curing conditions, the corresponding predetermined curing conditions can be used, but they should remain consistent within the same round of candidate comparison.

[0053] The 60° gloss was measured according to the 60° measurement method specified in GB / T9754—2025. Three test plates were prepared for each candidate material being fed, and five non-overlapping measurement positions with the same layout were selected for each test plate, resulting in a total of fifteen measurement values.

[0054] Record the arithmetic mean, minimum, and maximum values ​​of fifteen measurements, and use the maximum value among the fifteen measurements as the gloss evaluation value Gi. Three test plates, five points per plate, and taking the maximum value are in accordance with the formulation screening rules specified in this invention.

[0055] Experimental Example: Gradient Test of Compatibilizer C1 Dosage:

[0056] In a low-gloss powder coating system with a P / A ratio of 70 / 30, a polyester-polyacrylate block or multi-block compatibilizer was selected as compatibilizer C1, with feed amounts of 0, 0.25, 0.5, 1.0, 1.5, 2.0, 3.0, and 5.0 phr, respectively. The P / A ratio for each group of flakes was recorded as 70.0 / 30.0, and the fine powder content, fine powder P / A, finished powder P / A, and 60° gloss data were obtained under the same comparison conditions.

[0057]

[0058] like Figure 1 As shown, the proportion of acrylic resin in the fine powder of the zero-feed control was 56.0%, and the proportion of acrylic resin in the finished powder was 26.95%. As the amount of C1 feed increased, the proportion of acrylic resin in the fine powder gradually approached the 30.0% standard of the flake material, and the proportion of acrylic resin in the finished powder also gradually recovered.

[0059] Calculated from the data in the table, the decrease in composition of the finished powder (D0) in the zero-feed control group was 3.05 percentage points; when C1 was 0.5, 1.0 and 1.5 phr, the decrease in composition was 1.52, 0.70 and 0.40 percentage points, respectively, indicating that low doses of C1 can reduce the shift in the composition of the main resin after pulverization and classification.

[0060] Further calculations based on the flake and fine powder data in the table show that the fine powder enrichment E0 in the zero-feed control was 26.0 percentage points; when C1 was 0.5, 1.0, 1.5, and 2.0 phr, the fine powder enrichment Ei was 15.0, 8.0, 5.0, and 2.0 percentage points, respectively, all lower than E0. This indicates that as the compatibilizer dosage increases, the enrichment degree of acrylic resin in the graded fine powder continuously decreases, a change that corroborates the recovery trend in the composition of the finished powder.

[0061] like Figure 2 As shown, when C1 increases from 0 to 1.0–1.5 phr, the gloss representative value remains at a low level; when C1 continues to increase to 3.0 phr and 5.0 phr, the gloss representative value rises to 17.1 GU and 32.0 GU, respectively. This indicates that continuing to increase the compatibilizer after composition retention has been improved does not necessarily benefit low gloss retention.

[0062] The gloss data from the above experiments are listed as representative values ​​and ranges from the test group records, used to illustrate the relationship between compatibilizer dosage, main resin composition retention, and low-gloss performance. When implementing the method described in the claims, Gi is obtained according to the above-mentioned uniform sampling and gloss evaluation rules.

[0063] When compared on the basis that the composition decrease does not exceed 0.8 percentage points, the composition decrease corresponding to 1.0 phr and 1.5 phr is 0.70 and 0.40 percentage points respectively; the upper ends of the gloss recording range for the two are 13 GU and 15 GU respectively. This result indicates that, in the present test system, there is a relatively low compatibilizer feeding interval that balances composition retention and low-gloss performance.

[0064] The technical focus of the present invention is to determine the applicable feeding amount of K through physical trial production under the same conditions, quantification of the three main flow resins of sheet material - fine powder - finished powder, and unified gloss evaluation for specific P, A, K and powder preparation conditions, and prepare the low-gloss powder coating according to the determined feeding amount and corresponding preparation conditions.

[0065] After replacing P, A or K, or changing the melt mixing, pulverization, classification and feeding conditions, the enrichment degree of fine powder, the composition deviation of the finished product and the applicable K feeding amount may all change, so the feeding amount determination and preparation steps described above shall be re-executed.

[0066] The P / A ratio in the sheet material, fine powder and finished powder is a normalized composition index of the two main resins. When the mass fraction of fine powder and the P / A ratio adopt different mass bases, the simplified two-component mass conservation calculation shall not be directly carried out without verification of the main resin content of each stream and other discharges.

[0067] When the zero-feeding control does not have the phenomena of fine powder enrichment and finished product composition decrease to be solved, or none of the actually tested positive-feeding candidates simultaneously satisfy 0≤Di<D0, 0≤Ei<E0 and Gi≤30 GU, the evaluation of the current compatibilizer candidate can be terminated and the material can be replaced for re-implementation.

[0068] The technical features of the above-described embodiments can be combined arbitrarily. For the sake of brevity, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction between these combinations of technical features, they shall be regarded as the scope recorded in this specification.

[0069] The above-described embodiments only represent several implementations of the present application, which are described relatively specifically and in detail, but shall not be construed as a limitation on the protection scope of the present application. It should be pointed out that for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and all of these shall fall within the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the appended claims.

Claims

1. A method for preparing a low-gloss powder coating, characterized in that, comprising the following steps: S1. Selecting polyester resin P, acrylic resin A and the same compatibilizer candidate K, proportioning the polyester resin P and the acrylic resin A according to a preset feeding ratio, and setting a zero-feeding control of the compatibilizer candidate K and a plurality of different positive-feeding candidates; S2. Under the conditions that the types and feeding amounts of other formula components are the same and the main preparation conditions are the same, respectively subjecting the zero-feeding control and each positive-feeding candidate to premixing, melt extrusion, cooling, crushing and classification, to obtain pre-crushing sheet material S, fine powder F discharged by classification and retained finished powder T respectively; S3. Respectively measuring the mass percentages of the main acrylic resin A in the sum of the mass of the main polyester resin P and the main acrylic resin A in the sheet material S, fine powder F and finished powder T corresponding to each formula, which are respectively recorded as xS,i, xF,i and xT,i, wherein i=0 represents the zero-feeding control, i=1, 2, ..., n respectively represent different positive-feeding candidates, n is a positive integer not less than 2, and distinguishing the contributions of the compatibilizer candidate K and other components to the detection signal from the contributions of the main polyester resin P and the main acrylic resin A; S4. When the zero-feeding control satisfies xF,0>xS,0 and xT,0<xS,0, defining the finished powder composition reduction amount of the zero-feeding control as D0=xS,0-xT,0, and defining the fine powder enrichment amount of the zero-feeding control as E0=xF,0-xS,0; respectively determining the finished powder composition reduction amount Di=xS,i-xT,i and the fine powder enrichment amount Ei=xF,i-xS,i for the i-th positive-feeding candidate, and preparing the finished powder corresponding to each positive-feeding candidate into a test plate under the same predetermined curing condition, and obtaining the gloss evaluation value Gi corresponding to the i-th positive-feeding candidate according to the same 60° gloss measurement and sampling rule; S5. Determining the feeding amount of the compatibilizer candidate K that simultaneously satisfies 0≤Di<D0, 0≤Ei<E0 and Gi≤30GU from the actually tested positive-feeding candidates, and preparing the low-gloss powder coating according to the determined feeding amount and the same materials, other formula components and main preparation conditions as the corresponding candidate formula; 2. The preparation method according to claim 1, characterized in that, The feeding mass ratio of the polyester resin P to the acrylic resin A is 70:30; taking the total feeding mass of the polyester resin P and the acrylic resin A as 100 parts by mass, the positive-feeding candidates at least include three different feeding amounts of the compatibilizer candidate K; 3. The preparation method according to claim 1 or 2, characterized in that, The i-th positive-feeding candidate further satisfies 0≤Di≤0.8 percentage points, and Gi≤15GU; 4. The preparation method according to any one of claims 1 to 3, characterized in that, When there are a plurality of positive-feeding candidates that simultaneously satisfy the conditions of fine powder enrichment, finished product composition deviation and Gi≤30GU, selecting the feeding amount corresponding to the positive-feeding candidate with the smallest feeding amount of the compatibilizer candidate K among them; 5. The preparation method according to any one of claims 1 to 4, characterized in that, Defining the finished powder composition improvement amount of the i-th positive-feeding candidate relative to the zero-feeding control as Ii=D0-Di; determining the expanded uncertainty U(Ii) of Ii according to the measurement uncertainties and their covariances of xS,0, xT,0, xS,i and xT,i, and further requiring Ii>U(Ii).

6. The preparation method according to any one of claims 1 to 5, characterized in that, For each formulation, samples of equal mass increment are obtained along the front, middle and rear sections of the corresponding material flow for the flakes S, fine powder F and finished powder T, respectively, and at least three independent composite samples covering the entire batch of materials are formed. The independent composite samples are physically combined after being separated by equal mass to form a combined sample M for judgment. The combined sample M is resampled and measured at least three times, and the average value of each measurement result is used as xS,i, xF,i or xT,i of the corresponding material flow.

7. The preparation method according to any one of claims 1 to 6, characterized in that, The composition of the main resin was determined using a multivariate quantitative infrared method established with known composition calibration samples and verified by independent verification samples. The calibration samples were prepared by actually selected P, A, K and other formulation groups, and covered the range of variation of the main resin ratio, K content and pigment and filler content of the sample to be tested.

8. The preparation method according to any one of claims 1 to 7, characterized in that, For each candidate material being fed, three test plates were prepared. The 60° gloss of each test plate was measured at five different locations, and the maximum value among the fifteen measurements was taken as the gloss evaluation value Gi. The 60° gloss was measured according to the 60° measurement method specified in GB / T9754—2025. The predetermined curing conditions were that the test plate was cured at 200°C for 15 minutes, the coating thickness was 60-80 μm, and the cured test plate was placed at 23±2°C and 50±5% relative humidity for 24 hours before measurement.

9. The preparation method according to any one of claims 1 to 8, characterized in that, After determining the amount of compatibilizer candidate K, a new zero-feed control and a confirmation formulation prepared according to the determined amount of feed were prepared, and premixing, melt extrusion, cooling, pulverizing, grading, sampling, determination of main resin composition and 60° gloss evaluation were performed independently respectively. D0 and E0 were re-determined with the new zero-feed control. When the confirmation formulation once again met the conditions of fine powder enrichment, finished product composition shift and Gi≤30GU corresponding to claim 1, the amount of feed was confirmed.

10. A low-gloss powder coating, characterized in that, The coating is prepared by any one of claims 1 to 9, and the 60° gloss rating of the coating formed by the low-gloss powder coating is not higher than 15 GU.