An aqueous binder for silicon negative electrode, a silicon negative electrode sheet, and a lithium ion battery
By introducing polyphenolic compounds and small-molecule polycarboxylic acids into a water-soluble polymer binder, a dynamically cross-linked water-based binder is formed, which solves the structural failure problem caused by the volume expansion of silicon anodes and improves the cycle performance and stability of lithium-ion batteries.
Patent Information
- Application Number
- CN202611258621.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional graphite anodes have limited theoretical specific capacity, while silicon anodes suffer structural failure due to volume expansion during charging and discharging. Existing water-soluble polymer binders are insufficient to maintain the structural stability of silicon anodes over the long term.
A water-soluble polymer binder is used as a continuous film-forming component. Polyphenolic compounds and small molecule polycarboxylic acids are introduced to form a dynamically cross-linked water-based binder, which improves the bonding force between silicon active materials, conductive agents and current collectors.
It enhances the structural stability of silicon anodes and battery cycle performance, improves reversible specific capacity and cycle stability, and reduces the risk of particle pulverization and electrode cracking.
Smart Images

Figure CN123063100A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion battery technology, and in particular to an aqueous binder for silicon anodes, silicon anode sheets, and lithium-ion batteries. Background Technology
[0002] With the rapid development of portable electronic devices, electric vehicles, and energy storage systems, lithium-ion batteries are facing higher demands for energy density, cycle life, and safety performance. Traditional graphite anodes, due to their limited theoretical specific capacity (372 mAh g⁻¹),... -1 The silicon anode has gradually become insufficient to meet the development needs of high-energy-density lithium-ion batteries. Silicon anodes possess a relatively high theoretical specific capacity (approximately 4200 mAh g⁻¹). -1 and a lower lithium intercalation potential (approximately 0.4 V vs. Li). + / Li) is considered an important candidate system for next-generation high-capacity lithium-ion battery anode materials.
[0003] However, silicon anodes undergo significant volume expansion (approximately 300%) during charge and discharge, which can easily lead to problems such as active particle pulverization, electrode structure cracking, conductive network damage, and repeated formation of solid electrolyte interfacial films, ultimately resulting in rapid capacity decay and reduced cycle life. Therefore, maintaining the integrity of the electrode structure during charge and discharge cycles is one of the key issues in the application of silicon anodes.
[0004] To address the problems associated with silicon anodes, current main solutions include nano-sizing, carbon coating, electrolyte optimization, and binder design. Among these solutions, functional binder design offers advantages such as low cost, good process compatibility, and high feasibility, and is considered one of the effective ways to mitigate volume expansion and structural failure in silicon anodes.
[0005] As a crucial component of the electrode, the binder connects the active material, conductive agent, and current collector, playing a vital role in maintaining the stability of the electrode structure. Traditional PVDF binders primarily rely on weak van der Waals forces, making it difficult to accommodate the volume expansion of the silicon anode. Water-soluble polymer binders (such as carboxymethyl cellulose, polyacrylic acid, and sodium alginate) offer advantages such as environmental friendliness, processing safety, and low cost. They can improve the structural stability of the silicon anode through polar functional groups; however, they may still exhibit poor adhesion, insufficient toughness, and irreversible chain slippage during long-term cycling, making it difficult to maintain the long-term structural stability of the silicon anode.
[0006] Therefore, it is necessary to develop a functionalized aqueous binder suitable for silicon anodes, which can maintain the advantages of aqueous processing while also possessing good film-forming properties, interfacial bonding ability, mechanical adaptability and ion transport compatibility, so as to alleviate problems such as particle pulverization, electrode cracking, conductive network damage and ion transport obstruction caused by volume changes during silicon anode cycling, thereby improving the structural stability of silicon anodes and battery cycle life. Summary of the Invention
[0007] In view of this, the purpose of this invention is to address the problems of insufficient structural retention, easy cracking of the electrode sheet, and rapid capacity decay of existing water-soluble polymer binders during silicon anode cycling. This invention uses a water-soluble polymer binder as the continuous film-forming component and introduces polyphenolic compounds and small-molecule polycarboxylic acids as functional regulating components to prepare a dynamically crosslinked water-based binder. This binder can improve the bonding force between the silicon active material, the conductive agent, and the current collector, improve the structural stability of the silicon anode during cycling, and thus improve the cycle performance of the battery.
[0008] To solve the above-mentioned technical problems, the present invention is implemented as follows:
[0009] In a first aspect, the present invention provides an aqueous adhesive comprising the following raw materials: a water-soluble polymer adhesive, a polyphenol compound, and a small molecule polycarboxylic acid;
[0010] Raw materials combine in the water system to form a network structure;
[0011] The mass ratio of the water-soluble polymer binder, the polyphenol compound, and the small molecule polycarboxylic acid is 1:(0.1-2):(0.1-2).
[0012] In one embodiment, the water-soluble polymer binder is selected from one or more of carboxymethyl cellulose and its salts, alginate and its salts, polyvinyl alcohol, hydroxyethyl cellulose, xanthan gum, and carboxymethyl chitosan.
[0013] In one embodiment, the polyphenolic compound is selected from one or more of gallic acid, dopamine, tannic acid, tea polyphenols, catechins, and chlorogenic acid.
[0014] In one embodiment, the small molecule polycarboxylic acid is selected from one or more of tartaric acid, malic acid, citric acid, succinic acid, oxalic acid, and aconitic acid.
[0015] As a specific embodiment of the present invention, the mass ratio of the water-soluble polymer binder, polyphenol compound and small molecule polycarboxylic acid is 1:(0.2-1.5):(0.2-1.5).
[0016] Secondly, the present invention also provides a method for preparing an aqueous adhesive, comprising the following steps:
[0017] S1. Dissolve the water-soluble polymer binder to obtain a water-soluble polymer binder solution;
[0018] S2. Dissolve the polyphenol compound and the small molecule polycarboxylic acid to obtain a mixed solution of functional components;
[0019] S3. Add the functional component mixture solution from step S2 to the water-soluble polymer binder solution obtained in step S1, and stir until homogeneous to obtain the water-based binder solution.
[0020] In one embodiment, the concentration of the water-soluble polymer binder solution in step S1 is 1 wt% to 10 wt%.
[0021] In one embodiment, the concentration of the functional component mixture solution in step S2 is 1 wt% to 20 wt%.
[0022] Thirdly, the present invention also provides a silicon anode sheet, the silicon anode sheet comprising a silicon active material, a conductive agent and an aqueous binder as described above, wherein the aqueous binder forms a composite cross-linked bonding network inside the silicon anode sheet.
[0023] As a specific embodiment of the present invention, the mass ratio of the silicon active material, the conductive agent and the aqueous binder is (60-90):(5-20):(5-20).
[0024] As a specific embodiment of the present invention, the conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, SuperP, and carbon nanotubes.
[0025] Fourthly, the present invention also provides a method for preparing a silicon anode sheet, comprising the following steps:
[0026] L1. Mix the silicon active material, conductive agent and the water-based binder as described above, add an aqueous solvent or a water / alcohol mixture, and stir until homogeneous to obtain the negative electrode slurry;
[0027] L2. The negative electrode slurry is coated onto the current collector, and the coated electrode is heated and dried to form a composite cross-linked bonding network inside the silicon negative electrode. After drying, a silicon negative electrode is obtained.
[0028] In a specific embodiment of the present invention, the heating and drying temperature in step L2 is 70-150 °C, and the drying time is 2-24 h.
[0029] Fifthly, the present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode comprises a silicon negative electrode sheet as described above or a silicon negative electrode sheet prepared by the above preparation method.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The dynamic crosslinking waterborne binder of the present invention is mainly composed of water-soluble polymer binder, polyphenol compound and small molecule polycarboxylic acid. The preparation process is simple, the raw materials are widely available, the cost is low, and the environment is environmentally friendly. It is suitable for the preparation and large-scale application of silicon anode slurry.
[0032] (2) This invention uses a water-soluble polymer binder as a continuous film-forming component, introduces polyphenolic compounds to form a multi-reversible hydrogen bond network, and provides carboxyl group interaction sites and flexible regulation effects to synergistically construct a dynamic cross-linked water-based binder network with flexible buffering, stress dissipation and interface anchoring functions. During the drying process of the silicon anode sheet, the carboxyl groups can undergo in-situ thermal cross-linking reactions with the hydroxyl groups in the water-soluble polymer binder molecular chain and the hydroxyl groups on the silicon surface, further improving the stability of the composite cross-linked network.
[0033] (3) The dynamic cross-linked aqueous binder described in this invention can effectively buffer and dissipate the mechanical stress generated by the volume change of silicon anode, enhance the bonding force between silicon particles, conductive agent and current collector, reduce the risk of particle pulverization, electrode cracking and conductive network damage, thereby improving the structural integrity of silicon anode and battery cycle performance.
[0034] (4) The coin cell prepared using the binder of the present invention has a current density of 1408 mAh g at 2 C. -1 The reversible specific capacity, after 200 cycles at a current density of 0.5 C, still retains 2142 mAh g⁻¹. -1 It has a reversible specific capacity with a capacity retention of 79.1%, exhibiting excellent rate performance and cycle stability. Attached Figure Description
[0035] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0036] Figure 1 The 180° peel test curves are for the silicon anode sheets prepared in Example 1, Comparative Example 1, and Comparative Example 3.
[0037] Figure 2 The image shows the nanoindentation load-displacement curves of the adhesive films prepared in Example 1, Comparative Example 1, and Comparative Example 3.
[0038] Figure 3 Electrochemical impedance spectroscopy (EIS) spectra of coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3 after 100 cycles.
[0039] Figure 4Scanning electron microscope images of the electrode surfaces of the coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3 after 100 cycles.
[0040] Figure 5 The graph shows a comparison of the cycle performance of the coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3.
[0041] Figure 6 Rate performance graphs of coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3 at different current densities.
[0042] The accompanying drawings have illustrated specific embodiments of the invention, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the invention in any way, but rather to illustrate the concept of the invention to those skilled in the art through reference to particular embodiments. Detailed Implementation
[0043] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.
[0044] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0045] In the description of this application, "A and / or B" can include any of the cases of A alone, B alone, or A and B, where A and B are merely examples and can be any technical feature connected by "and / or" in this application.
[0046] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0047] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0048] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.
[0049] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0050] To address the problems associated with silicon anodes, previous studies have attempted to modify water-soluble polymer binders by introducing polyphenolic compounds, utilizing the catechol groups of polyphenols to form a hydrogen-bonded network with the silicon surface to enhance interfacial bonding. However, the simple polyphenol-polymer binary system still has shortcomings in terms of crosslinking density and network structure control, making it difficult to balance mechanical strength and flexibility. Therefore, it is necessary to develop a functionalized waterborne binder suitable for silicon anodes, which, while maintaining the advantages of aqueous processing, also possesses good film-forming properties, interfacial bonding ability, mechanical adaptability, and ion transport compatibility, to alleviate problems such as particle pulverization, electrode cracking, conductive network damage, and ion transport obstruction caused by volume changes during silicon anode cycling.
[0051] The inventors have discovered that by using a water-soluble polymer binder as the continuous film-forming component and introducing polyphenolic compounds and small-molecule polycarboxylic acids as functional regulating components, a dynamically cross-linked aqueous binder can be prepared. This binder can improve the bonding force between the silicon active material, the conductive agent, and the current collector, and improve the structural stability of the silicon anode during cycling, thereby improving the cycle performance of the battery. Specifically, the technical solution of this application is as follows:
[0052] In a first aspect, the present invention provides an aqueous adhesive comprising the following raw materials: a water-soluble polymer adhesive, a polyphenol compound, and a small molecule polycarboxylic acid;
[0053] Raw materials combine in the water system to form a network structure;
[0054] The mass ratio of the water-soluble polymer binder, the polyphenol compound, and the small molecule polycarboxylic acid is 1:(0.1-2):(0.1-2).
[0055] In one specific embodiment, the water-soluble polymer binder is selected from one or more of carboxymethyl cellulose and its salts, alginate and its salts, polyvinyl alcohol, hydroxyethyl cellulose, xanthan gum, and carboxymethyl chitosan.
[0056] As a specific embodiment of the present invention, the polyphenolic compound is selected from one or more of gallic acid, dopamine, tannic acid, tea polyphenols, catechins, and chlorogenic acid.
[0057] As a specific embodiment of the present invention, the small molecule polycarboxylic acid is selected from one or more of tartaric acid, malic acid, citric acid, succinic acid, oxalic acid, and aconitic acid.
[0058] As a specific embodiment of the present invention, the mass ratio of the water-soluble polymer binder, polyphenol compound and small molecule polycarboxylic acid is 1:(0.2-1.5):(0.2-1.5).
[0059] In this invention, the mass ratio of water-soluble polymer binder, polyphenol compound, and small molecule polycarboxylic acid is 1:(0.1-2):(0.1-2), based on the total solid weight of the three components. The water-soluble polymer binder serves as the continuous film-forming and basic bonding component, the polyphenol compound provides dynamic hydrogen bond crosslinking functionality, and the small molecule polycarboxylic acid acts as a carboxyl group regulating component to adjust the network structure. When the amount of polyphenol compound added is less than 0.1 parts (based on 1 part of water-soluble polymer binder), there are insufficient hydrogen bond interaction sites in the binder system, making it difficult to form a sufficiently dynamic crosslinked network. The effect of improving interfacial bonding is limited, and the buffering effect on the volume expansion of the silicon anode is not significant. When the amount of polyphenol compound added is more than 2 parts, excessive polyphenol molecules may self-aggregate in the binder system, leading to a decrease in system uniformity. At the same time, excessive phenolic hydroxyl groups may form excessively strong interfacial interactions with the silicon particle surface, increasing the rigidity and decreasing the flexibility of the binder network, which is detrimental to stress dissipation during silicon volume changes.
[0060] When the amount of small molecule polycarboxylic acid added is less than 0.1 parts, there are insufficient carboxyl group interaction sites, making it difficult to effectively regulate the crosslinking density and microstructure of the binder network, and the regulatory effect on the flexibility of the binder is limited. When the amount of small molecule polycarboxylic acid added is more than 2 parts, excessive carboxyl groups may cause the crosslinking of the binder network to be too high, resulting in increased brittleness of the binder film. At the same time, excessive carboxyl groups may interact excessively with the silicon surface, affecting the stability of the electrode interface.
[0061] When the mass ratio of the water-soluble polymer binder, polyphenol compound, and small molecule polycarboxylic acid is selected within the above range, both the full construction of the dynamic cross-linking network and the flexibility control of the binder system can be taken into account, so that the binder has both good interfacial bonding ability and stress buffering ability. Specifically, the mass ratio of the water-soluble polymer binder, polyphenol compound, and small molecule polycarboxylic acid can be 1:0.1:0.1, 1:0.2:0.2, 1:0.5:0.5, 1:0.8:0.8, 1:1:1, 1:1.2:1.2, 1:1.5:1.5, 1:1.8:1.8, or 1:2:2, or any value within the range formed by any two of these values. In one example, the mass ratio is 1:(0.2~1.5):(0.2~1.5), within which the polyphenol compound and small molecule polycarboxylic acid can form a synergistically optimal hydrogen bond-carboxyl group complex cross-linking network.
[0062] Secondly, the present invention also provides a method for preparing an aqueous adhesive, comprising the following steps:
[0063] S1. Dissolve the water-soluble polymer binder to obtain a water-soluble polymer binder solution;
[0064] S2. Dissolve the polyphenol compound and the small molecule polycarboxylic acid to obtain a mixed solution of functional components;
[0065] S3. Add the functional component mixture solution from step S2 to the water-soluble polymer binder solution obtained in step S1, and stir until homogeneous to obtain the water-based binder solution.
[0066] In this invention, the concentration of the water-soluble polymer binder solution is 1 wt% to 10 wt%, based on the total weight of the water-soluble polymer binder solution. When the concentration is below 1 wt%, the inter-chain spacing of polymer molecules in the solution is too large, and the degree of entanglement between the molecular chains is insufficient, which is not conducive to the formation of a uniform cross-linked network structure with the functional components. Moreover, the low concentration will increase the amount of water introduced during the subsequent slurry preparation, prolonging the electrode drying time and increasing energy consumption. When the concentration is above 10 wt%, the solution viscosity is too high, which is not conducive to the uniform dispersion of the functional component mixture solution. Furthermore, the high viscosity solution may affect the dispersion uniformity of the active material and conductive agent when preparing the negative electrode slurry, resulting in uneven internal structure of the electrode. When the concentration of the water-soluble polymer binder solution is selected within the above range, it can balance the sufficient dissolution and dispersion of polymer molecules with the uniform mixing of subsequent functional components, and at the same time, it is beneficial to the control of solid content during slurry preparation and the smooth progress of the coating process. Specifically, the concentration of the water-soluble polymer binder solution can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, or 10 wt%, or any value within the range of any two of these values. In one example, the concentration is 1.5 wt% to 5 wt%, within which the polymer solution has a suitable viscosity for easy handling and subsequent mixing.
[0067] In this invention, the concentration of the functional component mixed solution is 1 wt% to 20 wt%, based on the total weight of the functional component mixed solution. The functional component mixed solution is formed by dissolving polyphenolic compounds and small-molecule polycarboxylic acids in water. When the concentration is below 1 wt%, the content of the functional components in the solution is too low, and the regulatory effect on the crosslinking network structure of the system after adding the polymer solution is not significant. Furthermore, the introduction of excessive solvent will affect the original concentration of the polymer solution and the solid content of the slurry. When the concentration is above 20 wt%, the polyphenolic compounds and small-molecule polycarboxylic acids may undergo self-aggregation or premature interaction in the solution due to the excessive concentration, affecting their uniform dispersion in the polymer matrix and thus reducing the structural uniformity of the binder network. When the concentration of the functional component mixed solution is selected within the above range, it can ensure that the polyphenolic compounds and small-molecule polycarboxylic acids are uniformly dispersed at the molecular level and rapidly form a uniform network after being added to the polymer solution. Specifically, the concentration of the functional component mixed solution can be 1 wt%, 2 wt%, 4 wt%, 6 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, or 20 wt%, or any value within the range of any two of these values. In one example, the concentration is 2 wt% to 10 wt%, within which the functional component exhibits optimal solubility, dispersibility, and miscibility with the polymer solution.
[0068] Thirdly, the present invention also provides a silicon anode sheet, the silicon anode sheet comprising a silicon active material, a conductive agent and the above-mentioned aqueous binder, wherein the aqueous binder forms a composite cross-linked bonding network inside the silicon anode sheet.
[0069] As a specific embodiment of the present invention, the mass ratio of the silicon active material, the conductive agent and the aqueous binder is (60-90):(5-20):(5-20).
[0070] In this invention, the mass ratio of silicon active material, conductive agent, and aqueous binder is (60-90):(5-20):(5-20), based on the total solid weight of the three. When the proportion of silicon active material is less than 60 parts, the content of active material in the negative electrode is too low, the reversible specific capacity of the electrode decreases, which is not conducive to improving the energy density of the battery. When the proportion of silicon active material is greater than 90 parts, the relative content of conductive agent and binder is insufficient, making it difficult to form a continuous and effective conductive network and stable bonding support inside the electrode, resulting in a decrease in the cohesive strength and interfacial bonding ability of the electrode, and structural failure is prone to occur during cycling.
[0071] When the amount of conductive agent is less than 5 parts, the insufficient conductive agent content makes it difficult to form a continuous and effective electron transport network between silicon active particles, resulting in limited electron conduction inside the electrode and thus affecting the rate performance of the battery. When the amount of conductive agent is more than 20 parts, the excessive conductive agent content will reduce the relative content of silicon active material in the electrode, thereby affecting the reversible specific capacity of the electrode. At the same time, excessive conductive agent is prone to agglomeration, which is not conducive to the formation of a uniform and stable conductive network, and may increase electrode porosity and electrolyte consumption, affecting the electrochemical performance of the silicon anode.
[0072] When the amount of binder is less than 5 parts, the binder content is insufficient, making it difficult to provide sufficient bonding force between the silicon active material, conductive agent and current collector, resulting in a decrease in the mechanical strength and interfacial bonding ability of the electrode, and making the electrode prone to cracking and particle shedding during cycling. When the amount of binder is more than 20 parts, the excessive binder will reduce the relative content of silicon active material and may increase particle surface coverage and lithium-ion transport resistance, thereby affecting the overall capacity and rate performance of the battery.
[0073] When the mass ratio of silicon active material, conductive agent, and binder is selected within the above-mentioned range, a balance can be achieved between high active material content, good conductive network construction, and sufficient adhesive support in the electrode. Specifically, the mass ratio of the three can be 60:20:20, 65:18:17, 70:15:15, 75:13:12, 80:10:10, 85:8:7, or 90:5:5, or any value within the range formed by any two of these values. In one example, the mass ratio is (70–80):(10–15):(10–15), within which the electrode exhibits the optimal balance of overall performance.
[0074] As a specific embodiment of the present invention, the conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, SuperP, and carbon nanotubes.
[0075] Fourthly, the present invention also provides a method for preparing a silicon anode sheet, comprising the following steps:
[0076] L1. Mix the silicon active material, conductive agent and the water-based binder as described above, add an aqueous solvent or a water / alcohol mixture, and stir until homogeneous to obtain the negative electrode slurry;
[0077] L2. The negative electrode slurry is coated onto the current collector, and the coated electrode is heated and dried to form a composite cross-linked bonding network inside the silicon negative electrode. After drying, a silicon negative electrode is obtained.
[0078] In a specific embodiment of the present invention, the heating and drying temperature in step L2 is 70-150 °C, and the drying time is 2-24 h.
[0079] In this invention, the coated electrode is heated and dried at a temperature of 70–150 °C for 2–24 h.
[0080] When the drying temperature is below 70 ℃, the solvent evaporation rate is slow, and the electrode drying time is prolonged, which is not conducive to improving the preparation efficiency. At the same time, the lower drying temperature is not conducive to the participation of small molecule polycarboxylic acids in the in-situ thermal cross-linking reaction, resulting in insufficient formation of the composite bonding network, which in turn limits the reinforcing effect of the binder on the silicon anode. When the drying temperature is above 150 ℃, the excessively high temperature may cause thermal decomposition or excessive cross-linking of the binder components, reducing the flexibility of the binder network. At the same time, high-temperature drying may also cause electrode shrinkage and warping, and increase energy consumption, which is not conducive to the stable preparation of silicon anodes.
[0081] When the drying time is less than 2 hours, the solvent is difficult to completely evaporate under the given temperature conditions. The residual solvent will affect the degree of cross-linking reaction of the binder and the mechanical properties of the electrode. When the drying time is more than 24 hours, although sufficient drying can be ensured, the excessively long drying time is not conducive to production efficiency and economy, and long-term high-temperature heating may have an adverse effect on the binder network and electrode structure.
[0082] When the heating and drying temperature and time are selected within the above range, both effective solvent removal and sufficient in-situ thermal crosslinking reaction can be achieved, while ensuring the structural integrity of the electrode and production efficiency. Specifically, the drying temperature can be 70℃, 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, or 150℃, and the drying time can be 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, 16 h, 20 h, or 24 h, or any value within any range of these values. In one example, a stepwise heating and drying method is used, first drying at 80℃ for 10 h to remove most of the solvent, and then drying at 120℃ for 2 h to fully trigger the in-situ thermal crosslinking reaction. Under these conditions, the binder network is most fully formed, and the electrode performance is optimal.
[0083] Fifthly, the present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode comprises a silicon negative electrode sheet as described above or a silicon negative electrode sheet prepared by the above preparation method.
[0084] This invention does not impose any particular limitation on the preparation method of the electrolyte; conventional methods well-known to those skilled in the art can be used. In a preferred embodiment of this invention, the electrolyte is obtained by uniformly mixing the various components. As an example, the preparation method of the electrolyte includes the following steps: in an argon glove box, the solvent components are first mixed to form a homogeneous solvent system, and then a lithium salt electrolyte is slowly added to avoid local overheating and decomposition of the lithium salt; after complete dissolution, trace particulate impurities are removed by pressure filtration through a 0.2 μm PTFE filter membrane to obtain the electrolyte.
[0085] The lithium-ion battery can also be a battery pack assembled from the aforementioned battery modules. The battery pack can contain one or more battery modules, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery pack. Specifically, the battery pack can include a battery box and multiple battery modules disposed within the battery box; the battery box includes an upper box and a lower box, the upper box covering the lower box and forming a closed space for accommodating the battery modules. The multiple battery modules can be arranged in any manner within the battery box.
[0086] In a specific embodiment of the present invention, the outer packaging of the battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc., or it can be a soft pack, such as a pouch-type soft pack; the material of the soft pack can be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0087] The present invention does not impose any particular restrictions on the shape of the battery; it can be cylindrical, square, or any other arbitrary shape, and those skilled in the art can choose according to specific practical needs.
[0088] According to another aspect of the present invention, an electrical device is provided, comprising the battery described in the above-described technical solution. Thus, the electrical device possesses all the features and advantages of the battery described in the above-described technical solution, which will not be repeated here. Specifically, the battery can serve as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks), electric trains, ships and satellites, and energy storage systems.
[0089] The present application will be described in detail below with reference to the accompanying drawings and embodiments. However, the implementation and protection of the present invention are not limited thereto. The following embodiments are only some embodiments of the present application and are not intended to limit the present application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0090] Example 1
[0091] A method for preparing an aqueous binder for silicon anodes, comprising the following steps:
[0092] (1) Weigh 0.1 g of lithium carboxymethyl cellulose and dissolve it in 6 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of lithium carboxymethyl cellulose.
[0093] (2) Weigh 0.1 g of tannic acid and 0.1 g of citric acid and dissolve them in 3.7 g of water. Stir at room temperature until completely dissolved to obtain a mixed solution of functional components.
[0094] (3) The mixed solution of functional components in step (2) is slowly added dropwise (within half an hour) to the lithium carboxymethyl cellulose aqueous solution obtained in step (1), and stirred evenly at room temperature to obtain a dynamic crosslinking waterborne adhesive.
[0095] Example 2
[0096] (1) Weigh 0.12 g of lithium carboxymethyl cellulose and dissolve it in 6 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of lithium carboxymethyl cellulose.
[0097] (2) Weigh 0.04 g of tannic acid and 0.04 g of citric acid and dissolve them in 3.8 g of water. Stir at room temperature until completely dissolved to obtain a mixed solution of functional components.
[0098] (3) The mixed solution of functional components in step (2) is slowly added dropwise (within half an hour) to the lithium carboxymethyl cellulose aqueous solution obtained in step (1), and stirred evenly at room temperature to obtain a dynamic crosslinking waterborne adhesive.
[0099] Example 3
[0100] This embodiment is basically the same as embodiment 2, except that gallic acid is used to replace tannic acid of the same mass. All other steps and raw material amounts are the same as in embodiment 2.
[0101] Example 4
[0102] (1) Weigh 0.15 g of lithium carboxymethyl cellulose and dissolve it in 7 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of lithium carboxymethyl cellulose.
[0103] (2) Weigh 0.025 g of tannic acid and 0.025 g of citric acid and dissolve them in 2.8 g of water. Stir at room temperature until completely dissolved to obtain a mixed solution of functional components.
[0104] (3) The mixed solution of functional components in step (2) is slowly added dropwise (within half an hour) to the lithium carboxymethyl cellulose aqueous solution obtained in step (1), and stirred evenly at room temperature to obtain a dynamic crosslinking waterborne adhesive.
[0105] Example 5
[0106] This embodiment is basically the same as embodiment 4, except that the same mass of sodium alginate is used to replace lithium carboxymethyl cellulose. All other steps and raw material amounts are the same as in embodiment 4.
[0107] Example 6
[0108] (1) Weigh 0.135 g of lithium carboxymethyl cellulose and dissolve it in 6 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of lithium carboxymethyl cellulose.
[0109] (2) Weigh 0.03 g of tannic acid and 0.135 g of citric acid and dissolve them in 3.7 g of water. Stir at room temperature until completely dissolved to obtain a mixed solution of functional components.
[0110] (3) The mixed solution of functional components in step (2) is slowly added dropwise (within half an hour) to the lithium carboxymethyl cellulose aqueous solution obtained in step (1), and stirred evenly at room temperature to obtain a dynamic crosslinking waterborne adhesive.
[0111] Example 7
[0112] This embodiment is basically the same as embodiment 4, except that the same mass of oxalic acid is used to replace citric acid. All other steps and raw material amounts are the same as in embodiment 4.
[0113] Example 8
[0114] (1) Weigh 0.15 g of carboxymethyl chitosan and dissolve it in 7 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of carboxymethyl chitosan.
[0115] (2) Weigh 0.025 g of dopamine and 0.025 g of citric acid and dissolve them in 2.8 g of water. Stir at room temperature until completely dissolved to obtain a mixed solution of functional components.
[0116] (3) Slowly add the mixed solution of functional components in step (2) to the aqueous solution of carboxymethyl chitosan obtained in step (1) within half an hour, and continue to stir evenly at room temperature to obtain a dynamic crosslinked waterborne adhesive.
[0117] Comparative Example 1
[0118] Weigh 0.1 g of lithium carboxymethyl cellulose and dissolve it in 9.9 g of water. Stir at room temperature until completely dissolved to obtain a single lithium carboxymethyl cellulose binder.
[0119] Comparative Example 2
[0120] Weigh 0.06 g of polyacrylic acid and dissolve it in 1.94 g of water. Stir at room temperature until completely dissolved to obtain a single polyacrylic acid adhesive.
[0121] Comparative Example 3
[0122] (1) Weigh 0.1 g of lithium carboxymethyl cellulose and dissolve it in 7 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of lithium carboxymethyl cellulose.
[0123] (2) Weigh 0.1 g of tannic acid and dissolve it in 2.8 g of water. Stir at room temperature until completely dissolved to obtain an aqueous solution of tannic acid.
[0124] (3) Slowly add the tannic acid aqueous solution from step (2) to the carboxymethyl cellulose lithium aqueous solution obtained in step (1) within half an hour, and continue to stir evenly at room temperature to obtain a binary composite water-based adhesive.
[0125] Comparative Example 4
[0126] Weigh 0.12 g of sodium carboxymethyl cellulose and add it to 7.63 g of water. Stir until completely dissolved, then add 0.25 g of styrene-butadiene rubber emulsion (solid content of 48 wt%) and continue stirring until homogeneous to obtain sodium carboxymethyl cellulose / styrene-butadiene rubber composite adhesive.
[0127] Implementation Results Example
[0128] To further demonstrate the beneficial effects of the present invention, the binders prepared in the above embodiments and comparative examples were used as binders for silicon anodes in lithium-ion batteries. The silicon anode preparation method is as follows:
[0129] Nanoscale silicon particles (100–200 nm) were used as the active material, and Super P was used as the conductive agent. The active material, conductive agent, and binder were mixed at a mass ratio of 70:15:15, with the binder amount calculated based on the mass of the solid component in the binder solution. A water / anhydrous ethanol mixture was then added, and the mixture was stirred in a glass bottle to form a homogeneous slurry. The slurry was then coated onto copper foil. The electrode was vacuum-dried at 80 °C for 10 h, and then vacuum-dried at 120 °C for 2 h. The electrode was cut into 12 mm diameter discs to serve as silicon anodes, with each disc containing 0.7–0.9 mg of nanoscale silicon active material.
[0130] The silicon anode sheet was transferred to an argon-filled glove box, with the moisture and oxygen content in the glove box controlled to be less than 0.1 ppm. A lithium sheet was used as the counter electrode, and the electrolyte was a 1.0 mol / L LiPF6 solution of ethylene carbonate (EC) / diethyl carbonate (DEC), with a volume ratio of EC to DEC of 1:1, and 5 wt% fluoroethylene carbonate (FEC) was added as an additive. Glass fiber filter paper was used as the separator, and CR2032 coin cells were assembled. The assembled coin cells were then allowed to stand at 30 °C for 12 h before electrochemical testing. Testing was performed using a Neware CT4008 (Shenzhen, China) battery testing system. The cells were first activated at 0.05 C for 3 cycles, followed by constant current charge-discharge cycle testing at a current density of 0.5 C, where 1 C corresponds to a current density of 3580 mA g. -1 The discharge cutoff voltage is 0.01 V, and the charging cutoff voltage is 3 V.
[0131] Performance analysis of the above batteries:
[0132] 1. Electrode peel strength test
[0133] To analyze the effect of different binders on the interfacial bonding strength of silicon anode sheets, 180° peel tests were performed on the silicon anode sheets prepared in Example 1, Comparative Example 1, and Comparative Example 3. Figure 1 As shown, Example 1 has the highest average peel force, followed by Comparative Example 3, while Comparative Example 1 has the lowest average peel force, indicating that the dynamic cross-linking aqueous adhesive of the present invention can effectively enhance the bonding force between the silicon anode active layer and the current collector.
[0134] 2. Mechanical property testing of adhesive films
[0135] Nanoindentation tests were performed on the adhesive films prepared in Example 1, Comparative Example 1, and Comparative Example 3. Figure 2 As shown, different binder films exhibit different load-displacement responses. At the same indentation depth, Comparative Example 3 requires the highest load, indicating that the introduction of polyphenolic compounds can enhance the rigidity and indentation resistance of the binder film. Example 1 requires the lowest load, suggesting that small-molecule polycarboxylic acids can modulate the flexibility of the binder network, giving it better compliance and deformation buffering capabilities, which is beneficial for mitigating volume change stress during silicon anode cycling.
[0136] 3. Electrochemical impedance spectroscopy (EIS) test
[0137] Figure 3 Electrochemical impedance spectroscopy (EIS) spectra of coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3 after 100 cycles. Figure 3 It can be seen that the impedance semicircle diameter of Example 1 is small, and the slope in the low-frequency region is large, indicating that it has low interfacial impedance and good ion transport characteristics. This result shows that the dynamic crosslinking aqueous binder of the present invention can improve the interfacial stability and electrochemical reaction kinetics of silicon anodes after cycling, thereby contributing to improved battery cycle performance.
[0138] 4. Analysis of electrode morphology after cycling
[0139] To further illustrate the effect of the dynamic crosslinking aqueous binder of the present invention on the structural stability of the silicon anode, scanning electron microscopy analysis was performed on the electrode sheets of coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 3 after 100 cycles. Figure 4 As shown, after 100 cycles, obvious cracks appeared on the surface of the electrodes in Comparative Example 1 and Comparative Example 3. In contrast, the electrode surface in Example 1 only had a few fine cracks, and the overall structure remained better, indicating that the dynamic cross-linked aqueous binder of the present invention helps to improve the structural integrity of the silicon anode after cycling.
[0140] 5. Electrochemical performance test results
[0141] Cyclic and rate performance tests were conducted on each embodiment and comparative example, and the results are shown in Table 1. The electrochemical performance curves of representative samples are shown in Table 1. Figure 5 and Figure 6 As shown.
[0142] Table 1. Electrochemical performance of silicon anodes prepared in Examples 1-8 and Comparative Examples 1-4
[0143]
[0144] As shown in Table 1, Example 1 still maintains 2142 mAh g after 200 cycles at 0.5 C. -1 The reversible specific capacity and capacity retention rate were 79.1%, significantly higher than those of the comparative examples. This result indicates that the silicon anode prepared by the preferred system of this invention has better long-term cycling stability and capacity retention. A comparison of Examples 1, 2, 4, and 6 shows that the proportions of the water-soluble polymer binder, polyphenol compound, and small molecule polycarboxylic acid affect the crosslinking degree and interfacial bonding ability of the binder system, thus affecting the electrochemical performance of the silicon anode. Compared to Example 2, Example 3, even after replacing tannic acid with gallic acid, still maintained good electrochemical performance. Compared to Example 4, Examples 5, 7, and 8 changed one or more components of the water-soluble polymer binder, polyphenol compound, or small molecule polycarboxylic acid, and the resulting silicon anodes still maintained good cycling stability, indicating that the dynamically crosslinked water-based binder described in this invention has good component compatibility. Compared to Comparative Examples 2 and 4, the silicon anode prepared by the ternary system of this invention shows a more significant advantage in long-term cycling stability and capacity retention. Compared to Comparative Example 3, Example 1 exhibited superior cycle stability and rate performance, indicating that the further introduction of small-molecule polycarboxylic acids into the water-soluble polymer binder / polyphenol compound binary system helps to construct a more stable composite crosslinking bonding network. In summary, the dynamic crosslinking waterborne binder of this invention can enhance the bonding force between the silicon active material, the conductive agent, and the current collector, improve the structural stability of the silicon anode during cycling, and thus improve the cycle performance of the silicon anode.
[0145] A water-soluble polymer binder (such as lithium carboxymethyl cellulose in Example 1) serves as a continuous film-forming component, constituting the basic framework of the binder system. Its molecular chain contains hydroxyl groups (-OH) and carboxylates (-COO). - The polymer contains polar functional groups such as α, β, and γ. On the one hand, these functional groups can form hydrogen bonds with the silanol groups (Si-OH) in the oxide layer on the surface of silicon particles, providing initial adhesion to the active material and current collector. On the other hand, the long polymer chains form a continuous film during electrode drying, connecting and fixing the silicon active material, conductive agent, and current collector. However, the single linear polymer molecular chains rely solely on physical entanglement and limited hydrogen bond interactions, making them prone to irreversible chain slippage during repeated volume expansion of silicon particles, leading to loosening or even collapse of the bonding network. The electrode of Comparative Example 1 (containing only CMC-Li) developed severe cracks after cycling. Figure 4 Its 2C rate capacity is 0 mAh g. -1After 200 cycles, the capacity is only 1235 mAh g. -1 The capacity retention rate was only 44.9%. These results indicate that although water-soluble polymer binders can provide basic film formation and bonding, their effect on improving the structural stability of silicon anodes during cycling is limited when used alone.
[0146] Polyphenolic compounds (such as tannic acid in Example 1) contain abundant phenolic hydroxyl structural units, enabling them to form a multi-reversible hydrogen bond network with polar groups on water-soluble polymer chains and silanol groups on the silicon surface. Their core functions are twofold: firstly, the introduction of polyphenolic compounds helps improve the bonding force between the binder and the silicon active material and current collector. Figure 1 It can be seen that the peel strength of Example 1 and Comparative Example 3, which contain tannic acid, is significantly higher than that of Comparative Example 1, which does not contain polyphenolic compounds. Secondly, the multiple hydrogen bonds, acting as "sacrificial bonds," preferentially break during silicon volume expansion to dissipate mechanical stress, and reform during volume contraction, endowing the electrode with dynamic adaptive mechanical response capabilities. Compared to Comparative Example 1, the 2C rate specific capacity of Comparative Example 3 (CMC-Li + tannic acid) increased from 0 to 822 mAh g. -1 After 200 cycles, the reversible specific capacity increased from 1235 mAh g to 1832 mAh g. -1 This indicates that the introduction of polyphenolic compounds is beneficial to improving the rate performance and cycle performance of silicon anodes. However, the nanoindentation loading of Comparative Example 3 is the highest among the three ( Figure 2 This indicates that the adhesive film is too rigid and lacks flexibility, and obvious cracks still appear on the electrode after cycling. Figure 4 The capacity retention rate was only 67.6%, indicating that although the simple polyphenol hydrogen bond network can improve the interfacial binding ability, its mechanical adaptability still has room for further improvement.
[0147] The small molecule polycarboxylic acid (such as citric acid in Example 1) is the core innovation of this invention, distinguishing it from existing binary systems. Its effects are manifested on two levels: First, during the electrode drying process (80→120 ℃), the carboxyl groups (-COOH) on the polycarboxylic acid undergo in-situ thermal crosslinking reactions with the hydroxyl groups (-OH) on the water-soluble polymer molecular chains and the silanol groups (Si-OH) on the silicon surface, thereby enhancing the stability of the binder network and the interfacial bonding ability. Second, the free small molecule polycarboxylic acid can regulate the hydrogen bonding, intermolecular interactions, and network structure in the binder system, giving the binder film better flexibility and deformation buffering ability, avoiding the problem of excessive rigidity in the binder system after simply introducing polyphenol compounds. A direct comparison between Example 1 (containing citric acid) and Comparative Example 3 (without citric acid) fully demonstrates the dual contribution of small molecule polycarboxylic acid in "toughness regulation + covalent crosslinking": with the same amount of polyphenol, the introduction of citric acid significantly increased the 2C rate specific capacity from 822 to 1408 mAh g.-1 (+71%), the reversible specific capacity after 200 cycles increased from 1832 mAh g to 2142 mAh g. -1 (+17%), capacity retention jumped from 67.6% to 79.1% (+11.5 percentage points), while nanoindentation load decreased from "highest" to "lowest" ( Figure 2 The adhesive film exhibits better flexible cushioning capabilities.
[0148] A synergistic mechanism of "skeleton support—dynamic energy dissipation—interfacial anchoring—flexible buffering" can be formed between water-soluble polymer binders, polyphenolic compounds, and small-molecule polycarboxylic acids. The water-soluble polymer binder, as a continuous film-forming component, provides basic adhesion and electrode structural support. The polyphenolic compound, through its abundant phenolic hydroxyl groups, forms multiple reversible hydrogen bonds with the polymer molecular chains and the surface of the silicon active material, thereby enhancing interfacial bonding and playing a role in stress dissipation during volume changes in the silicon active material. The small-molecule polycarboxylic acid participates in in-situ thermal cross-linking through its carboxyl groups, while simultaneously regulating intermolecular interactions and network flexibility, giving the binder network both good stability and deformation adaptability. The results of Example 1 and Comparative Examples 1 and 3 show that a single water-soluble polymer binder is insufficient to maintain the long-term structural stability of the silicon anode. The introduction of polyphenolic compounds improves interfacial bonding and electrochemical performance. Further introduction of small-molecule polycarboxylic acids achieves a better balance between interfacial bonding, stress buffering, and mechanical adaptability, resulting in superior rate performance and cycle stability for the silicon anode.
[0149] The parts of this invention not described in detail are techniques known to those skilled in the art.
[0150] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.
[0151] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An aqueous binder for silicon anodes, characterized in that, The water-based binder comprises the following raw materials: water-soluble polymer binder, polyphenol compound, and small molecule polycarboxylic acid; Raw materials combine in the water system to form a network structure; The mass ratio of the water-soluble polymer binder, the polyphenol compound, and the small molecule polycarboxylic acid is 1:(0.1-2):(0.1-2).
2. The water-based adhesive according to claim 1, characterized in that, The water-soluble polymer binder is selected from one or more of carboxymethyl cellulose and its salts, alginate and its salts, polyvinyl alcohol, hydroxyethyl cellulose, xanthan gum, and carboxymethyl chitosan; And / or, the polyphenolic compound is selected from one or more of gallic acid, dopamine, tannic acid, tea polyphenols, catechins, and chlorogenic acid; And / or, the small molecule polycarboxylic acid is selected from one or more of tartaric acid, malic acid, citric acid, succinic acid, oxalic acid, and aconitic acid.
3. The water-based adhesive according to claim 1 or 2, characterized in that, The mass ratio of the water-soluble polymer binder, the polyphenol compound, and the small molecule polycarboxylic acid is 1:(0.2-1.5):(0.2-1.5).
4. The water-based adhesive according to claim 1, characterized in that, The aqueous binder is a homogeneous solution formed by mixing the water-soluble polymer binder, the polyphenol compound, and the small molecule polycarboxylic acid in a solvent.
5. A method for preparing the water-based adhesive as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Dissolve the water-soluble polymer binder to obtain a water-soluble polymer binder solution; S2. Dissolve the polyphenol compound and the small molecule polycarboxylic acid to obtain a mixed solution of functional components; S3. Add the functional component mixture solution from step S2 to the water-soluble polymer binder solution obtained in step S1, and stir to obtain an aqueous binder solution.
6. The preparation method according to claim 5, characterized in that, The concentration of the water-soluble polymer binder solution in step S1 is 1 wt% to 10 wt%; And / or, the concentration of the functional component mixture solution in step S2 is 1 wt% to 20 wt%.
7. A silicon anode sheet, characterized in that, The silicon anode sheet comprises a silicon active material, a conductive agent, an aqueous binder as described in any one of claims 1 to 4, or an aqueous binder prepared by the preparation method described in claim 5 or 6; The aqueous binder forms a composite cross-linked bonding network inside the silicon anode sheet.
8. The silicon anode sheet according to claim 7, characterized in that, The mass ratio of the silicon-active material, the conductive agent, and the aqueous binder is (60-90):(5-20):(5-20). And / or, the conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, Super P, and carbon nanotubes.
9. A method for preparing a silicon anode sheet as described in claim 7 or 8, characterized in that, Includes the following steps: L1. Mix silicon active material, conductive agent and aqueous binder as described in any one of claims 1 to 4, add aqueous solvent or water / alcohol mixed solvent, stir evenly to obtain negative electrode slurry; L2. The negative electrode slurry is coated onto the current collector, and the coated electrode is heated and dried to allow the water-based binder to form a composite cross-linked bonding network inside the silicon negative electrode. After drying, a silicon negative electrode is obtained. Preferably, the heating and drying temperature in step L2 is 70–150 °C, and the drying time is 2–24 h.
10. A lithium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte, characterized in that, The negative electrode includes a silicon negative electrode sheet as described in claim 7 or 8, or a silicon negative electrode sheet prepared by the preparation method described in claim 9.